Covering articles with durable optical structures and functional coatings and methods of making same

By setting a fluorine-containing material easy-to-clean coating on the optical coating of the cover product and performing modification treatment, combined with the multi-layer optical structure, the problem of poor durability of the easy-to-clean coating in the prior art is solved, and high durability is achieved and excellent optical properties.

CN118922388APending Publication Date: 2024-11-08CORNING INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029253.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-21
Filing Date
2023-03-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing cover articles have poor durability on optical coatings and substrates, which limit their optical properties and fingerprint resistance when protecting electronic devices.

Method used

It adopts an easy-to-clean coating with fluorine-containing material and is modified on the outer surface of the optical coating to reduce surface roughness. Combined with multiple optical structures with high refractive index and low refractive index layers, a scratch-resistant layer is formed. Enhance the physical thickness and hardness of the optical structure.

Benefits of technology

The durability of the cover article and the wear resistance of the functional coating are significantly improved, ensuring that the water contact angle remains high in the steel wool wear test, improving the combination of optical and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922388A_ABST
    Figure CN118922388A_ABST
Patent Text Reader

Abstract

Described herein is a covering article comprising: a substrate having a major surface; an optical structure disposed on the major surface, where the optical structure includes an optical coating and a scratch resistant layer, and where the optical coating has an outer surface; and an easy-to-clean (ETC) coating disposed on the outer surface of the optical coating, wherein the ETC coating includes a fluorine-containing material. The outer surface of the optical coating has a surface roughness (Ra) of less than 1.5 nm. The optical structure has a physical thickness greater than or equal to 500 nm and a maximum hardness of 10 GPa or greater, as measured on the outer surface of the optical coating along an indentation depth of 50 nm or greater by a Berkovich indenter test. The scratch resistant layer has a physical thickness of from 200 nm to 5000 nm.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Priority claim

[0002] This application claims the benefit of priority under patent law to U.S. Provisional Application No. 63 / 321,909, filed on March 21, 2022, the contents of which are incorporated herein by reference in their entirety. Technical Field

[0003] The present disclosure relates to articles for protecting displays and other electronic devices, particularly cover articles having durable functional coatings (e.g., easy-to-clean coatings) and optical structures (e.g., antireflective coatings), and methods of making these articles, wherein the durable functional coatings and optical structures are configured to exhibit desired optical properties and enhance the durability of the functional coatings. Background Art

[0004] Covered articles with glass substrates are often used to protect key devices and components in electronic products and systems, such as mobile devices, smart phones, tablet computers, handheld devices, car displays, and other electronic devices with displays, cameras, light sources, and / or sensors. These covered articles can also be used for architectural products, transportation products (e.g., products for automotive applications, trains, airplanes, ships, etc.), appliance products, or any products that require a certain degree of transparency, scratch resistance, abrasion resistance, or a combination thereof.

[0005] These applications employing cover glass articles generally require a combination of mechanical and environmental durability, fingerprint resistance, breakage resistance, damage resistance, scratch resistance, and strong optical performance characteristics. In some applications, the cover article is required to cover and protect display devices, cameras, sensors, and / or light sources. Typically, the cover article is configured with a multi-layer optical coating that is configured so that the cover article exhibits a combination of certain optical properties. For example, the cover article may be required to exhibit high light transmittance, low reflectivity, and / or low transmission color in the visible spectrum, and employ an optical coating configured to achieve acceptable levels of these properties.

[0006] Conventional cover articles often employ hydrophobic and / or oleophobic functional coatings on their optical coatings and structures, commonly referred to as "anti-fingerprint," "anti-fouling," and "easy-to-clean" coatings. These easy-to-clean coatings can reduce surface damage due to their lubricating characteristics. They can also reduce or eliminate fingerprints and facilitate the cleaning of foreign objects and materials. However, when used in combination with an underlying optical coating, the durability of the easy-to-clean coating is poor. That is, it has been found that the durability of the easy-to-clean coating disposed on the optical coating and the substrate is significantly reduced or decreased relative to the easy-to-clean coating disposed directly on the substrate. Therefore, conventional cover articles are often limited in their ability to exhibit a combination of optical properties and anti-fingerprint properties.

[0007] Therefore, there is a need for improved cover articles to protect optical articles and devices, particularly cover articles having durable functional coatings (e.g., easy-to-clean coatings) and optical structures (e.g., anti-reflective coatings) configured to exhibit desired optical properties and enhance the durability of the functional coatings. There is also a need for methods of making these cover articles. The present disclosure addresses these needs and other needs. Summary of the invention

[0008] According to one aspect of the present disclosure, there is provided a covering article, the covering article comprising: a substrate having a major surface; an optical structure disposed on the major surface, wherein the optical structure comprises an optical coating and a scratch-resistant layer, and wherein the optical coating has an outer surface opposite to the major surface of the substrate; and an easy-to-clean (ETC) coating disposed on the outer surface of the optical coating, wherein the ETC coating comprises a fluorine-containing material. The outer surface of the optical coating has a surface roughness (Ra) of less than 1.5 nm. The optical structure has a physical thickness greater than or equal to 500 nm and a maximum hardness of 10 GPa or greater, as measured on the outer surface of the optical coating at an indentation depth of 50 nm or greater by a Berkovich indenter test. The scratch-resistant layer has a physical thickness of 200 nm to 5000 nm.

[0009] According to one aspect of the present disclosure, a covering product is provided, the covering product comprising: a substrate having a major surface; an optical structure disposed on the major surface, wherein the optical structure comprises an optical coating and a scratch-resistant layer, and wherein the optical coating has an outer surface opposite to the major surface of the substrate; and an easy-to-clean (ETC) coating disposed on the outer surface of the optical coating, wherein the ETC coating comprises a fluorine-containing material. The outer surface of the optical coating has a surface roughness (Ra) of less than 1.5 nm. The optical structure has a physical thickness greater than or equal to 500 nm and a maximum hardness of 10 GPa or greater, as measured on the outer surface of the optical coating along an indentation depth of 50 nm or greater by a Berkovich indenter test. The scratch-resistant layer has a physical thickness of 200 nm to 5000 nm. Further, the optical coating comprises a plurality of high refractive index (RI) layers and low RI layers, wherein the refractive index of each of the low RI layers is less than or equal to about 1.8, and the refractive index of each of the high RI layers is greater than 1.8. Each high RI layer includes one of AlOxNy, Nb2Ox, TiO2, Si3N4, SiNx and SiOxNy, and each low RI layer includes one of SiO2, SiOx and MgF2. In addition, the scratch-resistant layer includes any one of AlOxNy, Si3N4, SiNx and SiOxNy.

[0010] According to one aspect of the present disclosure, a covering product is provided, the covering product comprising: a substrate having a major surface; an optical structure disposed on the major surface, wherein the optical structure comprises an optical coating and a scratch-resistant layer, and wherein the optical coating has an outer surface opposite to the major surface of the substrate; and an easy-to-clean (ETC) coating disposed on the outer surface of the optical coating, wherein the ETC coating comprises a fluorine-containing material. The outer surface of the optical coating has a surface roughness (Ra) of less than 1.5 nm. The optical structure has a physical thickness greater than or equal to 750 nm and a maximum hardness of 10 GPa or greater, as measured on the outer surface of the optical coating along an indentation depth of 50 nm or greater by a Berkovich indenter test. The scratch-resistant layer has a physical thickness of 250 nm to 2500 nm. In addition, the scratch-resistant layer is within the optical coating. Further, the optical coating comprises a plurality of high refractive index (RI) layers and low RI layers, wherein the refractive index of each of the low RI layers is less than or equal to about 1.8, and the refractive index of each of the high RI layers is greater than 1.8. Each high RI layer includes one of Si3N4, SiNx and SiOxNy, and each low RI layer includes one of SiO2 and SiOx. In addition, the scratch-resistant layer includes any one of Si3N4, SiNx and SiOxNy.

[0011] According to another aspect of the present disclosure, a method for manufacturing a covered article is provided, the method comprising: providing a substrate having a major surface; depositing an optical structure on the major surface, wherein the optical structure comprises an optical coating and a scratch-resistant layer, and wherein the optical coating has an outer surface opposite to the major surface of the substrate; modifying the outer surface of the optical coating, wherein after the step of modifying the outer surface, the outer surface of the optical coating has a surface roughness (Ra) of less than 1.5 nm; after the step of modifying the outer surface, depositing an easy-to-clean (ETC) coating on the outer surface of the optical coating, wherein the ETC coating comprises a fluorine-containing material; and curing the ETC coating. The optical structure has a physical thickness greater than or equal to 500 nm and a maximum hardness of 10 GPa or greater, as measured on the outer surface of the optical coating at an indentation depth of 50 nm or greater by a Berkovich indenter test. Further, the scratch-resistant layer has a physical thickness of 200 nm to 5000 nm. Furthermore, after the step of curing the ETC coating, the ETC coating exhibited a water contact angle of greater than 95° after 1000 cycles in a Steel Wool Abrasion Test.

[0012] Additional features and advantages will be set forth in the detailed description that follows and, to the extent possible, will be readily apparent to those skilled in the art from this description or may be recognized by practicing the embodiments as described herein, including the detailed description that follows, the claims, and the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] It should be understood that the foregoing summary and the following detailed description are merely exemplary and are intended to provide an overview or framework for understanding the nature and character of the claims. The accompanying drawings are included to provide a further understanding and are incorporated into and constitute a part of this specification. The accompanying drawings illustrate one or more embodiments and, together with the description, serve to explain the principles and operation of the various embodiments, wherein:

[0014] Figure 1A is a cross-sectional side view of a cover article (e.g., for a display device) according to an embodiment of the present disclosure;

[0015] Figure 1B is a cross-sectional side view of a covered article according to an embodiment of the present disclosure;

[0016] Figures 2A-2C is a schematic cross-sectional view of an easy-to-clean coating on a substrate and an easy-to-clean coating on each of two antireflective films having different surface roughness levels on the substrate;

[0017] Figure 3A is a schematic cross-sectional view of an apparatus for performing a steel wool abrasion test on a covered article according to an embodiment of the present disclosure;

[0018] Figure 3B is a schematic cross-sectional view of a covered article according to an embodiment of the present disclosure after being subjected to a steel wool test;

[0019] Figure 4 is a schematic diagram of a flow chart of a method of manufacturing a cover article according to an embodiment of the present disclosure;

[0020] Figure 4A According to the embodiments of the present disclosure Figure 4 A schematic diagram of the steps of modifying the outer surface of the covered article by the method depicted;

[0021] Figure 5A is a plan view of an exemplary electronic device including any of the cover articles disclosed herein;

[0022] Figure 5B yes Figure 5A A perspective view of an exemplary electronic device;

[0023] Figure 6is a graph of average water contact angle measurements of samples of various comparative articles (relative to covered articles of the present disclosure) after being subjected to 0, 1000, 2000 and 3000 cycles of steel wool abrasion testing;

[0024] Fig. 7A is a graph of surface roughness versus treatment time of an outer surface of an optical coating covering an article after being subjected to plasma treatment at various power levels according to an embodiment of the present disclosure;

[0025] Figure 7B According to the embodiments of the present disclosure, Fig. 7A A graph of the relationship between the first surface reflectance and visible wavelength of the covered article prepared by the process shown in ; and

[0026] Figure 7C and 7D According to the embodiments of the present disclosure, Fig. 7A Graph of average water contact angle measurements of covered article samples prepared by the treatments depicted in FIG. 5 after being subjected to 2000 and 3000 cycles of steel wool abrasion testing, respectively. DETAILED DESCRIPTION

[0027] In the following specific embodiments, for the purpose of explanation rather than limitation, the exemplary embodiments disclosing specific details are set forth to provide a thorough understanding of the various principles of the present disclosure. However, it will be apparent to those of ordinary skill in the art that, after benefiting from the present disclosure, the present disclosure can be practiced in other embodiments that depart from the specific details disclosed herein. In addition, the description of well-known equipment, methods, and materials may be omitted so as not to obscure the description of the various principles of the present disclosure. Ultimately, where applicable, the same reference numerals refer to the same elements.

[0028] Ranges may be expressed herein as from "about" one particular value and / or to "about" another particular value. When such ranges are expressed, another embodiment includes from the one particular value and / or to the other particular value. Similarly, when values ​​are expressed as approximations by using the antecedent "about," it is understood that the particular value forms another embodiment. It is also understood that each of the end values ​​in a range is meaningful relative to the other end value and independently of the other end value.

[0029] Directional terms used herein—eg, “upper,” “lower,” “right,” “left,” “front,” “back,” “top,” “bottom”—refer only to the drawings drawn and are not intended to represent absolute directions.

[0030] Unless otherwise expressly stated, it is not intended that any method set forth herein be construed as requiring that its steps be performed in a particular order. Therefore, in the absence of a method claim actually reciting an order in which its steps are to be followed or otherwise specifically stating in the claim or description that the steps are to be limited to a particular order, no order is intended to be inferred in any respect. This applies to any possible non-express basis for interpretation, including: logical matters regarding the arrangement of steps or operational flow; explicit meaning derived from grammatical organization or punctuation; the number or type of embodiments described in this specification.

[0031] As used herein, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a component" includes aspects having two or more such components unless the context clearly dictates otherwise.

[0032] As used herein, the term "disposed" includes coating, depositing and / or molding a material onto a surface using any method known or to be developed in the art. The disposed material may constitute a layer as defined herein. As used herein, the phrase "disposed on..." includes embodiments in which a material is molded onto a surface so that the material is in direct contact with the surface, as well as embodiments in which the material is molded onto a surface and one or more intermediate materials are disposed between the material and the surface. The intermediate material may constitute a layer as defined herein.

[0033] As used herein, the terms "low RI layer" and "high RI layer" refer to the relative values ​​of the refractive index ("RI") of each layer of the optical structure of the cover article according to the present disclosure (i.e., low RI layer < high RI layer). Therefore, the refractive index value of the low RI layer is less than the refractive index value of the high RI layer. In addition, as used herein, "low RI layer" and "low refractive index layer" can be interchanged with the same meaning. Similarly, "high RI layer" and "high refractive index layer" can be interchanged with the same meaning.

[0034] As used herein, the term "strengthened substrate" refers to a substrate employed in the cover article of the present disclosure that has been chemically strengthened, for example, by ion exchange of larger ions for smaller ions in the surface of the substrate. However, other strengthening methods known in the art, such as thermal tempering, or utilizing mismatches in thermal expansion coefficients between portions of the substrate to produce compressive stress and central tension regions, may also be utilized to form a strengthened substrate.

[0035] As used herein, "Berkovich Indenter Hardness Test," "Berkovich Hardness Test," and "Berkovich Indenter Test" are used interchangeably and refer to a test that measures the hardness of a material at the surface of the material by pressing into the surface with a diamond Berkovich indenter. The Berkovich indenter hardness test includes pressing a diamond Berkovich indenter into the outermost surface (e.g., exposed surface) of a single optical structure or an external optical structure of a cover article of the present disclosure to form an indentation having a depth in the range of about 50 nm to about 1000 nm (or the entire thickness of the external or internal optical structure, whichever is less) and measuring the maximum hardness of the indentation along the entire indentation depth range or a segment of the indentation depth (e.g., in the range of about 100 nm to about 600 nm), generally using the method described in: Oliver, W.C.; Pharr, G.M. An improved technique for determining hardness and elastic modulus using load and displacement sensing indentation experiments. J. Mater. Res., Vol. 7, No. 6, 1992, 1564-1583; and Oliver, W.C.; Pharr, G.M. Measurement of Hardness and Elastic Modulus by Instrument Indentation: Advances in Understanding and Refinements to Methodology. J. Mater. Res., Vol. 19, No. 1, 2004, 3-20. As used herein, each of "hardness" and "maximum hardness" interchangeably refers to the maximum hardness as measured along an indentation depth range, rather than an average hardness.

[0036] As used herein, the term "transmittance" is defined as the percentage of incident light power within a given wavelength range that is transmitted through a material (e.g., an article, substrate, or optical film, or a portion thereof). The term "reflectivity" is similarly defined as the percentage of incident light power within a given wavelength range that is reflected from a material (e.g., a cover article, its substrate, an optical structure or an optical coating, or a portion thereof). Transmittance and reflectance are measured using a specific line width. As used herein, "average transmittance" refers to the average amount of incident light power transmitted through a material within a defined wavelength range. As used herein, "average reflectivity" refers to the average amount of incident light power reflected by a material.

[0037] As used herein, "photopic reflectance" simulates the response of the human eye by weighting the reflectance or transmittance and the wavelength spectrum according to the sensitivity of the human eye. Photopic reflectance can also be defined as the brightness or tristimulus Y value of the reflected light according to known conventions (such as the CIE color space conventions). As used herein, "average photopic reflectance" for a wavelength range of 380nm to 720nm is defined in the following formula as the spectral reflectance R(λ) multiplied by the light source spectrum I(λ) and the CIE color matching function (related to the spectral response of the eye):

[0038]

[0039] In addition, "average reflectivity" can be determined in the visible spectrum or other wavelength ranges according to measurement principles understood by those skilled in the art of the present disclosure, such as in the infrared spectrum from 840nm to 950nm, etc. Unless otherwise stated, all reflectivity values ​​reported or otherwise referenced in this disclosure are associated with tests conducted through the two major surfaces and optical structures of the substrate of the cover article of the present disclosure, such as "dual-surface" average bright reflectivity. Where "single-sided" or "first-surface" reflectivity is specified, the reflectivity of the back surface of the cover article is eliminated by optical bonding with a light absorber, allowing only the reflectivity of the first surface to be measured.

[0040] The usability of a cover article in an electronic device (e.g., as a protective cover) may be related to the total amount of reflection in the article. Bright reflectivity is particularly important for display devices that use visible light. Lower reflectivity of a cover article on a lens and / or display associated with a device can reduce multiple-bounce reflections in the device that can produce "ghosting." Therefore, reflectivity has an important relationship to the image quality associated with the device, particularly its display and any other optical components thereof (e.g., a camera lens). Low reflectivity displays can also improve display readability, reduce eye fatigue, and speed up user response time (e.g., in automotive displays, display readability may also be related to driver safety). Low reflectivity displays can also reduce display energy consumption and extend device battery life because the display brightness of a low reflectivity display can be reduced compared to a standard display while still maintaining a target display readability level in bright ambient environments.

[0041] As used herein, "brightness transmittance" is defined in the following formula as the spectral transmittance T(λ) multiplied by the light source spectrum I(λ) and the CIE color matching function (related to the spectral response of the eye):

[0042]

[0043] In addition, "average transmittance" or "average bright light transmittance" can be determined in the visible spectrum or other wavelength ranges according to measurement principles understood by those skilled in the art of the present disclosure, such as in the infrared spectrum from 840nm to 950nm, etc. Unless otherwise stated, all transmittance values ​​reported or otherwise referenced in the present disclosure and claims are relative to the optical transmission through the two major surfaces of the substrate covering the article and the optical structure (e.g., Figure 1A and 1B The substrate 110, major surfaces 112, 114, and optical structure 120 shown, as described below, are correlated to tests performed, such as "dual-surface" average bright light transmittance.

[0044] In general, the present disclosure relates to covered articles that employ structures on glass and glass-ceramic substrates (including reinforced substrates). In addition, these covered articles include functional, high-durability coatings (e.g., easy-to-clean coatings) on high-hardness optical structures, which are configured to ensure that the covered articles exhibit certain optical properties, such as low reflectivity. Notably, the structural characteristics of the optical structures can be configured to improve and affect the durability of the functional coatings. In addition, the present disclosure also includes methods for making these covered articles, including method steps for configuring optical structures to improve and affect the durability of overlying functional coatings (e.g., plasma surface treatment processes, mechanical polishing, chemical etching, etc.).

[0045] The cover articles disclosed herein can be used to protect and / or cover displays, camera lenses, sensors and / or light source components within or in part of electronic devices, as well as to protect other components (e.g., buttons, speakers, microphones, etc.). These cover articles with protective functions use an optical structure disposed on a substrate so that the article exhibits a combination of high hardness, high damage resistance and desirable optical properties (including low reflectivity). The optical structure may include a scratch-resistant layer at any of a plurality of locations within the structure. In addition, the optical structure of these cover articles may include a plurality of alternating high refractive index layers and low refractive index layers, wherein each high refractive index layer and scratch-resistant layer include a nitride or an oxynitride, and each low refractive index layer includes an oxide.

[0046] Generally, these covered articles include functional coatings (e.g., easy-to-clean coatings including fluorinated materials) with high durability, such as a water contact angle greater than 95° after 1000 cycles in a steel wool abrasion test (see Figure 3A and 3B, and the corresponding description later in this disclosure). It is worth noting that the durability of the functional coating of these cover articles may be driven or otherwise affected by the surface roughness of their optical structures. For example, aspects of the cover articles of the present disclosure are configured such that the outer surface of the optical coating of the optical structure has a surface roughness (Ra) of less than 1.5 nm, less than 1.2 nm, or even less than 1.0 nm. In some aspects, the functional coating of the cover article is particularly durable, with a water contact angle still greater than 100° or even 105° after 2000 cycles or even 3000 cycles in a steel wool abrasion test.

[0047] In terms of mechanical properties, the cover articles of the present disclosure and / or the optical structures of these cover articles may exhibit a maximum hardness of 10 GPa or greater, or 12 GPa or greater (or in some cases even greater than 14 GPa), as measured by the Berkovich hardness test along an indentation depth of 50 nm or greater. In terms of optical properties, the cover articles of the present disclosure may exhibit a first surface average bright reflectance of less than 10%, less than 5%, or even less than 1% at any incident angle from normal or near normal (e.g., 5°) to about 20° at wavelengths in the visible spectrum (e.g., 450 nm to 650 nm).

[0048] refer to Figure 1A and 1B The cover article 100 according to one or more embodiments includes a substrate 110, and an optical structure 120 disposed on the substrate 110, the optical structure defining an outer surface 120a and an inner surface 120b. The substrate 110 includes opposing major surfaces 112, 114. Figure 1A and 1B The optical structure 120 is shown with its inner surface 120b disposed on the first opposing major surface 112, and the optical structure disposed on the second opposing major surface 114 is not shown. However, in some embodiments, the optical structure 120 may also (or alternatively) be disposed on the second opposing major surface 114.

[0049] The optical structure 120 includes at least one layer of material. As used herein, the term "layer" may include a single layer or may include one or more sublayers. These sublayers may be in direct contact with each other. The sublayers may be formed of the same material or two or more different materials. In one or more alternative embodiments, an intermediate layer of different materials may be provided between such sublayers. In one or more embodiments, the layer may include one or more continuous and uninterrupted layers and / or one or more discontinuous and discontinuous layers (i.e., layers with different materials formed adjacent to each other). The layer or sublayer may be formed by any method known in the art, including discrete deposition or continuous deposition methods. In one or more embodiments, a continuous deposition method may be used alone or alternatively, a discrete deposition method may be used alone to form a layer.

[0050] In one or more embodiments, a single layer or multiple layers of the optical structure 120 can be deposited onto the substrate 110 by a vacuum deposition technique, such as chemical vapor deposition (e.g., plasma enhanced chemical vapor deposition (PECVD), low pressure chemical vapor deposition, atmospheric pressure chemical vapor deposition, and plasma enhanced atmospheric pressure chemical vapor deposition), physical vapor deposition (e.g., reactive or non-reactive sputtering or laser ablation), thermal evaporation or electron beam evaporation, and / or atomic layer deposition. Liquid-based methods such as spraying, dipping, spin coating, or slit coating (e.g., using sol-gel materials) can also be used. In general, vapor deposition techniques may include a variety of vacuum deposition methods that can be used to produce thin films. For example, physical vapor deposition uses a physical method (such as heating or sputtering) to generate a material vapor, which is then deposited on the object to be coated. Preferred methods for manufacturing the optical structure 120 may include reactive sputtering, metal mode reactive sputtering, and PECVD methods.

[0051] The optical structure 120 may have a thickness of about 500 nm to about 10 microns. Figure 1A and 1B In the illustrated embodiment of the cover article 100, the optical structure 120 can have a thickness of greater than or equal to about 500 nm, 600 nm, 700 nm, 750 nm, 800 nm, 900 nm, 1 micrometer (i.e., 1000 nm), 1.25 micrometers, 1.5 micrometers, 1.75 micrometers, 2 micrometers, 3 micrometers, 4 micrometers, 5 micrometers, 6 micrometers, 7 micrometers, or even 8 micrometers, and less than or equal to about 10 micrometers. For example, the optical structure 120 can have a thickness of about 500 nm, 750 nm, 1000 nm, 1250 nm, 1500 nm, 1750 nm, 2000 nm, 2500 nm, 3000 nm, 4000 nm, 5000 nm, 7500 nm, 10000 nm, and all thickness values ​​between the aforementioned ranges and sub-ranges.

[0052] In e.g. Figure 1A and 1B In the illustrated embodiment, the optical structure 120 includes an optical coating 130 that is divided into an outer structure 130a and an inner structure 130b, wherein a scratch-resistant layer 150 (as further described below) is disposed between the structures 130a and 130b. In these embodiments, the outer optical structure 130a and the inner optical structure 130b of the optical coating 130 can have the same thickness or different thicknesses and each include one or more layers.

[0053] Reference again Figure 1A and 1B In the illustrated cover article 100, the optical structure 120 includes one or more scratch-resistant layers 150. For example, Figure 1A and 1B The illustrated cover article 100 includes an optical structure 120 having a scratch resistant layer 150 disposed on the major surface 112 of the substrate 110. According to one embodiment, the scratch resistant layer 150 may include one or more materials selected from the following: Si u Al v O x N y 、Ta2O5、Nb2O5、AlN、AlN x 、SiAl x N y 、AlN x / SiAl x N y 、Si3N4、AlO x N y 、SiO x N y 、SiN y 、SiN x :H y , HfO2, TiO2, ZrO2, Y2O3, Al2O3, MoO3, diamond-like carbon, or a combination thereof. Exemplary materials used in the scratch-resistant layer 150 may include inorganic carbides, nitrides, oxides, diamond-like materials, or a combination thereof. Examples of materials suitable for the scratch-resistant layer 150 include metal oxides, metal nitrides, metal oxynitrides, metal carbides, metal oxycarbides, and / or a combination thereof. Exemplary metals include B, Al, Si, Ti, V, Cr, Y, Zr, Nb, Mo, Sn, Hf, Ta, and W. Specific examples of materials that can be used for the scratch-resistant layer 150 may include Al2O3, AlN, AlO x N y 、Si3N4、SiO x N y 、Si u Al v Ox N y , diamond, diamond-like carbon, Si x C y 、Si x O y C z 、ZrO2、TiO x N y In some embodiments, the scratch resistant layer 150 may include AlO x N y 、Si3N4、SiN y 、SiO x N y and combinations thereof.

[0054] like Figure 1A and 1B As shown in the exemplary form of the illustrated covering article 100, each scratch resistant layer 150 can be relatively thick compared to other layers (e.g., low RI layer 130A, high RI layer 130B, upper cover layer 131, etc.), such as greater than or equal to about 200nm, 250nm, 300nm, 325nm, 350nm, 375nm, 400nm, 425nm, 450nm, 475nm, 500nm, 525nm, 550nm, 575nm, 600nm, 700nm, 800nm, 900nm, 1 micron, 2 microns, 3 microns, 4 microns, 5 microns, 6 microns, 7 microns or even 8 microns. For example, the scratch resistant layer 150 can have a thickness of about 200 nm to about 10 microns, about 200 nm to about 5 microns, about 250 nm to about 10 microns, about 250 nm to about 5 microns, about 250 nm to about 2.5 microns, about 500 nm to about 10 microns, about 500 nm to 7500 nm, about 500 nm to about 6000 nm, about 500 nm to about 5000 nm, and all thickness levels and ranges between the foregoing ranges. In other embodiments, the scratch resistant layer 150 can have a thickness of about 200 nm to about 10,000 nm, about 200 nm to about 3000 nm, or about 500 nm to about 2500 nm.

[0055] like Figure 1A and 1BAs shown and summarized above, the cover article 100 of the present disclosure includes an optical structure 120, which includes an optical coating 130. In an implementation, the optical coating 130 includes one or more of an outer structure 130a and an inner structure 130b. Each of the outer structure 130a and the inner structure 130b of the optical coating 130 includes a plurality of alternating low refractive index (RI) layers 130A and high refractive index (RI) layers 130B, respectively. According to an embodiment, each of the outer structure 130a and the inner structure 130b includes a period 132 of two or more layers, such as a low RI layer 130A and a high RI layer 130B (see Figure 1A ), or a high RI layer 130B and a low RI layer 130A. In addition, each of the outer structure 130a and the inner structure 130b of the optical coating 130 may include a plurality of periods 132, such as 1 to 30 periods, 1 to 25 periods, 1 to 20 periods, and all periods within the aforementioned ranges. In addition, the number of periods 132, the number of layers of the outer structure 130a and the inner structure 130b, and / or the number of layers within a given period 132 may be different or the same. Furthermore, in some implementations, the total number of layers constituting the plurality of alternating low RI layers 130A and high RI layers 130B and the scratch resistant layer 150 can be in the range of 2 to 50 layers, 3 to 50 layers, 4 to 50 layers, 5 to 50 layers, 6 to 50 layers, 6 to 40 layers, 6 to 30 layers, 6 to 28 layers, 6 to 26 layers, 6 to 24 layers, 6 to 22 layers, 6 to 20 layers, 6 to 18 layers, 6 to 16 layers, and 6 to 14 layers, as well as all ranges and numbers of layers between the foregoing values.

[0056] For example, Figure 1A and 1B For the illustrated cover article 100, the period 132 of the outer structure 130a or the inner structure 130b may include a continuous low RI layer 130A and a high RI layer 130B (see Figure 1A ), or a continuous high RI layer 130B and a low RI layer 130A (see Figure 1B ). When multiple periods are included in either or both of the outer structure 130a and the inner structure 130b, the low RI layers 130A (denoted as "L") and the high RI layers 130B (denoted as "H") may alternate in the following layer order: L / H / L / H... or H / L / H / L..., such that the low RI layers 130A and the high RI layers 130B alternate along the physical thickness of the outer structure 130a and the inner structure 130b of the optical coating 130. In addition, the scratch-resistant layer 150 (generally including a high RI material) of the optical structure 120 may be included in the period 132 with the adjacent low RI layer 130A.

[0057] In an exemplary implementation of the covering article 100, as Figure 1AAs shown, the number of periods 132 of the outer structure 130a and the inner structure 130b of the optical coating 130 can be configured to be a total of six (6) periods 132. Specifically, the outer structure 130a includes at least five (5) layers (e.g., two (2) periods 132 of alternating low RI layers 130A and high RI layers 130B plus the upper cover layer 131), and the inner structure 130b includes at least seven (7) layers (e.g., four (4) periods 132 of eight (8) layers, alternating low RI layers 130A and high RI layers 130B and alternating low RI layers 130A and scratch resistant layers 150). That is, the inner structure 130b includes the low RI layer 130A directly on the major surface 112 of the substrate 110. Furthermore, in this implementation of the cover article 100, the optical structure 120 includes an upper cover layer 131 (similar in structure and thickness to the low RI layer 130A) on the outer structure 130a; and a scratch-resistant layer 150 between the outer structure 130a and the inner structure 130b.

[0058] In another exemplary implementation of the covering article 100, as Figure 1B As shown, the number of periods 132 of the outer structure 130a and the inner structure 130b of the optical coating 130 can be configured to be a total of six (6) periods 132. Specifically, the outer structure 130a includes at least five (5) layers (e.g., three (3) periods 132, including the scratch-resistant layer 150 and the low RI layer 130A, alternating high RI layers 130B and low RI layers 130A, and alternating high RI layers 130B and the upper cover layer 131), and the inner structure 130b includes at least six (6) layers (e.g., three (3) periods 132 of six (6) layers, alternating high RI layers 130B and low RI layers 130A). That is, the inner structure 130b includes the low RI layer 130A directly on the major surface 112 of the substrate 110. Furthermore, in this implementation of the cover article 100 , the structure and thickness of the upper cover layer 131 are similar to the low RI layer 130A, and the scratch resistant layer 150 is between the outer structure 130a and the inner structure 130b of the optical coating 130 .

[0059] According to an embodiment of the covering article 100, Figure 1B Exemplary designs of the illustrated cover articles are detailed in Table 1 below. In these four (4) designs, the optical structures 120, optical coating 130, and the configurations of the outer structures 130a and inner structures 130b are similar in design, with the high RI layer 130B disposed directly on the substrate 110. In addition, the scratch resistant layer 150 employed in these designs has the same composition (i.e., SiO 2) with different thicknesses (e.g., 500 to 2000 nm). x N y). In addition, in each configuration, the functional coating 140 is an easy-to-clean (ETC) coating including a fluorine-containing material having a thickness of about 5 to 20 nm.

[0060] Table 1: Figure 1B Exemplary configurations of the illustrated covering articles

[0061]

[0062] according to Figure 1A and 1B In some embodiments of the illustrated cover article 100, a functional coating 140 is disposed on the outermost cover layer 131 of the optical structure 120. In some embodiments, the functional coating 140 (e.g., an easy-to-clean coating 140) is disposed on the outer surface 120a of the optical coating 130. In some implementations of the cover article 100, the optical structure 120 and each high RI layer 130B of the outer structure 130a and the inner structure 130b include a nitride, a silicon-containing nitride (e.g., SiN x , Si3N4), oxynitrides or silicon-containing oxynitrides (e.g., SiAl x O y N z or SiO x N y ). In addition, according to some embodiments, the optical structure 120 and each low RI layer 130A of the outer structure 130a and the inner structure 130b include an oxide or a silicon-containing oxide (e.g., SiO2, SiO x or SiO2, doped with Al, N or F).

[0063] exist Figure 1A and 1BIn one or more embodiments of the illustrated cover article 100, the term "low RI" includes a refractive index range of about 1.3 to about 1.7 or 1.75 when used with the low RI layer 130A and / or the upper cover layer 131. In one or more embodiments, the term "high RI" includes a refractive index range of about 1.7 to about 2.5 (e.g., about 1.85 or greater) when used with the high RI layer 130B and / or the scratch-resistant layer 150. In some embodiments, the ranges of low RI and / or high RI may overlap; however, in most cases, the layers of each of the outer structure 130a and the inner structure 130b of the optical coating 130 of the optical structure 120 have a general relationship with respect to RI: low RI < high RI. In one or more embodiments, the refractive index difference between each of the low RI layer 130A (and / or the upper cover layer 131) and the high RI layer 130B (and / or the scratch-resistant layer 150) may be about 0.01 or greater, about 0.05 or greater, about 0.1 or greater, or even about 0.2 or greater.

[0064] Applies to Figure 1A and 1B Exemplary materials for the outer structure 130a and the inner structure 130b of the optical coating 130 of the optical structure 120 of the illustrated covering article 100 include, but are not limited to, SiO2, SiO x 、Al2O3、SiAl x O y 、GeO2、SiO、AlO x N y 、AlN、AlN x 、SiAl x N y 、SiN x 、SiO x N y 、SiAl x O y N z , Ta2O5, Nb2O5, TiO2, ZrO2, TiN, MgO, MgF2, BaF2, CaF2, SnO2, HfO2, Y2O3, MoO3, DyF3, YbF3, YF3, CeF3, diamond-like carbon, and combinations thereof. Some examples of materials suitable for the low RI layer 130A include, but are not limited to, SiO2, SiO x 、Al2O3、SiAl x O y 、GeO2、SiO、AlO x N y 、SiO x N y 、SiAl x O y Nz 、MgO、MgAl x O y , MgF2, BaF2, CaF2, DyF3, YbF3, YF3 and CeF3. In some implementations of the cover article 100, each of the low RI layers 130A thereof includes a silicon-containing oxide (e.g., SiO2 or SiO x The nitrogen content of the material used in the low RI layer 130A can be minimized (for example, in materials such as Al2O3 and MgAl x O y Some examples of materials suitable for the high RI layer 130B include, but are not limited to, SiAl x O y N z 、Ta2O5、Nb2O5、Nb2O x 、AlN、AlN x 、SiAl x N y 、AlN x / SiAl x N y 、Si3N4、AlO x N y 、SiO x N y 、SiN y 、SiN x :H y , HfO2, TiO2, ZrO2, Y2O3, Al2O3, MoO3 and diamond-like carbon. According to some implementation schemes, each high RI layer 130B of the outer structure 130a and the inner structure 130b includes a silicon-containing nitride or a silicon-containing oxynitride (e.g., Si3N4, SiN y or SiO x N y ). In one or more embodiments, each of the high RI layers 130B may have a high hardness (eg, a hardness greater than 8 GPa), and the high RI materials listed above may include high hardness and / or scratch resistance.

[0065] The oxygen content of the material of the high RI layer 130B can be minimized, especially in the case of SiN x In addition, the exemplary SiO x N y High RI materials may include about 0 atomic % to about 20 atomic % oxygen, or about 5 atomic % to about 15 atomic % oxygen, and 30 atomic % to about 50 atomic % nitrogen. The foregoing materials may be hydrogenated up to about 30 weight %. When a medium refractive index material is desired as a medium RI layer, some embodiments may utilize AlN and / or SiO x Ny It should be understood that the scratch resistant layer 150 may include any material disclosed as suitable for use with the high RI layer 130B.

[0066] In one or more embodiments of the cover article 100, the optical structure 120 includes a scratch-resistant layer 150 that can be integrated as a high RI layer 130B, and one or more low RI layers 130A, high RI layers 130B, and / or an upper cover layer 131 can be on the scratch-resistant layer 150. In addition, with respect to the scratch-resistant layer 150, as Figure 1A and 1B As shown, the functional coating 140 is generally located on the layer 150. Alternatively, the scratch-resistant layer 150 can be defined as the thickest high RI layer 130B in the overall optical structure 120 and / or the outer structure 130a and the inner structure 130b of the optical coating 130. Without being bound by theory, it is believed that when a relatively small amount of material is deposited on the scratch-resistant layer 150, the cover article 100 can exhibit increased hardness at the indentation depth. However, including the low RI layer 130A and the high RI layer 130B on the scratch-resistant layer 150 can enhance the optical properties of the cover article 100.

[0067] In one or more embodiments, Figure 1A and 1B The illustrated cover article 100 includes one or more functional coatings 140 disposed on the outer surface 120a of the optical coating 130 (typically the outer surface 120a of the outer structure 130a). In one or more embodiments, the functional coating 140 includes an easy-to-clean coating. Examples of suitable easy-to-clean coatings are described in U.S. Patent Application Publication No. 2014 / 0113083, entitled "Method for Making Glass Articles Having Optical Coatings and Easy-to-Clean Coatings," published on April 24, 2014, which is incorporated herein by reference in its entirety. In an implementation scheme of the cover article 100, the functional coating 140 is an easy-to-clean coating that includes a fluorine-containing material, such as a fluorinated silane. According to some embodiments, the functional coating 140 is an easy-to-clean coating that includes a perfluoropolyether (PFPE) having an alkoxysilane at the end. For example, the functional coating 140 can be an easy-to-clean coating that includes a silane-modified PFPE having a silane functional group for bonding to the outer surface 120a of the optical coating 130. According to some embodiments, the easy-to-clean coating of the functional coating 140 is made by one or more suitable methods, as understood by those skilled in the art of the present disclosure, such as dip coating, spin coating, spray coating, and physical vapor deposition.

[0068] In an implementation of the cover article 100, the functional coating 140 (e.g., an easy-to-clean coating) has a thickness in the range of about 2 nm to 75 nm, about 5 nm to about 50 nm, or about 5 nm to 25 nm. The easy-to-clean coating may replace or additionally include a low-friction coating or surface treatment. Exemplary low-friction coating materials may include diamond-like carbon, silanes (e.g., fluorosilanes), phosphonates, olefins, and alkynes.

[0069] In some embodiments, the functional coating 140 (e.g., an easy-to-clean coating) may have a thickness in the range of about 1 nm to about 40 nm, about 1 nm to about 30 nm, about 1 nm to about 25 nm, about 1 nm to about 20 nm, about 1 nm to about 15 nm, about 1 nm to about 10 nm, about 5 nm to about 50 nm, about 10 nm to about 50 nm, about 15 nm to about 50 nm, about 7 nm to about 20 nm, about 7 nm to about 15 nm, about 7 nm to about 12 nm, about 7 nm to about 10 nm, about 1 nm to about 90 nm, about 5 nm to about 90 nm, about 10 nm to about 90 nm, or about 5 nm to about 100 nm, and all ranges and sub-ranges therebetween.

[0070] The functional coating 140 may additionally include one or more scratch-resistant layers, the scratch-resistant layer including any material disclosed as being suitable for the scratch-resistant layer 150. In some embodiments, the functional coating 140 includes a combination of an easy-to-clean material and a scratch-resistant material. In one example, the combination includes an easy-to-clean material and diamond-like carbon. Such a functional coating 140 may have a thickness in the range of about 5 nm to about 20 nm. The components of the functional coating 140 may be provided in separate layers. For example, diamond-like carbon may be provided as a first layer, and an easy-to-clean material may be provided as a second layer on the first layer of diamond-like carbon. The thickness of the first layer and the second layer may be within the range provided above for the additional coating. For example, the first layer of diamond-like carbon may have a thickness of about 1 nm to about 20 nm or about 4 nm to about 15 nm (or more specifically about 10 nm), while the second layer of easy-to-clean material may have a thickness of about 1 nm to about 10 nm (or more specifically about 6 nm). The diamond-like coating may include tetrahedral amorphous carbon (Ta-C), Ta-C:H and / or aCH.

[0071] according to Figure 1A and 1BIn the illustrated embodiment of the cover article 100, each high RI layer 130B in the outer structure 130a and the inner structure 130b of the optical coating 130 of the optical structure 120 can have a physical thickness ranging from about 5 nm to 2000 nm, about 5 nm to 1500 nm, about 5 nm to 1000 nm, and all thicknesses and thickness ranges between these values. For example, these high RI layers 130B can have a physical thickness of 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 250 nm, 500 nm, 750 nm, 1000 nm, 1250 nm, 1500 nm, 1750 nm, 2000 nm, and all thickness values ​​between these levels. In addition, each high RI layer 130B of the inner structure 130b may have a physical thickness ranging from about 5 nm to 500 nm, about 5 nm to 400 nm, about 5 nm to 300 nm, and all thicknesses and thickness ranges between these values. For example, each of these high RI layers 130B may have a physical thickness of 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, and all thickness values ​​between these levels. In addition, according to Figure 1A and 1B In some embodiments of the illustrated cover article 100, each low RI layer 130A of the outer structure 130a and the inner structure 130b can have a physical thickness of about 5nm to 300nm, about 5nm to 250nm, about 5nm to 200nm, and all thicknesses and thickness ranges between these values. For example, each of these low RI layers 130A can have a physical thickness of 5nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 150nm, 200nm, 250nm, 300nm, and all thickness values ​​between these levels.

[0072] As previously described, the cover article 100 includes a functional coating 140 with high durability (e.g., an easy-to-clean coating including a fluorine-containing material). It is worth noting that the durability of the functional coating 140 of the cover article 100 of the present disclosure may be affected by the surface roughness of its optical structure 120 and / or optical coating 130. For example, an implementation of the cover article 100 is configured such that the outer surface 120a of the optical coating 130 of the optical structure 120 has a surface roughness (Ra) of less than 1.5 nm, less than 1.2 nm, or even less than 1.0 nm. According to some embodiments, the surface roughness (Ra) of the outer surface 120a of the optical coating 130 of the optical structure 120 is 1.45nm, 1.40nm, 1.35nm, 1.30nm, 1.25nm, 1.20nm, 1.15nm, 1.10nm, 1.05nm, 1.0nm, 0.9nm, 0.8nm, 0.7nm, 0.6nm, 0.5nm, and all surface roughness (Ra) values ​​between the aforementioned ranges and sub-ranges.

[0073] According to embodiments of the cover article 100 of the present disclosure, configuring or otherwise adjusting the outer surface 120a of the optical coating 130 to be smooth and have a low surface roughness can improve the durability of the functional coating 140 disposed on the outer surface 120a, as measured or evaluated using a steel wool abrasion test. Without being bound by theory, the smoother outer surface 120a of the optical coating 130 tends to improve the adhesion between the functional coating 140 (e.g., an easy-to-clean coating including a fluorine-containing material) and the optical coating 130, the optical structure 120, and the underlying substrate 110, thereby improving the durability of the functional coating 140 from a wear perspective, as measured by the steel wool abrasion test.

[0074] According to embodiments of the covered article 100 of the present disclosure, the functional coating 140 (e.g., an easy-to-clean coating including a fluorine-containing material) may exhibit a water contact angle greater than 95° in a steel wool abrasion test after 1000 cycles, 2000 cycles, or even 3000 cycles (see Figure 3A and 3B , and corresponding descriptions later in this disclosure). In some aspects, the functional coating 140 covering the article 100 is particularly durable, with a water contact angle greater than 100° or even 105° in a steel wool abrasion test after 1000 cycles, 2000 cycles, or even 3000 cycles. For example, in a steel wool abrasion test, the functional coating 140 can exhibit a contact angle greater than 95°, 100°, or 105° (and all cycles and contact angles between the aforementioned ranges) after being subjected to 1000 cycles, 1250 cycles, 1500 cycles, 1750 cycles, 2000 cycles, 2250 cycles, 2500 cycles, 2750 cycles, or even 3000 cycles.

[0075] Figure 1A and 1B The substrate 110 of the illustrated cover article 100 may include an inorganic material having an amorphous portion and a crystalline portion. The substrate 110 may be formed of an artificial material and / or a natural material (e.g., quartz). In some specific embodiments, the substrate 110 may specifically exclude polymers, plastics, and / or metal substrates. The substrate 110 may be characterized as an alkali-containing substrate (i.e., the substrate includes one or more alkalis). In some implementations, the substrate 110 includes a glass composition, a glass-ceramic composition, or a ceramic composition. In one or more embodiments, the substrate 110 exhibits a refractive index in the range of about 1.5 to about 1.6.

[0076] Suitable substrates 110 may exhibit an elastic modulus (or Young's modulus) in the range of about 60 GPa to about 130 GPa. In some cases, the elastic modulus of substrate 110 may be in the range of about 70 GPa to about 120 GPa, about 80 GPa to about 110 GPa, about 80 GPa to about 100 GPa, about 80 GPa to about 90 GPa, about 85 GPa to about 110 GPa, about 85 GPa to about 105 GPa, about 85 GPa to about 100 GPa, about 85 GPa to about 95 GPa, and all ranges and sub-ranges therebetween (e.g., ~103 GPa). In some embodiments, the elastic modulus of substrate 110 may be greater than 85 GPa, greater than 90 GPa, greater than 95 GPa, or even greater than 100 GPa. In some examples, Young's modulus may be measured by acoustic wave resonance (ASTM E1875), resonant ultrasonic spectroscopy, or nanoindentation using a Berkovich indenter.

[0077] In one or more embodiments, substrate 110 may include glass, which may be reinforced or non-reinforced. Examples of suitable glass include soda lime glass, alkali aluminosilicate glass, alkali borosilicate glass, and alkali aluminoborosilicate glass. In some variants, the glass may not contain lithium oxide. In one or more alternative embodiments, substrate 110 may include a crystalline substrate, such as a glass ceramic substrate (the glass ceramic substrate may be reinforced or non-reinforced), or may include a single crystal structure, such as sapphire. In one or more specific embodiments, substrate 110 includes an amorphous substrate (e.g., glass) and a crystalline cladding (e.g., a sapphire layer, a polycrystalline alumina layer, and / or a spinel (MgAl2O4) layer).

[0078] In one or more embodiments, the substrate 110 includes one or more glass-ceramic materials and can be reinforced or non-reinforced. In one or more embodiments, the substrate 110 may include one or more crystalline phases, such as lithium disilicate, lithium metasilicate, petalite, beta quartz and / or beta spodumene, possibly combined with residual glass in the structure. In one embodiment, the substrate 110 includes a disilicate phase. In another embodiment, the substrate 110 includes a disilicate phase and a petalite phase. According to one embodiment, the substrate 110 has a crystallinity of at least 40% by weight. In some implementations, the substrate 110 has a crystallinity of at least about 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85% or more (by weight), and the remainder is a glass phase.

[0079] According to implementations, the substrate 110 is substantially optically clear, transparent, and free of light scattering. In such embodiments, the substrate 110 may exhibit an average light transmittance over an optical wavelength range of about 80% or greater, about 81% or greater, about 82% or greater, about 83% or greater, about 84% or greater, about 85% or greater, about 86% or greater, about 87% or greater, about 88% or greater, about 89% or greater, about 90% or greater, about 91% or greater, about 92% or greater, about 93% or greater, or even about 94% or greater. In some embodiments, these light reflectance and transmittance values ​​may be total reflectance or total transmittance (taking into account the reflectance or transmittance on both major surfaces of the substrate 110) or may be observed on a single side of the substrate 110 (i.e., only on the major surface 112, without taking into account the opposite surface 114). Unless otherwise specified, the average reflectivity or transmittance of the substrate 110 alone is measured at an incident illumination angle of 0 degrees relative to the major surface 112 (however, such measurements may also be made at incident illumination angles of 45 degrees or 60 degrees).

[0080] A variety of different methods may be used to provide the substrate 110. For example, when the substrate 110 includes or consists essentially of an amorphous portion or phase such as glass, various forming methods may include float glass methods and down-draw methods such as fusion draw and slot draw.

[0081] Once formed, the substrate 110 can be strengthened to form a strengthened substrate. When the substrate 110 is chemically strengthened by an ion exchange method, the ions in the surface layer of the substrate 110 are replaced or exchanged by larger ions with the same valence or oxidation state. The ion exchange method is usually carried out by immersing the substrate in a molten salt bath, which contains larger ions and exchanges with smaller ions in the substrate. It should be understood by those skilled in the art that the parameters of the ion exchange method (including but not limited to bath composition and temperature, immersion time, the number of immersions of the substrate 110 in the salt bath (or multiple salt baths), the use of multiple salt baths, additional steps such as annealing, washing, etc.) are generally determined by the composition of the substrate 110 and the required compressive stress (CS), the depth (or layer depth) of the compressive stress layer of the substrate 110 generated by the strengthening operation. For example, the ion exchange of an alkali-containing glass ceramic or glass substrate can be achieved by immersing in at least one molten bath containing a salt, such as but not limited to nitrates, sulfates and hydrochlorides of larger alkali metal ions. The temperature of the molten salt bath is typically in the range of about 380° C. to about 530° C., while the immersion time is in the range of about 15 minutes to about 40 hours. However, temperatures and immersion times different from those described above may also be used.

[0082] The degree of chemical strengthening achieved by ion exchange can be quantified according to the parameters of central tension (CT), surface CS, depth of compression (DOC) (i.e., the point at which the stress state in the substrate changes from compression to tension) and depth of potassium ion layer (DOL). Compressive stress (including surface CS) is measured by a surface stress meter (FSM), using commercially available instruments, such as the FSM-6000 manufactured by Orihara Industrial Co., Ltd. (Japan). Surface stress measurement relies on the accurate measurement of stress optical coefficient (SOC), which is related to the birefringence of glass ceramic materials. SOC is measured according to the procedure C (glass disk method) described in ASTM standard C770-16, which is called "Standard Test Method for Measurement of Glass Stress-Optical Coefficients", and its content is incorporated herein by reference as a whole. Stress distribution can be measured using a refractive near field (RNF) method or a scattered light polarizer (SCALP) technique. When the RNF method is used to measure the pressure distribution, the RNF method uses the maximum CT value provided by SCALP. Specifically, the stress distribution measured by the RNF is force balanced and calibrated to provide a maximum CT value for the SCALP measurement. The RNF method is described in U.S. Patent No. 8,854,623, issued on October 7, 2014, entitled "System and Method for Measuring Distribution Characteristics of Glass Samples," which is incorporated herein by reference in its entirety. Specifically, the RNF method includes placing a covered article near a reference block, generating a polarization switching beam that switches between orthogonal polarizations at a rate between 1 Hz and 50 Hz, measuring the amount of power in the polarization switching beam and generating a polarization switching reference signal, wherein the amount of power measured in each orthogonal polarization is within 50% of each other. The method also includes transmitting the polarization switching beam through the sample and the reference block to enter different depths of the sample, and then relaying the transmitted polarization switching beam to a signal photodetector using a relay optical system, wherein the signal photodetector generates a polarization switching detector signal. The method also includes dividing the detector signal by the reference signal to form a standardized detector signal, and determining the distribution characteristics of the sample based on the standardized detector signal. The maximum CT value is measured using a scattered light polarizer (SCALP) technique known in the art.

[0083] In one embodiment of the cover article 100 (see Figure 1A and 1B), the strengthening substrate 110 can have a surface CS of 200 MPa or more, 250 MPa or more, 300 MPa or more, or 350 MPa or more. In another implementation, the strengthening substrate 110 can exhibit a surface compressive stress (CS) of about 200 MPa to about 600 MPa, about 200 MPa to about 500 MPa, about 200 MPa to about 400 MPa, about 225 MPa to about 400 MPa, 250 MPa to about 400 MPa, and all CS sub-ranges and values ​​within the foregoing ranges. The reinforcement substrate 110 may have a DOL of 1 μm to 5 μm, 1 μm to 10 μm, or 1 μm to 15 μm, and / or a central tension (CT) of 50 MPa or greater, 75 MPa or greater, 100 MPa or greater, 125 MPa or greater (e.g., 80 MPa, 90 MPa, or 100 MPa or greater) but less than 250 MPa (e.g., 200 MPa or less, 175 MPa or less, 150 MPa or less, etc.).

[0084] The depth of compression (DOC) of the substrate 110 may be 0.1·(thickness of the substrate (t)) to about 0.25·t, such as about 0.15·t to about 0.25·t or about 0.15·t to about 0.20·t, and all DOC values ​​between the foregoing ranges. For example, the substrate 110 may have a DOC of 20% of the thickness of the substrate, while the DOC of the ion-exchanged glass substrate is 15% or less. In an embodiment, the depth of compression of the substrate material may be from 8% to 20% of the thickness of the substrate 110. It should be noted that the foregoing DOC values ​​are measured with respect to one of the major surfaces 112 or 114 of the substrate 110. Therefore, for a substrate 110 having a thickness of 600 μm, the DOC may be 20% of the thickness of the substrate, from 120 μm to each of the major surfaces 112, 114 of the substrate 110, or a total of 240 μm for the entire substrate. In one or more specific embodiments, the reinforced substrate 110 can exhibit one or more of the following mechanical properties: surface CS of about 200 MPa to about 400 MPa, DOL greater than 30 μm, DOC of about 0.08·t to about 0.25·t, and CT of about 80 MPa to about 200 MPa.

[0085] According to embodiments of the present disclosure, the substrate 110 (without the optical structure 120 disposed thereon for measurement purposes) can exhibit a maximum hardness of 8.5 GPa or greater, 9 GPa or greater, or 9.5 GPa or greater (or in some cases even greater than 10 GPa), as measured by the Berkovich hardness test over an indentation depth range of 100 nm to about 500 nm in the substrate 110. For example, the substrate 110 can exhibit a maximum hardness of 8.5 GPa, 8.75 Gpa, 9 Gpa, 9.25 Gpa, 9.5 Gpa, 9.75 Gpa, 10 GPa, and higher hardness levels, as measured by the Berkovich hardness test over an indentation depth range of 100 nm to about 500 nm in the substrate 110.

[0086] Exemplary glasses that can be used for the substrate 110 may include an alkali aluminosilicate glass composition or an alkali aluminoborosilicate glass composition, but other glass compositions are also contemplated. Such glass compositions can be chemically strengthened by ion exchange methods. An exemplary glass composition includes SiO2, B2O3, and Na2O, wherein (SiO2+B2O3)≥66mol.%, and Na2O≥9mol.%. In one embodiment, the glass composition includes at least 6 wt.% aluminum oxide. In another embodiment, the substrate includes a glass composition having one or more alkaline earth oxides such that the content of the alkaline earth oxides is at least 5 wt.%. In some embodiments, suitable glass compositions also include at least one of K2O, MgO, and CaO. In a particular embodiment, the glass composition used in the substrate may include 61-75 mol.% SiO2; 7-15 mol.% Al2O3; 0-12 mol.% B2O3; 9-21 mol.% Na2O; 0-4 mol.% K2O; 0-7 mol.% MgO; and 0-3 mol.% CaO.

[0087] Another exemplary glass composition suitable for substrate 110 includes: 60-70 mol.% SiO2; 6-14 mol.% Al2O3; 0-15 mol.% B2O3; 0-15 mol.% Li2O; 0-20 mol.% Na2O; 0-10 mol.% K2O; 0-8 mol.% MgO; 0-10 mol.% CaO; 0-5 mol.% ZrO2; 0-1 mol.% SnO2; 0-1 mol.% CeO2; less than 50 ppm As2O3; and less than 50 ppm Sb2O3; wherein 12 mol.% ≤ (Li2O + Na2O + K2O) ≤ 20 mol.% and 0 mol.% ≤ (MgO + CaO) ≤ 10 mol.%.

[0088] Yet another exemplary glass composition suitable for substrate 110 includes: 63.5-66.5 mol.% SiO2; 8-12 mol.% Al2O3; 0-3 mol.% B2O3; 0-5 mol.% Li2O; 8-18 mol.% Na2O; 0-5 mol.% K2O; 1-7 mol.% MgO; 0-2.5 mol.% CaO; 0-3 mol.% ZrO2; 0.05-0.25 mol.% SnO2; 0.05-0.5 mol.% CeO2; less than 50 ppm As2O3; and less than 50 ppm Sb2O3; wherein 14 mol.% ≤ (Li2O + Na2O + K2O) ≤ 18 mol.% and 2 mol.% ≤ (MgO + CaO) ≤ 7 mol.%.

[0089] In a particular embodiment, an alkali aluminosilicate glass composition suitable for use in substrate 110 includes aluminum oxide, at least one alkali metal, and in some embodiments greater than 50 mol.% SiO2, in other embodiments at least 58 mol.% SiO2, and in yet other embodiments at least 60 mol.% SiO2, wherein the ratio (Al2O3+B2O3) / ∑ modifier (i.e., the sum of modifiers) is greater than 1, wherein each component in the ratio is expressed in mol.%, and the modifier is an alkali metal oxide. In a particular embodiment, this glass composition includes: 58-72 mol.% SiO2; 9-17 mol.% Al2O3; 2-12 mol.% B2O3; 8-16 mol.% Na2O; and 0-4 mol.% K2O, wherein the ratio (Al2O3+B2O3) / ∑ modifier (i.e., the sum of modifiers) is greater than 1.

[0090] In yet another embodiment, the substrate 110 may include an alkali aluminosilicate glass composition comprising: 64-68 mol.% SiO2; 12-16 mol.% Na2O; 8-12 mol.% Al2O3; 0-3 mol.% B2O3; 2-5 mol.% K2O; 4-6 mol.% MgO; and 0-5 mol.% CaO, wherein: 66 mol.%≤SiO2+B2O3+CaO≤69 mol.%; Na2O+K2O+B2O3+MgO+CaO+SrO>10 mol.%; 5 mol.%≤MgO+CaO+SrO≤8 mol.%; (Na2O+B2O3)-Al2O3≤2 mol.%; 2 mol.%≤Na2O-Al2O3≤6 mol.%; and 4 mol.%≤(Na2O+K2O)-Al2O3≤10 mol.%.

[0091] In an alternative embodiment, the substrate 110 may include an alkali aluminosilicate glass composition including: 2 mol.% or more of Al2O3 and / or ZrO2, or 4 mol.% or more of Al2O3 and / or ZrO2.

[0092] When the substrate 110 comprises a crystalline substrate, the substrate may comprise a single crystal, which may comprise Al2O3. Such a single crystal substrate is referred to as sapphire. Other materials suitable for the crystalline substrate include polycrystalline aluminum oxide layers and / or spinel (MgAl2O4).

[0093] Optionally, the substrate 110 can be crystalline and include a glass ceramic substrate, which can be strengthened or non-strengthened. Examples of glass ceramics suitable for the substrate 110 can include Li2O-Al2O3-SiO2 system (i.e., LAS system) glass ceramics, MgO-Al2O3-SiO2 system (i.e., MAS system) glass ceramics, and / or glass ceramics including a main crystalline phase containing β-quartz solid solution, β-spodumene solid solution, cordierite and lithium disilicate. The chemical strengthening method disclosed herein can be used to strengthen the glass ceramic substrate. In one or more embodiments, the MAS system glass ceramic substrate can be strengthened in a Li2SO4 molten salt, where 2Li + Exchange Mg 2+ .

[0094] According to one or more embodiments, the substrate 110 may have a physical thickness in the range of about 100 μm to about 5 mm in various portions of the substrate 110. Exemplary physical thickness ranges of the substrate 110 are, for example, about 100 μm to about 500 μm (e.g., 100, 200, 300, 400, or 500 μm), about 500 μm to about 1000 μm (e.g., 500, 600, 700, 800, 900, or 1000 μm), and about 500 μm to about 1500 μm (e.g., 500, 750, 1000, 1250, or 1500 μm). In some embodiments, the substrate 110 may have a physical thickness greater than about 1 mm (e.g., about 2, 3, 4, or 5 mm). In one or more specific embodiments, the substrate 110 may have a physical thickness of 2 mm or less, or less than 1 mm. The substrate 110 may be acid polished or otherwise treated to remove or reduce the effects of surface imperfections.

[0095] for Figure 1A and 1BThe hardness of the depicted cover article 100, in general, in a nanoindentation measurement method (such as by using a Berkovich indenter), when the optical structure 120 is harder than the underlying substrate, the measured hardness may initially appear to increase due to the formation of a plastic zone at a shallow indentation depth (e.g., less than 25nm or less than 50nm), and then increase and reach a maximum or plateau at a deeper indentation depth (e.g., 50nm to about 500nm or 1000nm). Thereafter, the hardness begins to decrease at even deeper indentation depths due to the influence of the underlying substrate. The same effect can be seen when the substrate 110 utilized has a greater hardness than the optical structure 120; however, the hardness increases at deeper indentation depths due to the influence of the underlying substrate.

[0096] Further references Figure 1A and 1B The illustrated covered article 100 can select indentation depth ranges and hardness values ​​within certain indentation depth ranges to identify specific hardness responses of the optical structure 120, optical coating 130, and its outer structure 130a and inner structure 130b layers described herein, without being affected by the underlying substrate 110. When the hardness of the optical structure 120 (when disposed on the substrate 110) is measured with a Berkovich indenter, the permanent deformation region (plastic zone) of the material is related to the hardness of the material. During indentation, the elastic stress field extends far beyond this permanent deformation region. As the indentation depth increases, the apparent hardness and modulus are affected by the interaction of the stress field with the underlying substrate 110. The effect of the substrate 110 on the hardness occurs at deeper indentation depths (i.e., typically at depths greater than about 10% of the total thickness of the optical structure 120). In addition, an additional complicating factor is that the hardness response requires a certain minimum load to exert full plasticity during the indentation process. Before reaching a certain minimum load, the hardness generally shows an increasing trend.

[0097] At small indentation depths (which can also be characterized as small loads) in the optical structure 120 (e.g., up to about 50 nm), the apparent hardness of the material appears to increase dramatically with respect to the indentation depth. This small indentation depth range does not represent a true indicator of hardness, but rather reflects the development of the plastic zone described above, which is related to the finite radius of curvature of the indenter. At moderate indentation depths, the apparent hardness approaches a maximum level. At deeper indentation depths, the effect of the substrate 110 becomes more pronounced as the indentation depth increases. Once the indentation depth exceeds about 30% of the optical coating thickness, the hardness may begin to drop dramatically.

[0098] In one or more embodiments, Figure 1A and 1BAs depicted, the cover article 100 and / or the optical structure 120 may exhibit a maximum hardness of about 10 GPa or greater, about 11 GPa or greater, or about 12 GPa or greater, 13 GPa or greater, or 14 GPa or greater, as measured by the Berkovich Indenter Hardness Test along an indentation depth of 50 nm or greater, about 100 nm to about 500 nm, or about 100 nm to about 900 nm from the outer surface 120a of the optical structure 120. For example, the cover article 100 and / or its optical structure 120 may exhibit a maximum hardness of 10 GPa, 11 GPa, 12 GPa, 13 GPa, 14 GPa, 15 GPa, 16 GPa, 17 GPa, 18 GPa, 19 GPa, 20 GPa, or greater, as measured by the Berkovich Indenter Hardness Test along an indentation depth of 50 nm or greater from the outer surface 120a of the optical structure 120. In some embodiments, the maximum hardness of the cover article 100 and / or the optical structure 120 is greater than 10 GPa, 11 GPa, 12 GPa, 13 GPa, 14 GPa, 15 GPa, 16 GPa, 17 GPa, 18 GPa or 19 GPa at an indentation depth of 50 nm or 100 nm. In some implementation schemes, the maximum hardness of the cover article 100 and / or the optical structure 120 is greater than 10 GPa, 12 GPa, 14 GPa, 16 GPa, 17 GPa, 18 GPa or 19 GPa at an indentation depth of 500 nm.

[0099] Further references Figure 1A and 1B The hardness of the depicted cover article 100 and / or optical structure 120 may specifically characterize the hardness of the material of the high RI layer 130B and / or the scratch resistant layer 150. In some embodiments, the maximum hardness of the high RI layer 130B and / or the scratch resistant layer 150 may be about 10 GPa or greater, about 12 GPa or greater, about 15 GPa or greater, about 18 GPa or greater, or even about 20 GPa or greater, as measured by the Berkovich indenter hardness test. The hardness of a given layer (e.g., high RI layer 130B) may be measured by analyzing the cover article 100, wherein the layer measured is the uppermost layer in the optical structure 120. If the layer whose hardness is to be measured is a buried layer, the hardness of the buried layer may be measured by producing a transparent article that does not include the upper layer and then testing the hardness of the article. This measured hardness value can be exhibited by the covering article 100, the optical structure 120, the optical coating 130, the outer structure 130a and the inner structure 130b, the high RI layer 130B and / or the scratch-resistant layer 150 along an indentation depth of about 50 nm or greater or about 100 nm or greater, and can be maintained above a certain hardness value within a continuous range of indentation depths.

[0100] According to the implementation scheme, Figure 1A and Figure 1B The illustrated cover article 100 may exhibit an average dual-side or dual-surface (i.e., through the two major surfaces 112, 114 of the substrate 110) bright light transmittance (or average transmittance) in the visible spectrum in the range of 400 to 700 nm or 450 to 650 nm of light wavelength at normal incidence angles of 0 to 10 degrees, 0 to 20 degrees, 5 to 20 degrees, 0 to 30 degrees, 0 to 40 degrees, 0 to 50 degrees, or even 0 to 60 degrees of about 80% or more, about 85% or more, about 90% or more, about 91% or more, about 92% or more, about 93% or more, or even about 94% or more.

[0101] According to some implementation plans, Figure 1A and 1B The illustrated cover article 100 may exhibit a transmission color of a D65 illuminant, as given by √(a* 2 +b* 2 ), less than 4, less than 3.5, less than 3, less than 2.5, less than 2, less than 1.5, or even less than 1, as measured at normal incidence, 0 to 10 degrees, or at all angles of incidence from 0 to 90 degrees. For example, the cover article 100 can exhibit a transmittance color of less than 4, 3.75, 3.5, 3.25, 3, 2.75, 2.5, 2.25, 2, 1.9, 1.8, 1.7, 1.6, 1.5, 1.4, 1.3, 1.2, 1.1, 1.0, 0.9, 0.8, 0.7, 0.6, 0.5, or even lower, as measured at normal incidence, 0 to 10 degrees, 5 to 20 degrees, or at all angles of incidence from 0 to 90 degrees.

[0102] According to the implementation scheme, Figure 1A and Figure 1B The illustrated cover article 100 may exhibit an average single-side or first surface (i.e., through one of the major surfaces 112, 114 of the substrate 110) bright reflectance (or average reflectance) (i.e., first surface or dual surface reflectance) of less than 20%, less than about 15%, less than about 13%, less than about 12%, less than about 10%, less than about 8%, less than about 6%, less than about 4%, less than about 2%, or even less than 1% at normal incidence, 0 to 10 degrees or 5 to 20 degrees, through one or both major surfaces of the substrate 110 in the wavelength range of light from 400 to 700 nm or 450 to 650 nm. For example, the cover article 100 may exhibit a first surface average bright reflectance of less than 20%, less than 15%, less than 10%, less than 5%, less than 2%, less than 1%, or even less than 0.8%, as measured at an incident angle of 0 to 10 degrees or 5 to 20 degrees.

[0103] According to some embodiments, Figure 1A and 1B The illustrated cover article 100 may exhibit a first surface (ie, through one of the major surfaces 112, 114 of the substrate 110) with a reflected color of a D65 illuminant, as given by √(a* 2 +b* 2 ), less than 10, less than 8, less than 6, less than 4, less than 3, or even less than 2, as measured at normal incidence, 0 to 10 degrees, 5 to 20 degrees, or at all angles of incidence from 0 to 90 degrees. For example, the cover article 100 can exhibit a reflected color of less than 10, 9, 8, 7, 6, 5, 4, 3.75, 3.5, 3.25, 3, 2.75, 2.5, 2.25, 2, 1.9, 1.8, 1.7, 1.6, 1.5, 1.4, 1.3, 1.2, 1.1, 1, or even lower, as measured at normal incidence, 0 to 10 degrees, or at all angles of incidence from 0 to 90 degrees.

[0104] Reference now Figures 2A-2C , provides schematic cross-sectional views of an easy-to-clean (ETC) coating on a substrate and an easy-to-clean coating on each of two antireflective films having different surface roughness levels on the substrate. Figure 2A , comparative cover article 200a (Comparative Example 1A) is shown as being directly on a strengthened glass substrate (e.g., Gorilla The ETC coating is disposed on a main surface of the main surface, the main surface having a surface roughness (Ra) of about 0.2 to 0.5 nm. Figure 2B , comparative cover article 200b (Comparative Example 1B) is depicted as an ETC coating disposed directly on the outer surface of an anti-reflective (AR) film disposed on a major surface of a strengthened glass substrate. In addition, the outer surface of the AR film (thickness of ˜0.5 μm) had a surface roughness (Ra) of approximately 1.5 nm. Figure 2C , comparative cover article 200c (Comparative Example 1C) is depicted as an ETC coating disposed directly on the outer surface of an anti-reflective (AR) film disposed on a major surface of a strengthened glass substrate. In addition, the outer surface of the AR film (thickness ~2.0 μm) has a surface roughness (Ra) of about 2.5 nm.

[0105] Reference again Figures 2A-2C, the durability of the ETC coating of the comparative cover article 200a far exceeds the durability of the ETC coating of the comparative cover articles 200b and 200c. Without being bound by theory, it is believed that the ETC coating of the comparative article 200a exhibits superior durability than the ETC coating of the comparative articles 200b and 200c because the surface to which the ETC coating in the comparative article 200a is bonded is much smoother than the bonding surface of the ETC coating of the comparative articles 200b and 200c. These observations are consistent with the approach taken by the cover article 100 of the present disclosure, in which the smoothness of the outer surface 120a of the optical coating 130 is maximized to improve the durability of the functional coating 140 (e.g., ETC coating).

[0106] Reference now Figure 3A , provides a schematic cross-sectional view of an apparatus 300a for conducting a steel wool abrasion test on a cover article (e.g., the cover article 100 of the present disclosure) (see also Figure 1A and 1B As used herein, "steel wool abrasion test" or "steel wool test" interchangeably refers to the use of a test apparatus 300a to determine the optical structure 120 of a cover article 100 of the present disclosure (e.g., Figure 1A and 1B The durability test of the functional coating 140 (e.g., ETC coating) disposed on the outer surface 120a of the optical coating 130 shown in FIG. 1 and on the substrate 110. At the beginning of the steel wool abrasion test, the water contact angle of the water droplet 320 is measured one or more times on the cover article 100 to obtain a reliable initial water contact angle 330 (see FIG. 3 ). Figure 3B ). These water contact angle measurements can be performed using a Kruss GmbH DSA100 Drop Shape Analyzer or similar instrument. After measuring the initial water contact angle, a Bonstar #0000 steel wool pad 310 is fixed to Industries 5750 Linear Abrader Instrument Arm (see Figure 3A ). The steel wool pad 310 is then brought into contact with the covered article 100 (on the ETC coating 140) under a load of 1 kg and reciprocated at 60 cycles / minute. The average contact angle 330 of the sample is then measured after 1000 cycles, 1500 cycles, 2000 cycles, 3000 cycles, 3500 cycles, and / or another specified duration.

[0107] Reference now Figure 4 According to an embodiment of the present disclosure, a method for manufacturing a covering article 100 (see Figure 1A and 1Band corresponding description). According to one embodiment, method 400 for manufacturing a covered article (e.g., covered article 100) includes step 410 of providing a substrate (e.g., substrate 110) having a major surface. The method also includes an optional step 420 of washing the major surface of the substrate using a suitable method (e.g., a water cleaning method using deionized water) according to the composition of the substrate. Method 400 also includes step 430 of depositing an optical structure (e.g., optical structure 120) on the major surface of the substrate. More specifically, step 430 can be used to deposit the various layers constituting the optical structure 120, including the scratch-resistant layer 150, the optical coating 130, and the upper cover layer 131. As will be appreciated by those skilled in the art of the present disclosure, various sputtering methods can be used in step 430, including plasma enhanced chemical vapor deposition (PECVD), reactive sputtering methods, chemical vapor deposition (CVD), physical vapor deposition (PVD), and the like. Finally, step 430 is performed to form an optical structure on the substrate, the optical structure comprising an optical coating (e.g., optical coating 130), the optical coating having an outer surface (e.g., outer surface 120a), the outer surface being opposite to the main surface of the substrate on which the optical structure is disposed. In a preferred aspect of method 400, step 430 is performed using a reactive sputtering method, and the optical structure formed by step 430 comprises a plurality of continuous layers.

[0108] Reference again Figure 4 The illustrated method 400 for manufacturing the cover article 100 further includes a step 440 of modifying the outer surface of the optical coating (e.g., the outer surface 120a of the optical coating 130), wherein after the step of modifying the outer surface is completed, the outer surface of the optical coating has a surface roughness (Ra) of less than 1.5 nm. In some aspects, the step 440 of modifying the outer surface of the optical coating can be performed using one or more of an inductively coupled plasma (ICP) method, an ion beam (IB) method, a chemical etching method (e.g., plasma treatment in a CF4 atmosphere), and a mechanical polishing method (e.g., using a CeO2 polishing medium). In a preferred embodiment, the step 440 of modifying the outer surface of the optical coating can be performed using a plasma treatment method and / or a mechanical polishing method. In an embodiment, as Figure 4A As shown, step 440 of modifying the outer surface of the optical coating may be performed in two steps 440a and 440b to remove a few nanometers of thickness of the optical coating (step 440a) and reduce the roughness of the outer surface of the optical coating and further reduce its thickness (step 440b).

[0109] Still refer to Figure 4The method 400 for manufacturing the cover article 100 is shown, and the method further includes a step 450 of depositing a functional coating (e.g., the functional coating 140, such as an easy-to-clean (ETC) coating) on ​​the outer surface of the optical coating after the step 440 of modifying the outer surface. In addition, the ETC coating formed in step 450 includes a fluorine-containing material. In addition, the method 400 includes a step 460 of curing the ETC coating. A person skilled in the art of the present disclosure can set the time and temperature of step 460 according to the composition of the functional coating cured according to this step. In addition, after completing step 460 of method 400, the resulting cover article (e.g., Figure 1A and 1B The covered article 100 depicted in FIG. 1 includes an optical structure having a physical thickness greater than or equal to 500 nm and a maximum hardness of 10 GPa or greater, as measured by a Berkovich indenter test along an indentation depth of 50 nm or greater on the outer surface of the optical coating. In addition, the scratch-resistant layer of the optical structure has a physical thickness of 200 nm to 5000 nm. In addition, after step 460 of curing the ETC coating, the functional coating (e.g., the ETC coating) exhibits a water contact angle greater than 95° after 1000 cycles in a steel wool abrasion test.

[0110] The cover article 100 disclosed herein (e.g., Figure 1A and 1B The present invention (as shown) can be incorporated into equipment products, for example, equipment products with displays (or display equipment products) (for example, consumer electronics, including mobile phones, tablet computers, computers, navigation systems, wearable devices (for example, watches), etc.), augmented reality displays, head-up displays, glasses-based displays, architectural equipment products, transportation equipment products (for example, cars, trains, airplanes, ships, etc.), household equipment products, or any device that benefits from low reflectivity, scratch resistance, abrasion resistance, damage resistance, or a combination thereof. Figure 5A and 5B An exemplary device article (e.g., with Figure 1A and 1B Specifically, Figure 5A and 5B A consumer electronic device 500 is shown, comprising a housing 502 having a front surface 504, a rear surface 506, and sides 508; electronic components (not shown) at least partially or completely within the housing and including at least a controller, memory, and display 510 at or adjacent to the housing front surface; and a cover substrate 512 at or above the housing front surface such that it is above the display. In some embodiments, cover substrate 512 can include any cover article 100 disclosed herein.

[0111] Example

[0112] The following examples describe various features and advantages provided by the present disclosure but are in no way intended to limit the present invention and the appended claims.

[0113] In these examples (Examples 1A-1C; and Examples 2A-2E) and comparative examples (i.e., Comparative Examples 1A-1D; and Comparative Example 2), covered articles were formed according to the methods of the present disclosure, as depicted in Tables 2 and 3 below. More specifically, unless otherwise stated, the optical structures of these examples were formed using a metal mode reactive sputtering method in a rotary drum coater that independently controls the metal deposition and sputtering powers in the inductively coupled plasma (ICP) (gas reaction) zone. The reactive gas (e.g., N2 gas and O2 gas) is separated from the metal target in the ICP (gas reaction) zone. In addition, the metal sputtering zone only uses an inert gas flow (i.e., Ar gas).

[0114] Comparative Example 1

[0115] A comparative cover article comprising a strengthened glass substrate was prepared for this example, and its structure was Figures 2A-2C , as also described previously in this disclosure. The glass substrate is an ion-exchanged aluminosilicate glass substrate having a thickness of 550 μm and a refractive index of 1.509. The composition of the substrate is as follows: 61.81% SiO2; 3.9% B2O3; 19.69% Al2O3; 12.91% Na2O; 0.018% K2O; 1.43% MgO; 0.019% Fe2O3; and 0.223% SnO2 (wt %, based on oxides). A molten salt bath is used to strengthen the substrate to achieve a maximum compressive stress (CS) of 850 MPa and a depth of layer (DOL) of 40 μm.

[0116] Also like Figures 2A-2CAs shown, three groups of comparative cover articles were prepared according to this embodiment. Specifically, one group was prepared as an easy-to-clean (ETC) coating on a substrate (Comparative Example 1A), and two groups were prepared as easy-to-clean coatings on each of two anti-reflective films having different surface roughness levels on a substrate (Comparative Examples 1B and 1C). For Comparative Example 1A comparative cover article 200a, the major surface of the substrate had a surface roughness (Ra) of about 0.2 to 0.5 nm. For Comparative Example 1B comparative cover article 200b, the ETC coating was directly disposed on the outer surface of an anti-reflective (AR) film (thickness of ~0.5 μm), and the anti-reflective (AR) film was disposed on the major surface of a strengthened glass substrate having a surface roughness (Ra) of about 1.5 nm. For Comparative Example 1C comparative cover article 200c, the ETC coating was directly disposed on the outer surface of an anti-reflective (AR) film (thickness of ~2.0 μm), and the anti-reflective (AR) film was disposed on the major surface of a strengthened glass substrate having a surface roughness (Ra) of about 2.5 nm.

[0117] refer to Figure 6 , provides a graph of average water contact angle measurements after subjecting samples of various comparative cover articles from this Example to 0, 1000, 2000 and 3000 cycles of steel wool abrasion testing (using a Bonstar #0000 abrader, 1 kg load, 60 cycles / minute and 15 mm stroke length). Figure 6 As shown, the durability of the ETC coating of the comparative cover article Comparative Example 1A far exceeds the durability of the ETC coating of the comparative cover articles Comparative Examples 1B and 1C. That is, the ETC coatings of Comparative Examples 1B and 1C began to show some decrease in contact angle at 2000 and 3000 cycles in the steel wool abrasion test. In addition, as previously described, the surface roughness of the AR film deposited with the ETC coating is significantly higher in Comparative Examples 1B and 1C than in the control comparative article in which the ETC coating is directly deposited on a glass substrate having a lower inherent surface roughness.

[0118] Example 1

[0119] For this example, a covered article including a strengthened glass substrate was prepared, the structure of which is depicted in Table 2 below. The glass substrate was an ion-exchanged aluminosilicate glass substrate having a thickness of 550 μm and a refractive index of 1.509. The composition of the substrate was as follows: 61.81% SiO2; 3.9% B2O3; 19.69% Al2O3; 12.91% Na2O; 0.018% K2O; 1.43% MgO; 0.019% Fe2O3; and 0.223% SnO2 (wt %, based on oxides). The substrate was strengthened using a molten salt bath to achieve a maximum compressive stress (CS) of 850 MPa and a depth of layer (DOL) of 40 μm.

[0120] In this embodiment, each sample listed in Table 2 below is a cover article having an anti-reflective optical structure having a thickness of about 0.5 μm disposed on a glass substrate. In each embodiment, an ETC coating is disposed on an AR film structure and cured according to the method disclosed herein. More specifically, a comparative cover article (Comparative Example 1D) was manufactured without any surface treatment of the outer surface of the AR film structure before the ETC coating was applied and cured. In contrast, each of the inventive cover article embodiments (Examples 1A-1C) was prepared in a manner similar to the comparative cover article (Comparative Example 1D), except that the outer surface of the AR film of the inventive embodiment was subjected to an inductively coupled plasma (ICP) surface treatment step according to the method disclosed herein in accordance with the parameters listed in Table 2 below.

[0121] Table 2 - Covered Article Processing Conditions for Examples 1A-1C and Comparative Example 1D

[0122]

[0123]

[0124] Reference now Fig. 7A , provides a graph of surface roughness of the outer surface of the optical coating of the covered article of the embodiment after being subjected to plasma treatment at various power levels versus treatment time. From this graph, it can be clearly seen that the surface roughness of the comparative example (Comparative Example 1D) is the highest, and the surface roughness of the examples of the present invention (Examples 1A-1C) is greatly reduced as the surface treatment duration and ICP power level change.

[0125] Reference now Figure 7B , provides a graph of the reflectance of the first surface of the cover article of this embodiment versus visible wavelength. It is apparent from this graph that the reflectance levels of the comparative cover article and the inventive cover article of this embodiment are substantially similar. Therefore, the surface treatment methods used in the inventive embodiments of this sample do not significantly reduce or otherwise affect the reflectance in these embodiments.

[0126] Reference now Figure 7C and 7D , provide graphs of the average water contact angles after subjecting the covered article samples of this embodiment to 2000 and 3000 steel wool abrasion tests (represented as "CA(°)SW 2K" and "CA(°)SW 3K", respectively, in Table 2 above). It can be clearly seen from these graphs that there is a clear correlation between the surface roughness of the outer surface of the optical structure and the durability of the upper ETC coating. That is, the comparative covered article (Comparative Example 1D) has the highest surface roughness level (i.e., about 1.8nm) on the surface provided with the ETC, and has the lowest water contact angle after 2000 and 3000 cycles in the steel wool abrasion test. In contrast, the covered articles of the present invention (Examples 1A-1C) having a low surface roughness level (i.e., less than 1.5nm) exhibit the highest water contact angles (≥104°) after 2000 and 3000 cycles in the steel wool abrasion test.

[0127] Example 2

[0128] For this example, a covered article including a strengthened glass substrate was prepared, the structure of which is depicted in Table 3 below. The glass substrate was an ion-exchanged aluminosilicate glass substrate having a thickness of 550 μm and a refractive index of 1.509. The composition of the substrate was as follows: 61.81% SiO2; 3.9% B2O3; 19.69% Al2O3; 12.91% Na2O; 0.018% K2O; 1.43% MgO; 0.019% Fe2O3; and 0.223% SnO2 (wt %, based on oxides). The substrate was strengthened using a molten salt bath to achieve a maximum compressive stress (CS) of 850 MPa and a depth of layer (DOL) of 40 μm.

[0129] In this embodiment, each sample listed in Table 3 below is a cover product having an anti-reflective optical structure having a thickness of about 2 μm disposed on a glass substrate. In each embodiment, an ETC coating is disposed on the AR film structure and cured according to the method disclosed herein. More specifically, a comparative cover product (Comparative Example 2) was manufactured without any surface treatment of the outer surface of the AR film structure before the ETC coating was applied and cured. Instead, each of the cover product embodiments of the present invention (Examples 2A-2E) was prepared in a manner similar to the comparative cover product (Comparative Example 2), except that the outer surface of the AR film of the embodiment of the present invention was subjected to a mechanical polishing surface treatment step according to the method disclosed herein in accordance with the parameters listed in Table 3 below. Specifically, the number of polishing cycles and the polishing medium concentration of the CeO2 polishing medium used in the surface treatment step are shown in Table 3 below. It is apparent from Table 3 that a surface roughness level of the outer surface of the AR film of less than 1.8 nm can be achieved by mechanical polishing (Examples 2A-2E), while a surface roughness level of less than 1.5 nm can be achieved at a CeO2 concentration of 10 wt% with 15 polishing cycles or longer.

[0130] Table 3 - Examples 2A-2E and Comparative Example 2 Covered Article Processing Conditions

[0131]

[0132] The various features described in this specification may be combined in any and all combinations, for example, as listed in the following embodiments.

[0133] Embodiment 1. Provides a covering article, the covering article comprising: a substrate having a major surface; an optical structure disposed on the major surface, wherein the optical structure comprises an optical coating and a scratch-resistant layer, and wherein the optical coating has an outer surface opposite to the major surface of the substrate; and an easy-to-clean (ETC) coating disposed on the outer surface of the optical coating, wherein the ETC coating comprises a fluorine-containing material. The outer surface of the optical coating has a surface roughness (Ra) of less than 1.5 nm. The optical structure has a physical thickness greater than or equal to 500 nm and a maximum hardness of 10 GPa or greater, as measured on the outer surface of the optical coating along an indentation depth of 50 nm or greater by a Berkovich indenter test. The scratch-resistant layer has a physical thickness of 200 nm to 5000 nm.

[0134] Embodiment 2. Provided is an article according to embodiment 1, wherein the outer surface of the optical coating has a surface roughness (Ra) less than 1.2 nm.

[0135] Embodiment 3. Provided is an article according to embodiment 1, wherein the outer surface of the optical coating has a surface roughness (Ra) less than 1.0 nm.

[0136] Embodiment 4 provides an article according to any one of embodiments 1-3, wherein the optical structure is derived from multiple consecutive sputtered layers.

[0137] Embodiment 5. Provided is an article according to any one of Embodiments 1-4, wherein the optical coating comprises a first low refractive index (RI) layer directly on and in contact with the major surface of the substrate.

[0138] Embodiment 6. Provided is an article according to any one of Embodiments 1-5, wherein the optical coating is an antireflective (AR) coating, and further, wherein the article exhibits a first surface average bright reflectance (%R) of less than 1% at any incident angle of about 5° to 20° from normal at a wavelength of 450nm to 650nm.

[0139] Embodiment 7. Provided is an article according to any one of Embodiments 1-5, wherein the optical coating is an antireflective (AR) coating, and further, wherein the article exhibits a first surface average bright reflectance (%R) of less than 10% at any incident angle of about 5° to 20° from normal at a wavelength of 450nm to 650nm.

[0140] Embodiment 8. Provided is an article according to any one of Embodiments 1-5, wherein the optical coating is an antireflective (AR) coating, and further, wherein the article exhibits a first surface average bright reflectance (%R) of less than 20% at any incident angle of about 5° to 20° from normal at a wavelength of 450nm to 650nm.

[0141] Embodiment 9. Provided is an article according to any one of embodiments 1-8, wherein the ETC coating exhibits a water contact angle greater than 95° after 1000 cycles in a steel wool abrasion test.

[0142] Embodiment 10. Provided is an article according to any one of Embodiments 1-8, wherein the ETC coating exhibits a water contact angle greater than 105° after 3000 cycles in a steel wool abrasion test, and the physical thickness of the optical structure is about 1000 nm or greater.

[0143] Embodiment 11 provides an article according to any one of embodiments 1-10, wherein the substrate is a strengthened glass substrate or a glass ceramic substrate.

[0144] Embodiment 12. Provides a covering article, the covering article comprising: a substrate having a major surface; an optical structure disposed on the major surface, wherein the optical structure comprises an optical coating and a scratch-resistant layer, and wherein the optical coating has an outer surface opposite to the major surface of the substrate; and an easy-to-clean (ETC) coating disposed on the outer surface of the optical coating, wherein the ETC coating comprises a fluorine-containing material. The outer surface of the optical coating has a surface roughness (Ra) of less than 1.5 nm. The optical structure has a physical thickness greater than or equal to 500 nm and a maximum hardness of 10 GPa or greater, as measured on the outer surface of the optical coating along an indentation depth of 50 nm or greater by a Berkovich indenter test. The scratch-resistant layer has a physical thickness of 200 nm to 5000 nm. Further, the optical coating comprises a plurality of high refractive index (RI) layers and low RI layers, wherein the refractive index of each of the low RI layers is less than or equal to about 1.8, and the refractive index of each of the high RI layers is greater than 1.8. Each high RI layer comprises AlO x N y 、Nb2O x 、TiO2、Si3N4、SiN x and SiO x N y and each low RI layer comprises SiO2, SiO x and MgF2. In addition, the scratch-resistant layer includes AlO x N y 、Si3N4、SiN x and SiO x N y Any of .

[0145] Embodiment 13. Provided is an article according to Embodiment 12, wherein the outer surface of the optical coating has a surface roughness (Ra) less than 1.0 nm, wherein the ETC coating exhibits a water contact angle greater than 105° after 3000 cycles in a steel wool abrasion test.

[0146] Embodiment 14 provides an article according to Embodiment 12 or Embodiment 13, wherein the optical structure is derived from multiple consecutive sputtered layers.

[0147] Embodiment 15. Provided is an article according to any one of Embodiments 12-14, wherein the optical coating comprises a first low refractive index (RI) layer directly on and in contact with the major surface of the substrate.

[0148] Embodiment 16 provides an article according to any one of Embodiments 12-15, wherein the substrate is a strengthened glass substrate or a glass ceramic substrate.

[0149] Embodiment 17. Provides a covering article, the covering article comprising: a substrate having a major surface; an optical structure disposed on the major surface, wherein the optical structure comprises an optical coating and a scratch-resistant layer, and wherein the optical coating has an outer surface opposite to the major surface of the substrate; and an easy-to-clean (ETC) coating disposed on the outer surface of the optical coating, wherein the ETC coating comprises a fluorine-containing material. The outer surface of the optical coating has a surface roughness (Ra) of less than 1.5 nm. The optical structure has a physical thickness greater than or equal to 750 nm and a maximum hardness of 10 GPa or greater, as measured on the outer surface of the optical coating along an indentation depth of 50 nm or greater by a Berkovich indenter test. The scratch-resistant layer has a physical thickness of 250 nm to 2500 nm. In addition, the scratch-resistant layer is within the optical coating. Further, the optical coating comprises a plurality of high refractive index (RI) layers and low RI layers, wherein the refractive index of each of the low RI layers is less than or equal to about 1.8, and the refractive index of each of the high RI layers is greater than 1.8. Each high RI layer includes Si3N4, SiN x and SiO x N y and each low RI layer comprises SiO2 and SiO x In addition, the scratch-resistant layer includes Si3N4, SiN x and SiO x N y Any one of .

[0150] Embodiment 18 provides an article according to embodiment 17, wherein the outer surface of the optical coating has a surface roughness (Ra) less than 1.2 nm.

[0151] Embodiment 19. Provided is a product according to Embodiment 17 or Embodiment 18, wherein the optical structure is derived from multiple consecutive sputtered layers.

[0152] Embodiment 20. Provided is an article according to any one of Embodiments 17-19, wherein the optical coating comprises a first low refractive index (RI) layer directly on and in contact with the major surface of the substrate.

[0153] Embodiment 21. Provided is an article according to any one of Embodiments 17-20, wherein the substrate is a strengthened glass substrate or a glass ceramic substrate.

[0154] Embodiment 22. Provided is a consumer electronic product, comprising: a housing including a front surface, a rear surface, and a side surface; an electronic component at least partially within the housing; and a cover disposed on at least one of the display and the sensor. The electronic component comprises at least one of a display and a sensor. The display is at or adjacent to the front surface of the housing, and the sensor is at or adjacent to the front surface or the rear surface of the housing. Further, at least a portion of the cover comprises a cover article as described in any one of Embodiments 1-11.

[0155] Embodiment 23. Provided is a consumer electronic product, comprising: a housing including a front surface, a rear surface, and a side surface; an electronic component at least partially within the housing; and a cover disposed on at least one of the display and the sensor. The electronic component comprises at least one of a display and a sensor. The display is at or adjacent to the front surface of the housing, and the sensor is at or adjacent to the front surface or the rear surface of the housing. Further, at least a portion of the cover comprises a cover article as described in any one of Embodiments 12-16.

[0156] Embodiment 24. Provided is a consumer electronic product, comprising: a housing comprising a front surface, a rear surface, and a side surface; an electronic component at least partially within the housing; and a cover disposed on at least one of the display and the sensor. The electronic component comprises at least one of a display and a sensor. The display is at or adjacent to the front surface of the housing, and the sensor is at or adjacent to the front surface or the rear surface of the housing. At least a portion of the cover comprises a cover article as described in any one of Embodiments 17-21.

[0157] Embodiment 25. Provides a method for manufacturing a covered article, the method comprising: providing a substrate having a major surface; depositing an optical structure on the major surface, wherein the optical structure comprises an optical coating and a scratch-resistant layer, and wherein the optical coating has an outer surface opposite to the major surface of the substrate; modifying the outer surface of the optical coating, wherein after the step of modifying the outer surface, the outer surface of the optical coating has a surface roughness (Ra) of less than 1.5 nm; after the step of modifying the outer surface, depositing an easy-to-clean (ETC) coating on the outer surface of the optical coating, wherein the ETC coating comprises a fluorine-containing material; and curing the ETC coating. The optical structure has a physical thickness greater than or equal to 500 nm and a maximum hardness of 10 GPa or greater, as measured on the outer surface of the optical coating along an indentation depth of 50 nm or greater by a Berkovich indenter test. Further, the scratch-resistant layer has a physical thickness of 200 nm to 5000 nm. Furthermore, after the step of curing the ETC coating, the ETC coating exhibits a water contact angle greater than 95° after 1000 cycles in a steel wool abrasion test.

[0158] Embodiment 26. A method according to Embodiment 25, wherein the step of depositing the optical structure is performed using a reactive sputtering method, and further, wherein the optical structure comprises a plurality of continuous layers.

[0159] Embodiment 27. The method of Embodiment 25 or Embodiment 26, wherein the step of modifying the outer surface of the optical coating is performed using a plasma treatment method.

[0160] Embodiment 28. The method of Embodiment 25 or Embodiment 26, wherein the step of modifying the outer surface of the optical coating is performed using a mechanical polishing method.

[0161] In the case of not departing from the spirit and various principles of the present disclosure in substance, many changes and modifications may be made to the above-described embodiments of the present disclosure. All these modifications and variations are intended to be included in the scope of the present disclosure and protected by the following claims.

Claims

1. A covering product, comprising: a substrate having a major surface; an optical structure disposed on the major surface, wherein the optical structure comprises an optical coating and a scratch-resistant layer, and wherein the optical coating has an outer surface opposite the major surface of the substrate; as well as an easy-to-clean (ETC) coating disposed on the outer surface of the optical coating, wherein the ETC coating comprises a fluorine-containing material, wherein the outer surface of the optical coating has a surface roughness (Ra) of less than 1.5 nm, wherein the optical structure has a physical thickness greater than or equal to 500 nm and a maximum hardness of 10 GPa or greater, as measured by a Berkovich indenter test at an indentation depth of 50 nm or greater on the outer surface of the optical coating, and Furthermore, the scratch-resistant layer has a physical thickness of 200 nm to 5000 nm.

2. The cover article of claim 1, wherein the outer surface of the optical coating has a surface roughness (Ra) of less than 1.2 nm.

3. The cover article of claim 1, wherein the outer surface of the optical coating has a surface roughness (Ra) of less than 1.0 nm.

4. The covered article according to any one of claims 1 to 3, wherein the optical structure is derived from a plurality of consecutive sputtered layers.

5. The cover article of any one of claims 1-4, wherein the optical coating comprises a first low refractive index (RI) layer directly on and in contact with the major surface of the substrate.

6. The covered article of any one of claims 1-5, wherein the optical coating is an antireflective (AR) coating, and further wherein the article exhibits a first surface average bright reflectance (%R) of less than 1% at any incident angle from about 5° to 20° from normal at a wavelength of 450 nm to 650 nm.

7. The covered article of any one of claims 1-5, wherein the optical coating is an antireflective (AR) coating, and further wherein the article exhibits a first surface average bright reflectance (%R) of less than 10% at any angle of incidence from about 5° to 20° from normal at a wavelength of 450 nm to 650 nm.

8. The covered article of any one of claims 1-5, wherein the optical coating is an antireflective (AR) coating, and further wherein the article exhibits a first surface average bright reflectance (%R) of less than 20% at any incident angle from about 5° to 20° from normal at a wavelength of 450 nm to 650 nm.

9. The covered article of any one of claims 1-8, wherein the ETC coating exhibits a water contact angle of greater than 95° after 1000 cycles in a steel wool abrasion test.

10. The covered article of any one of claims 1-8, wherein the ETC coating exhibits a water contact angle greater than 105° after 3000 cycles in a steel wool abrasion test, and the optical structure has a physical thickness of about 1000 nm or greater.

11. The covered article according to any one of claims 1 to 10, wherein the substrate is a strengthened glass substrate or a glass ceramic substrate.

12. A covering product, comprising: a substrate having a major surface; an optical structure disposed on the major surface, wherein the optical structure comprises an optical coating and a scratch-resistant layer, and wherein the optical coating has an outer surface opposite the major surface of the substrate; as well as an easy-to-clean (ETC) coating disposed on the outer surface of the optical coating, wherein the ETC coating comprises a fluorine-containing material, wherein the outer surface of the optical coating has a surface roughness (Ra) of less than 1.5 nm, wherein the optical structure has a physical thickness greater than or equal to 500 nm and a maximum hardness of 10 GPa or greater, as measured by a Berkovich indenter test at an indentation depth of 50 nm or greater on the outer surface of the optical coating, wherein the scratch-resistant layer has a physical thickness of 200 nm to 5000 nm, wherein the optical coating comprises a plurality of high refractive index (RI) layers and low RI layers, wherein the refractive index of each of the low RI layers is less than or equal to about 1.8 and the refractive index of each of the high RI layers is greater than 1.8, Each high RI layer includes AlO x N y 、Nb2O x 、TiO2、Si3N4、SiN x and SiO x N y and wherein each low RI layer comprises SiO2, SiO x and MgF2, and Furthermore, the scratch-resistant layer comprises AlO x N y 、Si3N4、SiN x and SiO x N y Any of .

13. The covered article of claim 12, wherein the outer surface of the optical coating has a surface roughness (Ra) of less than 1.0 nm, wherein the ETC coating exhibits a water contact angle greater than 105° after 3000 cycles in a steel wool abrasion test.

14. A covered article according to claim 12 or claim 13, wherein the optical structure is derived from a plurality of successive sputtered layers.

15. The cover article of any one of claims 12-14, wherein the optical coating comprises a first low refractive index (RI) layer directly on and in contact with the major surface of the substrate.

16. The covered article according to any one of claims 12 to 15, wherein the substrate is a strengthened glass substrate or a glass ceramic substrate.

17. A covering product, comprising: a substrate having a major surface; an optical structure disposed on the major surface, wherein the optical structure comprises an optical coating and a scratch-resistant layer, and wherein the optical coating has an outer surface opposite the major surface of the substrate; as well as an easy-to-clean (ETC) coating disposed on the outer surface of the optical coating, wherein the ETC coating comprises a fluorine-containing material, wherein the outer surface of the optical coating has a surface roughness (Ra) of less than 1.5 nm, wherein the optical structure has a physical thickness greater than or equal to 750 nm and a maximum hardness of 10 GPa or greater, as measured by a Berkovich indenter test at an indentation depth of 50 nm or greater on the outer surface of the optical coating, wherein the scratch-resistant layer has a physical thickness of 250 nm to 2500 nm, wherein the scratch-resistant layer is within the optical coating, wherein the optical coating comprises a plurality of high refractive index (RI) layers and low RI layers, wherein the refractive index of each of the low RI layers is less than or equal to about 1.8 and the refractive index of each of the high RI layers is greater than 1.8, Each high RI layer includes Si3N4, SiN x and SiO x N y and wherein each low RI layer comprises SiO2 and SiO x one of them, and Furthermore, the scratch-resistant layer includes Si3N4, SiN x and SiO x N y Any one of .

18. The cover article of claim 17, wherein the outer surface of the optical coating has a surface roughness (Ra) of less than 1.2 nm.

19. A covered article according to claim 17 or claim 18, wherein the optical structure is derived from a plurality of successive sputtered layers.

20. The cover article of any one of claims 17-19, wherein the optical coating comprises a first low refractive index (RI) layer directly on and in contact with the major surface of the substrate.

21. The covered article according to any one of claims 17 to 20, wherein the substrate is a strengthened glass substrate or a glass ceramic substrate.

22. A consumer electronic product, comprising: a housing, the housing comprising a front surface, a rear surface and side surfaces; an electronic component at least partially within the housing, the electronic component comprising at least one of a display and a sensor, the display being at or adjacent to the front surface of the housing, and the sensor being at or adjacent to the front surface or the rear surface of the housing; as well as a cover disposed on at least one of the display and the sensor, At least a portion of the covering comprises a covering article as claimed in any one of claims 1-11.

23. A consumer electronic product, comprising: a housing, the housing comprising a front surface, a rear surface and side surfaces; an electronic component at least partially within the housing, the electronic component comprising at least one of a display and a sensor, the display being at or adjacent to the front surface of the housing, and the sensor being at or adjacent to the front surface or the rear surface of the housing; as well as a cover disposed on at least one of the display and the sensor, At least a portion of the covering comprises a covering article as claimed in any one of claims 12-16.

24. A consumer electronic product, comprising: a housing, the housing comprising a front surface, a rear surface and side surfaces; an electronic component at least partially within the housing, the electronic component comprising at least one of a display and a sensor, the display being at or adjacent to the front surface of the housing, and the sensor being at or adjacent to the front surface or the rear surface of the housing; as well as a cover disposed on at least one of the display and the sensor, Wherein at least a portion of the covering comprises a covering article as claimed in any one of claims 17-21.

25. A method of preparing a covered article, the method comprising: providing a substrate having a major surface; depositing an optical structure on the major surface, wherein the optical structure comprises an optical coating and a scratch-resistant layer, and wherein the optical coating has an outer surface opposite the major surface of the substrate; modifying the outer surface of the optical coating, wherein after the step of modifying the outer surface, the outer surface of the optical coating has a surface roughness (Ra) of less than 1.5 nm; depositing an easy-to-clean (ETC) coating on the outer surface of the optical coating after the step of modifying the outer surface, wherein the ETC coating comprises a fluorine-containing material; as well as curing the ETC coating, wherein the optical structure has a physical thickness greater than or equal to 500 nm and a maximum hardness of 10 GPa or greater, as measured by a Berkovich indenter test at an indentation depth of 50 nm or greater on the outer surface of the optical coating, wherein the scratch resistant layer has a physical thickness of 200 nm to 5000 nm, and Further, wherein after the step of curing the ETC coating, the ETC coating exhibits a water contact angle greater than 95° after 1000 cycles in a steel wool abrasion test.

26. The method of claim 25, wherein the step of depositing the optical structure is performed using a reactive sputtering method, and further wherein the optical structure comprises a plurality of consecutive layers.

27. A method according to claim 25 or claim 26, wherein the step of modifying the outer surface of the optical coating is performed using a plasma treatment process.

28. A method according to claim 25 or claim 26, wherein the step of modifying the outer surface of the optical coating is performed using a mechanical polishing method.