Preparation of amino-functional polyorganosiloxane emulsions

By adding water-soluble salts and preservatives to the amino-functional polyorganosiloxane aqueous emulsion, the emulsion phase conversion is controlled, and the problem of increased emulsion viscosity is solved, and an oil-in-water structure with high stability and fluidity is achieved, suitable for high content Preparation of amino functional polyorganosiloxane.

CN118922500APending Publication Date: 2024-11-08DOW SILICONES CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029649.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-02-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing amino-functional polyorganosiloxane aqueous emulsions have significantly increased viscosity after adding certain preservatives, resulting in the emulsion being unflowing and unstable, and reducing the amino-functional polyorganosiloxane content to alleviate the viscosity problem is detrimental to consumers.

Method used

By adding water-soluble salts to the method of preparing amino functional polyorganosiloxane aqueous emulsions, adjusting the pH value and adding preservatives, the phase conversion of the emulsion is controlled, and an oil-in-water emulsion structure with low viscosity and high stability is formed.

Benefits of technology

The flowability and stability of the emulsion under relatively high amino functional polyorganosiloxane content and low water content is achieved, avoiding the problem of increasing viscosity, and the emulsion remains stable under different storage conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005055275470000081
    Figure BDA0005055275470000081
  • Figure BDA0005055275470000091
    Figure BDA0005055275470000091
  • Figure BDA0005055275470000151
    Figure BDA0005055275470000151
Patent Text Reader

Abstract

A method for preparing an aqueous emulsion of an amino-functional polyorganosiloxane is provided. The method comprises mixing A) an amino-functional polyorganosiloxane, B) a nonionic surfactant, and C) water; and then incorporating into an additional starting material comprising additional water, D) a water-soluble salt, E) a pH adjusting agent, and F) a preservative. Phase inversion occurs during the process such that the resulting emulsion has A) the amino-functional polyorganosiloxane in an inner discontinuous phase and C) the water in an outer continuous phase.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit under 35 U.S.C. §119(e) of U.S. Provisional Patent Application Serial No. 63 / 324,765, filed on March 29, 2022. U.S. Provisional Patent Application Serial No. 63 / 324,765 is hereby incorporated by reference. Technical Field

[0003] A method for preparing an amino-functional polyorganosiloxane emulsion is provided. Background Art

[0004] Amino-functional polyorganosiloxane emulsions are widely used in hair care compositions to provide various hair cosmetic benefits. Various types of emulsions have been commercially developed to provide water-based products of such amino-functional polyorganosiloxanes for use as hair conditioners. One method of preparing emulsions of amino-functional polyorganosiloxanes involves an emulsion polymerization technique that first emulsifies the siloxane monomers and subsequently polymerizes them to high molecular weight. Alternatively, mechanical emulsions can be prepared from preformed amino-functional polyorganosiloxanes. Summary of the invention

[0005] A method for preparing an aqueous emulsion of an aminofunctional polyorganosiloxane comprises: 1) mixing starting materials comprising: A) an aminofunctional polyorganosiloxane, B) a nonionic surfactant, and C) water to prepare a water-in-oil dispersion (having C) water in an inner discontinuous phase and A) the aminofunctional polyorganosiloxane in an outer continuous phase); and then mixing additional starting materials comprising additional water, D) a water-soluble salt, E) a pH adjuster, and F) a preservative. A phase inversion occurs so that the resulting emulsion has A) the aminofunctional polyorganosiloxane in the inner discontinuous phase and C) water in the outer continuous phase. DETAILED DESCRIPTION

[0006] A method for preparing an aqueous emulsion of an aminofunctional polyorganosiloxane is provided. The method comprises mixing starting materials comprising A) an aminofunctional polyorganosiloxane, B) a nonionic surfactant, and C) water; and then mixing additional starting materials comprising additional water, D) a water-soluble salt, E) a pH adjuster, and F) a preservative. Phase inversion occurs during the process, so that the emulsion produced by the method has A) an aminofunctional polyorganosiloxane in an inner discontinuous phase and C) water in an outer continuous phase.

[0007] The method of preparing the emulsion may comprise:

[0008] 1) Mixing starting materials, the starting materials comprising

[0009] 25 to 75 parts by weight of A) an amino-functional polyorganosiloxane,

[0010] 2 to 10 parts by weight of B) a nonionic surfactant, and

[0011] 4 to 20 parts by weight of C) water;

[0012] 2) mixing a starting material with the product of step 1), the starting material comprising

[0013] 0.02 to 1 parts by weight of D) a salt, and

[0014] Additional water; and

[0015] 3) Mixing starting materials, the starting materials comprising

[0016] E) a pH adjusting agent,

[0017] F) preservatives, and

[0018] Optionally G) a freezing inhibitor.

[0019] In the above method, step 1) is performed before steps 2) and 3). Steps 2) and 3) can be performed in any order. Alternatively, steps 2) and 3) can be performed sequentially. Alternatively, steps 2) and 3) can be performed simultaneously.

[0020] In the method described herein, step 1) can be carried out at a temperature of 10°C to 70°C (alternatively 25°C), for 70s -1 To 700s -1 (Alternatively 180s -1 ) and a pressure of 100 torr to 760 torr (alternatively 200 torr to 500 torr). Alternatively, step 1) may be performed under vacuum, for example <760 torr, to minimize foaming. Step 2) may be performed at a temperature of 10°C to 70°C (alternatively 25°C), 7s -1 To 90s -1 (Alternatively 45s -1 ) and a pressure of 100 torr to 760 torr (alternatively 200 torr). Step 3) may be performed at a temperature of 10°C to 70°C (alternatively 25°C), 7s -1 To 90s -1 (Alternatively 45s -1 ) and a pressure of 100 Torr to 760 Torr (alternatively 200 Torr).

[0021] The above method may optionally further comprise one or more additional steps selected from the following:

[0022] adding additional water and mixing after step 1) and before step 2);

[0023] adding additional water and mixing during or after step 2) and before step 3);

[0024] Additional water is added during or after step 3) and mixed. In addition, those skilled in the art will recognize that starting materials E), F) and G) (when present) can be added simultaneously, alternatively they can be added in any order. The method may also optionally include a post-processing step after preparing the emulsion as described above. For example, the method may also include filtering the emulsion after step 3) and / or packaging after step 3).

[0025] The method may also optionally include: first mixing A) amino-functional polyorganosiloxane and B) nonionic surfactant in step 1), and then adding C) water and mixing. The amount of water added in step 1) depends on various factors, including the shearing device selected for performing step 1). For example, a can mixer, a rotor-stator mixer, a sonographer, an extruder such as a twin-screw extruder, a colloid mill, a stirring tank, a conical screw or a homogenizer can be used for mixing in step 1). The same or different equipment can be used for other steps of the method described herein. The amount of water added in step 1) can be 4 to 20 parts by weight, alternatively 5 to 18 parts by weight, alternatively 5.5 to 16 parts by weight, alternatively 6 to 14 parts by weight, and alternatively 6.5 to 12 parts by weight. Alternatively, based on the combined weight of all starting materials in the emulsion, the amount of water added in step 1) can be 4% to 20%, alternatively 8%.

[0026] The starting materials used in the methods described herein include A) an amino-functional polyorganosiloxane, B) a nonionic surfactant, C) water, D) a water-soluble salt, E) a pH adjuster, F) a preservative, and optionally G) a freeze inhibitor, which are introduced above and described in detail below.

[0027] A) Polysiloxane

[0028] The amino-functional polyorganosiloxane comprises two or more siloxane units which may be independently selected from the group consisting of: 3 SiO 1 / 2 ) of the M unit, formula (R 2 SiO 2 / 2 ) of D unit, formula (RSiO 3 / 2 ) and the T unit of formula (SiO 4 / 2 ) wherein each R is independently selected from an alkyl group and an amino-alkyl-functional group, provided that at least one unit per molecule has an R that is an amino-alkyl-functional group. The amino-functional polyorganosiloxane further comprises a Q unit of formula (ZO 1 / 2 ) wherein Z is selected from H and R1 (alkyl groups having 1 to 6 carbon atoms), as described in further detail below. These siloxane units can be combined in various ways to form cyclic, linear or branched structures. Suitable amino-functional polyorganosiloxanes are disclosed, for example, in PCT published patent application number WO2013 / 082096.

[0029] Alternatively, the aminofunctional polyorganosiloxane may be substantially linear or linear. The aminofunctional polyorganosiloxane may include an aminofunctional polydiorganosiloxane. Alternatively, the aminofunctional polydiorganosiloxane may include units of formula (R 1 2 SiO 2 / 2 ) a (R 1 R 2 SiO 2 / 2 ) b (ZO 1 / 2 ) d (R 1 3 SiO 1 / 2 ) e Poly(dialkyl / alkyl, amino)siloxane, wherein each R 1 is an independently selected alkyl group of 1 to 6 carbon atoms; each R 2 is an independently selected amino-functional alkyl group; subscripts a, b, d, and e represent the average number per molecule of each unit in the unit formula, subscript a is 1 to 5, subscript b is 1 to 1000; subscript d is 0, 1 or 2, alternatively 1 or 2; subscript e is 0, 1 or 2, alternatively 0 or 1; and the number (d+e)=2. Alternatively, subscript a may be 2 to 5, alternatively 2 to 4, and alternatively 1 to 4. Alternatively, subscript b may be 50 to 900, alternatively 100 to 800, alternatively 150 to 700, alternatively 200 to 600, alternatively 300 to 550, alternatively 350 to 550, and alternatively 400 to 500. Alternatively, the amount (a+b) may be of a value sufficient for the poly(dialkyl / alkylamino)siloxane to have a viscosity of 3,000 to 8,000 centipoise at 25°C as measured with a Brookfield DV viscometer at 30 rpm using LV#4.

[0030] R 1 is an alkyl group of 1 to 6 carbon atoms, such as methyl, ethyl, propyl (including n-propyl and isopropyl) and butyl (including n-butyl, isobutyl, sec-butyl and tert-butyl). 1 It can be methyl or ethyl. Alternatively, each R 1 It may be methyl.

[0031] R 2is an amino-functional alkyl group. The amino-functional alkyl group may have the formula ZHN-R 3 -(ZNR 4 ) c -, where Z is as above, R 3 is an alkylene group of 2 to 6 carbon atoms, R 4 is an alkylene group of 2 to 6 carbon atoms, and the subscript c is 0 or 1. 3 and R 4 Examples of alkylene groups include the empirical formula -C r H 2r -, wherein the subscript r is 2 to 8. The alkylene group may be a straight chain alkylene group, such as -CH 2 -CH 2 -、-CH 2 -CH 2 -CH 2 -、-CH 2 -CH 2 -CH 2 -CH 2 -or-CH 2 -CH 2 -CH 2 -CH 2 -CH 2 -CH 2 -, or branched alkylene

[0032] For example

[0033] R 2 Examples of amino-functional alkyl groups include, but are not limited to, aminoethyl-, aminopropyl-, aminoisobutyl-, aminoethyl-aminopropyl-, and aminoethyl-aminoisobutyl-.

[0034] Amino-functional polyorganosiloxanes are known in the art and many are commercially available. Representative commercially available amino-functional organopolysiloxanes include XIAMETER TM OFX-8040 Fluid,XIAMETER TM OHX-8630 Fluid, XIAMETER TM OHX-8803 Fluid, DOWSIL TM AP-6087 Fluid, DOWSIL TM AP-8087 Fluid and DOWSIL TM2-8566Amino Fluid, all of which are commercially available from Dow Silicones Corporation, Midland, Michigan, USA. Amino-functional polyorganosiloxanes can be prepared by known methods, such as those disclosed in: U.S. Pat. No. 11,028,233 to Suthiwangcharoen et al.; U.S. Pat. No. 11,028,229 to Suthiwangcharoen et al.; U.S. Pat. No. 7,781,505 to Cook et al.; U.S. Patent Application Publication No. 2004 / 0210074; U.S. Pat. No. 7,238,768 to Hupfield et al.; U.S. Pat. No. 6,171,515 to Evans et al.; and U.S. Pat. No. 2,947,771 to Bailey.

[0035] In the emulsion prepared as described herein, one or more of the above amino-functional polyorganosiloxanes can be used as starting material A). The amount in the emulsion produced by the method can be 25 to 75 parts by weight, alternatively 30 to 70 parts by weight, alternatively 35 to 65 parts by weight, alternatively 40 to 60 parts by weight, alternatively 45 to 55 parts by weight, and alternatively 50 parts by weight. Alternatively, the amount of A) amino-functional polyorganosiloxane can be 35 to 75 parts by weight, alternatively 40 to 70 parts by weight, alternatively 45 to 65 parts by weight, alternatively 50 to 75 parts by weight, and alternatively 50 to 65 parts by weight. Without wishing to be bound by theory, it is believed that the method for preparing the emulsion described herein allows for relatively high loadings (e.g., at least 35%, alternatively at least 50% of the emulsion produced is A) amino-functional polyorganosiloxane).

[0036] B) Nonionic surfactants

[0037] The starting material B) in the emulsion prepared herein is a nonionic surfactant. The emulsion may not contain a cationic surfactant. Without wishing to be bound by theory, it is believed that the presence of a cationic surfactant may lead to the undesirable formation of cyclic siloxanes (e.g., octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane and / or dodecamethylcyclohexasiloxane) when the emulsion is stored for a period of time before use.

[0038] Some suitable nonionic surfactants that can be used herein include polyoxyethylene alkyl ethers (such as lauryl, hexadecyl, octadecyl or octyl), polyoxyethylene alkylphenol ethers, alkyl glycosides, polyoxyethylene fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitan monooleate, polyoxyethylene alkyl esters, polyoxyethylene sorbitan alkyl esters, polyethylene glycols (such as polyethylene glycols having 23 ethylene oxide units), polypropylene glycol, diethylene glycol, ethoxylated trimethylnonanol, tristyrylphenol ether (TSP), distyrylphenol ether (DSP) and polyoxyalkylene glycol-modified silicone surfactants.

[0039] Commercially available nonionic surfactants include compositions such as the following: marketed under the name TERGITOL by The Dow Chemical Company, Midland, Michigan, USA TM TMN-6 and TERGITOL TM 2,6,8-trimethyl-4-nonyloxypolyoxyethylene ethanol (6EO) and (10EO) sold as TMN-10; C 11-15 Secondary alkyl polyoxyethylene ether (e.g., C 11-15 Secondary alcohol ethoxylates 7EO, 9EO and 15EO, under the name TERGITOL TM 15-S-7, TERGITOL TM 15-S-9 and TERGITOL TM 15-S-15 is sold with an HL value of 15.4), other C 11-15 Secondary alcohol ethoxylates are sold under the trade name ECOSURF TM EH-40 and TERGITOL TM 15-S-12, TERGITOL TM 15-S-30 and TERGITOL TM 15-S-40; sold by Dow Chemical Company under the name TRITON TM X405 Octylphenyl polyoxyethylene (40) ether; sold by Stepan Company under the name MAKON TM 10; ethoxylated alcohol sold under the name Trycol 5953 by Henkel Corp. / Emery Group, Cincinnati, Ohio, USA; and BRIJ sold under the name by Croda Inc., Edison, New Jersey, USA. TM L23 (HLB value is 16.9) and BRIJ TMThe ethoxylated alcohol L4 (HLB value 9.7) is sold by ICI Surfactants, Wilmington, Delaware under the trademark BRIJ TM 23 sold by the polyoxyethylene 23 lauryl ether (Laureth-23); and RENEX TM 30, polyoxyethylene ether alcohols sold by ICI Surfactants, Wilmington, Delaware, USA; alkyl-oxyalcohol polyglycol ethers such as GENAPOL TM UD 050 (HLB value 11.4) and GENAPOL TM UD110 (HLB value 14.4), alkyl polyglycol ether based on C10-Guerbet alcohol and ethylene oxide, such as LUTENSOL TM XP 79, and alkyl polyglycosides such as those sold by BASF under the trade name Glucopon TM Those sold under the trade name EcoSense, and alkyl glucosides such as those sold under the trade name EcoSense by The Dow Chemical Company, Midland, Michigan, USA TM Decyl glucoside, lauryl glucoside and cocoyl glucoside are sold as TERGITOL GLUCOSIDE. Other commercially available nonionic surfactants include TERGITOL TM 15-S-5, also available from The Dow Chemical Company, has an HLB value of 10.5; Lutensol XP 50 has an HLB value of 10 and Lutensol XP 140 has an HLB value of 16.

[0040] Suitable nonionic surfactants also include poly(oxyethylene)-poly(oxypropylene)-poly(oxyethylene) triblock copolymers. Poly(oxyethylene)-poly(oxypropylene)-poly(oxyethylene) triblock copolymers are also commonly referred to as poloxamers. They are nonionic triblock copolymers consisting of a polyoxypropylene (poly(propylene oxide)) hydrophobic chain in the middle and polyoxyethylene (poly(ethylene oxide)) hydrophilic chains on both sides. Poly(oxyethylene)-poly(oxypropylene)-poly(oxyethylene) triblock copolymers are commercially available from BASF, Florham Park, New Jersey, USA and are marketed under the trade name PLURONIC TM Such as PLURONIC TM L61, L62, L64, L81, P84 for sale.

[0041] The nonionic surfactant may also be a silicone polyether (SPE). As a surfactant, the silicone polyether may have a rake-type structure in which polyoxyethylene or polyoxyethylene-polyoxypropylene copolymer units are grafted onto a siloxane backbone, or the SPE may have an ABA block copolymer structure in which A represents a polyether moiety and B represents a siloxane moiety of an ABA structure. Alternatively, the SPE may have a resin structure, such as a polyorganosilicate resin having a polyether group bonded to a silicon atom. Suitable SPEs include DOWSIL® from Dow Silicones Corporation, Midland, Michigan, USA. TM OFX-5329 fluid. Alternatively, the nonionic surfactant may be selected from polyoxyalkylene substituted silicones, silicone alkanolamides, silicone esters and silicone glycosides. Such silicone-based surfactants are useful in forming such aqueous emulsions and are known in the art and have been described, for example, in U.S. Pat. No. 4,122,029 to Gee et al., U.S. Pat. No. 5,387,417 to Rentsch, and U.S. Pat. No. 5,811,487 to Schulz et al. Other silicone polyether surfactants are known in the art and are also commercially available, such as DOWSIL TM 502W and DOWSIL TM 67 additive is commercially available from Dow Silicones Corporation, Midland, Michigan, USA.

[0042] Alternatively, the nonionic surfactant may include a polyvinyl alcohol compound. Polyvinyl alcohol compounds are known in the art and are disclosed in, for example, U.S. Patent Application Publication 2007 / 0099007, paragraphs

[0172] and

[0173] . The polyvinyl alcohol compound can be prepared by saponification of polyvinyl acetate, so up to 15% of the polyvinyl acetate can be retained in the polyvinyl alcohol compound used herein. Alternatively, the polyvinyl alcohol compound can be 88% to 92% polyvinyl alcohol (with a balance of 12% to 8% polyvinyl acetate). At 20°C, the polyvinyl alcohol compound can have a minimum viscosity of 5 cP at 4% aqueous solution.

[0043] In the emulsion prepared as described herein, one or more of the above nonionic surfactants may be used. The exact amount of the nonionic surfactant in the emulsion depends on various factors, including the selected amino-functional polyorganosiloxane, the selection of the nonionic surfactant, and the amount of water and other components of the emulsion, however, the amount of the nonionic surfactant may be 2 to 10 parts by weight, alternatively 2.5 to 8 parts by weight, alternatively 3 to 6 parts by weight, alternatively 3.5 to 5 parts by weight, alternatively 4 to 5 parts by weight, alternatively 4 to 4.5 parts by weight, and alternatively 4.3 parts by weight.

[0044] C) Water

[0045] Water is generally not limited and can be used in a neat form (i.e., without any carrier medium / solvent) and / or a pure form (i.e., free of or substantially free of minerals and / or other impurities). For example, prior to step (1), the water may be treated or untreated. Examples of methods that can be used to purify water include distillation, filtration, deionization, and combinations of two or more thereof, such that the water can be deionized, distilled, and / or filtered. Alternatively, the water can be untreated (e.g., it can be tap water, i.e., provided by a municipal water supply or well water, and used without further purification).

[0046] Water can be added in one or more aliquots in different process steps, which will be selected by those skilled in the art according to various factors, such as the ease of mixing and the ease of adding other starting materials to the emulsion. The total amount of water can be 25 to 75 parts by weight, alternatively 30 to 70 parts by weight, alternatively 35 to 65 parts by weight, alternatively 40 to 60 parts by weight, alternatively 45 to 55 parts by weight, and alternatively 50 parts by weight. Alternatively, the total amount of water in the emulsion can be 25 to 50 parts by weight, alternatively 30 to <50 parts by weight, alternatively 35 to 45 parts by weight, and alternatively 35 to 40 parts by weight.

[0047] D) Salt

[0048] The starting material D) in the emulsion prepared as described herein is a salt. A salt is a molecule having positive and negative ions that are held together by the strong attraction of oppositely charged particles. A salt is water-soluble if it dissolves in water to give a solution in which the ions are dispersed at room temperature. A salt is insoluble if the concentration of the aqueous solution is less than 0.001 M at room temperature; insoluble salts are not used herein. Examples of water-soluble salts suitable for use as starting material D) are Solubility (purdue.edu) and shown in Table 1 below.

[0049]

[0050]

[0051] Alternatively, the soluble salt selected for the starting material D) may have the formula MR 5 x , wherein M is selected from calcium (Ca), magnesium (Mg), potassium (K), ammonium (NH 4 ) and sodium (Na); R 5 Selected from the group consisting of halogen atoms, acetate groups, benzoate groups and sulfate groups; and the subscript x is 1 or 2. Alternatively, the halogen atom can be selected from the group consisting of bromine (Br), chlorine (Cl), fluorine (F) and iodine (I). Alternatively, D) the water-soluble salt can be selected from the group consisting of ammonium chloride, calcium bromide, calcium chloride, calcium iodide, calcium sulfate, magnesium chloride, potassium bromide, potassium chloride, sodium acetate, sodium benzoate, sodium bromide, sodium chloride, sodium iodide and a combination of two or more of them. Alternatively, D) the water-soluble salt may include sodium benzoate and one or more of the following: ammonium chloride, calcium bromide, calcium chloride, calcium iodide, calcium sulfate, magnesium chloride, potassium bromide, potassium chloride, sodium acetate, sodium bromide, sodium chloride and sodium iodide. The above salts are commercially available from various sources. Without wishing to be bound by theory, it is believed that Ca 3 (PO 4 ) 2 It is not suitable for use as a salt herein because its solubility in water is insufficient for this application.

[0052] D) The amount of salt is sufficient to provide the beneficial viscosity effect described below. The amount of salt can be 0.02 to 1 parts by weight, alternatively 0.025 to 0.8 parts by weight, alternatively 0.03 to 0.6 parts by weight, alternatively 0.035 to 0.5 parts by weight, alternatively 0.04 to 0.4 parts by weight, alternatively 0.045 to 0.3 parts by weight, alternatively 0.05 to 0.2 parts by weight, alternatively 0.055 to 0.1 parts by weight, alternatively 0.06 parts by weight.

[0053] E) pH adjuster

[0054] The starting material E) in the emulsion prepared as described herein is a pH adjusting agent. Suitable pH adjusting agents can be any acid or base that does not react with A) the amino-functional polyorganosiloxane. Suitable acids include acetic acid, maleic acid or lactic acid. Suitable bases include tertiary amines, such as triethanolamine. Acids and bases suitable as pH adjusting agents are known in the art and are commercially available. The amount of pH adjuster depends on various factors, such as how C) the water is treated prior to use and any impurities in the water, however, the amount of pH adjuster can be 0.02 to 0.2 parts by weight, alternatively 0.03 to 0.19 parts by weight, alternatively 0.04 to 0.18 parts by weight, alternatively 0.05 to 0.17 parts by weight, alternatively 0.06 to 0.16 parts by weight, alternatively 0.07 to 0.15 parts by weight, alternatively 0.08 to 0.14 parts by weight, alternatively 0.09 to 0.13 parts by weight, alternatively 0.1 to 0.12 parts by weight, and alternatively 0.12 parts by weight.

[0055] F) Preservatives

[0056] Starting material F) is a preservative added to the emulsion to prevent microbial growth. The preservative may be -OH functional. Representative preservatives that may be used include phenoxyethanol, ethylhexylglycerin, benzyl alcohol, caprylyl glycol, chlorphenesin, and combinations of two or more thereof. These preservatives are commercially available from a variety of sources, such as MICROCARE® from ECOCERT. TM Products, phenoxyethanol and blends, and available from the website of THOR Especialidades, SA, Barcelona, ​​Spain Preservatives-THORPersonalCare–Microcare The exact amount of preservative depends on various factors, including the choice of preservative and other starting materials used to prepare the emulsion. However, the amount of preservative can be 0.3 to 2 parts by weight, alternatively 0.5 to 1.9 parts by weight, alternatively 0.75 to 1.8 parts by weight, alternatively 1 to 1.7 parts by weight, alternatively 1.5 to 1.6 parts by weight.

[0057] Adding D) salt to the emulsion in the process described herein can result in a significant and surprising decrease in bulk viscosity. Without wishing to be bound by theory, it is believed that the combination of A) amino-functional polyorganosiloxane, B) nonionic surfactant and -OH functional preservative (e.g., phenoxyethanol and benzyl alcohol) can result in the formation of large emulsion particles, which is believed to result in a significant increase in bulk viscosity, which is undesirable. In the past, viscosity could be reduced by adding additional water. Without wishing to be bound by theory, it is believed that D) salt destabilizes the large emulsion particles and releases water, thereby reducing the viscosity of the resulting emulsion. The inventors surprisingly found that even in the presence of relatively low amounts of water in the emulsion prepared as described herein, the viscosity remains low enough to make the emulsion flowable at room temperature, and the emulsion is stable over time (e.g., no significant increase in viscosity that would make the emulsion non-flowable or separate the emulsion components was observed after 30 days at 50°C, in contrast, the inventors surprisingly found that storage under these conditions helped to reduce the viscosity of the emulsion). It is believed that the ions formed by the dissolved salts produce a viscosity reduction (dilution effect) in the emulsion prepared as described herein. The flowable nature of the product of step 2) allows for easy incorporation of the remaining starting materials E), F) and G) (when present), thereby saving energy and increasing the capacity of the manufacturing facility. The lower viscosity also allows for easy filtering and packaging of the produced emulsion upon completion of the process. The consumer benefits from easier incorporation of the emulsion into end-use formulations.

[0058] Optional G) Freeze Inhibitor

[0059] The starting material G) in the emulsion is an optional freezing inhibitor. Suitable freezing inhibitors are known in the art and are commercially available. The freezing inhibitor can be a glycol, such as propylene glycol, ethylene glycol, or a combination thereof. The amount of the freezing inhibitor can be 0 to 2, alternatively 0.1 to 1.75, alternatively 0.2 to 1.5, alternatively 0.3 to 1.25, alternatively 0.4 to 1, and alternatively 0.5 parts by weight.

[0060] When selecting starting materials for the emulsion, there can be overlap between the types of starting materials because some of the starting materials described herein can have more than one function. For example, certain diols can be used as both a freezing inhibitor and a preservative. When the starting materials are added during the process of forming the emulsion, the starting materials are different from each other.

[0061] The method described herein produces an emulsion which is an oil-in-water emulsion. By adjusting the amount of shear applied in step 1) and the amount of water used, the emulsion having different particle sizes can be produced. The particle size diameter measured by the 50% volume of the cumulative population can vary from 0.18 microns to 10 microns in size. Alternatively, a particle size of 0.25 microns to 0.75 microns can be produced, which can be kept stable in an emulsified form to prevent instability. The particle size can be measured by laser diffraction using a Malvern Mastersizer 3000 and according to ISO 13320 (2009).

[0062] How to use

[0063] Aminofunctional polyorganosiloxanes are used as fiber lubricants in the textile industry, for example, for polyester, polyamide, acrylic, cotton or wool fibers; as fabric softeners; and as anti-wrinkle agents. Aminofunctional polyorganosiloxanes can also be used in the personal care industry, for example, in hair care compositions such as shampoos, conditioners and styling products, and in skin care compositions such as cosmetic compositions. The emulsions prepared as described above can be used to deliver aminofunctional polyorganosiloxanes in one or more of the above-mentioned applications. For example, the emulsions prepared as described herein can be used to supplement or replace any emulsions described in, for example, U.S. Patent No. 7,781,505 to Cook et al.; U.S. Patent Application Publication No. 2018 / 0353396 to Paul et al.; U.S. Patent Application Publication No. 2022 / 0008320 to Liang et al. and U.S. Patent No. 6,171,515 to Evans et al. Therefore, a method includes using the above-mentioned emulsion in a hair care composition. For example, the method may include applying the emulsion or a hair care composition comprising the emulsion to the hair. Alternatively, the method for treating a textile comprises applying the emulsion prepared as described above or a textile treating agent comprising the emulsion to the textile.

[0064] Example

[0065] These examples are intended to illustrate the present invention to one of ordinary skill in the art and should not be construed as limiting the scope of the present invention described in the claims.All measurements and experiments were performed at 23°C unless otherwise specified.

[0066] Example 1 - Preparation of Emulsion A

[0067] In a 3L stainless steel beaker, add 500.00 g of aminofunctional polyorganosiloxane, 5.65 g of TERGITOL TM 15-S-7, 37.50g TERGITOL TM15-S-12. The beaker and contents are placed under an overhead bench mixer having a shaft containing a three-blade propeller directly above the propeller of six 90° blades. The contents are mixed at 150 rpm for 5 minutes or until they are uniform. The mixer is stopped and 75.00 g of water is added. Mixing is continued at 700 rpm for 5 minutes. After 5 minutes, the mixer is stopped and the phase inversion of the beaker contents is observed, which is subsequently confirmed by particle size analysis on a Malvern Mastersizer 3000. The emulsion is scraped off the sidewall and blade with a rubber scraper and continued to mix for another 15 minutes at 350 rpm. The particle size is measured again. The emulsion is diluted twice, 354.85 g of water is added in total, and mixed at 350 rpm and 150 rpm, respectively, for 10 minutes each time. 20% acetic acid solution, phenoxyethanol, benzyl alcohol and propylene glycol are all added separately, mixing for 10 minutes between each of these starting materials. The mixer was stopped and scraped from time to time to ensure that the starting materials were fully incorporated into the emulsion at each step. After mixing was complete and uniformity was ensured, the emulsion was collected. Visual observations, viscosity, and particle size were recorded. Viscosity was measured using a Brookfield DVII viscometer spindle #4 at 0.5 rpm.

[0068] Example 2 - Preparation of Emulsion B

[0069] In a 1 ounce glass bottle, 1 g of water and 0.03 g of sodium benzoate were added. The vial was vortexed to ensure that the sodium benzoate salt was dissolved to form a clear solution. 48.94 g of Emulsion A and sodium benzoate solution from Example 1 were added to a 60 g Speedmixer dental mixer cup. The dental mixer cup contents were sheared at 3500 rpm for 30 seconds on a Hauschild Speedmixer (model DAC 150FVZ). The cup was scraped with a spatula and the contents were mixed at 3500 rpm for another 30 seconds. Visual observations, viscosity, and particle size were recorded. Viscosity was measured at 60 rpm using a Brookfield DVII viscometer spindle #3.

[0070] Example 3 - Preparation of Emulsion C

[0071] In a 1 ounce glass bottle, 1 g of water and 0.03 g of sodium chloride were added. The vial was vortexed to ensure that the sodium chloride salt was dissolved to form a clear solution. 48.94 g of Emulsion A from Example 1 and sodium chloride solution were added to a 60 g Speedmixer dental mixer cup. The dental mixer cup contents were sheared at 3500 rpm for 30 seconds on a Hauschild Speedmixer (model DAC 150FVZ). The cup was scraped with a spatula and the contents were mixed at 3500 rpm for another 30 seconds. Visual observations, viscosity, and particle size were recorded. Viscosity was measured at 60 rpm using a Brookfield DVII viscometer spindle #3.

[0072] Example 4 - Preparation of Emulsion D

[0073] In a 1 ounce glass bottle, 1 g of water and 0.03 g of sodium bromide were added. The vial was vortexed to ensure that the sodium bromide salt was dissolved to form a clear solution. 48.94 g of Emulsion A and sodium bromide solution from Example 1 were added to a 60 g Speedmixer dental mixer cup. The dental mixer cup contents were sheared at 3500 rpm for 30 seconds on a Hauschild Speedmixer (model DAC 150FVZ). The cup was scraped with a spatula and the contents were mixed at 3500 rpm for another 30 seconds. Visual observations, viscosity, and particle size were recorded. Viscosity was measured at 60 rpm using a Brookfield DVII viscometer spindle #3.

[0074] Example 5 - Preparation of Emulsion E

[0075] In a 1 ounce glass bottle, 1 g of water and 0.03 g of sodium acetate were added. The vial was vortexed to ensure that the sodium acetate salt was dissolved to form a clear solution. 48.94 g of Emulsion A and sodium acetate solution from Example 1 were added to a 60 g Speedmixer dental mixer cup. The dental mixer cup contents were sheared at 3500 rpm for 30 seconds on a Hauschild Speedmixer (model DAC 150FVZ). The cup was scraped with a spatula and the contents were mixed at 3500 rpm for another 30 seconds. Visual observations, viscosity, and particle size were recorded. Viscosity was measured at 60 rpm using a Brookfield DVII viscometer spindle #3.

[0076] Example 6 - Preparation of Emulsion F

[0077] In a 1 ounce glass bottle, 1 g of water and 0.03 g of sodium iodide were added. The vial was vortexed to ensure that the sodium iodide salt was dissolved to form a clear solution. 48.94 g of Emulsion A and sodium iodide solution from Example 1 were added to a 60 g Speedmixer dental mixer cup. The dental mixer cup contents were sheared at 3500 rpm for 30 seconds on a Hauschild Speedmixer (model DAC 150FVZ). The cup was scraped with a spatula, and the contents were mixed at 3500 rpm for another 30 seconds. Visual observations, viscosity, and particle size were recorded. Viscosity was measured at 60 rpm using a Brookfield DVII viscometer spindle #3.

[0078] Example 7 - Preparation of Emulsion G

[0079] In a 1 ounce glass bottle, 1 g of water and 0.03 g of calcium chloride were added. The vial was vortexed to ensure that the calcium chloride salt was dissolved to form a clear solution. 48.94 g of Emulsion A and calcium chloride solution from Example 1 were added to a 60 g Speedmixer dental mixer cup. The dental mixer cup contents were sheared at 3500 rpm for 30 seconds on a Hauschild Speedmixer (model DAC 150FVZ). The cup was scraped with a spatula and the contents were mixed at 3500 rpm for another 30 seconds. Visual observations, viscosity, and particle size were recorded. Viscosity was measured at 60 rpm using a Brookfield DVII viscometer spindle #3.

[0080] Example 8 - Preparation of Emulsion H

[0081] In a 1 ounce glass bottle, 1 g of water and 0.03 g of calcium bromide were added. The vial was vortexed to ensure that the calcium bromide salt was dissolved to form a clear solution. 48.94 g of Emulsion A and calcium bromide solution from Example 1 were added to a 60 g Speedmixer dental mixer cup. The dental mixer cup was sheared at 3500 rpm for 30 seconds on a Hauschild Speedmixer (model DAC 150FVZ). The cup was scraped with a spatula and the contents were mixed at 3500 rpm for another 30 seconds. Visual observations, viscosity, and particle size were recorded. Viscosity was measured at 60 rpm using a Brookfield DVII viscometer spindle #3.

[0082] Example 9 - Preparation of Emulsion I

[0083] In a 1 ounce glass bottle, 1 g of water and 0.03 g of calcium sulfate were added. The vial was vortexed to ensure that the calcium sulfate salt was dissolved to form a clear solution. 48.94 g of Emulsion A and calcium sulfate solution from Example 1 were added to a 60 g Speedmixer dental mixer cup. The dental mixer cup contents were sheared at 3500 rpm for 30 seconds on a Hauschild Speedmixer (model DAC 150FVZ). The cup was scraped with a spatula and the contents were mixed at 3500 rpm for another 30 seconds. Visual observations, viscosity, and particle size were recorded. Viscosity was measured at 60 rpm using a Brookfield DVII viscometer spindle #3.

[0084] Example 10 - Preparation of Emulsion J

[0085] In a 1 ounce glass bottle, 1 g of water and 0.03 g of calcium iodide were added. The vial was vortexed to ensure that the calcium iodide salt was dissolved to form a clear solution. 48.94 g of Emulsion A and calcium iodide solution from Example 1 were added to a 60 g Speedmixer dental mixer cup. The dental mixer cup contents were sheared at 3500 rpm for 30 seconds on a Hauschild Speedmixer (model DAC 150FVZ). The cup was scraped with a spatula and the contents were mixed at 3500 rpm for another 30 seconds. Visual observations, viscosity, and particle size were recorded. Viscosity was measured at 60 rpm using a Brookfield DVII viscometer spindle #3.

[0086] Example 11 - Preparation of Emulsion K

[0087] In a 1 ounce glass bottle, 1 g of water and 0.03 g of ammonium chloride were added. The vial was vortexed to ensure that the ammonium chloride salt was dissolved to form a clear solution. 48.94 g of Emulsion A and ammonium chloride solution from Example 1 were added to a 60 g Speedmixer dental mixer cup. The dental mixer cup contents were sheared at 3500 rpm for 30 seconds on a Hauschild Speedmixer (model DAC 150FVZ). The cup was scraped with a spatula and the contents were mixed at 3500 rpm for another 30 seconds. Visual observations, viscosity, and particle size were recorded. Viscosity was measured at 60 rpm using a Brookfield DVII viscometer spindle #3.

[0088] Example 12 - Preparation of Emulsion L

[0089] In a 1 ounce glass bottle, 1 g of water and 0.03 g of potassium chloride were added. The vial was vortexed to ensure that the potassium chloride salt was dissolved to form a clear solution. 48.94 g of Emulsion A from Example 1 and potassium chloride solution were added to a 60 g Speedmixer dental mixer cup. The dental mixer cup contents were sheared at 3500 rpm for 30 seconds on a Hauschild Speedmixer (model DAC 150FVZ). The cup was scraped with a spatula and the contents were mixed at 3500 rpm for another 30 seconds. Visual observations, viscosity, and particle size were recorded. Viscosity was measured at 60 rpm using a Brookfield DVII viscometer spindle #3.

[0090] Example 13 - Preparation of Emulsion M

[0091] In a 1 ounce glass bottle, 1 g of water and 0.03 g of potassium bromide were added. The vial was vortexed to ensure that the potassium bromide salt was dissolved to form a clear solution. 48.94 g of Emulsion A from Example 1 and potassium bromide solution were added to a 60 g Speedmixer dental mixer cup. The dental mixer cup contents were sheared at 3500 rpm for 30 seconds on a Hauschild Speedmixer (model DAC 150FVZ). The cup was scraped with a spatula and the contents were mixed at 3500 rpm for another 30 seconds. Visual observations, viscosity, and particle size were recorded. Viscosity was measured at 60 rpm using a Brookfield DVII viscometer spindle #3.

[0092] Example 14 - Preparation of Emulsion N

[0093] In a 1 ounce glass bottle, 1 g of water and 0.03 g of magnesium chloride were added. The vial was vortexed to ensure that the magnesium chloride salt was dissolved to form a clear solution. 48.94 g of Emulsion A from Example 1 and magnesium chloride solution were added to a 60 g Speedmixer dental mixer cup. The dental mixer cup contents were sheared at 3500 rpm for 30 seconds on a Hauschild Speedmixer (model DAC 150FVZ). The cup was scraped with a spatula and the contents were mixed at 3500 rpm for another 30 seconds. Visual observations, viscosity, and particle size were recorded. Viscosity was measured at 60 rpm using a Brookfield DVII viscometer spindle #3.

[0094] Example 15 - Preparation of Emulsion O

[0095] In a 1 ounce glass bottle, 1 g of water and 0.03 g of calcium phosphate were added. The vial was vortexed and it was noted that the solution was turbid. 48.94 g of Emulsion A and calcium phosphate solution from Example 1 were added to a 60 g Speedmixer dental mixer cup. The dental mixer cup contents were sheared at 3500 rpm for 30 seconds on a Hauschild Speedmixer (model DAC 150FVZ). The cup was scraped with a spatula and the contents were mixed at 3500 rpm for another 30 seconds. Visual observations, viscosity, and particle size were recorded. Viscosity was measured at 0.5 rpm using a Brookfield DVII viscometer spindle #4.

[0096] The starting materials used to prepare the emulsions in Examples 1 to 18 are described below. The aminofunctional polyorganosiloxane is DOWSIL TM AP 6087 Fluid, nonionic surfactant is TERGITOL TM 15-S-7 and TERGITOL TM A mixture of 15-S-12, acetic acid (from Haviland), phenoxyethanol (from Clariant), benzyl alcohol (from Univar) and propylene glycol (The Dow Chemical Company).

[0097] Table 1 shows the salts used in Examples 2 to 15.

[0098]

[0099]

[0100] Table 2 shows the weight % composition of each of the above emulsions.

[0101] *qs=appropriate amount

[0102] Table 2 (continued)

[0103]

[0104] *qs=appropriate amount

[0105] Table 3 shows the particle size measured by Malvern Mastersizer 3000, the viscosity measured by Brookfield DVII viscometer with different spindles and visual observation of each example.

[0106]

[0107] Issues to be resolved

[0108] An aqueous emulsion of an aminofunctional polyorganosiloxane containing a nonionic surfactant package was produced using a preservative package that was found to increase viscosity. The emulsion was found to be no longer flowable. The increase in viscosity was only partially mitigated by reducing the level of aminofunctional polyorganosiloxane from 50% to 37.5%, and having 50% or less aminofunctional polyorganosiloxane in the emulsion may be undesirable for some consumers. Attempts to accelerate thinning by adding a heating step during the process were not effective within a reasonable manufacturing time frame.

[0109] Solution :

[0110] The process described herein produces an emulsion that is stable in viscosity and particle size, even after the emulsion has been stored at room temperature for 6 months or at 50° C. for 30 days. The emulsion can also withstand freezing conditions. The process allows the production of emulsions having a relatively high amino-functional polyorganosiloxane content and a relatively low water content.

[0111] Definition and usage of terms

[0112] Unless otherwise indicated, all amounts, ratios and percentages are by weight. Unless otherwise indicated, the words "a", "an" and "the" each refer to one (one) or more (multiple). The disclosure of a range includes the range itself and any values ​​and endpoints contained therein. Similarly, the disclosure of a Markush group includes the entire group and also includes any individual members and subgroups contained therein. For example, the disclosure of the Markush group methyl, ethyl, propyl and butyl includes the individual member ethyl; the subgroup methyl and ethyl; and any other individual members and subgroups contained therein.

[0113] Abbreviations used herein are defined as follows. The abbreviation "cP" means centipoise. The abbreviation "g" means gram. "L" means liter. The abbreviation "oz" means ounce. The abbreviation "rpm" means revolutions per minute. "RT" means room temperature, 23°C ± 2°C.

Claims

1. A method for preparing an emulsion, wherein the method include: 1) Mixing starting materials, the starting materials comprising 25 to 75 parts by weight of A) an amino-functional polyorganosiloxane; 2 to 10 parts by weight of B) a nonionic surfactant; and 4 to 20 parts by weight of C) water; 2) mixing the starting material with the product of step 1), wherein the starting material comprises 0.02 to 1 parts by weight of D) a salt, and Additional water; and 3) mixing starting materials, the starting materials comprising E) a pH adjusting agent, F) preservatives, and Optionally G) a freezing inhibitor; A prerequisite is that the emulsion contains no cationic surfactant.

2. The method according to claim 1, wherein the starting material A) comprises a unit of formula (R 1 2 SiO 2 / 2 ) a (R 1 R 2 SiO 2 / 2 ) b (ZO 1 / 2 ) d (R 1 3 SiO 1 / 2 ) e A poly(dialkyl / alkylamino)siloxane wherein each R 1 is an independently selected alkyl group of 1 to 6 carbon atoms; each R 2 Is independently selected type ZHN-R 3 -(ZNR 4 ) c - an amino-functional alkyl group, wherein R 3 is an alkylene group of 2 to 6 carbon atoms, R 4 is an alkylene group of 2 to 6 carbon atoms, and the subscript c is 0 or 1; each Z is independently selected from H and R 1 Subscripts a, b, d and e represent the average number of each unit per molecule in the unit formula, subscript a is 1 to 5, subscript b is 1 to 1000, subscript d is 0, 1 or 2; subscript e is 0, 1 or 2; And the number (d+e)=2.

3. The method according to claim 1, wherein B) the nonionic surfactant comprises a secondary alcohol ethoxylate.

4. The method according to claim 1, wherein step 1) is carried out at a temperature of 10°C to 70°C for 70s -1 To 700s -1 The reaction was carried out at a shear rate of 100 torr and a pressure of 760 torr.

5. The method according to claim 1, wherein step 1) comprises first mixing A) the amino-functional polyorganosiloxane and B) the nonionic surfactant; and then mixing C) the water with the mixture of A) and B).

6. The method of claim 1, wherein D) the salt has the formula MR 5 x , wherein M is selected from calcium (Ca), magnesium (Mg), potassium (K), ammonium (NH 4 ) and sodium (Na); R 5 is selected from the group consisting of a halogen atom, an acetate group, a benzoate group, and a sulfate group; and the subscript x is 1 or 2.

7. The method according to claim 6, wherein the halogen atom is selected from the group consisting of Br, Cl and I.

8. The method of claim 6, wherein D) the salt is selected from the group consisting of ammonium chloride, calcium bromide, calcium chloride, calcium iodide, calcium sulfate, magnesium chloride, potassium bromide, potassium chloride, sodium acetate, sodium benzoate, sodium bromide, sodium chloride, sodium iodide, and a combination of two or more thereof.

9. The method of claim 8, wherein D) the salt comprises sodium benzoate and one or more of the following: ammonium chloride, calcium bromide, calcium chloride, calcium iodide, calcium sulfate, magnesium chloride, potassium bromide, potassium chloride, sodium acetate, sodium bromide, sodium chloride, and sodium iodide.

10. The method according to claim 1, wherein step 2) and step 3) are carried out at a temperature of 10°C to 70°C for 7s -1 To 90s -1 The reaction was carried out at a shear rate of 100 torr and a pressure of 760 torr.

11. The method according to claim 1, further comprising one or more additional steps selected from the group consisting of: adding additional water and mixing after step 1) and before step 2); adding additional water and mixing during or after step 2) and before step 3); and Additional water is added during or after step 3) and mixed.

12. The method of claim 1, wherein E) the pH adjuster comprises acetic acid.

13. The method of claim 1, wherein F) the preservative comprises phenoxyethanol, benzyl alcohol, or a combination thereof.

14. The method of claim 1, wherein G) the freezing inhibitor is present, and wherein the freezing inhibitor is selected from the group consisting of propylene glycol, ethylene glycol, and combinations thereof.

15. An emulsion prepared by the method according to any one of the preceding claims, wherein the emulsion comprises: 25 to 75 parts by weight of A) the amino-functional polyorganosiloxane, 2 to 10 parts by weight of B) the nonionic surfactant, 25 to 75 parts by weight of C) water, 0.02 to 1 parts by weight of D) the salt, 0.02 to 0.2 parts by weight of E) the pH adjuster, 0.3 to 2 parts by weight of F) the preservative, and 0 to 2 parts by weight of G) the freezing inhibitor.