Multilayer material for moulding, conveying system and fiber products

Through multi-layer substrate structure and high-pressure and high-temperature molding technology, the problem of low strength and volume efficiency of fiber products during molding is solved, efficient production and high regeneration are achieved, and suitable for press forming operations and regenerating slurry operations.

CN118922287APending Publication Date: 2024-11-08BLUE OCEAN CLOSURES AB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029340.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-21
Filing Date
2023-03-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The low strength and volume efficiency of existing fiber products during the molding process lead to increased production complexity and cost and difficulty in regeneration.

Method used

Using a multi-layer substrate structure, including an outer layer that provides high tensile strength and an intermediate layer that is low initial tensile strength, a multi-layer product with enhanced mechanical and resistance properties is formed by high voltage and high temperature molding, and after use, it is regenerated slurry Operation for fiber separation.

Benefits of technology

It improves the tensile strength and volume efficiency of fiber products, reduces production complexity and cost, while maintaining high regenerative and degradability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922287A_ABST
    Figure CN118922287A_ABST
Patent Text Reader

Abstract

The invention relates to a multilayer material for moulding, a transport system and a resulting fibrous product. In addition, a method for regeneration is disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a material for moulding fibre products, the fibre products being formed under high pressure and temperature, preferably by means of a press pad and a punching device to form said material into a fibre product. The present invention also relates to an efficient conveying system for said moulding and to a final product having enhanced mechanical and electrical resistance properties. The present invention also relates to a three-layer material concept for enhanced product and recycling properties. The present invention also relates to a method for recycling. Background Art

[0002] Fiber products can be made by pressing fiber webs or fiber sheets. Typically, a combination of natural fibers (e.g., wood pulp fibers), synthetic fibers (e.g., polyolefin-based fibers, which may be polyethylene or polypropylene) and other additives (such as adhesives or dyes). In some applications, it is preferred that such a web is substantially composed of natural fibers only, with or without additives. Typical process conditions are temperature 150-250°C and pressure 100-10000 bar (200-2000 bar). The water content may generally be less than 20%. In many applications, the material is produced in an integrated operation consistent with the pressing operation so as to provide sufficient molding flexibility by using materials with very little internal strength. Examples of the above-mentioned known methods are shown in EP 3736099 and WO2020 / 165780. The fiber product may be in the form of a hollow product, such as a package or closure (lid, nut or the like), but may also be a flat product. The product may be formed of a material web and punched / cut during the molding process, for example, the product is completely or partially separated from the web for further forming. This is usually done by cutting the material into a shape suitable for the final shape close to the forming process. For example, round objects are often cut to form round packages.

[0003] Compression molding is usually performed with two tools, where both the outer tool (pad) and the inner tool (punch) can consist of several parts to enable ejection of the finished product. Usually, the punch is folded while the pad is opened. The piston, parts of the piston or parts of the pad can also be made of a compressible material that can generate a greater vertical compression force, usually acting on the sides of the cavity, by reshaping the tool material during compression.

[0004] If the material is not produced (or laid) directly adjacent to or following the stamping and forming process, it needs to have a certain strength (physical properties) to withstand operations such as production, drying, cutting into roll widths, winding, unwinding, cutting into blanks, and feeding. Typically, the material is subject to tensile forces from line tension, as well as sharing forces from cutting and handling. The material also needs a certain stiffness, mainly bending stiffness, for handling and feeding operations. In particular, when the material is stored, such as in rolls or on delivery pallets, there is a risk that the surface of the material will interlock or fuse with the connecting surfaces, resulting in difficulty in separating the material, dusting during separation, or damage during separation. This is a known problem with strong materials and is called blocking, but the problem becomes much greater in the case of soft materials or less clear materials commonly used in press forming.

[0005] Typically, fibrous materials for 3D pressing or folding into packaging products are delivered flat in one of three main ways: rolls, sheets, or blanks. The drawback of existing methods is that rolls have low volumetric efficiency, both from the circular shape and from the void created by the central unwinding core. For blanks and sheets, the volumetric efficiency can be very high, but the nature of the system is to cut the material into individual items, creating additional fuss and complexity in the feed system, increasing costs and reducing production efficiency.

[0006] When the material is formed into a product, internal bonding between the multiple fibers is less desirable or non-existent. This is due to the fact that the material partially changes shape by partial reorganization of the fibers or at least by breaking of bonds (e.g. by delamination). Usually, in the press forming operation, the material has an optimum moisture content. Because fiber-based materials usually become weaker at higher moisture contents. This places additional demands on the green strength and relative wet strength of the incoming material.

[0007] The final product needs to have certain minimum strength and resistance properties. These are partly affected by process parameters such as pressure, temperature and molding time, but also by material composition and additives. In some applications, higher strength and resistance properties may be required on the top and bottom or internal and external surfaces of the product. For example, a packaged product will have additional stresses on the outside due to handling, and on the inside due to interaction with the packaged product. For items with some kind of closure mechanism, stresses come from the interaction between different parts of the opening mechanism, such as the interaction between the lid and the container or between internal and external threads.

[0008] Many end products will be recycled, where the fibers are separated for use in new products. This places special demands on the product so that only a minimum amount of fibers are bound in a way that cannot be separated in the recycling operation (usually a repulping operation). Since the repulping operation benefits from thinner materials and objects, it is an advantage if weaker layers are introduced, thereby allowing the object to delaminate and the resulting harder layers to be better exposed to the repulping operation and separated more effectively.

[0009] Therefore, there remains a need to provide products that are easily regenerable and / or degradable. Summary of the invention

[0010] The first aspect of the present invention solves / mitigates one or more problems by providing a multilayer substrate comprising at least one layer providing tensile strength, and a layer comprising fibers having an internal strength low enough to deform during a compression molding operation, thereby at least partially forming new bonds in new relative positions.

[0011] Furthermore, in a second aspect of the present invention, there is provided a method for processing a multilayer substrate according to any one of the preceding claims for providing a multilayer product, the method comprising the following steps:

[0012] a) providing the multilayer substrate,

[0013] b) subjecting the substrate to high pressure, and

[0014] c) subjecting the substrate to elevated temperatures, thereby providing a multi-layer product.

[0015] In addition, a third aspect of the present invention provides a multi-layer product obtainable by the method of the second aspect.

[0016] In addition, in a fourth aspect of the present invention, there is provided the use of the multilayer product of the third aspect, wherein the product is a moulded product such as a nut, a container, a bread clip or a package, wherein the container may be a disposable drinking cup or a dairy carton or a pressure cooker package or a dish, or a plate for eating or storing food, or paper or paperboard, such as folding box board.

[0017] In addition, a fifth aspect of the present invention provides a method for regenerating the multilayer product of the third aspect to provide a regenerated pulp, comprising the following steps:

[0018] i) providing said multilayer product, preferably after its use,

[0019] ii) immersing the product in a liquid, preferably water, most preferably warm water,

[0020] iii) optionally adding one or more decoupling agents to the liquid,

[0021] iv) exposing said product to said liquid for subjecting it to shear forces, thereby providing a regenerated pulp. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Schematic diagram of the production of the multilayer material of the present invention, wherein usually one or two of the outer forming layers are solid and carry the other layers loosely held together.

[0023] Figure 2 is a schematic diagram of a slitting operation, where a larger roll of loosely held material is rewound and slit into several smaller rolls to be taken, thereby facing high tensile tensions in the web and the sharing forces from the slitting operation.

[0024] Figure 3 is a schematic diagram of a forming operation in which a partially loosely held together fiber material is unwound, cut, pulled, cover pressed, and possibly post-cut into a multi-layer structure with extra strong inner and / or outer surfaces.

[0025] Figure 4 Schematic diagram of a multi-layer molding structure in which one or two of the outer layers have high resistance to repulping operations, while the center layer is easier to separate and the repulpability and recyclability are improved through the layered structure. DETAILED DESCRIPTION

[0026] The expressions "fibre" or "fiber" are used interchangeably in this specification and have the same meaning as "fiber".

[0027] According to a preferred embodiment of the first aspect, the layer providing tensile strength provides a tensile strength at least about 10%, preferably at least about 20%, most preferably at least about 50% higher than the tensile strength of the other layer.

[0028] According to a preferred embodiment of the first aspect, the substrate is at least three layers of material. The substrate may further have more than three layers, such as four, five, six, seven, eight, nine or ten layers.

[0029] According to a preferred embodiment of the first aspect, said higher tensile strength is provided by at least one of the outer layers, preferably having a minimum tensile strength of about 75 N / m (CD). CD = Cross Machine Direction.

[0030] According to a preferred embodiment of the first aspect, the higher tensile strength is provided by the two outer layers, preferably with a total minimum tensile strength of about 150 N / m (MD). Thus, the layers provide about 75 N / m, with the middle layer providing a substantially smaller portion. MD = Machine Direction.

[0031] According to a preferred embodiment of the first aspect, the layer with higher tensile strength is thinner than the central layer.

[0032] According to a preferred embodiment of the first aspect, the material with a low initial tensile strength provides one or more layers with better repulpability.

[0033] According to a preferred embodiment of the first aspect, at least one of the outer layers is preferably made more hydrophobic and / or oleophobic by using a water- and / or oil-repellent agent, such as AKD (alkyl ketene dimer), ASA (alkenyl succinic anhydride) or wax or a combination thereof. This can be achieved by at least one or two of the outer layers as follows:

[0034] In this method, a bulk cellulosic material (which may have a specific volume of about 7 to about 8 cm 3 / g) is pressed after passing through a decurler unit, whereby a water and / or oil repellent is applied (e.g. using a spray) prior to pressing. The cellulosic material may be wet or dust-free. A combination of pressure (about 10 to about 100 MPa, preferably about 20 to about 30 MPa) and heat (about 120 to about 250°C, preferably about 120 to about 180°C) is applied to the material for 0.5-2 s, and this produces a high density cellulosic object (about 1.11 to about 1.25 kg / dm) with relatively limited porosity and relatively capillary-free structure. 3 ). This process affects the material in several ways:

[0035] a) The high temperature at which the material is pressed allows the fiber mat to be heated above the melting point of the agent for water / grease repellency. This allows the agent to be more evenly redistributed / spread over / around the fibers during pressing and achieve a more even coverage of the fibers and therefore a higher hydrophobicity and / or oleophobicity.

[0036] b) The very high densification of the material during pressing creates a smooth, closed surface object with a low specific volume compared to other cellulosic materials (such as paperboard or wet mold cellulose). The densification of the fiber network allows the creation of a network of hydrophobic and / or oleophobic agents (i.e. water and / or oil repellent agents) around the fibers, which are then locked into the structure due to the lack of available flow space. In addition, the smooth, closed surface further reduces the possibility of flow and locks the agents into the material and reduces the possibility of hydrolysis, thus improving performance. Finally, the densification of the material increases the volume fraction of hydrophobic and / or oleophobic agents (i.e. water and / or oil repellent agents) in a given amount of material, causing further densification of the network and improved performance.

[0037] The decurler unit that can be used in conjunction with the above method can be a roll-type decurling assembly provided by Maxson Automatic Machinery or a decurling unit provided by Ricoh. The decurling unit can include a sponge roller, two metal rollers and two paths for paper or other cellulosic materials. The decurling strength and curling direction can be adjusted. There can be a "sandwich" configuration, in which there is an upper pressure roller, a decurling roller and a lower pressure roller.

[0038] According to a preferred embodiment of the first aspect, at least one of the outer layers has a high relative wet strength.

[0039] According to a preferred embodiment of the first aspect, at least one of the outer layers has a higher density.

[0040] According to a preferred embodiment of the first aspect, the density is less than about 0.5 kg / dm 3 , preferably from about 0.1 to about 0.4 kg / dm 3 .

[0041] According to a preferred embodiment of the first aspect, the grammage is about 100 to about 2000 g / m 2 , preferably from about 300 to about 1500 g / m 2 If tissue paper is used as the starting material for one layer (preferably the outer layer), its grammage may be from about 15 to about 18 g / m 2 , preferably about 16.5 g / m 2 .

[0042] According to a preferred embodiment of the first aspect, the water content is from about 4% to about 25%, preferably from about 7% to about 15%.

[0043] According to a preferred embodiment of the first aspect, at least one of the outer layers comprises one or more additives for additional strength and wet strength, preferably wherein at least one component of said additives comprises fibers of a man-made polymer.

[0044] The above-mentioned substrate used in the embodiments of the first aspect can be derived from CTMP (Chemical Thermomechanical Pulp), TMP (Thermomechanical Pulp), Kraft pulp, sulfate pulp, sulfite pulp, recycled pulp material, paperboard or carton pulp, or a combination thereof. In addition, the substrate can be derived from bleached or unbleached pulp, or a combination thereof. In addition, the substrate can be derived from hardwood or softwood, bagasse or straw, or a combination thereof.

[0045] According to a preferred embodiment of the second aspect, the high pressure and high temperature of step b) and / or c) are provided by a pressure pad device and an embossing device.

[0046] According to a preferred embodiment of the second aspect, the substrate is derived from CTMP (Chemical Thermomechanical Pulp), TMP (Thermomechanical Pulp), Kraft pulp, sulfate pulp, sulfite pulp, recycled pulp material, paperboard or carton, or a combination thereof.

[0047] According to a preferred embodiment of the second aspect, the substrate is derived from bleached or unbleached pulp, or a combination thereof.

[0048] According to a preferred embodiment of the second aspect, the substrate is derived from hardwood or softwood, bagasse, algae or straw, or a combination thereof.

[0049] According to a preferred embodiment of the second aspect, step a) is preceded by a conveying step which comprises forming the substrate into a strip and subsequently folding said strip.

[0050] According to a preferred embodiment of the third aspect, the multilayer product according to the third aspect is a moulded product, such as a nut, a container, a bread clip or a package, wherein the container may be a disposable drinking cup or a dairy carton or an autoclave package or a dish, or a plate for eating or preserving food, or paper or paperboard, such as folding box board.

[0051] According to a preferred embodiment of the third aspect, a multi-layer product is provided such that one of the outer layers forms a thread or click feature for use in a sealable package, such as a container, a closure or a portion of a container or a closure.

[0052] Thanks to the present invention, a material can be produced which can be used in press molding operations, in which the fibers can be partially separated and reattached, which has high tensile strength, shared strength and surface strength, and can be fed into the molding operation in an efficient manner. In addition, the outer layer and surface properties of the molded product can be sufficiently strong and durable, while minimizing the amount of strengthening agent and maintaining high repulpability and, therefore, high renewability.

[0053] In one application of the invention, the multi-layer material is folded during or before the pressing and forming operation, thereby creating an inner structure of stronger material where the outer layers interact. In this way, the structure can be locally reinforced while minimizing the use of strength additives and maintaining reproducibility.

[0054] The novel material in this invention allows for a new conveying system through its tensile strength and handling properties, where the material can be conveyed in the form of strips folded on a pallet. This has two distinct advantages for the production of items, especially bulky packaged items. The conveying method is made possible by using a strong but flexible material resulting from a multi-layer structure in which the strength and possibility of folding does not create creases that affect the final product, allowing for a system with high volumetric efficiency. When the folding creates a continuous piece of material, it combines the volumetric efficiency of a sheet on a pallet with the production advantages where the material is continuously fed from a roll.

[0055] The preferred features of each aspect of the present invention are the same as those in the other aspects after making necessary changes in details. The prior art documents described herein are incorporated to the maximum extent permitted by law. The present invention is further described in the following examples together with the accompanying drawings, which do not limit the scope of the present invention in any way.

[0056] Embodiments of the invention are described in more detail by means of examples of embodiments together with the accompanying drawings, which have the sole purpose of illustrating the invention and are in no way intended to limit the scope thereof.

[0057] 1. Exemplary Description

[0058] A. Forming of the first outer or inner layer

[0059] B. Forming of the second center layer

[0060] C. Forming of the third outer or inner layer

[0061] D. Additional manufacturing processes where the material is exposed to mechanical or chemical stresses. Mechanical stresses are usually applied through compression (calendering) and tensile stresses in mechanical or drying operations. Chemical stresses are usually applied through moisture or water, such as from the addition of water-soluble or dispersible additives.

[0062] E. Winding operation, in which the material is exposed to stretching forces in order to form a sufficiently stable roll. If the tension in the winding operation is not high enough, the tension in the roll will not be sufficient to prevent the so-called handling telescoping.

[0063] F. Rewinding operations where web tension is required to pull the material from a larger original roll and the web tension is high enough to create sufficient web tension in the smaller resulting roll for safe handling. Tension is usually achieved by driving the smaller roll and preventing or braking the rotation of the larger roll.

[0064] G. Unwinding in converting operations. Web tension creating a material stretching force is required to create a flat and controlled web. This is usually achieved by pulling the material by a feed unit and stopping the roll by a brake mechanism. Unwinding means that if the surface strength of the material is not high enough, the roll layers where the inner material rests towards the outer part of the material need to be separated, thus applying a stretching force, which also creates tension out of the plane or creates a sharing force, with the risk of breaking the material, dusting or one part of one surface resting on another part.

[0065] H. In some operations, the material is cut into billets prior to the feeding operation, thereby exerting tensile and sharing forces on the material.

[0066] I. The material, whether web or sheet (or blank), is usually fed to the pressing operation (J.) by a push operation of a feeder so as to avoid stretching forces, and then the material is punched or covered into the die (see Figure 1 and Figure 2 The pushing action exerts compressive and buckling forces on the material, requiring the material to be strong and rigid enough not to be compressed, folded or buckled as it is fed.

[0067] J. Pressing device (see also below Figure 1 and Figure 2 ). The material is usually pushed flat into the pressing area and then pushed or covered into the press pad device with a punch or special tool. The material needs to be strong enough not to break due to the tensile or sharing forces applied from the pressing device and the pad wall, and at the same time, the large number of fibers needs to be loose enough to reposition under the pressing operation. During the pressing operation, the material will form and form new bonds. The properties of the material and the added additives will determine the properties of the new laminate structure. Generally, the material will contain strength, wet strength and hydrophobic properties, and may be stronger and / or more water resistant, while materials without these additives will produce better repulping properties. In the case of folding the material in the push-down or covering operation, the inner or outer material will be in direct contact with the additives, forming a generally stronger reinforced structure.

[0068] K. The forming and pressing operations result in a multilayer structure, usually with outer and / or inner layers gaining additional strength from additives initially added to form one or a few strong layers during the manufacturing and converting operations. If the formed article is to be cut, the strength of the outer layers aids the cutting operation by providing better resistance to sharing and bending.

[0069] Molded products will benefit from the additional strength.

[0070] As a non-limiting example, the minimum tensile strength may be 150 N / m (MD) in total, with essentially no strength in the middle layer. Thus, there would be a tensile strength of about 75 N / m (CD) in each outer layer.

[0071] L. After use, the fibers in the article need to be regenerated to enable new use as packaging or other products. This is typically accomplished by collecting, shipping, and repulping the article with other fibers and paper products. Repulping, which constitutes the fifth aspect of the invention, is typically performed in an operation where the article is immersed in warm water, with or without a decoupling agent, and exposed to the forces that cause the fiber bonds to separate. In general, stronger bonds, additive-assisted bonds, and thick structures are more difficult to repulp.

[0072] M. If one or more of the layers in a multilayer material delaminate or partially delaminate more easily, it will be easier to repulp that layer to separate into individual fibers. The layers that are more difficult to separate will eventually become thinner layers or sheets, and through this geometric transformation they will be easier to separate into individual fibers than if they remained in a thicker structure. If all or some of the stronger layers cannot be completely separated, these layers will be screened so that the main part of the structure can be recycled into new paper or fiber products.

[0073] 2. Measurement

[0074] If the dust-free test material (carrier sheet), i.e. the multilayer material of the present invention, is handled during the test and the tensile strength of the entire material (including the tissue) is subsequently measured, the data (test results) can be collected and can be expressed as follows:

[0075] parameter Test Method unit Target LSL USL Basis Weight EN 12625-6 <![CDATA[(g / m 2 )]]> 16.5 15 17.5 thickness EN 12625-3 (μm) 1300 Tensile strength MD (dry) EN 12625-4 (N / m) 150 120 Elongation MD EN 12625-4 (%) 25 20 Air Permeability Internal Method DPMK 001 (l / m2 / s) 2400 1870 Moisture EN 287 % 5.5 6

[0076] The elongation and air permeability of the tissue carrier are two important parameters for conversion on a cleanroom machine.

[0077] Additional measurements on an exemplary thermally bonded dust-free tissue carrier gave the following values:

[0078]

[0079] Various embodiments of the present invention have been described above, and further minor modifications made by those skilled in the art fall within the scope of protection of the present invention. The breadth and scope of the present invention should not be limited by any of the above exemplary embodiments, but should only be defined according to the attached claims and their equivalents. For example, any of the above layered configurations or methods can be combined with other known methods. Other aspects, advantages and modifications within the scope of the present invention will be apparent to those skilled in the art.

Claims

1. A multilayer substrate comprising at least one layer providing tensile strength and a layer comprising fibers having an internal strength low enough to deform during a compression molding operation, thereby at least partially forming new bonds in new relative positions.

2. The multilayer substrate of claim 1, wherein the layer providing tensile strength provides a tensile strength at least about 10%, preferably at least about 20%, and most preferably at least about 50% greater than the tensile strength of the other layer.

3. The multi-layer substrate of claim 1, wherein the substrate is at least three layers of material.

4. The multilayer substrate according to claim 3, wherein the higher tensile strength is provided by at least one of the outer layers, preferably having a minimum tensile strength of about 75 N / m (CD).

5. The multilayer substrate according to claim 3, wherein the higher tensile strength is provided by two outer layers, preferably having a total minimum tensile strength of about 150 N / m (MD).

6. The multilayer substrate of claim 3, wherein the layer having higher tensile strength is thinner than the center layer.

7. The multilayer substrate of claim 1, 2 or 3, wherein the material having a low initial tensile strength provides one or more layers with better repulpability.

8. The multilayer substrate according to claim 3, wherein at least one of the outer layers is rendered more hydrophobic and / or oleophobic, preferably by using a water and / or oil repellent, such as an alkyl ketene dimer, alkenyl succinic anhydride or wax or a combination thereof.

9. The multilayer substrate of claim 3, wherein at least one of the outer layers has a high relative wet strength.

10. The multilayer substrate of claim 3, wherein at least one of the outer layers has a higher density.

11. The multilayer substrate of claim 1, 2 or 3, wherein the density is less than about 0.5 kg / dm 3 , preferably from about 0.1 to about 0.4 kg / dm 3 .

12. The multilayer substrate of claim 1, 2 or 3, wherein the grammage is from about 100 to about 2000 g / m 2 , preferably from about 300 to about 1500 g / m 2 .

13. The multi-layer substrate of claim 1, 2 or 3, wherein the moisture content is from about 4% to about 25%, preferably from about 7% to about 15%.

14. The multilayer substrate of claim 3 wherein at least one of the outer layers comprises one or more additives for additional strength and wet strength, preferably wherein at least one component of the additives comprises fibers of a man-made polymer.

15. A method for treating a multilayer substrate according to any one of the preceding claims for providing a multilayer product, comprising the steps of: a) providing the multilayer substrate, b) subjecting the substrate to high pressure, and c) subjecting the substrate to elevated temperatures, thereby providing a multi-layer product.

16. The method according to claim 15, wherein the high pressure and the high temperature of step b and / or c) are provided by a pressure pad device and a stamping device.

17. The method of claim 15, wherein the substrate is derived from chemithermomechanical pulp, thermomechanical pulp, kraft pulp, sulfate pulp, sulfite pulp, recycled pulp material, paperboard or carton, or a combination thereof.

18. The method of claim 15, wherein the substrate is derived from bleached or unbleached pulp, or a combination thereof.

19. The method of claim 15, wherein the substrate is derived from hardwood or softwood, bagasse, algae or straw, or a combination thereof.

20. The method of claim 15, wherein step a) is preceded by a conveying step comprising forming the substrate into a strip and subsequently folding the strip.

21. A multi-layer product obtainable by a method according to any one of claims 15 to 20.

22. The multilayer product according to claim 21, wherein the product is a moulded product such as a nut, a container, a bread clip or a package, wherein the container may be a disposable drinking cup or a dairy carton or an autoclave package or a dish, or a plate for eating or holding food, or paper or paperboard such as folding box board.

23. A multilayer product according to claim 21 wherein the product is provided such that one of the outer layers forms a thread or click feature for use in a sealable package such as a container, a closure or a portion of a container or closure.

24. Use of a multilayer product according to claim 21, wherein the product is a moulded product such as a nut, a container, a bread clip or a part of a package, wherein the container may be a disposable drinking cup or a dairy carton or an autoclave package or a dish or a plate for eating or holding food, or paper or paperboard such as folding box board.

25. A method for regenerating a multilayer product according to any one of claims 21 to 23 for providing a regenerated pulp, comprising the steps of: i) providing said multilayer product, preferably after its use, ii) immersing the product in a liquid, preferably water, most preferably warm water, iii) optionally adding one or more decoupling agents to the liquid, iv) exposing the product to the liquid to apply shear forces to provide a regenerated pulp.