Method for manufacturing expanded polymer material
By using preforms in foam injection molding technology to dissolve foaming agent in the mold and release pressure, the heterogeneity problem caused by premature foaming is solved, the fine adjustment of density and structure is achieved, and the relatively low density is successfully produced The product at 0.5 has improved material performance.
Patent Information
- Application Number
- CN202380023369.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-24
- Filing Date
- 2023-01-30
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing foam injection molding technology, it is difficult to avoid heterogeneity problems caused by premature foaming, resulting in poor foaming morphology and characteristics, and it is difficult to produce foamed products with a relative density below 0.5.
Using the preform method, the foaming agent is dissolved in the polymer material at high pressure and temperature in the mold, and the pressure is suddenly released at the end of dissolution to promote foaming, and the dissolution time is adjusted by thin structural design and heating. Density distribution, finely adjusting foam density and structure.
The foam injection molding technology has been simplified, overcome density limitations, and can produce products with a relative density below 0.5, and finely adjust the density and bubble orientation, improving the structural and functional performance of the material.
Smart Images

Figure CN118922289A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing an expanded polymer material and an object / product made of such an expanded polymer material. In particular, the method comprises a step of manufacturing a preform of the polymer material, a step of dissolving a physical foaming agent in the preform under pressure, and an expansion step during which the pressure is released. More particularly, the preform is manufactured with a filling degree equal to or lower than 90%, the dissolution step of the physical foaming agent is carried out under heat and pressure in a mold having a desired shape, and the expansion step is carried out by suddenly releasing the pressure. Background Art
[0002] Foam injection molding is a complex polymer processing technology for mass production of lightweight parts with advanced structural and functional properties. The method has various applications in fields such as medicine, automobiles and aerospace. In order to meet the growing consumer demand for greater functionality, an advanced foaming process that allows the inclusion of a foaming agent in the formula to achieve an expanded structure has been developed. By producing an expanded structure, improvements in functional and / or structural performance can be obtained, as well as a reduction in the weight of objects produced with the same volume and shape. Foam injection molding shows high potential in manufacturing objects with less environmental impact (Llewelyn et al., "Advance in Microcellular Injection Moulding, Journal of Cellular Plastics, Vol. 56, No. 6, pp. 646-674, 2020).
[0003] The process involves injection molding of a stable high pressure polymer / blowing agent solution which is allowed to foam in a mold where the solution is brought to a supersaturated state by a sudden pressure reduction.
[0004] The complexity lies in the transition from continuous (extrusion) to discontinuous (injection), a characteristic of this technology, and in the proper management of the solutions at the different processing stages. In fact, when, for example, the processing pressure p drops below the equilibrium pressure pe=pe(ω AE , T), the polymer / foaming agent solution tends to phase separate, and the equilibrium pressure pe=pe(ω AE , T) is at the general processing temperature T and composition ω AE The pressure of the blowing agent in equilibrium with the solution at 100 °C (i.e., based on the mass flow fraction metered by the feed system).
[0005] At any point and at any time before the final pressure release <p eIn the case of a premature foaming / phase separation, the ensuing (even if only partial) may also lead to heterogeneity in the final foam morphology, where prematurely formed bubbles and bubbles formed under the final pressure release coexist in the mold.
[0006] In general, heterogeneity due to premature foaming is detrimental to the morphology and final appearance of the foam as well as to the resulting foam properties (both structural and functional). Many advances have been proposed in the technical and scientific literature for preventing premature formation of bubbles / foam in injection molding: backpressure control valves (to avoid pressure drops in the barrel residue after injection), duct geometry design (to avoid stagnation points), techniques for generating backpressure in the mold (to avoid foam formation at the feed front during mold filling) and core-back techniques (to induce a sudden drop in pressure in the mold by a sudden increase in mold volume).
[0007] However, it is very difficult or impossible to avoid premature formation of foam. The current state of the art in foam injection molding solves this problem by utilizing a post-injection dissolution phase in which early bubbles are allowed to melt again under pressure to form a polymer / foaming agent solution again before a sudden pressure reduction through the core-back system (Ishikawa et al., "Visual Observation and Numerical Studies of N2 vs. CO2 Foaming Behavior in Core-Back Foam Injection Molding" Polym. Eng. Sci., Vol. 52, No. 4, pp. 875-883, 2012).
[0008] This solution, which is common today, is expensive, complicated and does not make it possible to produce foamed products having a relative density below 0.5 with respect to the density of the starting polymer. Summary of the invention
[0009] The applicant has solved the problem of manufacturing products comprising expanded polymer materials by injection molding. In this regard, the applicant has found a different solution that avoids the complex management of the polymer / blowing agent solution in the extruder and the injection of this solution into the mold to produce foamed plastic objects with complex geometries.
[0010] The Applicant has discovered a method that uses a preform of polymer material to be inserted into a mold in which a blowing agent is dissolved in the polymer material of the preform at high pressure and temperature and at the end of the dissolution the pressure is suddenly released to allow the desorption of the blowing agent and the consequent expansion. In the context of the method of the invention, the mold used comprises a cavity having a volume equal to or greater than the total volume of the preform and corresponding to the geometry of the product to be manufactured.
[0011] Taking into account the mass transfer characteristics represented by the diffusion of the blowing agent in the polymer at the operating temperature, the applicant has found that the preform must be manufactured in such a way that:
[0012] - Accelerate the dissolution step,
[0013] - determining the desired degree of foaming by foaming,
[0014] - Ensure that the mold is completely filled with the appropriate increase in volume after expansion.
[0015] The Applicant has found that the preform must at least partially comprise thin structures with characteristic dimensions of a millimeter, preferably a tenth of a millimeter, wherein the dissolution time of the blowing agent is of the order of a few seconds, at most a few tens of seconds.
[0016] Applicants have also observed that the empty spaces defined by the thin structures are preferably connected in a manner that allows the blowing agent to flow into all the cavities defined by the preform.
[0017] The applicant has also found that in this way, depending on the shape, size and spatial distribution of the thin structures, and according to the shape and size of the mold, the spatial distribution of the foam density, as well as the spatial distribution of the polymer structure in terms of molecular orientation and the orientation and degree of crystalline phases, can be designed in detail.
[0018] The Applicant has also observed that, depending on the precise definition of the spatial distribution of the foam density and of the spatial distribution of the polymer structure, it is possible to locally impart isotropic or anisotropic properties to the material, for example triangular, rhombic, or orthotropic properties.
[0019] Applicants have also observed that in order to accelerate dissolution and enable expansion into desired areas, the preform polymer may be locally heated prior to dissolution.
[0020] Again, the reduced thickness of the thin structures and the characteristic properties of the polymer material allow this step to be performed rapidly, with characteristic times on the order of a few seconds, at most tens of seconds.
[0021] The Applicant has also observed that the above-mentioned heating can be performed by injecting a blowing agent at an appropriate temperature in order to bring the polymer material to the desired temperature.
[0022] If the characteristic thickness of interest in the conveying mechanism is of the order of mm, typical thermal and mass diffusion of polymers allow that the characteristic time for heating and the characteristic time for saturating the polymer volume of interest with blowing agent are of the order of 1 second to 10 seconds, compatible with company production rates and current production processes / standards.
[0023] Using the present invention, with respect to the foam injection molding technology, the extruder is simplified because it is no longer necessary to inject the blowing agent into the barrel (valves, syringes, feeders, special screw configurations and lengths to allow complete dissolution of the blowing agent), and a complex core return operation with equipment components, core return time and geometric restrictions on the mold is not necessary.
[0024] Use the present invention, overcome the density restriction of the product that is used for foam injection molding at present.In fact, there is no product that produces relative density lower than 0.5 at present.
[0025] Using the present invention, by adjusting the preform saturation time and heating time, the size of the thin layer, and the positioning and geometry of the thin layer in the preform, the spatial distribution of the density, as well as the orientation of the bubbles and the structure of the polymer, for example in terms of molecular orientation and the orientation and degree of crystallization, can be finely and locally adjusted.
[0026] Therefore, a first aspect of the present invention is a method for manufacturing a product comprising a polymer material expanded by using one or more blowing agents, characterised in that the method comprises the following steps:
[0027] manufacturing a preform of polymer material having a filling degree equal to or less than 90% and a thin structure with a thickness equal to or less than 3 mm, preferably equal to or less than 2 mm,
[0028] making a mould comprising a cavity having the shape of the desired product and a size equal to or greater than the total volume of the preform,
[0029] inserting the preform into the cavity of the mold,
[0030] dissolving one or more blowing agents under pressure in the preform within the mold cavity,
[0031] Relieve stress, and
[0032] v Remove the product comprising the expanded polymer material from the mold. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] FIG. 1 shows a CAD model of a preform of Example 1 (a) and a CAD model of a preform of Example 2 (b).
[0034] FIG. 2 shows a detail of a CAD model of a preform of Example 1 (a) and a detail of a CAD model of a preform of Example 2 (b).
[0035] FIG. 3 shows the printing result of the preform of Example 1 (a) and the printing result of the preform of Example 2 (b).
[0036] FIG. 4 shows a detail of the printing result of the preform of Example 1 (a) and a detail of the printing result of the preform of Example 2 (b).
[0037] FIG. 5 shows the object obtained after dissolution and expansion of Example 1 (a) and the object obtained after dissolution and expansion of Example 2 (b).
[0038] FIG. 6 shows a CAD model of a preform (a) and a CAD model of its detail (b) for producing a helmet with a filling degree of about 70%.
[0039] FIG. 7 shows a CAD model of a preform (a) and a CAD model of its detail (b) for producing a helmet with a filling degree of about 50%.
[0040] FIG8 shows a CAD model (a) of a preform for manufacturing a helmet with a "gradient" filling degree (comprising a first layer of 50% and a second layer of 25%), and detailed CAD models (b), (c) and (d).
[0041] FIG. 9 shows a CAD model of the resulting helmet (a) and a CAD model of its detail (b).
[0042] Fig.10 A CAD model of a preform (a) and an expanded product (b) manufactured as described in Example 3 are shown, as well as pictures of the real preform (c) and expanded product (d to e).
[0043] Fig.11 A CAD model of a preform (a) and an expanded product (b) manufactured as described in Example 4 are shown, as well as pictures of the real preform (c) and expanded product (d to e).
[0044] Fig.12 A CAD model of a preform (a) and an expanded product (b) manufactured as described in Example 5 are shown, as well as pictures of the real preform (c) and expanded product (d to e).
[0045] Fig.13A CAD model of a preform (a) and an expanded product (b) manufactured as described in Example 6 are shown, as well as pictures of the real preform (c) and expanded product (d to e).
[0046] Fig.14 A CAD model of a preform (a) and an expanded product (b) manufactured as described in Example 7 are shown, as well as pictures of the real preform (c) and expanded product (d to e).
[0047] Fig.15 A CAD model of a preform (a) and an expanded product (b) manufactured as described in Example 8 are shown, as well as pictures of the real preform (c) and expanded product (d to e).
[0048] Fig.16 A CAD model of a preform (a) and a CAD model of an expanded product (b) manufactured as described in Example 9 are shown.
[0049] Fig.17 A CAD model of a preform (a) and a CAD model of an expanded product (b) manufactured as described in Example 10 are shown. DETAILED DESCRIPTION
[0050] The expression "polymer material" denotes a polymer material comprising a thermoplastic homopolymer or copolymer.
[0051] The expression "expandable polymer material" refers to a polymer material that is capable of absorbing a blowing agent at a certain temperature and pressure, capable of allowing the nucleation and growth of gas bubbles when the pressure is released, and capable of withstanding tensile stress during the growth of the gas bubbles until solidification.
[0052] The term "blowing agent" refers to a substance that is capable of causing expansion of a polymeric material by forming gas bubbles within the polymeric material.
[0053] The term "expanded polymer material" means a polymer material in which gas bubbles have been formed by a blowing agent.
[0054] The expression "filling degree" in relation to a preform means the ratio between the volume of material actually used to manufacture the preform on a millimeter or sub-millimeter scale and the macroscopic volume or total volume occupied by the preform itself (including the millimeter or sub-millimeter space not actually occupied by the material in this volume or total volume). The filling degree is a complementary index to the amount of voids in the preform, and the greater the amount of voids, the lower the value of the filling degree.
[0055] The term "cavity of the mold" refers to the space of the preform available for making the final object when expanded. The cavity of the mold is greater than or equal to the total volume of the preform and is capable of accommodating the preform.
[0056] The term "density" refers to the ratio between the weight of a given volume of a layer of polymeric material and that volume.
[0057] The term "relative density" refers to the ratio of the density of the expanded polymer material to the starting polymer.
[0058] The term "thin structure" means any shape or mass distribution in which at least one characteristic dimension is small and lower than the others. This definition includes, for example, wire (insulating sleeve) structures, parallel laminated structures, folded or twisted structures, and cavity structures.
[0059] The term "morphology" refers to the shape, size, number and distribution per unit volume of the gas bubbles formed within the expanded polymer material.
[0060] A first object of the invention is represented by a process for manufacturing a product comprising a polymer material expanded by using one or more blowing agents, characterized in that said process comprises the following steps:
[0061] manufacturing a preform of a polymer material having a filling degree equal to or lower than 90% and a thin structure with a thickness equal to or lower than 3 mm, preferably equal to or lower than 2 mm,
[0062] making a mould comprising a cavity having the shape of the desired product and a size equal to or greater than the total volume of the preform,
[0063] inserting the preform into the cavity of the mold,
[0064] dissolving one or more blowing agents under pressure in the preform within the mold cavity,
[0065] Relieve stress, and
[0066] v Remove the product comprising the expanded polymer material from the mold.
[0067] According to the first object of the present invention, said polymer material is preferably selected from thermoplastic polymer materials.
[0068] Advantageously, the thermoplastic polymer material is selected from polyolefins, polyurethanes, polyesters, polyamides, and mixtures thereof. Preferably, the polymer material is a polymer and copolymer of styrene, ethylene, propylene and other olefins, such as polystyrene, polyethylene and polypropylene, and mixtures thereof. Optionally, the polymer material can include one or more comonomers. Comonomers can include, for example, alkyl styrene, divinyl benzene, acrylonitrile, diphenyl ether, alpha-methyl styrene or a combination thereof. As an example, the polymer material can include about 0 wt % to about 30 wt %, preferably about 0.1 wt % to about 15 wt %, and more preferably about 1 wt % to about 10 wt % comonomers.
[0069] Preferably, the polymeric material may exhibit a molecular weight Mw (measured by GPC) ranging from about 10,000 Daltons to about 500,000 Daltons, more preferably ranging from about 150,000 Daltons to about 400,000 Daltons, and even more preferably from about 200,000 Daltons to about 350,000 Daltons.
[0070] Advantageously, the polymeric material exhibits a melt flow index ranging from 1.0 g / 10 min to 20 g / 10 min, measured according to ASTM D 1238 at a temperature of 200° C. and a load of 10 kg.
[0071] In one embodiment, the polymer material can be mixed with a fiber material, and the fiber material is preferably selected from natural plant and animal fibers, mineral fibers and synthetic fibers. Plant fibers are, for example, cotton, flax and hemp fibers. Animal fibers are, for example, wool and silk fibers. Mineral fibers are, for example, carbon fibers and silicate fibers, such as, for example, glass fibers, chrysotile fibers, sepiolite, palygorskite (also referred to as attapulgite), wollastonite, imogolite, and mixtures thereof. Synthetic fibers are, for example, polyester fibers, polyamide fibers (nylon), acrylics, aramids (Kevlar and Nomex), vinyl, polyolefins (polyethylene and polypropylene), polytetrafluoroethylene (Gore-tex) and polyurethane (Elastam) fibers.
[0072] The polymer material may contain the fiber material in an amount ranging from 5 to 70 volume %, preferably ranging from 10 to 50 volume %, relative to the volume of the polymer material.
[0073] The preform may be manufactured using methods known in the art such as injection molding, compression molding, 3D molding, rotational molding, blow molding, extrusion and by thermoforming, lamination, additive manufacturing and subtractive manufacturing.
[0074] The preform can also be produced directly in the mold using a counter mold in a step prior to dissolution.
[0075] In any case, the model is first constructed using CAD / CAM / CAE software (e.g. Solidworks by Dassault Systèmes). TM and CATIA TM 、Autodesk's AutoCAD TM The geometry of the preform is processed using a three-dimensional computer model created by a computer programmable controller. The resulting model is then sent to the production plant.
[0076] Advantageously, the degree of filling of the preform in polymeric material is equal to or lower than 70%, preferably lower than 50%.
[0077] Applicants have observed that lower filling levels allow for a greater amount of voids within the preform to enable rapid circulation of the blowing agent within the preform.
[0078] At the same time, the Applicant has observed that the dissolution of the blowing agent in the polymer material of the preform is faster with the thickness of the thin structure of the preform itself.
[0079] Advantageously, the thickness of the thin structure of the preform is greater than 0.1 mm, preferably greater than 0.2 mm, more preferably greater than 0.3 mm, and even more preferably greater than 0.4 mm. In particular, the thickness of the thin structure of the preform is lower than 2 mm, preferably lower than 1.9 mm, more preferably lower than 1.7 mm, and even more preferably lower than 1.6 mm. According to a particularly preferred embodiment, the thickness of the thin structure of the preform ranges from 0.5 mm to 1.5 mm.
[0080] The Applicant has observed that the thin structure of the preform, with the indicated thickness, allows obtaining a rapid and uniform dissolution of the blowing agent within the polymer material, avoiding the drawbacks known in the prior art.
[0081] The thin structure of the preform may consist of flakes and / or filaments that are ultimately interconnected to form a three-dimensional structure. The flake and / or filament structure allows the manufacture of a preform with a desired filling degree, leaving hollow spaces interconnected to each other within the preform, through which the blowing agent can be more effectively transported in the areas where the flakes or filaments are located and more advantageously absorbed by the polymer material during the dissolution step relative to areas with larger characteristic dimensions.
[0082] The preform may have a uniform structure or a gradient structure. A uniform structure means a uniform distribution of the preform structure, e.g. Figures 1a to 4a The structure exemplified in FIG. 1 , wherein the filling degree is uniform throughout the preform. The gradient structure presents a distribution of changes in the preform structure, such as Figures 1b to 4b The structure illustrated in FIG. 1 , wherein there are portions with different filling degrees.
[0083] The structure and final shape of the preform are not particularly limited and may present any appearance achievable according to methods known in the art and according to the shape and size requirements of the object to be manufactured.
[0084] According to a first object of the present invention, the dissolving step is carried out with a blowing agent or with a mixture of two or more blowing agents, preferably with a mixture of two blowing agents.
[0085] According to the first object of the present invention, the one or more blowing agents are selected from inert gases, carbon dioxide and substituted or unsubstituted (linear, branched or cyclic) aliphatic hydrocarbons having 3 to 8 carbon atoms. Advantageously, the blowing agent is selected from the group comprising nitrogen, carbon dioxide, n-butane, isobutane, n-pentane and isopentane. Preferably, the substituted aliphatic hydrocarbons include halogenated hydrocarbons, in particular chlorocarbons, chlorofluorocarbons and fluorocarbons, such as, for example, 1,1,1,2-tetrafluoroethane (Freon R-134a), 1,1-difluoroethane (Freon R-152a), difluoromethane (Freon R-32), pentafluoroethane (Freon R-125).
[0086] According to the first object of the invention, the dissolving step is preferably carried out at a temperature ranging from 20°C to 350°C, more preferably ranging from 30°C to 250°C and advantageously ranging from 50°C to 200°C.
[0087] According to the first object of the present invention, the dissolving step is preferably carried out at a pressure ranging from 20 bar to 400 bar, preferably ranging from 40 bar to 300 bar, more preferably ranging from 60 bar to 250 bar, and even more preferably ranging from 80 bar to 200 bar.
[0088] Advantageously, the dissolution step comprises a stabilization step under isobaric and isothermal conditions for a time ranging from 5 seconds to 300 seconds, preferably ranging from 10 seconds to 180 seconds, more preferably ranging from 15 seconds to 120 seconds.
[0089] Preferably, according to the first object of the present invention, the pressure is released instantaneously at a rate of not less than 20 bar / sec, preferably not less than 50 bar / sec, more preferably not less than 100 bar / sec.
[0090] The release of the pressure causes desorption and expansion of the blowing agent dissolved in the polymer material of the preform and the consequent formation of gas bubbles within the polymer material, thereby forming an expanded polymer material having a desired shape.
[0091] Depending on the structural distribution and saturation history of the preform, the morphology and density of the expanded polymer material can be uniform or gradient.
[0092] In particular, as described, for example, in international patent applications published under the numbers WO2019 / 202407 and WO2021 / 014371, the dissolution step can be carried out with a constant or time-varying pressure history of one or more foaming agents, in a periodic or non-periodic manner, in a waveform such as a sinusoidal, triangular, square, sawtooth, or a combination thereof.
[0093] Using a time-varying pressure history, a multilayer structure can be produced that includes at least two layers having different densities and / or morphologies without morphological and density discontinuities at the interface between the at least two layers.
[0094] Advantageously, the dissolving step may be performed by varying the concentration of the blowing agent over time. In particular, the concentration of the blowing agent may vary over time.
[0095] The formation of different concentration distributions of the blowing agent in different regions of the preform is determined by a dissolution step that varies the pressure or concentration of the blowing agent over time, as required to locally obtain the desired expansion and flow to impart a defined 3D pattern of density, structure, morphology, material and pore orientation to the part.
[0096] Figure 5a The object obtained with the preform of Example 1 is shown, with which an expanded polymer material having a uniform morphology and density is obtained.
[0097] Figure 5b An object obtained using the preform of Example 2 is shown, from which an expanded polymer material with varying morphology and density is obtained, wherein a partial foamed structure is formed inside a parallelepiped, which essentially corresponds to an arched structure with a 100% filling level of the preform, and the partial foamed structure has a different morphology and density relative to the majority of the foamed structure, which essentially corresponds to a layered structure.
[0098] In the following Experimental section, the present invention will now be described with reference to the materials and methods described for illustrative but non-limiting purposes.
[0099] Experimental Section
[0100] Example 1 (Uniform Expanded Material)
[0101] A preform consisting of a parallelepiped of thermoplastic polyurethane (TPU3D Printer Filament-YOYI) with dimensions of 40 mm × 40 mm × 10 mm, characterized by a filling degree equal to 50% and a thickness of 0.5 mm for thin structures, was produced by a 3D printer (Cetus MKIII 3D Printer-Tiertime). The preform is shown as a whole and in detail in Figures 1a to 4a middle.
[0102] The preform is then included in a mold comprising a cavity having the same dimensions as the total volume of the preform and subjected to the method described by the following steps:
[0103] 1. Heating from room temperature to 130°C within 15 minutes;
[0104] 2. Pressurization with CO2 from ambient pressure to 100 bar within 2 minutes;
[0105] 3. Wait for 30 seconds under isobaric and isothermal conditions;
[0106] 4. Release the pressure at a rate of 100 bar / s.
[0107] When the mold is opened, the object obtained from the preform (shown in Figure 5a The relative density of the samples was 0.5 and the average bubble size was about 200 microns.
[0108] Example 2 (Gradient expansion material)
[0109] A preform consisting of a parallelepiped of thermoplastic polyurethane (TPU3D Printer Filament-YOYI) with dimensions of 40 mm×40 mm×10 mm was produced by a 3D printer (Cetus MKIII 3D Printer—Tiertime).
[0110] As a whole and in detail shown in Figures 1b to 4b The preform in the embodiment 1 consists of domes with a filling degree of 100% and flakes with a thickness of about 0.5 mm with a filling degree of 30% distributed in the volume to occupy the entirety thereof.
[0111] The preform is then included in a mold comprising a cavity having the same dimensions as the total volume of the preform and subjected to the method described by the following steps:
[0112] 1. Heating from room temperature to 130°C within 15 minutes;
[0113] 2. Pressurization with CO2 from ambient pressure to 100 bar within 2 minutes;
[0114] 3. Wait for 30 seconds under isobaric and isothermal conditions;
[0115] 4. Release the pressure at a rate of 100 bar / s.
[0116] When the mold is opened, the object obtained from the preform (shown in Figure 5bThe preform is expanded in the middle and has an average relative density of 0.5. However, the construction of the preform results in a complex structure of partial foaming inside the parallelepiped that is not noticeable to the naked eye.
[0117] Example 3
[0118] A preform of thermoplastic polypropylene (E02ES of Sinopec Shanghai Gaoqiao Company) having a total volume with dimensions of 40 mm×40 mm×9 mm was produced by thermoforming.
[0119] Fig.10 a(CAD) and Fig.10 The preform shown in c (real object) with a filling degree of 45% is formed from a vertical sheet with a thickness of about 0.4 mm and two horizontal sheets with a thickness of about 2 mm.
[0120] The preform is then included in a mold comprising a cavity having the same dimensions as the total volume of the preform and subjected to the method described by the following steps:
[0121] 1. Heating from room temperature to 156°C in 15 minutes, followed by stabilization at a temperature of 142°C;
[0122] 2. Pressurization from ambient pressure to 100 bar with CO2 within 10 seconds;
[0123] 3. Release the pressure at a rate of 100 bar / s.
[0124] When the mold is opened, the object obtained from the preform (shown in Fig.10 b(CAD) and Fig.10 d to Fig.10 e (the real object that expands) expands, and the average relative density is 0.10g / cm 3 However, the structure of the preform determines the Fig.10 d to Fig.10 e is also perceptible to the naked eye. Fig.10 The high-density and unfoamed areas (0.95 g / cm 3 ) and in Fig.10 The low-density expansion area (0.09 g / cm 3 )’s complex structure manufacturing.
[0125] Example 4
[0126] A preform of thermoplastic polypropylene (E02ES of Sinopec Shanghai Gaoqiao Company) having a total volume with dimensions of 40 mm×40 mm×9 mm was produced by thermoforming.
[0127] Fig.11 a(CAD) and Fig.11 The preform with a filling degree of 20% shown in c (real object) is formed by a sheet with a thickness of about 1.0 mm placed perpendicularly to a flat plate with a thickness of about 1.0 mm.
[0128] The preform is then included in a mold comprising a cavity having the same dimensions as the total volume of the preform and subjected to the method described by the following steps:
[0129] 1. Heating from room temperature to 156°C in 15 minutes, followed by stabilization at a temperature of 142°C;
[0130] 2. Pressurization with CO2 from ambient pressure to 120 bar within 2 minutes;
[0131] 3. Wait for 1 minute under isobaric and isothermal conditions;
[0132] 4. Release the pressure at a rate of 100 bar / s.
[0133] When the mold is opened, the object obtained from the preform (shown in Fig.11 b(CAD) and Fig.11 d to Fig.11 e (the real object that expands) expands, and the average relative density is 0.10g / cm 3 .
[0134] Example 5
[0135] A preform of thermoplastic polypropylene (E02ES of Sinopec Shanghai Gaoqiao Company) having a total volume with dimensions of 40 mm×40 mm×9 mm was produced by thermoforming.
[0136] Fig.12 a(CAD) and Fig.12 The preform shown in c (real object) with a filling degree of 67% is formed of vertical sheets having a thickness gradient varying from a maximum value of 3 mm to a minimum value of 1 mm in both vertical and horizontal directions.
[0137] The preform is then included in a mold comprising a cavity having the same dimensions as the total volume of the preform and subjected to the method described by the following steps:
[0138] 1. Heating from room temperature to 156°C in 15 minutes, followed by stabilization at a temperature of 142°C;
[0139] 2. Pressurization with CO2 from ambient pressure to 120 bar within 2 minutes;
[0140] 3. Wait for 1 minute under isobaric and isothermal conditions;
[0141] 4. Release the pressure at a rate of 100 bar / s.
[0142] When the mold is opened, the object obtained from the preform (shown in Fig.12 b(CAD) and Fig.12 d to Fig.12 e (the real object that expands) expands, and the average relative density is 0.65g / cm 3 However, the structure of the preform determines the Fig.12 d to Fig.12 The lower high-density unfoamed area (0.95 g / cm 3 ) and in Fig.12 d to Fig.12 The low-density expansion area (0.11 g / cm 3 )’s complex structure manufacturing.
[0143] Example 6
[0144] A preform of thermoplastic polypropylene (E02ES of Sinopec Shanghai Gaoqiao Company) having a total volume with dimensions of 40 mm×40 mm×9 mm was produced by thermoforming and by assembling two sheets with a thickness of 2 mm obtained by compression molding thermoplastic polypropylene with flax fibers (40 volume %) in an aluminum mold at 200° C. with 5 sheets with a thickness of 1 mm obtained by compression molding thermoplastic polypropylene in an aluminum mold at 180° C.
[0145] Fig.13 a(CAD) and Fig.13 c (real object) shows a preform with a filling degree of 67%.
[0146] The preform is then included in a mold comprising a cavity having the same dimensions as the total volume of the preform and subjected to the method described by the following steps:
[0147] 1. Heating from room temperature to 156°C in 15 minutes, followed by stabilization at a temperature of 142°C;
[0148] 2. Pressurization with CO2 from ambient pressure to 120 bar within 2 minutes;
[0149] 3. Wait for 1 minute under isobaric and isothermal conditions;
[0150] 4. Release the pressure at a rate of 100 bar / s.
[0151] When the mold is opened, the object obtained from the preform (shown in Fig.13 b(CAD) and Fig.13 d to Fig.13 e (the real object that expands) expands, and the average relative density is 0.65g / cm 3 The object obtained is a thermoplastic sandwich having an outer polypropylene wall with fiber reinforcement and an inner polypropylene foam core. In particular, the thickness of the inner foam core has a constant thickness equal to about 5 mm.
[0152] Example 7
[0153] A preform of thermoplastic polypropylene (E02ES from Sinopec Shanghai Gaoqiao Company) having a total volume with dimensions of 40 mm×40 mm×9 mm was produced by thermoforming and by assembling two sheets with a thickness of 2 mm obtained by compression molding thermoplastic polypropylene with flax fibers (40% by volume) in an aluminum mold at 200° C. and four sheets with a thickness of 1 mm obtained by compression molding thermoplastic polypropylene in an aluminum mold at 180° C.
[0154] Fig.14 a(CAD) and Fig.14 A preform with a filling degree of 50% is shown in c (real object).
[0155] The preform is then included in a mold comprising a cavity having the same dimensions as the total volume of the preform and subjected to the method described by the following steps:
[0156] 1. Heating from room temperature to 156°C in 15 minutes, followed by stabilization at a temperature of 142°C;
[0157] 2. Pressurization with CO2 from ambient pressure to 120 bar within 2 minutes;
[0158] 3. Wait for 1 minute under isobaric and isothermal conditions;
[0159] 4. Release the pressure at a rate of 100 bar / s.
[0160] When the mold is opened, the object obtained from the preform (shown in Fig.14 b(CAD) and Fig.14 d to Fig.14 e (real object with expansion) expands, with an average relative density of 0.5 g / cm 3 The object obtained is a thermoplastic sandwich having an outer polypropylene wall with fiber reinforcement and an inner polypropylene foam core. In particular, the thickness of the inner foam core has a constant thickness that can vary from about 5 mm to zero (on the thinner side).
[0161] Example 8
[0162] A preform of thermoplastic polypropylene (E02ES of Sinopec Shanghai Gaoqiao Company) having a total volume with dimensions of 40 mm×40 mm×9 mm was produced by thermoforming. Fig.15 a(CAD) and Fig.15 The preform with a filling degree of 15% shown in c (real object) is formed from vertical sheets with a thickness of about 1 mm and curved sheets with a thickness of about 2 mm.
[0163] The preform is then included in a mold comprising a cavity having the same dimensions as the total volume of the preform and subjected to the method described by the following steps:
[0164] 1. Heating from room temperature to 156°C in 15 minutes, followed by stabilization at a temperature of 142°C;
[0165] 2. Pressurization with CO2 from ambient pressure to 120 bar within 2 minutes;
[0166] 3. Wait for 1 minute under isobaric and isothermal conditions;
[0167] 4. Release the pressure at a rate of 100 bar / s.
[0168] When the mold is opened, the object obtained from the preform (shown in Fig.15 b(CAD) and Fig.15 d to Fig.15 e (the real object that expands) expands, and the average relative density is 0.15g / cm 3 .
[0169] Example 9
[0170] A preform of thermoplastic polypropylene (E02ES of Sinopec Shanghai Gaoqiao Company) having a total volume with dimensions of 40 mm×40 mm×9 mm was produced by thermoforming. Fig.16 Half of the preform shown in a (CAD) is formed of vertical sheets of about 0.4 mm thickness and the other half is formed of 2 mm sheets. All sheets are held together by a flat plate of 0.4 mm thickness.
[0171] The preform is then included in a mold comprising a cavity having the same dimensions as the total volume of the preform and subjected to the method described by the following steps:
[0172] 1. Heating from room temperature to 156°C in 15 minutes, followed by stabilization at a temperature of 142°C;
[0173] 2. Pressurization from ambient pressure to 120 bar with CO2 within 10 minutes;
[0174] 3. Gas exchange from CO2 to N2 at 120 bar in 10 seconds;
[0175] 4. Release the pressure at a rate of 100 bar / s.
[0176] When the mold is opened, the object obtained from the preform (shown in Fig.16 b (CAD)) expands, with an average relative density of 0.2 g / cm 3 In this way, the part obtained from a thickness of 2 mm foamed with CO2 has a cell morphology of about 100 μm, and the part obtained from a sheet of 0.4 mm foamed with N2 has a cell morphology of about 10 μm. The density of each part given by the filling degree is about 0.2 g / cm 3 , the degree of filling is in this case equal between the two parts and is 20%.
[0177] Example 10
[0178] A preform of thermoplastic polypropylene (E02ES of Sinopec Shanghai Gaoqiao Company) having a total volume with dimensions of 40 mm×40 mm×9 mm was produced by thermoforming. Fig.17 The preform shown in a (CAD) with a filling degree of 20% is formed from vertical sheets with a thickness of about 0.4 mm. All sheets are held together by a flat plate with a thickness of 0.4 mm.
[0179] The preform is then included in a mold comprising a cavity having the same dimensions as the total volume of the preform and subjected to the method described by the following steps:
[0180] 1. Heating from room temperature to 156°C in 15 minutes, followed by stabilization at a temperature of 142°C;
[0181] 2. Pressurize with N2 from ambient pressure to 120 bar in 10 seconds;
[0182] 3. Release the pressure at a rate of 100 bar / s.
[0183] When the mold is opened, the object obtained from the preform (shown in Fig.17 b (CAD)) undergoes uniform expansion, with an average relative density of 0.2 g / cm 3 .
Claims
1. A method for manufacturing a product comprising a polymer material expanded by using one or more blowing agents, characterized in that The method comprises the following steps: manufacturing a preform of a polymer material having a filling degree equal to or less than 90% and a thin structure with a thickness equal to or less than 3 mm, preferably equal to or less than 2 mm, making a mould comprising a cavity having the shape of the desired product and a size equal to or greater than the total volume of the preform, inserting the preform into the cavity of the mold, dissolving one or more blowing agents under pressure in the preform within the mold cavity, releasing the pressure, and - Removing the product comprising expanded polymer material from the mould.
2. The method according to claim 1, characterized in that The degree of filling of the preform of polymer material is equal to or less than 70%, preferably less than 50%.
3. The method according to claim 1, characterized in that The thickness of the thin structure of the preform is greater than 0.1 mm, preferably greater than 0.2 mm, more preferably greater than 0.3 mm, and even more preferably greater than 0.4 mm.
4. The method according to claim 1, characterized in that The thickness of the thin structure of the preform is lower than 2 mm, preferably lower than 1.9 mm, more preferably lower than 1.7 mm, and even more preferably lower than 1.6 mm.
5. The method according to claim 1, characterized in that The dissolving step is performed at a temperature ranging from 20°C to 350°C, preferably ranging from 30°C to 250°C, and more preferably ranging from 50°C to 200°C.
6. The method according to claim 1, characterized in that The dissolving step is performed at a pressure ranging from 20 bar to 400 bar, preferably ranging from 40 bar to 300 bar, more preferably ranging from 60 bar to 250 bar, and even more preferably ranging from 80 bar to 200 bar.
7. The method according to claim 1, characterized in that The dissolving step is carried out with a constant or time-varying pressure history of the one or more blowing agents.
8. The method according to claim 7, characterized in that The pressure history varies over time in a periodic or non-periodic manner, in a waveform such as a sinusoidal, triangular, square, sawtooth, or a combination thereof.
9. The method according to claim 7, characterized in that The dissolving step is performed with a time-varying concentration history of the blowing agent.
10. The method according to claim 1, characterized in that The dissolution step comprises a stabilization step under isobaric and isothermal conditions for a time ranging from 5 seconds to 300 seconds, preferably ranging from 10 seconds to 180 seconds, more preferably ranging from 15 seconds to 120 seconds.
11. The method according to claim 1, characterized in that The pressure is released at a rate of not less than 20 bar / s, preferably not less than 50 bar / s, more preferably not less than 100 bar / s.
12. The method according to claim 1, characterized in that The one or more blowing agents are selected from inert gases, carbon dioxide and substituted or unsubstituted (linear, branched or cyclic) aliphatic hydrocarbons having 3 to 8 carbon atoms.
13. The method according to claim 1, characterized in that The one or more blowing agents are selected from nitrogen, carbon dioxide, n-butane, isobutane, n-pentane and isopentane.
14. The method according to claim 1, characterized in that The polymer material used to make the preform comprises a fibrous material.
15. The method of claim 14, wherein the fiber material is selected from natural plant and animal fibers, mineral fibers and synthetic fibers.
16. The method according to claim 14, wherein the polymer material comprises the fiber material in an amount ranging from 5 to 70 volume %, preferably ranging from 10 to 50 volume %, relative to the volume of the polymer material.
17. The method according to claim 1, characterized in that The step of manufacturing a preform is performed in the cavity of the mold.