Catalyst for methacrylic acid production, method for producing same, and method for producing methacrylic acid and methacrylic acid ester using same

By optimizing the structural parameters of heteropolyacid catalysts containing phosphorus, molybdenum and tungsten, the heat resistance of the catalyst and the high yield of methacrylic acid are improved, and the problem of low heat resistance of existing catalysts is solved. It is suitable for industrial-scale Methacrylic acid production.

CN118922249APending Publication Date: 2024-11-08MITSUBISHI CHEM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380029122.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2023-03-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing catalysts for methacrylic acid manufacturing have low heat resistance and insufficient catalytic life, which makes it difficult to efficiently manufacture methacrylic acid in industrial applications.

Method used

Use a heteropolyacid catalyst containing phosphorus, molybdenum and tungsten, and optimize its structural parameters through powder X-ray diffraction determination to ensure the stability of the catalyst and the presence of active sites at high temperatures, thereby improving the heat resistance of the catalyst and methacrylic acid high yield.

Benefits of technology

It has achieved improved heat resistance of the catalyst and high yield of methacrylic acid, extended the service life of the catalyst, and is suitable for industrial-scale methacrylic acid production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005052159240000171
    Figure BDA0005052159240000171
Patent Text Reader

Abstract

The present invention addresses the problem of providing a catalyst having high heat resistance and capable of producing methacrylic acid at a high yield, and a method for producing methacrylic acid and methacrylic acid ester using the catalyst, the problem being solved by using a catalyst having a specific peak in powder X-ray diffraction measurement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a catalyst for the manufacture of methacrylic acid, a method for manufacturing the same, and a method for manufacturing methacrylic acid and methacrylates using the catalyst. Background Art

[0002] As a catalyst for the production of methacrylic acid (hereinafter also referred to as "catalyst") used in the production of methacrylic acid by the oxidation of methacrolein, heteropolyacid catalysts containing, for example, molybdenum and phosphorus are known. Heteropolyacids are condensed oxyacids formed by oxides of the 12 coordinating atoms (hereinafter referred to as polyatoms) and heteroatoms that form the basic framework of the polyacid. Examples of heteropolyacid catalysts include proton-type heteropolyacids with proton-type cations as counter cations and heteropolyacid salts obtained by replacing part of the proton with cations other than protons (hereinafter, proton-type heteropolyacids are also simply referred to as "heteropolyacids", and at least one selected from proton-type heteropolyacids and heteropolyacid salts is simply referred to as "heteropolyacid (salt)").

[0003] Regarding the structure of heteropolyacids (salts), Non-Patent Literature 1 describes that phosphorus, silicon, arsenic, germanium, titanium, and antimony can be heteroatoms, while tungsten, molybdenum, vanadium, niobium, and tantalum can be polyatoms in heteropolyacids (salts). Furthermore, Keggin, Dawson, and Preyssler types are described as basic structures for heteropolyacids (salts).

[0004] In addition, Patent Document 1 discloses a catalyst composed of a Keggin-type heteropolyacid salt having a composition represented by the following formula as a catalyst for the manufacture of methacrylic acid.

[0005] P a Mo b V c X d Y e O f

[0006] (In the formula, P, Mo, V, and O represent phosphorus, molybdenum, vanadium, and oxygen, respectively; X represents at least one element selected from potassium, rubidium, cesium, and thallium; Y represents at least one element selected from copper, arsenic, antimony, boron, silver, bismuth, iron, cobalt, lanthanum, and cerium. a, b, c, d, e, and f represent the atomic ratios of P, Mo, V, X, Y, and O, respectively. When b = 12, a, c, d, and e are each independently a value greater than 0 and less than 3. f is a value determined by the oxidation state and atomic ratio of each element except oxygen.)

[0007] H3PMo is known to be a Keggin-type heteropolyacid. 12 O 40 H4PMo 11 VO 40 H3, PW12 O 40 In non-patent literature 1, it is shown that H3PMo... 12 O 40 H4PMo 11 VO 40 Compared to H3, PW 12 O 40 The thermal decomposition temperature is high. On the other hand, Non-Patent Document 2 describes the following: using H3PMo... 12 O 40 When used as a catalyst for the production of methacrylic acid, it yields methacrylic acid well, but using PW... 12 O 40 Its activity and selectivity are both very low.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2003-010691

[0011] Non-patent literature

[0012] Non-patent literature 1: Toshio Okuhara, Noritaka Mizuno, Makoto Misono, Advances in Catalysis, volume 41.

[0013] Non-patent literature 2: Shuhei Yasuda, Atsuki Iwakura, Jun Hirata, Mitsuru Kanno, Wataru Ninomiya, Ryoichi Otomo, Yuichi Kamiya, Catalysis Communications, 125(2019), 43-47. Summary of the Invention

[0014] However, known catalysts for the production of methacrylic acid have low heat resistance and insufficient catalytic lifetime. Therefore, it is desirable to develop catalysts with high heat resistance that can produce methacrylic acid in high yields for industrial use.

[0015] The object of this invention is to provide a catalyst with high heat resistance and capable of producing methacrylic acid in high yield. Furthermore, the object of this invention is to provide a method for producing methacrylic acid and methacrylates using this catalyst.

[0016] In view of the above-mentioned problems, the inventors conducted in-depth research and found that the above-mentioned problems could be solved by using a catalyst that has a specific peak in powder X-ray diffraction, thereby completing the present invention.

[0017] That is, the present invention includes the following technical solutions.

[0018] [1]: A catalyst for the production of methacrylic acid, used in the production of methacrylic acid by the oxidation of methacrolein.

[0019] It contains heteropolyacids containing phosphorus, molybdenum, and tungsten.

[0020] (a1) In powder X-ray diffraction measurements at 25℃, when the intensity of the diffraction peak (peak A) with 2θ = 26.1 ± 0.2° is set as IA, and the intensity of the diffraction peak (peak B) with 2θ = 23.0 ± 0.2° is set as IB, the ratio of IB / IA is less than 0.015.

[0021] (b) When powder X-ray diffraction measurements were performed at intervals of 10°C starting from 400°C while increasing the temperature by 10°C / min, the lowest temperature T1 at which the diffraction peak (peak E) with 2θ = 27.1 ± 0.2° appeared was above 440°C.

[0022] [2]: The catalyst for manufacturing methacrylic acid according to [1], wherein the above IB / IA is 0.01 or less.

[0023] [3]: According to the catalyst for the manufacture of methacrylic acid as described in [1] or [2], wherein, in the powder X-ray diffraction measurement at 25°C, when the intensity of the diffraction peak (peak C) at 2θ = 34.1 ± 0.2° is set as IC, IC / IA is less than 0.0055.

[0024] [4]: The catalyst for the manufacture of methacrylic acid according to [3], wherein the IC / IA is 0.0005 to 0.0055.

[0025] [5]: The catalyst for the manufacture of methacrylic acid according to [3] or [4], wherein the IC / IA is 0.001 to 0.0053.

[0026] [6]: The catalyst for manufacturing methacrylic acid according to any one of [1] to [5], wherein, in the powder X-ray diffraction measurement at 25°C, when the intensity of the diffraction peak (peak D) at 2θ = 48.3 ± 0.2° is set as ID, ID / IA is 0.003 or less.

[0027] [7]: A catalyst for the manufacture of methacrylic acid according to any one of [1] to [6], wherein the T1 is 440 to 500°C.

[0028] [8]: The catalyst for manufacturing methacrylic acid according to any one of [1] to [7] has a composition represented by the following formula (I).

[0029] P a Mo b W c V d Cu e A f E g G h O i (I)

[0030] In formula (I), P, Mo, W, V, Cu, and O represent phosphorus, molybdenum, tungsten, vanadium, copper, and oxygen, respectively. A represents at least one element selected from antimony, bismuth, arsenic, germanium, tellurium, selenium, and silicon. E represents at least one element selected from iron, zinc, chromium, tantalum, cobalt, nickel, manganese, titanium, and niobium. G represents at least one element selected from potassium, rubidium, and cesium. a to i represent the molar ratios of each component, b+c=12, a=0.5-3, c=0.22-5, d=0.01-3, e=0.01-2, f=0-3, g=0-3, h=0.01-3, and i is the molar ratio of oxygen required to satisfy the valences of the above components.

[0031] [9]: The catalyst for the manufacture of methacrylic acid according to [8], wherein in the above formula (I), c = 0.22 to 3.

[0032]

[10] : A method for manufacturing a catalyst for methacrylic acid production, which is the method for manufacturing a catalyst for methacrylic acid production as described in any one of [1] to [9], comprising:

[0033] Step (i) involves mixing phosphorus, molybdenum, and tungsten raw materials with a solvent to prepare a solution or slurry (solution A) with a pH of 0.1–4.

[0034] Step (ii) involves drying the above-mentioned liquid A to obtain a dried product, and

[0035] Step (iii) involves calcining the dried material to obtain a calcined product.

[0036]

[11] : According to the method for manufacturing a catalyst for methacrylic acid production as described in

[10] , in the above step (i), the tungsten raw material with a solubility of 4.1 g / 100 mL or more in water at 20 °C is 50% or more of the total tungsten raw material.

[0037]

[12] The method for manufacturing a catalyst for methacrylic acid production according to

[10] or

[11] , wherein in the above-mentioned step (i), the pH of the above-mentioned liquid A is 0.1 to 3.

[0038]

[13] : A method for manufacturing methacrylic acid, comprising the following steps: oxidizing methacrolein using any one of the catalysts for manufacturing methacrylic acid described in [1] to [9] to manufacture methacrylic acid.

[0039]

[14] : A method for manufacturing methacrylic acid, comprising the following steps: oxidizing methacrolein using a catalyst for manufacturing methacrylic acid produced by any one of the methods described in

[10] to

[12] to produce methacrylic acid.

[0040]

[15] : A method for manufacturing methacrylate, comprising the following steps: esterifying methacrylate manufactured by the method described in

[13] or

[14] .

[0041] According to the present invention, a catalyst with high heat resistance and capable of producing methacrylic acid in high yield can be provided. Detailed Implementation

[0042] The embodiments of the present invention will be described below, but the present invention is not limited to the following. It should be noted that in this specification, the numerical range represented by "~" means the range of values ​​described before and after "~" as the lower limit and upper limit, and "A~B" means above A and below B.

[0043] Catalyst for the manufacture of methacrylic acid

[0044] The catalyst for manufacturing methacrylic acid in this embodiment is a catalyst used in the production of methacrylic acid by oxidation of methacrolein, and contains a heteropolyacid comprising phosphorus, molybdenum and tungsten, satisfying the following conditions (a1) and (b).

[0045] (a1) In the powder X-ray diffraction measurement at 25℃, when the intensity of the diffraction peak (peak A) with 2θ = 26.1 ± 0.2° is set as IA and the intensity of the diffraction peak (peak B) with 2θ = 23.0 ± 0.2° is set as IB, the ratio of IB / IA is less than 0.015.

[0046] (b) When powder X-ray diffraction measurements were performed at intervals of 10°C starting from 400°C while increasing the temperature by 10°C / min, the lowest temperature T1 at which the diffraction peak (peak E) with 2θ = 27.1 ± 0.2° appeared was above 440°C.

[0047] Such catalysts have high heat resistance and can produce methacrylic acid in high yields.

[0048] Furthermore, the catalyst for manufacturing methacrylic acid in this embodiment preferably further satisfies the following conditions (a2) or (a3), and more preferably satisfies (a2) and (a3).

[0049] (a2) In powder X-ray diffraction measurements at 25°C, when the intensity of the diffraction peak (peak C) at 2θ = 34.1 ± 0.2° is set as IC, IC / IA is below 0.0055.

[0050] (a3) In powder X-ray diffraction measurements at 25°C, when the intensity of the diffraction peak (peak D) at 2θ = 48.3 ± 0.2° is set as ID, ID / IA is less than 0.003.

[0051] <Powder X-ray Diffraction Determination of Catalysts>

[0052] (Conditions (a1)~(a3))

[0053] When a heteropolyacid catalyst containing phosphorus, molybdenum, and tungsten was subjected to powder X-ray diffraction at 25 °C, the diffraction peaks observed at 2θ = 26.1 ± 0.2° (peak A) and 2θ = 23.0 ± 0.2° (peak B) primarily originated from the heteropolyacid structure. Specifically, peak A mainly originated from a structure where the heteroatom is phosphorus and more than 10 of the polyatoms are molybdenum (hereinafter also referred to as structure A). Conversely, peak B mainly originated from a structure where the heteroatom is phosphorus, 6–11 of the polyatoms are tungsten, vanadium, or other elements besides molybdenum, and the remaining portion is molybdenum (hereinafter also referred to as structure B). Structure B is the cause of the reduced activity in the oxidation reaction of methacrolein.

[0054] Furthermore, the diffraction peaks observed at 2θ = 34.1 ± 0.2° (peak C) and 2θ = 48.3 ± 0.2° (peak D) primarily originate from oxide structures composed of elements that have not formed heteropolyacid structures. Specifically, peak C mainly originates from oxide structures containing molybdenum. Peak D, on the other hand, primarily originates from oxide structures containing tungsten. These oxides contribute to the reduced selectivity of methacrylic acid by promoting stepwise oxidation in the oxidation reaction of methacrolein.

[0055] In the powder X-ray diffraction analysis of the catalyst for methacrylic acid production in this embodiment at 25°C, when the intensity of peak A is set as IA and the intensity of peak B is set as IB, the IB / IA ratio is 0.015 or less. At this value, it is considered that the content of structure B, which is unsuitable for methacrylic acid production, is sufficiently low, resulting in a good yield of methacrylic acid. The upper limit of IB / IA is preferably 0.01 or less, and more preferably 0.005 or less.

[0056] Furthermore, when the intensity of peak C is set to IC, IC / IA is preferably 0.0055 or less. At this value, it is considered that the content of molybdenum-containing oxides, which are unsuitable for the production of methacrylic acid, is sufficiently low, resulting in a good yield of methacrylic acid. The upper limit of IC / IA is more preferably 0.0053 or less, and even more preferably 0.0052 or less. Additionally, from the viewpoint of improving the reactivity of the methacrolein oxidation reaction, the lower limit of IC / IA is preferably 0.0005 or more, and more preferably 0.001 or more.

[0057] As a method for obtaining catalysts with IB / IA and IC / IA within a specified range, for example, the following method can be used: the catalyst is manufactured by means of steps (i) to (iii) described later, and the amount of tungsten raw material used in step (i) and the pH of the resulting liquid A are adjusted.

[0058] Furthermore, when the intensity of peak D is set to ID, ID / IA is preferably 0.003 or less, more preferably 0.002 or less, and even more preferably 0.001 or less.

[0059] As a method for obtaining a catalyst with an ID / IA within a specified range, for example, the following method can be used: the catalyst is manufactured by means of steps (i) to (iii) described below, and in step (i) a tungsten raw material of 50% by mass or more of the total tungsten raw material with a solubility of 4.1 g / 100 mL or more in water at 20 °C is used.

[0060] (Condition (b))

[0061] When a heteropolyacid catalyst containing phosphorus, molybdenum, and tungsten is heated while powder X-ray diffraction (PXRD) is performed, the peak (peak E) observed at 2θ = 27.1 ± 0.2° originates from molybdenum oxide generated by the decomposition of the heteropolyacid. In this embodiment, when the catalyst for the production of methacrylic acid is heated at 10°C / min while PXRD is performed at 10°C intervals starting from 400°C, the lowest temperature T1 at which peak D appears is 440°C or higher. A catalyst with T1 of 440°C or higher indicates that the heteropolyacid in the catalyst has formed a thermodynamically metastable crystal structure. It is believed that the heteropolyacid has high heat resistance and possesses active sites suitable for the oxidation reaction of methacrolein. The lower limit of T1 is preferably 450°C or higher, more preferably 460°C or higher, and even more preferably 470°C or higher. Furthermore, the upper limit of T1 is preferably 500°C or lower, more preferably 490°C or lower, and even more preferably 480°C or lower.

[0062] As a method for obtaining a catalyst with a specified range of T1, for example, the following method can be used: the catalyst is manufactured by means of steps (i) to (iii) described later, and the amounts of tungsten raw material and G element raw material used in step (i) are adjusted.

[0063] Powder X-ray diffraction measurements of catalysts can be performed using, for example, a PANalytical X'PertProMPD X-ray diffractometer and an Anton Paar high-temperature ribbon heating chamber. CuKα rays (λ = 0.154 nm) are used in the measurements, with an output of 45 kV and 40 mA, and a measurement range of 5–60°. The goniometer radius is 240 mm, and either an automatically continuously adjustable slit or a fixed slit is used for the divergence. It should be noted that with an automatically continuously adjustable slit, the slit size is 0–8.0 mm; with a fixed slit, the slit size is 1.75 mm, and the slit opening angle is 1.00°. For the obtained X-ray diffraction pattern, Kα2 rays are separated for peak finding to determine IA, IB, IC, and ID. The peak finding conditions are a minimum significance of 1 degree, a minimum peak tip of 0.2 degrees, a maximum peak tip of 1 degree, and a peak base width of 2 degrees, using the minimum value of the second derivative. Peak finding can be performed using, for example, Panalytical High Score Plus. Furthermore, the lowest temperature at which peak E appears refers to the lowest temperature at which the peak is detected at 2θ = 27.1 ± 0.2° when the X-ray diffraction pattern obtained by performing powder X-ray diffraction measurements on the catalyst at 10°C / min increments from 400°C at 10°C intervals is found using the method described above.

[0064] <Composition of the catalyst>

[0065] From the viewpoint of methacrylic acid yield, the catalyst for methacrylic acid production in this embodiment preferably has the composition represented by the following formula (I). It should be noted that the catalyst may contain small amounts of elements not described in the following formula (I).

[0066] P a Mo b W c V d Cu e A f E g G h O i (I)

[0067] In formula (I), P, Mo, W, V, Cu, and O represent phosphorus, molybdenum, tungsten, vanadium, copper, and oxygen, respectively. A represents at least one element selected from antimony, bismuth, arsenic, germanium, tellurium, selenium, and silicon. E represents at least one element selected from iron, zinc, chromium, tantalum, cobalt, nickel, manganese, titanium, and niobium. G represents at least one element selected from potassium, rubidium, and cesium. a to i represent the molar ratios of each component, b+c=12, a=0.5-3, c=0.22-5, d=0.01-3, e=0.01-2, f=0-3, g=0-3, h=0.01-3, and i is the molar ratio of oxygen required to satisfy the valences of the above components.

[0068] In formula (I) above, c, which is the molar ratio of W (tungsten), satisfies c = 0.22 to 5. Therefore, a catalyst satisfying conditions (a1) and (b) can be easily obtained. The lower limit of c is preferably 0.23 or more, more preferably 0.3 or more. Furthermore, the upper limit of c is preferably 3 or less, more preferably 2 or less, even more preferably 1 or less, and particularly preferably 0.8 or less.

[0069] Furthermore, in formula (I) above, from the viewpoint of improving the yield of methacrylic acid, the lower limit of a is preferably 0.6 or more, more preferably 0.7 or more. The upper limit of a is preferably 2.5 or less, more preferably 2 or less. The lower limit of d is preferably 0.1 or more, more preferably 0.15 or more, and even more preferably 0.2 or more. The upper limit of d is preferably 2.5 or less, more preferably 2 or less, and even more preferably 1.5 or less. The lower limit of e is preferably 0.03 or more, more preferably 0.05 or more. The upper limit of e is preferably 2.5 or less, more preferably 2 or less. The lower limit of f is preferably 0.01 or more, more preferably 0.1 or more. The upper limit of f is preferably 2.5 or less, more preferably 2 or less. The upper limit of g is preferably 2 or less, more preferably 1.5 or less, and even more preferably 1 or less. The lower limit of h is preferably 0.1 or more, more preferably 0.3 or more. The upper limit of h is preferably 2.8 or less, more preferably 2.5 or less.

[0070] It should be noted that the molar ratios of each component were determined by analyzing the components of the catalyst dissolved in ammonia using ICP emission spectroscopy.

[0071] [Method for manufacturing catalysts for methacrylic acid production]

[0072] The catalyst for manufacturing methacrylic acid according to this embodiment can be manufactured according to a known catalyst manufacturing method as long as it contains phosphorus, molybdenum and tungsten and meets the above conditions (a1) and (b), preferably by a method including the following steps (i) to (iii).

[0073] Step (i) involves mixing phosphorus, molybdenum, and tungsten raw materials with a solvent to prepare a solution or slurry (solution A) with a pH of 0.1 to 4.

[0074] Step (ii) involves drying the above-mentioned liquid A to obtain a dried product.

[0075] Step (iii) involves calcining the dried material to obtain a calcined product.

[0076] Furthermore, the method for manufacturing the catalyst for methacrylic acid production in this embodiment may further include the molding process described later.

[0077] The following is a detailed description of each process.

[0078] <Process (i)>

[0079] In step (i), phosphorus raw materials, molybdenum raw materials, and tungsten raw materials are mixed with a solvent to prepare a solution or slurry (solution A) with a pH of 0.1 to 4. Solution A may be mixed with raw materials of elements other than phosphorus, molybdenum, and tungsten in the above formula (I), and preferably with raw materials of element G.

[0080] Solution A can be prepared by dissolving or suspending a catalyst component containing phosphorus, molybdenum, and tungsten raw materials in a solvent.

[0081] (Raw materials for catalyst components)

[0082] The raw materials for the above-mentioned catalyst components are not particularly limited. Nitrates, carbonates, acetates, ammonium salts, oxides, halides, oxyacids, oxyacids, and oxyacid salts of the constituent elements of the catalyst can be used individually or in combination of two or more.

[0083] Examples of phosphorus raw materials include phosphoric acid, phosphorus pentoxide, and ammonium phosphate. Examples of molybdenum raw materials include molybdenum oxide (such as molybdenum trioxide), ammonium molybdate (such as ammonium paramolybdate and ammonium dimolybdate), and molybdenum chloride.

[0084] Examples of tungsten raw materials include tungsten oxide, sodium tungstate, phosphotungstic acid, and ammonium metatungstate. The tungsten raw material having a solubility in water of 4.1 g / 100 mL or more at 20°C is preferably 50% by mass or more of the total tungsten raw material. This allows for the easy acquisition of catalysts that satisfy conditions (a1) and (b). Examples of tungsten raw materials having a solubility in water of 4.1 g / 100 mL or more at 20°C include phosphotungstic acid and ammonium metatungstate. More preferably, the tungsten raw material having a solubility in water of 4.1 g / 100 mL or more at 20°C is 70% by mass or more, and even more preferably 90% by mass or more.

[0085] In the manufacture of catalysts further containing vanadium and copper, examples of vanadium raw materials include, for example, ammonium metavanadate, vanadium pentoxide, vanadium chloride, and vanadium oxalate. Examples of copper raw materials include, for example, copper sulfate, copper nitrate, copper oxide, copper carbonate, copper acetate, and copper chloride.

[0086] The concentration of the catalyst component in solution A is not particularly limited, but is preferably in the range of 5% to 90% by mass.

[0087] (Solvent)

[0088] Examples of solvents mentioned above include water, ethanol, and acetone. One or more of these can be used. From an industrial point of view, water is preferred.

[0089] (Preparation of Solution A)

[0090] Solution A is preferably prepared by adding the catalyst component to the solvent in a preparation vessel while heating and stirring. This ensures the sufficient generation of a suitable heteropolyacid during the production of methacrylic acid.

[0091] The heating temperature can typically be in the range of 30–150°C, preferably in the range of 60–150°C. By setting the heating temperature to 60°C or higher, the formation rate of heteropoly acids can be sufficiently accelerated, while by setting it to 150°C or lower, solvent evaporation can be suppressed. The lower limit of the heating temperature is more preferably 80°C or higher, and even more preferably 90°C or higher. Furthermore, the upper limit of the heating temperature is more preferably 130°C or lower, and even more preferably 110°C or lower. Additionally, depending on the vapor pressure of the solvent used, concentration or reflux can be performed during heating, or the heating treatment can be carried out under pressure by operating in a closed container.

[0092] There is no particular limitation on the heating rate, but 0.8 to 15°C / minute is preferred. By using a heating rate of 0.8°C / minute or higher, the time required for step (i) can be shortened. Alternatively, by using a heating rate of 15°C / minute or lower, conventional heating equipment can be used.

[0093] The stirring is preferably performed with a stirring power of 0.01 kW / m. 3 The above is preferred, with 0.05kW / m 3 The above is performed. The stirring power is set to 0.01 kW / m. 3 The above measures reduce the temperature, composition, and local temperature inhomogeneities of solution A, resulting in a stable structure suitable for use as a catalyst in the production of α,β-unsaturated carboxylic acids. Furthermore, from the viewpoint of catalyst manufacturing cost, stirring is typically preferred at a stirring power of 3.5 kW / m³. 3 The following will proceed.

[0094] (Physical properties of liquid A)

[0095] The pH of solution A is 0.1 to 4, preferably 0.5 or higher at the lower limit and 3 or lower at the upper limit. This is suitable for stabilizing the formation reaction of heteropolyacids that produce α,β-unsaturated carboxylic acids. Methods for setting the pH of solution A to 0.1 to 4 include, for example, using molybdenum trioxide as a molybdenum raw material, or appropriately selecting the raw material compound and adjusting the content of nitrate ions and oxalate ions.

[0096] <Process (ii)>

[0097] In step (ii), liquid A obtained in step (i) is spray-dried to obtain a dried product.

[0098] Examples of drying methods include, for instance, drum drying, airflow drying, evaporative drying, and spray drying. Among these, spray drying is preferred because it yields granular dried material with a uniform spherical shape.

[0099] The drying temperature varies depending on the drying method, and is generally carried out between 100 and 500°C, with a lower limit preferably above 140°C and an upper limit preferably below 400°C. Drying is preferably carried out in a manner that results in a moisture content of 4.5% by mass or less in the dried product, and more preferably in a manner that results in a moisture content of 0.1% to 4.5% by mass in the dried product. These conditions are not particularly limited and can be appropriately selected according to the desired shape and size of the dried product.

[0100] The dried material obtained in step (ii) can be shaped as described later as needed.

[0101] <Molding Process>

[0102] In the molding process, the dried material obtained in step (ii) above is molded as needed. It should be noted that molding can be performed after step (iii) described later.

[0103] The molding method is not particularly limited; known dry and wet molding methods can be used, such as tablet molding, pressure molding, extrusion molding, and granulation molding. The shape of the molded article is not particularly limited; for example, cylindrical, ring-shaped, and spherical shapes can be used. Furthermore, during molding, it is preferable to mold only the dried material without adding carriers, but known additives such as graphite and talc can be added as needed. It should be noted that when using a carrier, the carrier is not particularly limited; silica is a preferred example.

[0104] <Process (iii)>

[0105] In the calcination process, the dried material obtained in step (iii) and the shaped dried material obtained in the molding process are calcined to obtain the calcined material.

[0106] Calcination can be carried out under the flow of at least one of an oxygen-containing gas such as air and an inactive gas, preferably under the flow of an oxygen-containing gas such as air. Here, an inactive gas refers to a gas that does not reduce the activity of the catalyst, such as nitrogen, carbon dioxide, helium, and argon. Only one of them can be used, or two or more can be mixed.

[0107] The shape of the calcination container is not particularly limited; box-shaped, tubular, or other similar containers can be used. Furthermore, multiple containers can be used for filling and calcination. Preferably, a cross-sectional area of ​​1–100 cm² is used. 2 A tubular container.

[0108] The calcination temperature (the highest temperature during calcination) is preferably 200 to 700°C, with a lower limit more preferably above 320°C and an upper limit more preferably below 450°C.

[0109] The calcined product obtained therefrom can be used as a catalyst for the manufacture of methacrylic acid. Alternatively, the calcined product can be shaped as described in the molding process above. In this embodiment, the calcined product and the shaped calcined product are collectively referred to as catalysts.

[0110] [Methacrylic acid manufacturing method]

[0111] In the method for producing methacrylic acid according to this embodiment, methacrolein is oxidized using the catalyst for producing methacrylic acid according to this embodiment. Furthermore, in the method for producing methacrylic acid according to this embodiment, methacrolein is oxidized using the catalyst for producing methacrylic acid manufactured by the method of this embodiment. Based on these methods, methacrylic acid can be produced in high yield.

[0112] The method for producing methacrylic acid according to this embodiment can be carried out by contacting the catalyst for producing methacrylic acid according to this embodiment with a feed gas containing methacrolein. A fixed-bed reactor can be used in this reaction. The reaction can be carried out by filling the reactor with a catalyst and supplying the reactor with the feed gas. The catalyst layer can be a single layer, or multiple layers of catalysts with different activities can be filled separately. In addition, in order to control the activity, the catalyst can be diluted with an inactive support before filling.

[0113] The concentration of methacrolein in the raw material gas is preferably 1 to 20% by volume, more preferably 3% by volume or more, and more preferably 10% by volume or less. The methacrolein used as a raw material may contain small amounts of impurities such as lower saturated aldehydes that do not substantially affect the reaction.

[0114] There are no particular limitations on the oxygen source for the feedstock gas, and using air is advantageous in industry. Alternatively, a gas mixed with pure oxygen in air or the like can be used as needed. The proportion of oxygen in the feedstock gas is not particularly limited, but it is preferably 0.4 to 4 moles relative to 1 mole of methacrolein, more preferably 0.5 moles or more, and more preferably 3 moles or less.

[0115] From an economic point of view, the feed gas can also be a gas diluted with inert gases such as nitrogen or carbon dioxide. Water vapor can be further added to the feed gas. By carrying out the reaction in the presence of water vapor, methacrylic acid can be obtained in a higher yield. The concentration of water vapor in the feed gas is preferably 0.1 to 50% by volume, more preferably 1% by volume or more, and more preferably 40% by volume.

[0116] The contact time between the raw material gas and the catalyst for the production of methacrylic acid is preferably 1.5 to 15 seconds, more preferably 2 seconds or more, and more preferably 10 seconds or less. The reaction pressure is preferably 0.1 to 1 MPa(G), where (G) refers to gauge pressure. The reaction temperature is preferably 200 to 450°C, more preferably 250°C or more, and more preferably 400°C or less.

[0117] There are no particular restrictions on the location of the catalyst in the reactor or the proportion of the catalyst in the reactor during the manufacture of methacrylic acid; commonly used methods can be applied.

[0118] [Methods for manufacturing methacrylates]

[0119] In the method for manufacturing methacrylate of this embodiment, the methacrylic acid manufactured by the method of this embodiment is esterified. That is, the method for manufacturing methacrylate of this embodiment includes: a step of manufacturing methacrylic acid by the method of this embodiment, and a step of esterifying the methacrylic acid.

[0120] The alcohol that reacts with methacrylic acid is not particularly limited, and examples include methanol, ethanol, n-propanol, isopropanol, n-butanol, and isobutanol. Examples of the resulting methacrylates include methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, butyl methacrylate, and isobutyl methacrylate. The esterification reaction can be carried out in the presence of an acidic catalyst such as a sulfonic acid-type cation exchange resin. The preferred temperature for the esterification reaction is 50–200°C.

[0121] There are no particular limitations on the pressure, the location of the catalyst in the reactor, or the proportion of the catalyst in the reactor during the esterification reaction; commonly used methods can be applied.

[0122] Example

[0123] Hereinafter, examples of catalyst manufacturing and reaction using the catalyst according to this embodiment will be described together with comparative examples. In the following examples and comparative examples, "parts" refers to parts by mass.

[0124] (Catalyst composition ratio)

[0125] The molar ratios of each component were determined by analyzing the components of the catalyst dissolved in ammonia using ICP emission spectroscopy.

[0126] (Powder X-ray diffraction analysis of the catalyst)

[0127] The powder X-ray diffraction of the catalyst was performed using a Panalytical X'PertProMPD X-ray diffractometer and an Anton Paar high-temperature ribbon heating chamber. CuKα rays (λ = 0.154 nm) were used, with an output of 45 kV and 40 mA, and a measurement range of 5–60°. The goniometer radius was 240 mm, and either an automatically adjustable or fixed slit was used for divergence. It should be noted that with the automatically adjustable slit, the slit size ranged from 0 to 8.0 mm; with the fixed slit, the slit size was 1.75 mm, and the slit opening angle was 1.00°. For the obtained X-ray diffraction pattern, the Kα2 rays were separated using a Panalytical High ScorePlus for peak finding, thereby determining IA, IB, IC, and ID. The peak finding conditions were a minimum significance of 1 degree, a minimum peak tip of 0.2 degrees, a maximum peak tip of 1 degree, and a peak base width of 2 degrees, using the minimum value of the second derivative. In addition, for the X-ray diffraction pattern obtained by increasing the temperature of the catalyst by 10 °C / min while performing powder X-ray diffraction measurements at 10 °C intervals starting from 400 °C, the lowest temperature at which the peak was detected at 2θ = 27.1 ± 0.2 °C was recorded as T1 when the peak was found using the above method.

[0128] (Thermal decomposition temperature of the catalyst)

[0129] The thermal decomposition temperature, an indicator of the catalyst's heat resistance, was determined using a TG / DTA apparatus as follows. Using 50 mg of alumina as a control, 50 mg of powdered catalyst was heated from room temperature to 550 °C at a rate of 10 °C / min in air. The thermal decomposition temperature was defined as the temperature at which heat generation exceeding 1.8 μV was observed at a 15 °C increase within the temperature range above 380 °C in the obtained DTA curve. A higher thermal decomposition temperature indicates higher heat resistance.

[0130] (Analysis of feedstock gases and products)

[0131] The analysis of the feed gas and products was performed using the following gas chromatography.

[0132] GC-2014 manufactured by Shimadzu Corporation (column: DB-FFAP manufactured by J&W Corporation, 30m × 0.32mm, film thickness 1.0μm)

[0133] GC-8A manufactured by Shimadzu Corporation (Column: Molecular sieve, 2.0M × 3.0mm ID)

[0134] Shimadzu Corporation GC-8A (Pillar: Porapak Q, 2.0M x 3.0mm ID)

[0135] The yield of the generated methacrylic acid is calculated using the following formula.

[0136] Yield of methacrylic acid (%) = (N2 / N1) × 100

[0137] Here, N1 is the number of moles of methacrolein supplied, and N2 is the number of moles of methacrylic acid produced.

[0138] (Tungsten raw materials)

[0139] The tungsten raw materials used in the examples and comparative examples are described below.

[0140] Ammonium metatungstate (manufactured by Japan Inorganic Chemical Industry) solubility in water at 20°C: 10 g / 100 mL

[0141] Solubility of phosphotungstic acid (manufactured by Japan Inorganic Chemical Industry) in water at 20°C: ≥40g / 100mL

[0142] <Example 1>

[0143] A mixture of 294.0 parts molybdenum trioxide, 10.2 parts ammonium metavanadate, 10.6 parts ammonium metatungstate, 30.0 parts of 85% phosphoric acid aqueous solution diluted with 36 parts of pure water, and 6.3 parts copper(II) nitrate trihydrate dissolved in 9.0 parts of pure water was prepared. The resulting slurry was heated to 95°C at 2°C / min and stirred for 2 hours. Next, a mixture of 40.4 parts cesium bicarbonate dissolved in 60 parts of pure water at room temperature was prepared and stirred at 95°C for 15 minutes. Then, a mixture of 27.5 parts ammonium carbonate dissolved in 78 parts of pure water was prepared and stirred at 95°C for 15 minutes to obtain solution A. The pH of solution A is shown in Table 1.

[0144] The obtained liquid A is heated to evaporate and solidify, yielding a dried product.

[0145] The dried material was pressurized, pulverized, and classified using a sieve in a particle size range of 710 μm to 2.36 mm. The resulting granules were calcined at 380 °C for 5 hours under air circulation, and the calcined product was used as a catalyst. The catalyst, excluding oxygen, has a composition of P. 1.5 Mo 11.8 W 0.2 V 0.5 Cu 0.15 Cs 1.2 In addition, powder X-ray diffraction and thermal decomposition temperature of the catalyst were determined. The results are shown in Table 1.

[0146] The obtained catalyst (8 g) was diluted with 10 g of silicon carbide and packed into a fixed-bed flow-through reactor. Then, a feed gas consisting of 5% by capacity of methacrolein, 10% by capacity of oxygen, 30% by capacity of water vapor, and 55% by capacity of nitrogen was passed through the reactor at a contact time of 178 hr·g / mol, and the oxidation of methacrolein was carried out at a reaction temperature of 300 °C. The reaction results are shown in Table 1.

[0147] <Example 2>

[0148] Solution A was prepared using the same method as in Example 1, with 292.1 parts of molybdenum trioxide and 13.6 parts of ammonium metatungstate. The pH of solution A is shown in Table 1.

[0149] The obtained liquid A is heated to evaporate and solidify, yielding a dried product.

[0150] Using the obtained dried material, a catalyst was obtained using the same method as in Example 1. The catalyst, excluding oxygen, had a composition of P. 1.5 Mo 11.7 W 0.3 V 0.5 Cu 0.15 Cs 1.2 In addition, powder X-ray diffraction and thermal decomposition temperature of the catalyst were determined. The results are shown in Table 1.

[0151] The obtained catalyst was used to carry out the oxidation reaction of methacrolein using the same method as in Example 1. The reaction results are shown in Table 1.

[0152] <Example 3>

[0153] Solution A was prepared using the same method as in Example 1, with 287.1 parts of molybdenum trioxide and 22.6 parts of ammonium metatungstate. The pH of solution A is shown in Table 1.

[0154] The obtained liquid A is heated to evaporate and solidify, yielding a dried product.

[0155] Using the obtained dried material, a catalyst was obtained using the same method as in Example 1. The catalyst, excluding oxygen, had a composition of P. 1.5 Mo 11.5 W 0.5 V 0.5 Cu 0.15 Cs 1.2 In addition, powder X-ray diffraction and thermal decomposition temperature of the catalyst were determined. The results are shown in Table 1.

[0156] The obtained catalyst was used to carry out the oxidation reaction of methacrolein using the same method as in Example 1. The reaction results are shown in Table 1.

[0157] <Example 4>

[0158] Solution A was prepared using the same method as in Example 1, with 285.0 parts of molybdenum trioxide, 29.0 parts of 85% (w / w) aqueous phosphoric acid solution, and 29.7 parts of phosphotungstic acid instead of 10.6 parts of ammonium metatungstate. The pH of solution A is shown in Table 1.

[0159] The obtained liquid A is heated to evaporate and solidify, yielding a dried product.

[0160] Using the obtained dried material, a catalyst was obtained using the same method as in Example 1. The catalyst, excluding oxygen, had a composition of P. 1.5 Mo 11.4 W 0.6 V 0.5 Cu 0.15 Cs 1.2 In addition, powder X-ray diffraction and thermal decomposition temperature of the catalyst were determined. The results are shown in Table 1.

[0161] The obtained catalyst was used to carry out the oxidation reaction of methacrolein using the same method as in Example 1. The reaction results are shown in Table 1.

[0162] <Example 5>

[0163] The molybdenum trioxide content was 277.2 parts, and the ammonium metatungstate content was 40.8 parts. Otherwise, solution A was obtained using the same method as in Example 1. The pH of solution A is shown in Table 1.

[0164] The obtained liquid A is heated to evaporate and solidify, yielding a dried product.

[0165] Using the obtained dried material, a catalyst was obtained using the same method as in Example 1. The catalyst, excluding oxygen, had a composition of P. 1.5 Mo 11.1 W 0.9 V 0.5 Cu 0.15 Cs1.2 In addition, powder X-ray diffraction and thermal decomposition temperature of the catalyst were determined. The results are shown in Table 1.

[0166] The obtained catalyst was used to carry out the oxidation reaction of methacrolein using the same method as in Example 1. The reaction results are shown in Table 1.

[0167] <Comparative Example 1>

[0168] Solution A was prepared using the same method as in Example 1, with 270.0 parts of molybdenum trioxide and 53.2 parts of ammonium metatungstate. The pH of solution A is shown in Table 1.

[0169] The obtained liquid A is heated to evaporate and solidify, yielding a dried product.

[0170] Using the obtained dried material, a catalyst was prepared using the same method as in Example 1. The catalyst, excluding oxygen, had a composition of P. 1.5 Mo 10.8 W 1.2 V 0.5 Cu 0.15 Cs 1.2 In addition, powder X-ray diffraction and thermal decomposition temperature of the catalyst were determined. The results are shown in Table 1.

[0171] The obtained catalyst was used to carry out the oxidation reaction of methacrolein using the same method as in Example 1. The reaction results are shown in Table 1.

[0172] <Comparative Example 2>

[0173] Solution A was prepared using the same method as in Example 1, with 270.0 parts of molybdenum trioxide, 27.4 parts of 85% (w / w) aqueous phosphoric acid solution, and 59.4 parts of phosphotungstic acid instead of 10.6 parts of ammonium metatungstate. The pH of solution A is shown in Table 1.

[0174] The obtained liquid A is heated to evaporate and solidify, yielding a dried product.

[0175] Using the obtained dried material, a catalyst was prepared using the same method as in Example 1. The catalyst, excluding oxygen, had a composition of P. 1.5 Mo 10.8 W 1.2 V 0.5 Cu 0.15 Cs 1.2 In addition, powder X-ray diffraction and thermal decomposition temperature of the catalyst were determined. The results are shown in Table 1.

[0176] The obtained catalyst was used to carry out the oxidation reaction of methacrolein using the same method as in Example 1. The reaction results are shown in Table 1.

[0177] <Comparative Example 3>

[0178] 300.0 parts of phosphotungstic acid were pressurized and pulverized, and then classified using a sieve to a particle size range of 710 μm to 2.36 mm. The resulting solid particles were calcined at 380 °C for 5 hours under air circulation, and the calcined product was used as a catalyst. The composition of this catalyst, excluding oxygen, is P1W. 12 In addition, powder X-ray diffraction and thermal decomposition temperature of the catalyst were determined. The results are shown in Table 1.

[0179] The obtained catalyst was used to carry out the oxidation reaction of methacrolein using the same method as in Example 1. The reaction results are shown in Table 1.

[0180] <Comparative Example 4>

[0181] 300 parts of phosphomolybdic acid (manufactured by Nippon Inorganic Chemical Industry) were calcined at 380°C for 5 hours, and the resulting powder was pulverized and classified using a sieve with a particle size ranging from 710 μm to 2.36 mm. The resulting solid particles were then calcined at 380°C for 5 hours under air circulation to produce a catalyst. The catalyst, excluding oxygen, has a composition of P1Mo. 12 In addition, powder X-ray diffraction and thermal decomposition temperature of the catalyst were determined. The results are shown in Table 1.

[0182] The obtained catalyst was used to carry out the oxidation reaction of methacrolein using the same method as in Example 1. The reaction results are shown in Table 1.

[0183] [Table 1]

[0184]

[0185] As shown in Table 1, Examples 1-5 using catalysts that meet conditions (a1) and (b) exhibit high heat resistance and can yield methacrylic acid in high yields because the heteropolyacids in the catalysts form thermodynamically metastable crystal structures.

[0186] It should be noted that esterification of the methacrylic acid obtained in this embodiment can yield methacrylate.

[0187] Industrial availability

[0188] According to the present invention, a catalyst with high heat resistance and capable of producing methacrylic acid in high yield can be provided.

Claims

1. A methacrylic acid production catalyst, which is a catalyst used when producing methacrylic acid by oxidation of methacrolein. It contains a heteropolyacid comprising phosphorus, molybdenum and tungsten, (a1) in a powder X-ray diffraction measurement at 25°C, when the intensity of the diffraction peak A at 2θ=26.1±0.2° is denoted as IA, and the intensity of the diffraction peak B at 2θ=23.0±0.2° is denoted as IB, IB / IA is not more than 0.015, (b) When powder X-ray diffraction measurement is performed at 10°C intervals from 400°C while increasing the temperature at 10°C / min, the lowest temperature T1 at which a diffraction peak E with 2θ=27.1±0.2° appears is 440°C or higher.

2. The catalyst for producing methacrylic acid according to claim 1, in, The IB / IA is less than 0.

01.

3. The catalyst for producing methacrylic acid according to claim 1 or 2, in, (a2) In a powder X-ray diffraction measurement at 25°C, when the intensity of peak C which is a diffraction peak at 2θ=34.1±0.2° is defined as IC, IC / IA is 0.0055 or less.

4. The catalyst for producing methacrylic acid according to claim 3, in, The IC / IA is 0.0005 to 0.0055.

5. The catalyst for producing methacrylic acid according to claim 3 or 4, in, The IC / IA is 0.001 to 0.0053.

6. The catalyst for producing methacrylic acid according to any one of claims 1 to 5, in, (a3) In a powder X-ray diffraction measurement at 25°C, when the intensity of peak D which is a diffraction peak at 2θ=48.3±0.2° is defined as ID, ID / IA is 0.003 or less.

7. The catalyst for producing methacrylic acid according to any one of claims 1 to 6, in, The T1 is 440-500°C.

8. The catalyst for producing methacrylic acid according to any one of claims 1 to 7, which has a composition represented by the following formula (I): Q a Mo b W c V d Cu e A f HAVE BEEN g G h O i (I) In formula (I), P, Mo, W, V, Cu and O represent phosphorus, molybdenum, tungsten, vanadium, copper and oxygen, respectively; A represents at least one element selected from antimony, bismuth, arsenic, germanium, tellurium, selenium and silicon; E represents at least one element selected from iron, zinc, chromium, tantalum, cobalt, nickel, manganese, titanium and niobium; G represents at least one element selected from potassium, rubidium and cesium; a to i represent the molar ratio of each component, b+c=12, a=0.5~3, c=0.22~5, d=0.01~3, e=0.01~2, f=0~3, g=0~3, h=0.01~3, and i is the molar ratio of oxygen required to satisfy the valence of each component.

9. The catalyst for producing methacrylic acid according to claim 8, in, In the above formula (I), c=0.22-3.

10. A method for producing a catalyst for producing methacrylic acid, the method for producing a catalyst for producing methacrylic acid according to any one of claims 1 to 9, include: Step (i) is to mix a phosphorus raw material, a molybdenum raw material and a tungsten raw material with a solvent to prepare a solution or slurry having a pH of 0.1 to 4, i.e., a liquid A. Step (ii), drying the liquid A to obtain a dried product, and In step (iii), the dried product is calcined to obtain a calcined product.

11. The method for producing a catalyst for producing methacrylic acid according to claim 10, in, In the step (i), the tungsten raw material having a solubility of 4.1 g / 100 mL or more in water at 20° C. accounts for 50% by mass or more of the entire tungsten raw material.

12. The method for producing a catalyst for producing methacrylic acid according to claim 10 or 11, in, In the step (i), the pH of the solution A is 0.1-3. 13 . A method for producing methacrylic acid, comprising the step of producing methacrylic acid by oxidizing methacrolein using the catalyst for producing methacrylic acid according to claim 1 . 14 . A method for producing methacrylic acid, comprising the step of producing methacrylic acid by oxidizing methacrolein using the catalyst for producing methacrylic acid produced by the method according to claim 10 .

15. A method for producing methacrylic acid ester, comprising the step of esterifying methacrylic acid produced by the method according to claim 13 or 14.

Citation Information

Patent Citations

  • Catalyst precursor, method for producing catalyst, method for producing methacrylic acid and acrylic acid, and method for producing methacrylic acid ester and acrylic acid ester

    CN110944747A

  • Catalyst for methacrylic acid production, coated catalyst, and process for producing the same

    CN1461236A

  • Method for producing catalyst for use in manufacturing methacrylic acid

    JP2004008834A

  • Vanadotungstomolybdophosphoric acid oxidation catalyst

    US4522934A