Composition

By using powder coatings prepared by using epoxy resin, imidazoline ring curing agent and other materials, the problem of damage to the battery cell coating after contact with the electrolyte is solved, high bond strength and electrolyte resistance are achieved, and fire risk is reduced. In new energy vehicle battery cells.

CN118922505APending Publication Date: 2024-11-08JOTUN AS LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380027746.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-22
Filing Date
2023-03-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing battery cell coating is prone to damage after contact with the electrolyte, losing its insulation and adhesion. The softening of traditional PET tape at high temperature increases the risk of fire, which cannot meet the high bond strength and electrolyte resistance of new energy vehicles. need.

Method used

Using powder coating compositions containing epoxy resin, imidazoline ring curing agent, filler and degassing agent, granular coating is formed by blending and extrusion, applied to the surface of the battery cell and cured to form electrolyte resistance and high viscosity. Coating of junction strength.

Benefits of technology

It realizes the electrical insulation and beautiful appearance of the coating after the electrolyte contact, enhances the adhesion to the battery cell, reduces the risk of fire, and meets the requirements of new energy vehicles for high bond strength and electrolyte resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005042898640000121
    Figure BDA0005042898640000121
  • Figure BDA0005042898640000281
    Figure BDA0005042898640000281
  • Figure BDA0005042898640000291
    Figure BDA0005042898640000291
Patent Text Reader

Abstract

The present invention provides a particulate coating composition, and preferably a powder coating composition, the composition comprising: (i) an epoxy resin, (ii) a curing agent wherein the curing agent comprises an imidazoline ring; (iii) a filler; and (iv) a degassing agent, preferably benzoin, where the total amount of the epoxy binder system is from 40 to 99% by weight, based on the total weight of the particulate coating composition, where the system comprises the epoxy resin and the curing agent.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] introduction

[0002] The present invention relates to a granular coating composition, in particular a powder coating composition, comprising an epoxy resin, a curing agent comprising an imidazoline ring, a filler and a degassing agent. The present invention also relates to a container containing the composition and a method for preparing the composition. In addition, the present invention relates to a coating comprising the composition, a substrate coated with the composition and a method for coating a substrate with the composition.

[0003] The coatings of the present invention advantageously have strong electrolyte resistance, i.e. they retain their electrical insulation after contact with an electrolyte, as well as their aesthetic appearance. Therefore, the present invention also relates to a battery assembly comprising a battery cell having a coating formed on at least one surface thereof, wherein the coating is formed from a powder coating composition comprising an epoxy resin, a curing agent including an imidazole ring, an imidazoline ring or an imidazolidine ring, a filler and a degassing agent. Background Art

[0004] Electric vehicles have become one of the fastest growing sectors in recent years, driven by the growing demand for more environmentally friendly modes of transportation, especially to reduce CO2 emissions. The battery is the heart of the electric vehicle.

[0005] An electric vehicle typically includes a battery assembly containing a plurality of battery cells, each of which contains an electrolyte. The battery cells may be arranged in different configurations, but are interconnected to provide an overall battery assembly. Typically, the assembly includes modules and fixtures for holding the battery cells.

[0006] Blue PET tape is traditionally used for insulation of battery cells in electric vehicles. However, there are some disadvantages to the use of PET tape, for example, because it is a thermoplastic film, it softens at higher temperatures and dimensional stability becomes a problem at higher temperatures. In addition, PET melts at temperatures above about 110°C, which increases the risk of battery fires. This is a particular concern for battery manufacturers because battery cells made with PET film allow fires to spread quickly. Finally, in the case of PET film, a reduction in adhesion occurs when rapid temperature changes occur, which can short-circuit the battery.

[0007] At the same time, the demand for energy density of batteries in the automotive industry is growing. As a result, there is a trend to remove modules and fixtures present in the battery assembly to provide more space for battery cells. This technology is called "Cell to Pack (CTP)" technology. Because there are no fixtures in the CTP battery assembly or pack, the battery cells in the battery pack must be bonded together with structural adhesive to form a block. The bonded units need to survive vibrations during the service life of the electric vehicle. Therefore, the bonding strength between the battery cells is crucial. PET tape has a low bonding strength of about 5MPa to the aluminum substrate of the battery and cannot meet the high requirements of new technologies.

[0008] As a possible alternative to conventional PET tapes, powder coatings with no volatile organic compounds (VOCs) and excellent adhesion to both the aluminum substrate of the battery cell and the structural adhesive for CTP battery assembly are gaining more and more attention. One of the main challenges to overcome in turning this concept into reality is to provide a coating with electrolyte resistance, i.e., a coating with properties that are not negatively affected by contact with electrolytes.

[0009] The minimum powder coating curing temperature is 120-130°C. However, if the electrolyte present in the battery cell is exposed to these temperatures, the electrolyte will be damaged. Therefore, the battery cell must be coated with powder coating first and then filled with electrolyte. Unfortunately, spillage is inevitable during electrolyte filling and there will also be some electrolyte evaporation. The powder coating must maintain its designed electrical insulation and other properties after contact with the electrolyte.

[0010] This is a challenge because the chemicals present in the electrolyte are highly corrosive. For example, lithium batteries contain solvents, additives and lithium salts, primarily lithium hexafluorophosphate (LiPF6) and other lithium-based salts. When the electrolyte overflows during filling, the coating on the battery cell comes into contact with harmful hydrofluoric acid produced by the reaction of LiPF6 and water present in the air. If a large overflow occurs, the coating is destroyed very quickly, and even if a small overflow occurs, the coating is irreversibly damaged, such as losing insulation. Other chemicals present in the electrolyte, such as solvents, similarly have a negative impact on the key properties of the coating in the event of contact. For example, contact with the electrolyte typically causes the coating to discolor, lose its insulating effect and / or lose adhesion to the substrate.

[0011] Other types of batteries may contain different salts, for example based on nickel, cobalt and manganese salts, but they all tend to contain similar solvents. The main components of the solvents are ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), carboxylates and fluoroethers. Coatings suitable for battery cells must be able to withstand contact with these solvents and the corrosive compounds formed in the event of a leak. Summary of the invention

[0012] Viewed from a first aspect, the present invention provides a granular coating composition, and preferably a powder coating composition, comprising:

[0013] (i) epoxy resin,

[0014] (ii) a curing agent, wherein the curing agent comprises an imidazoline ring;

[0015] (iii) fillers; and

[0016] (iv) a degassing agent, preferably benzoin,

[0017] The total amount of the epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0018] Viewed from another aspect, the invention provides a container containing a granular coating composition, and preferably a powder coating composition, as hereinbefore described.

[0019] Viewed from another aspect, the present invention provides a process for preparing a granular coating composition, and preferably a powder coating composition, as hereinbefore described, the process comprising:

[0020] (i) blending an epoxy resin, a curing agent, a filler, and a degassing agent to form a mixture, wherein the curing agent comprises an imidazoline ring; and

[0021] (ii) extruding the mixture to form granules.

[0022] Viewed from another aspect the invention provides the use of a granular coating composition, and preferably a powder coating composition, as hereinbefore described for coating a substrate, preferably a metal substrate such as aluminium.

[0023] Viewed from another aspect, the invention provides a method for coating a substrate, preferably a metal substrate such as aluminium, with a granular coating composition, preferably a powder coating composition as hereinbefore described, the method comprising:

[0024] i) applying the granular coating composition to the substrate; and

[0025] ii) curing the granular coating composition.

[0026] Viewed from another aspect the invention provides a coating, preferably a cured coating, comprising a granular coating composition, and preferably a powder coating composition, as hereinbefore described.

[0027] Viewed from another aspect the invention provides a substrate, preferably a metal substrate such as aluminium, coated with a granular coating composition and preferably a powder coating composition as hereinbefore described or a coating as hereinbefore described.

[0028] Viewed from another aspect, the present invention provides a battery assembly comprising at least one battery cell, wherein the at least one battery cell has a coating formed on at least one surface, and the coating is formed from a composition comprising:

[0029] (i) epoxy resin,

[0030] (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0031] (iii) fillers; and

[0032] (iv) a degassing agent, preferably benzoin, and

[0033] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0034] Preferably, the composition is as described above.

[0035] Viewed from another aspect, the present invention provides the use of a granular coating composition comprising the following components for forming an electrolyte-resistant coating on at least one surface of a substrate, preferably a battery cell:

[0036] (i) epoxy resin,

[0037] (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0038] (iii) fillers; and

[0039] (iv) a degassing agent, preferably benzoin;

[0040] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0041] Viewed from another aspect, the present invention provides the use of a granular coating composition comprising the following components for protecting a substrate, in particular a battery cell, from electrolyte:

[0042] (i) epoxy resin,

[0043] (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0044] (iii) fillers; and

[0045] (iv) a degassing agent, preferably benzoin;

[0046] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0047] Viewed from another aspect, the present invention provides the use of a granular coating composition comprising the following components for coating at least one aluminum surface of a battery cell:

[0048] (i) epoxy resin,

[0049] (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0050] (iii) fillers; and

[0051] (iv) a degassing agent, preferably benzoin;

[0052] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0053] Viewed from another aspect, the present invention provides the use of a granular coating composition comprising the following components for forming at least a base layer on a battery cell:

[0054] (i) epoxy resin,

[0055] (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0056] (iii) fillers; and

[0057] (iv) a degassing agent, preferably benzoin;

[0058] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0059] Viewed from another aspect, the present invention provides the use of a granular coating composition comprising the following components for coating a battery cell:

[0060] (i) epoxy resin,

[0061] (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0062] (iii) fillers; and

[0063] (iv) a degassing agent, preferably benzoin;

[0064] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0065] Viewed from another aspect, the invention provides a method for protecting a surface from electrolyte damage, the method comprising:

[0066] (a) applying a particulate coating composition to the surface; and

[0067] (b) curing the coating composition to obtain a coating,

[0068] The granular coating composition comprises:

[0069] (i) epoxy resin,

[0070] (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0071] (iii) fillers; and

[0072] (iv) a degassing agent, preferably benzoin,

[0073] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0074] Viewed from another aspect, the invention provides a method of retaining electrical insulation of a coating on a substrate after the coating has been exposed to (e.g., contacted with) an electrolyte, the method comprising:

[0075] (a) applying a particulate coating composition to the surface; and

[0076] (b) curing the coating composition to obtain a coating,

[0077] The granular coating composition comprises:

[0078] (i) epoxy resin,

[0079] (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0080] (iii) fillers; and

[0081] (iv) a degassing agent, preferably benzoin.

[0082] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0083] definition

[0084] As used herein, the term "particulate coating composition" refers to a mixture of particles that, when applied to a surface and heated, such as to cure, form a coating on the surface.

[0085] As used herein, the term "powder coating composition" refers to a dry free-flowing powder that forms a coating on a surface when applied to the surface and heated, for example, cured. Typically, the average diameter of the particles making up the powder is from 10 to 120 μm.

[0086] As used herein, the term "epoxy" refers to a three-atom cyclic ether.

[0087] As used herein, the term "epoxy" refers to a polymer or oligomer containing epoxy groups and / or modified epoxy groups. The term epoxy adhesive covers adhesives having a traditional epoxy backbone but wherein the epoxy end groups are modified with, for example, acrylic acid or methacrylic acid functional groups, which can be cured with the same curing agent as the epoxy groups. Epoxy adhesives will contain at least some epoxy groups. The terms "epoxy" and "epoxide" are used interchangeably.

[0088] As used herein, the term "solid epoxy resin" refers to an epoxy polymer that is solid at ambient temperature and pressure (25°C and 1 atm). Thus, the term "solid" refers to the physical state of the epoxy-based adhesive.

[0089] As used herein, the phrase "epoxy equivalent weight" or "EEW" refers to the number of grams of epoxy resin required to provide 1 mole of epoxy groups. It is measured by ASTM D-1652.

[0090] Unless otherwise indicated, as used herein, the term "molecular weight" refers to weight average molecular weight (Mw).

[0091] As used herein, the term "curing agent" refers to a compound that, when mixed with an epoxy resin, produces a cured or hardened coating by creating crosslinks within the polymer. Sometimes, a curing agent is referred to as a hardener.

[0092] As used herein, the terms "cure accelerator" and "accelerator" are used synonymously and refer to compounds that increase the rate of the curing reaction that causes a coating to cure or harden.

[0093] As used herein, the term "filler" refers to solid particles. Typically, fillers are incorporated into granular coating compositions to increase their capacity. Sometimes, fillers are referred to as "extenders."

[0094] As used herein, the term "spherical" when used with respect to particles encompasses both substantially spherical and spherical particles. Substantially spherical particles have the same size in each of the x, y and z dimensions within ±1.2 μm, more preferably ±0.6 μm.

[0095] As used herein, the term "average diameter" refers to the Z-average diameter size determined by ISO 22412:2017 using a Malvern Mastersizer 2000.

[0096] As used herein, the term D 90 It refers to the size at which 90% of the particles have diameters smaller than the reported value.

[0097] As used herein, the term D 50 It refers to the size at which 50% of the particles have diameters smaller than the reported value.

[0098] As used herein, the term D 10 It refers to the size at which 10% of the particles have a diameter smaller than the stated value.

[0099] As used herein, the term "degassing agent" refers to a compound added to a composition to remove gases, such as air, and / or to promote the dissolution of gases to avoid the formation of pinholes or bubbles in the formed coating.

[0100] As used herein, the term "leveling agent" refers to a compound added to a granular coating composition during the melting stage to facilitate powder flow, for example by breaking weak bonds between particles within the powder and / or by lubricating the movement.

[0101] As used herein, the term "flow additive" or "flow agent" refers to a compound added to a granular coating composition to reduce surface tension and reduce surface defects (such as craters, pinholes and fish eyes) and improve surface smoothness.

[0102] As used herein, the term "color pigment" is a pigment added to a composition to provide color. Color pigments include white pigments, such as TiO2.

[0103] As used herein, the term "rheology modifier" refers to a compound that improves the consistency uniformity and coating properties of a coating composition.

[0104] As used herein, when the term "weight % (wt%)" is used with respect to a coating composition, it refers to the weight of each component in the composition relative to the total weight of the composition. The total weight % of any given coating composition is 100 weight %. DETAILED DESCRIPTION

[0105] The present invention relates to a granular coating composition, comprising:

[0106] (i) epoxy resin,

[0107] (ii) a curing agent, wherein the curing agent comprises an imidazoline ring;

[0108] (iii) fillers; and

[0109] (iv) a degassing agent, preferably benzoin,

[0110] The total amount of the epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0111] Preferably, the granular coating composition is a powder coating composition.

[0112] Optionally, the coating composition of the present invention further comprises: (v) a flow additive; (vi) a color pigment; (vii) a leveling agent and / or (viii) an additive.

[0113] Compared to other granular coatings, the granular coating compositions of the present invention advantageously produce coatings that are more resistant to contact with electrolytes (e.g., electrolytes present in lithium batteries). More specifically, the coating compositions of the present invention produce coatings that retain their insulation and voltage resistance even after immersion in electrolytes (i.e., extreme conditions). The coating compositions of the present invention also produce coatings that are less prone to discoloration after contact with electrolytes than other powder coatings, which means that they retain a pleasing aesthetic appearance longer. The coatings produced by the coating compositions of the present invention achieve improved resistance to damage caused by electrolyte contact while maintaining suitable adhesion to metals, such as aluminum substrates.

[0114] Epoxy resin

[0115] The granular coating composition of the present invention comprises an epoxy resin, which is preferably a solid epoxy resin.

[0116] Preferred epoxy resins present in the coating composition of the present invention have an epoxy equivalent weight (EEW) of 200-1950 g / eq, more preferably 200 to 1300 g / eq, and still more preferably 400-1300 g / eq.

[0117] There are two main types of epoxy resins, namely glycidyl epoxy resins and non-glycidyl epoxy resins. Some types of glycidyl epoxy resins include glycidyl ether type epoxy resins, glycidyl ester type epoxy resins, and glycidyl amine type epoxy resins. Some types of non-glycidyl epoxy resins include aliphatic epoxy resins and alicyclic epoxy resins.

[0118] Preferably, the solid epoxy resin present in the granular coating composition of the present invention comprises a glycidyl epoxy resin, and more preferably a glycidyl ether type epoxy resin. Glycidyl ether type epoxy resins are generally prepared by a condensation reaction of a dihydroxy compound with epichlorohydrin. Preferably, the dihydroxy compound is a bisphenol compound. Therefore, preferably, the epoxy resin is a bisphenol-based epoxy resin.

[0119] Representative examples of solid epoxy resins suitable for use in the composition of the present invention include bisphenol A epoxy resins, bisphenol F epoxy resins, novolac-modified bisphenol A epoxy resins, isocyanate-modified bisphenol A epoxy resins, cresol novolac-type epoxy resins, o-cresol epoxy resins, silane-modified bisphenol A epoxy resins, rubber-modified bisphenol A epoxy resins, silicone-modified bisphenol A epoxy resins, and various mixtures thereof. In a preferred granular coating composition, the solid epoxy resin is selected from bisphenol A epoxy resins, bisphenol F epoxy resins, novolac-modified bisphenol A epoxy resins, isocyanate-modified bisphenol A epoxy resins, cresol novolac-type epoxy resins, o-cresol epoxy resins, and various mixtures thereof. In a particularly preferred granular coating composition, the solid epoxy resin is selected from bisphenol A epoxy resins, novolac-modified bisphenol A epoxy resins, bisphenol F epoxy resins, isocyanate-modified bisphenol A epoxy resins, and various mixtures thereof. Bisphenol A epoxy resins, novolac-modified bisphenol A epoxy resins, and various mixtures thereof are particularly preferred. Bisphenol A epoxy resins are particularly preferred.

[0120] The epoxy equivalent weight (EEW) of the preferred solid epoxy resin (e.g., bisphenol A epoxy resin, novolac-modified bisphenol A epoxy resin) present in the coating composition of the present invention is 200-1950 g / eq, more preferably 200 to 1300 g / eq, still more preferably 400-1300 g / eq, still more preferably 700-1300 g / eq, and especially preferably 700 to 1000 g / eq. It is believed that EEW plays an important role in the performance of the coating. Epoxy resins with relatively lower EEW tend to have lower viscosity and better wettability, and thus better adhesion, but too low EEW leads to sagging and / or bubbles in the final coating. On the other hand, epoxy resins with relatively high EEW tend to slow down the degassing of air in the coating when it is cured, which is believed to be detrimental to electrolyte resistance. Furthermore, if the EEW of the epoxy resin is too low or too high, handling of the composition during coating is challenging and the final coating produced from the composition tends to have poor appearance, poor coverage at the edges of the substrate (resulting in poor protection at the edges), and poor storage stability.

[0121] The granular coating composition of the present invention may include one or more solid epoxy resins. In some preferred granular coating compositions of the present invention, only one type of solid epoxy resin is present, and in particular, a bisphenol A-based epoxy resin, a novolac-modified bisphenol A-based epoxy resin, or an isocyanate-modified bisphenol A-based epoxy resin. Other preferred coating compositions of the present invention contain a mixture of two or more, for example, 2 types of solid epoxy resins. A mixture of a bisphenol A-based epoxy resin and a novolac-modified bisphenol A-based epoxy resin is particularly preferred. When a mixture of a bisphenol A-based epoxy resin and a novolac-modified bisphenol A-based epoxy resin is used, the weight ratio of the bisphenol A-based epoxy resin to the novolac-modified bisphenol A-based epoxy resin is preferably 10:1 to 1:10, more preferably 5:1 to 1:5, and still more preferably 2:1 to 1:2.

[0122] Suitable epoxy resins are commercially available. Representative examples of suitable epoxy resins include KD-213, KD-214C, KD-242K, KD-2200, KD-242G, KD-243G, KD-2103, KD-214M, KD-2203, KD-2104, KD214L, KD-9002, KD-9003, KD-9004, KD-213C, KD-213H, DER 6805, NPCN-704, DER6224, DER6225, DER662E, KD-211G, DER662UH, DER6635, DER663U, DER663UE, DER664, DER664U, DER664UE, DER672U DER6510HT, YDCN-500-90P, BE501H, BE502L, BE502, BE503L, BE503, BE504, BE504H, BE 505H, BE507, YD-017, BE574P, BFE107, MOE-380, MOE-400, CNE202, CNE220, CNE220H, BE 502S, BE503S, NPES-901, NPES-901H, NPES-902, NPES-902H, NPES-903K, NPES-903, NPES-903H, NPES-904, NPES-303, NPES-904H, NPES-304, NPES-907, NPCN-704 and NPER-450.

[0123] The total amount of epoxy resin present in the granular coating composition of the present invention is preferably 38-99 wt%, and more preferably 38-95 wt%, based on the total weight of the granular coating composition. Preferably, the weight of the epoxy resin present in the granular coating composition is 40-99 wt% (e.g., 40-95 wt%), more preferably 50-95 wt%, and still more preferably 60-90 wt%, based on the total weight of the granular coating composition.

[0124] Curing agent

[0125] The granular coating composition of the present invention also includes a curing agent. The curing agent reacts with the epoxy resin during curing to form a coating, such as a film coating. Therefore, the curing agent is beneficial to provide a coating composition with an acceptable curing time.

[0126] The curing agent present in the granular coating composition of the present invention comprises an imidazoline ring. The imidazoline ring may be 2-imidazoline, 3-imidazoline or 4-imidazoline. Preferably, the imidazoline ring is 2-imidazoline.

[0127] The imidazoline ring present in the curing agent present in the granular coating composition of the present invention may be unsubstituted or substituted. Preferably, the imidazoline ring is substituted. Any number of substituents may be present, more preferably one or two substituents are present, and still more preferably one substituent.

[0128] When substituted, the imidazoline ring may be substituted at any position. Preferably, the imidazoline ring is substituted at the 2-position, for example, a preferred curing agent comprises an imidazoline ring substituted at the 2-position. Optionally, the imidazoline ring present in the curing agent present in the granular coating composition of the present invention is a dimer, the dimer being connected, for example, by an alkylene linker between the two 2-positions of the imidazoline ring.

[0129] Examples of suitable substituents that may be present on the imidazoline ring include aromatic substituents, C1–C 12 Alkyl substituents, C1-C6 alkylene substituents, alcohols, amines, halides, C1-C6 alkoxy groups, and nitriles. Preferred substituents include aromatic substituents (e.g., phenyl or benzyl) and C1-C 12 Alkyl substituents (such as methyl). More preferred substituents include aromatic substituents (such as phenyl or benzyl) and C2-C 12 Alkyl substituents. Still more preferably, the imidazoline ring has aromatic substituents. Examples of suitable aromatic substituents include phenyl and heterocycles such as pyridine, imidazole, furan and thiophene. A preferred aromatic substituent is phenyl, especially unsubstituted phenyl.

[0130] The nitrogen atom of the imidazoline ring may be substituted or unsubstituted. Examples of suitable substituents include C1-C 12 Alkyl groups, alkyl alcohols and alkyl amines. The nitrogen atom is preferably unsubstituted.

[0131] When a phenyl group is present as a substituent on the imidazoline ring, the phenyl group may be unsubstituted or substituted. Examples of suitable substituents include C1-C6 alkyl, C1-C6 alkoxy, nitrile, hydroxy, halide, thiol and amine. The phenyl substituent may have one or more substituents located at any position on the aromatic ring. Preferably, the phenyl group present as a substituent is unsubstituted.

[0132] Particularly preferred granular coating compositions of the present invention comprise a curing agent comprising a 2-imidazoline ring.

[0133] Particularly preferred curing agents present in the coating composition of the present invention comprise a 2-imidazoline ring substituted at the 2-position (e.g. consist of a 2-imidazoline ring substituted at the 2-position). Still more preferably, the substituent is an aromatic substituent (e.g. phenyl) or a C1-C 12 More preferably, the substituent is an aromatic substituent (e.g., phenyl) or a C2-C12 Alkyl substituents.

[0134] Particularly preferably, the curing agent present in the granular coating composition of the present invention comprises (eg consists of) 2-phenyl-2-imidazoline (Cas No: 936-49-2).

[0135]

[0136] More typically, imidazolines act as accelerators. Without being bound by theory, it is believed that they act as curing agents in the present coating compositions.

[0137] The curing agent preferably comprises 2-phenyl-2-imidazoline, for example in an amount of >50 wt %, more preferably >75 wt %, still more preferably >90 wt % and still more preferably >95 wt % of the curing agent.

[0138] The purity of 2-phenyl-2-imidazoline preferably present in the granular coating composition is preferably 98% or more, more preferably 99% or more.

[0139] Suitable curing agents containing imidazoline rings are commercially available. For example, 2-phenyl-2-imidazoline for use in the granular coating composition of the present invention is commercially available, for example, under the trade name HC31 from Huangshan Huahui Technology Co. Ltd., under the trade name Vestagon B31 from Evonik Degussa Coatings & Colour, and under the trade name MB 31 from Huangshan Deping Chemical Co. Ltd.

[0140] It will be appreciated that the curing agent and epoxy resin need to react in order to cure the coating. The appropriate amounts of curing agent and epoxy resin depend on the relative amounts of reactive groups, i.e., the epoxide in the epoxy resin and the amine in the curing agent. Generally speaking, the amount of curing agent present (in wt%) is preferably 1-35 wt%, more preferably 1.5-20 wt%, and still more preferably 2-15 wt%, based on the amount of epoxy resin present (in wt%).

[0141] It is preferred that these components be mixed in a ratio such that the curing agent is present in a stoichiometric amount of 80-120%, more preferably 90-115%, and still more preferably 100-110%, based on the number of reactive groups present in the curing agent relative to the number of reactive groups present in the epoxy resin.

[0142] The total amount of epoxy binder system, comprising one or more epoxy resins and one or more curing agents, is preferably 40-99 wt%, more preferably 50-95 wt%, and still more preferably 60-90 wt%, based on the total weight of the granular coating composition.

[0143] In the preferred coating composition of the present invention, the binder system is a pure epoxy resin system. Therefore, preferably, no other type of resin (such as a copolymer) is present in the binder system.

[0144] Fillers

[0145] The granular coating composition of the present invention comprises a filler. Preferred fillers present in the granular coating composition are inorganic fillers. Suitable inorganic filler particles exist in different forms, such as spherical, lamellar, nodular and irregular forms.

[0146] The amount of filler present in the granular coating composition of the present invention is 50 It is preferably 0.5 to 25 μm, more preferably 1 to 20 μm, still more preferably 1 to 15 μm, still more preferably 1 to 10 μm.

[0147] In the preferred granular coating composition of the present invention, the filler is selected from barium sulfate (preferably precipitated barium sulfate), mica, talc, wollastonite (calcium metasilicate), glass flakes, nepheline, kaolin, dolomite, diatomaceous earth, boron nitride, aluminum oxide, aluminum hydroxide and various mixtures thereof, and more preferably selected from barium sulfate (preferably precipitated barium sulfate), kaolin and various mixtures thereof. In particularly preferred granular coating compositions, the filler is selected from precipitated barium sulfate, kaolin, mica and various mixtures thereof.

[0148] The granular coating composition of the present invention may contain a single filler or a combination of two or more fillers. In some preferred granular coating compositions, a single filler is present. When a single filler is present, the filler is preferably selected from precipitated barium sulfate, wollastonite (calcium metasilicate), glass flakes, nepheline, kaolin, dolomite, diatomaceous earth, boron nitride, aluminum oxide, aluminum hydroxide, and various mixtures thereof.

[0149] In some other preferred granular coating compositions, a combination of two fillers is preferred. Representative examples of some preferred combinations include: precipitated barium sulfate and mica, precipitated barium sulfate and talc, precipitated barium sulfate and kaolin, mica and talc, kaolin and talc, and kaolin and mica. Particularly preferred filler combinations are precipitated barium sulfate and kaolin, kaolin and talc, and kaolin and mica.

[0150] Suitable fillers are commercially available. Representative examples of suitable fillers include Blanc Fine GM-80 from Gemme Speciality Chemicals Co. Ltd., Blanc Fixe L from Yillong Chemical Group Limited, GL-2500 from Jiangsu Qunxin powder technology Co. Ltd., Specs white and Micro Mica W1 from Imerys Minerals Ltd., JLH-60D and H6 from Shenzhen JinHaoHui Industrial Development Co. Ltd., and GA-1 from Chuzhou Gera Minerals Co. Ltd.

[0151] The total amount of filler present in the granular coating composition of the present invention is preferably 0.01 - 60 wt%, more preferably 1.5-50 wt%, and still more preferably 10-38 wt%, based on the total weight of the granular coating composition.

[0152] Degassing agent

[0153] The granular coating composition of the present invention contains a degassing agent. Conventional commercially available degassing agents can be used.

[0154] Representative examples of suitable degassing agents include cyclohexanedimethanol dibenzoate, benzoin, benzoin derivatives and various mixtures thereof. Preferably, the degassing agent is benzoin or a benzoin derivative, and particularly preferably benzoin. Suitable degassing agents can be obtained from numerous commercial suppliers, for example benzoin can be obtained from Miwon Speciality Chemical Co. Ltd. under the trade name Miwon benzoin, and as benzoin, from Orgamine Chemicals PVT Ltd. and Ningbo South Sea Chemical Co. Ltd.

[0155] Preferred coating compositions of the present invention comprise 0.15-0.45 wt. %, more preferably 0.17-0.4 wt. % and still more preferably 0.2-0.35 wt. % of degassing agent, based on the total weight of the granular coating composition.

[0156] Flowability Additives

[0157] The granular coating composition of the present invention preferably comprises a flow additive. The presence of the flow additive tends to improve surface smoothness, for example by reducing or eliminating surface defects such as pits, fish-eye cracks and pinholes. This is achieved by improving the melt flow characteristics of the granular coating composition.

[0158] Conventional commercially available flowability additives may be used, such as PCL-100 from Kscnt Co. Ltd., Rheoflow PLP 100H(A) from KS Chemical Co. Ltd., and Resiflow PV 88 from Worlee-Chemie GmbH.

[0159] Representative examples of suitable flow additives include acrylic resins, silicon-containing compounds, and fluorine-based polymers.Preferred granular coating compositions of the present invention contain a flow additive which is an acrylic resin.

[0160] Preferred coating compositions of the present invention comprise 0.01 to 5 wt%, more preferably 0.1 to 3 wt%, and still more preferably 0.5 to 1.5 wt% of a flow additive, based on the total weight of the granular coating composition.

[0161] Color Pigments

[0162] The granular coating composition of the present invention preferably comprises at least one color pigment. The color pigment may be an inorganic or organic color pigment. Organic color pigments are preferred.

[0163] Representative examples of inorganic color pigments suitable for inclusion in the granular coating composition of the present invention include titanium dioxide, red iron oxide, black pigments, yellow pigments, chrome pigments, carbon black, and various combinations thereof.

[0164] Representative examples of organic pigments suitable for inclusion in the granular coating composition of the present invention include phthalocyanine, azo, dioxazine, perylene, anthraquinone, thioindigo, isodibenzanthrone, triphendioxane, quinacridone pigments, vat dye pigments, and various combinations thereof.

[0165] Preferred color pigments for inclusion in the granular coating composition of the present invention are selected from titanium dioxide, carbon black, organic red pigments, organic yellow pigments, organic blue pigments, ultramarine blue and organic green pigments.

[0166] Other preferred granular coating compositions of the present invention contain less than 5 wt%, more preferably less than 2 wt%, and still more preferably less than 1.1 wt% carbon black. Without wishing to be bound by theory, it has been found that when higher levels of carbon black are present, the electrolyte resistance of the resulting coating is compromised. This is believed to be due to the electrical conductivity of carbon black.

[0167] Suitable color pigments are commercially available, for example, NTR-606, Beablack 2669F, Beablack 2870F, Red 122, DPP Red SR2P, Yellow 139, Sudafast blue 2789, Blue 51, Green 2730K.

[0168] In general, the color pigment should be included in the granular coating composition in the minimum amount necessary to provide the desired color. The amount of color pigment required depends to a certain extent on the type of color pigment. For example, titanium dioxide can be present in an amount of 25% by weight, while carbon black can be present in an amount of up to 1.1% by weight. The technician will be able to determine the appropriate amount for different types of pigments.

[0169] When present, the color pigment is preferably present in the granular coating composition of the present invention in an amount of 0.0005-30 wt%, more preferably 0.001-25 wt%, and still more preferably 0.01-20 wt%, based on the total weight of the granular coating composition.

[0170] Leveling agent

[0171] The granular coating composition of the present invention preferably comprises a leveling agent. Examples of suitable leveling agents include copolymers of methyl acrylate and butyl acrylate. Suitable leveling agents are commercially available, such as BLC701B from Ningbo South Sea Chemical Co. Ltd. and WK701 from Ningbo Wecan Chemical Co., Ltd. The leveling agent improves the melt flow characteristics of the composition and helps eliminate surface defects during curing.

[0172] When present, the leveling agent is preferably present in the granular composition of the present invention in an amount of 0.01 to 5 wt%, more preferably 0.1 to 3 wt%, and still more preferably 0.5 to 1.5 wt%, based on the total weight of the granular coating composition.

[0173] additive

[0174] The granular coating composition of the present invention optionally comprises one or more additives. Examples of additives optionally present in the composition of the present invention include metal phosphates, metal borates, amino alcohols, adhesion promoters, gloss modifiers, driers, waxes, ethylene bisstearamide (EBS), antioxidants, rheological additives, matting agents, and surface modifiers. Preferred additives present in the granular coating composition of the present invention are gloss modifiers, rheological modifiers, surface modifiers, matting agents, and various mixtures thereof. Representative examples of suitable rheological modifiers are hydrogenated castor oil and low melting point polyethylene wax.

[0175] The further additives are preferably present in an amount of 0-10 wt %, more preferably 0.1-5 wt %, still more preferably 0.2-4 wt % and particularly preferably 0.5-3 wt %, based on the total weight of the granular coating composition.

[0176] Composition

[0177] A preferred granular coating composition of the present invention comprises:

[0178] (i) epoxy resin,

[0179] (ii) a curing agent, wherein the curing agent comprises an imidazoline ring;

[0180] (iii) fillers;

[0181] (iv) a degassing agent, preferably benzoin;

[0182] (v) flow additives;

[0183] (vi) preferably a colour pigment; and

[0184] (vii) leveling agent,

[0185] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0186] Another preferred granular coating composition of the present invention comprises:

[0187] (i) epoxy resin,

[0188] (ii) a curing agent, wherein the curing agent comprises an imidazoline ring;

[0189] (iii) a filler selected from the group consisting of barium sulfate (preferably precipitated barium sulfate), mica, talc, wollastonite (calcium metasilicate), glass flakes, nepheline, kaolin, dolomite, diatomaceous earth, boron nitride, aluminum oxide, aluminum hydroxide, and various mixtures thereof;

[0190] (iv) benzoin;

[0191] (v) flow additives;

[0192] (vi) colour pigments; and

[0193] (vii) leveling agent,

[0194] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0195] Yet another preferred granular coating composition of the present invention comprises:

[0196] (i) an epoxy resin, wherein the epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac-modified bisphenol A epoxy resin, isocyanate-modified bisphenol A epoxy resin, cresol novolac-type epoxy resin, o-cresol epoxy resin, silane-modified bisphenol A epoxy resin, rubber-modified bisphenol A epoxy resin, silicone-modified bisphenol A epoxy resin, and mixtures thereof;

[0197] (ii) a curing agent, wherein the curing agent comprises an imidazoline ring;

[0198] (iii) a filler selected from the group consisting of barium sulfate (preferably precipitated barium sulfate), mica, talc, wollastonite (calcium metasilicate), glass flakes, nepheline, kaolin, dolomite, diatomaceous earth, boron nitride, aluminum oxide, aluminum hydroxide, and various mixtures thereof;

[0199] (iv) benzoin;

[0200] (v) flow additives;

[0201] (vi) colour pigments; and

[0202] (vii) leveling agent,

[0203] The total amount of the epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0204] Another preferred granular coating composition of the present invention comprises:

[0205] (i) 38-95 wt %, preferably 40-95 wt %, more preferably 50-95 wt % and still more preferably 60-90 wt % of an epoxy resin;

[0206] (ii) 1-35 wt %, preferably 1.5-20 wt %, and more preferably 2-15 wt % of a curing agent based on the epoxy resin, wherein the curing agent contains an imidazoline ring;

[0207] (iii) 0.01-60 wt % filler, preferably 1.5-50 wt % and more preferably 10-38 wt % filler;

[0208] (iv) 0.15-0.45 wt. %, preferably 0.17-0.4 wt. % and more preferably 0.2-0.35 wt. % of a degassing agent, preferably benzoin,

[0209] Unless otherwise indicated, all weight % are based on the total weight of the granular composition.

[0210] In a particularly preferred granular coating composition of the present invention, the curing agent is 2-phenyl-2-imidazoline.

[0211] Preferred granular coating compositions of the present invention have a pigment volume concentration (PVC) of 0-25, more preferably 7-18, and still more preferably 9-13, for example, calculated from the theoretical density of the components of the coating and their weight %.

[0212] Some particularly preferred granular coating compositions of the present invention are as follows:

[0213] -Bisphenol F epoxy resin: 65.9 wt%, 2-phenylimidazoline: 4.1 wt%, pigment: 8.4 wt%, precipitated barium sulfate: 20.2 wt%, benzoin, flow agent and additives: 1.4 wt%,

[0214] - Epoxy type 3: 64.8 wt%, 2-phenylimidazoline: 5.2 wt%, pigment: 8.4 wt%, precipitated barium sulfate: 20.2 wt%, benzoin, flow agent and additives: 1.4 wt%,

[0215] - Epoxy resin type 3: 64.2 wt.%, 2-phenylimidazoline: 5.8 wt.%, pigment: 8.4 wt.%, precipitated barium sulfate: 20.2 wt.%, benzoin, flow agent and additives: 1.4 wt.%,

[0216] - Epoxy resin type 3: 66.5 wt%, 2-phenylimidazoline: 3.5 wt%, precipitated barium sulfate: 27.1 wt%, organic green pigment: 1.5 wt%, benzoin, flow agent and additives: 1.4 wt%,

[0217] - Epoxy resin type 3: 66.5 wt%, 2-phenylimidazoline: 3.5 wt%, carbon black: 1.1 wt%, precipitated barium sulfate: 27.5 wt%, benzoin, flow agent and additives: 1.4 wt%,

[0218] - Epoxy resin type 3: 66.5 wt.%, 2-phenylimidazoline: 3.5 wt.%, pigment: 8.4 wt.%, kaolin: 20.2 wt.%, benzoin, flow agent and additives: 1.4 wt.%,

[0219] - Epoxy resin type 3: 66.5 wt.%, 2-phenylimidazoline: 3.5 wt.%, pigment: 8.4 wt.%, precipitated barium sulfate: 10.1 wt.%, kaolin: 10.1 wt.%, benzoin, flow agent and additives: 1.4 wt.%,

[0220] - Epoxy resin type 3: 66.5 wt %, 2-phenylimidazoline: 3.5 wt %, pigment: 8.4 wt %, talc: 10.1 wt %, kaolin: 10.1 wt %, benzoin, flow agent and additives: 1.4 wt %

[0221] - Epoxy resin type 3: 66.5 wt %, 2-phenylimidazoline: 3.5 wt %, pigment: 8.4 wt %, precipitated barium sulfate: 20.2 wt %, benzoin, flow agent and additives: 1.4 wt %, and

[0222] Epoxy resin type 3: 66.5% by weight, 2-phenylimidazoline: 3.5% by weight, titanium dioxide: 25% by weight, precipitated barium sulfate: 3.6% by weight, benzoin, flow agents and additives: 1.4% by weight.

[0223] The granular coating composition of the present invention preferably provides a coating having electrical insulation properties (i.e., high electrical resistance and high withstand voltage). Preferably, the granular coating composition of the present invention provides a coating having a DC resistance of 1000V and a resistance of >500MΩ. Preferably, the granular coating composition of the present invention provides a coating having a DC resistance of 2700V and a maximum leakage current of no more than 0.1mA.

[0224] A feature of the present invention is that the granular coating composition provides a coating that is resistant to electrolytes. Thus, the granular coating composition provides a coating that has electrical insulating properties after exposure to an electrolyte.

[0225] Preferably, the granular coating composition of the present invention provides a coating having an insulation resistance that meets the standards described in the examples herein after immersion in an electrolyte, and is resistant to 1000V DC, and has a resistance>500MΩ, and / or a resistance below the limit of 500MΩ, but does not break through the coating. Preferably, the granular coating composition of the present invention provides a coating having a voltage resistance that meets the standards described in the examples herein after immersion in an electrolyte, and is resistant to 2700V DC, and has a maximum leakage current of no more than 0.1mA, and / or a small current leakage above the limit of 1mA at a voltage below 2700V DC. Preferably, the granular coating composition of the present invention provides an insulation resistance and voltage resistance that meet the standards described in the examples herein after immersion in an electrolyte, and is resistant to 1000V DC, and has a resistance>500MΩ, and / or a resistance below the limit of 500MΩ, but does not break through the coating, and is resistant to 2700V DC, and has a maximum leakage current of no more than 0.1mA, and / or a small current leakage above the limit of 1mA at a voltage below 2700V DC.

[0226] Preferably, the granular coating composition provides a coating having an insulation resistance that meets the standards described in the examples herein after immersion in an electrolyte, and is resistant to 1000V DC, and has a resistance of >500MΩ. Preferably, the granular coating composition provides a coating having a voltage resistance that meets the standards described in the examples herein after immersion in an electrolyte, and is resistant to 2700V DC, and has a maximum leakage current of no more than 0.1mA. Preferably, the granular coating composition provides a coating having an insulation resistance and voltage resistance that meets the standards described in the examples herein after immersion in an electrolyte, and is resistant to 1000V DC, and has a resistance of >500MΩ, and is resistant to 2700V DC, and has a maximum leakage current of no more than 0.1mA.

[0227] Yet another feature of the present invention is that the granular coating composition provides a coating having good adhesion to a substrate, preferably a metal substrate, such as an aluminum substrate, and to a structural adhesive. Preferably, the granular coating composition provides a coating that passes the cross cut test as described in ISO 2409:2013 (E).

[0228] Yet another feature of the present invention is that the particulate coating composition provides a coating that resists discoloration due to electrolytes. Preferably, the coating exhibits only slight discoloration when it is immersed in an electrolyte, for example, as described in the Examples section herein.

[0229] Another feature of the present invention is that the particulate coating composition provides a coating that is water resistant (ie, does not lose adhesion, swell significantly, or blister after exposure to water), even at elevated temperatures.

[0230] container

[0231] The present invention also relates to a container containing a granular coating composition as described above. Suitable containers include a cardboard box lined with a plastic bag and multiple plastic bags (so-called "big bags").

[0232] manufacture

[0233] The present invention also relates to a method for preparing a granular coating composition as described above, the method comprising:

[0234] (i) blending an epoxy resin, a curing agent, a filler, and a degassing agent to form a mixture, wherein the curing agent comprises an imidazoline ring; and

[0235] (ii) extruding the mixture to form granules.

[0236] The extruded particles can take any form, such as spherical particles, fragments or flakes. Preferred methods of the present invention also include grinding the extruded particles to form a powder. Grinding can be performed in any conventional mill to a particle size that is most suitable for powder coating. Other preferred methods of the present invention also include screening the milled particles.

[0237] Therefore, a preferred method of the present invention comprises:

[0238] (i) blending an epoxy resin, a curing agent, a filler, and a degassing agent to form a mixture, wherein the curing agent comprises an imidazoline ring;

[0239] (ii) extruding the mixture to form granules;

[0240] (iii) milling the extruded particles to form milled particles; and

[0241] (iv) sieving the milled particles.

[0242] In a particularly preferred method of the invention, the curing agent is 2-phenyl-2-imidazoline.

[0243] After grinding, screening is preferably performed to remove coarse particles.

[0244] Optionally, a fluidizing agent (eg, fumed silica or alumina) is added during milling and / or sieving.

[0245] Any conventional mixing, extrusion and milling methods may be used. Preferred extrusion conditions are conventional and will generally be maintained at low temperatures, for example below 140°C, to avoid premature curing. Particle size distribution D of the granular coating composition 50 Preferably in the range of 10 to 120 μm, and still more preferably in the range of 15 to 100 μm. Preferred particle size D 50At least 20 or 25 μm, and advantageously not more than 80 μm, for example 30 to 70 μm. Typically, the particle size may be determined using a Malvern particle size analyzer.

[0246] Application and coating to substrates

[0247] The present invention also relates to a method for coating a substrate with a granular coating composition as described above, the method comprising:

[0248] i) applying a granular coating composition to the substrate; and

[0249] ii) curing the granular coating composition.

[0250] Optionally, prior to application of the granular coating composition, the substrate is pretreated, for example degreasing, desalting, shot or sand blasting, dust removal.

[0251] In some methods of the invention, the substrate is pretreated and the heat in the substrate cures the coating.

[0252] Thus, some methods of the invention include:

[0253] i) preheating the substrate, for example, to a temperature above the curing temperature of the particulate coating composition;

[0254] ii) applying a particulate coating composition to the preheated substrate; and

[0255] iii) curing the granular coating composition.

[0256] The granular coating composition of the present invention can be applied to the substrate by any conventional particle (e.g., powder) coating method (e.g., electrostatic spray or fluidized bed). A cold or preheated substrate can be coated, for example, in a spray booth, or the preheated substrate is immersed in a fluidized bed of powder. The preheating preferably heats the substrate to a temperature above the melting temperature of the powder, and keeps enough time for the coating to flow, fuse, and solidify into a continuous coating. Coating techniques are well known in the art and will be familiar to the technician. Electrostatic spraying is preferred.

[0257] The present invention also relates to the use of a granular coating composition as described above for coating a substrate, preferably a metal substrate, such as aluminium.

[0258] Preferably, the dry thickness of the coating is from 60 to 250 microns, such as from 80 to 200 microns, especially from 90 to 150 microns.

[0259] The present invention also relates to a coating comprising a granular coating composition as described above. Preferably, the coating is cured. Alternatively, the present invention relates to a coating obtainable by spraying or dipping and curing the granular coating composition as described above.

[0260] The granular coating composition of the present invention can be used to form a single layer coating, or can be part of a multi-layer structure. The granular coating composition of the present invention is preferably used to form a first layer or base layer on a substrate (e.g., a battery cell). Preferably, the coating of the present invention is the top or outermost layer that can be exposed to the electrolyte.

[0261] Curing

[0262] Once the substrate is coated with the granular coating composition of the present invention, the coating is preferably cured. Curing can be performed by continuous heating, subsequent heating, or residual heat in the substrate. Additionally or alternatively, the granular coating composition of the present invention can be cured by placing the substrate in a post cure oven. The heating process allows the particles to melt and fuse, and then cure.

[0263] The granular coating composition preferably flows freely during the curing operation. Advantageously, this results in a smooth, uniform topcoat. The thickness of the cured coating is preferably 60 to 250 microns, such as 80 to 200 microns, especially 90 to 150 microns.

[0264] The coating formed by the granular coating composition of the present invention is preferably electrically insulating, i.e., has high electrical resistance and high voltage resistance. Preferably, the coating formed by the granular coating composition of the present invention withstands 1000V DC and has a resistance of >500MΩ. Preferably, the coating formed by the granular coating composition of the present invention withstands 2700V and has a maximum leakage current of no more than 0.1mA.

[0265] A feature of the present invention is that the coating formed by the granular coating composition of the present invention is resistant to electrolytes. Therefore, the coating has electrical insulation after exposure to an electrolyte. Preferably, the coating has an insulation resistance that meets the standards described in the embodiments of this article after being immersed in an electrolyte, and is resistant to direct current 1000V, and the resistance is>500MΩ. Preferably, the coating has a voltage resistance that meets the standards described in the embodiments of this article after being immersed in an electrolyte, and is resistant to 2700V, and the maximum leakage current does not exceed 0.1mA. Preferably, the coating has an insulation resistance and voltage resistance that meet the standards described in the embodiments of this article after being immersed in an electrolyte, and is resistant to direct current 1000V, and the resistance is>500MΩ, and is resistant to 2700V, and the maximum leakage current does not exceed 0.1mA.

[0266] Another feature of the present invention is that the coating formed from the granular coating composition of the present invention has good adhesion to the substrate (preferably a metal substrate, such as an aluminum substrate) and to the structural adhesive. Preferably, the coating formed from the granular coating composition of the present invention passes the cross cut test as described in ISO 2409:2013 (E).

[0267] Yet another feature of the present invention is that the coating formed from the granular coating composition of the present invention resists discoloration due to electrolytes. Preferably, the coating exhibits only slight discoloration when it is immersed in an electrolyte, for example, as described in the Examples section herein.

[0268] Another feature of the present invention is that coatings formed from the granular coating compositions of the present invention are water resistant, ie, do not lose adhesion, swell significantly, or blister after exposure to water, even at elevated temperatures.

[0269] Substrate and products

[0270] The present invention also relates to a substrate coated with a granular coating composition as described above or a coating as described above. The granular coating composition of the present invention can be applied to any substrate. A preferred substrate is a metal, and still more preferably, the substrate is aluminum. Particularly preferably, the substrate is an aluminum surface of a battery cell, and especially preferably an aluminum surface of a battery cell present in a battery assembly, such as a battery assembly of an electric vehicle.

[0271] The substrate, e.g. the aluminum surface of a battery cell, may be partially or completely coated with the granular coating composition or coating of the invention. Preferably, however, substantially all of the substrate is coated with the granular coating composition or coating of the invention. In the case of a battery cell, this preferably includes the entire outer wall of the battery cell except for the electrical contacts.

[0272] The present invention also relates to a battery assembly comprising at least one battery cell, wherein the at least one battery cell has a coating formed on at least one surface, and the coating is formed from a composition comprising the following components:

[0273] (i) epoxy resin,

[0274] (ii) a curing agent, wherein the curing agent comprises an imidazoline ring;

[0275] (iii) fillers; and

[0276] (iv) optionally a degassing agent, preferably benzoin.

[0277] Preferably, the battery assembly comprises a plurality of battery cells having a coating formed on at least one surface, wherein the coating is formed from a composition as described herein.

[0278] Preferred battery components include a coating formed from the preferred particulate coating composition as described above.

[0279] Further preferred battery components comprise the preferred coatings as described above.

[0280] Battery components, uses and methods

[0281] The present invention also relates to a battery assembly comprising at least one battery cell, wherein the at least one battery cell has a coating formed on at least one surface, and the coating is formed from a composition comprising the following components:

[0282] (i) epoxy resin,

[0283] (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0284] (iii) fillers; and

[0285] (iv) a degassing agent, preferably benzoin.

[0286] Preferably, the battery assembly comprises a plurality of battery cells having a coating formed on at least one surface, wherein the coating is formed from a composition as described herein.

[0287] The present invention also relates to the use of a granular coating composition comprising the following components for forming an electrolyte-resistant coating on at least one surface of a substrate, preferably a battery cell:

[0288] (i) epoxy resin,

[0289] (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0290] (iii) fillers; and

[0291] (iv) a degassing agent, preferably benzoin;

[0292] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0293] The present invention also relates to the use of a granular coating composition comprising the following components for protecting a substrate, in particular a battery cell, from an electrolyte:

[0294] (i) epoxy resin,

[0295] (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0296] (iii) fillers; and

[0297] (iv) a degassing agent, preferably benzoin;

[0298] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0299] The present invention also relates to the use of a granular coating composition comprising the following components for coating at least one aluminum surface of a battery cell:

[0300] (i) epoxy resin,

[0301] (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0302] (iii) fillers; and

[0303] (iv) a degassing agent, preferably benzoin;

[0304] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0305] The present invention also relates to the use of a granular coating composition comprising the following components for forming at least a base layer on a battery cell:

[0306] (i) epoxy resin,

[0307] (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0308] (iii) fillers; and

[0309] (iv) a degassing agent, preferably benzoin;

[0310] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0311] The present invention also relates to the use of a granular coating composition comprising the following components for coating a battery cell:

[0312] (i) epoxy resin,

[0313] (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0314] (iii) fillers; and

[0315] (iv) a degassing agent, preferably benzoin;

[0316] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0317] The present invention also relates to a method for protecting a surface from electrolyte damage, the method comprising:

[0318] (a) applying a particulate coating composition to the surface; and

[0319] (b) curing the coating composition to obtain a coating,

[0320] The granular coating composition comprises:

[0321] (v) epoxy resin,

[0322] (vi) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0323] (vii) fillers; and

[0324] (viii) a degassing agent, preferably benzoin,

[0325] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0326] The present invention also relates to a method of retaining electrical insulation of a coating on a substrate after the coating has been exposed to (e.g., contacted with) an electrolyte, the method comprising:

[0327] (a) applying a particulate coating composition to the surface; and

[0328] (b) curing the coating composition to obtain a coating,

[0329] The granular coating composition comprises:

[0330] (v) epoxy resin,

[0331] (vi) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring;

[0332] (vii) fillers; and

[0333] (viii) a degassing agent, preferably benzoin.

[0334] Preferably, the total amount of epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

[0335] Preferred battery components, uses and methods include a coating formed from the preferred epoxy resin, filler and degassing agent as described above with respect to the composition itself.

[0336] Preferred battery components, uses and methods include coatings formed from curing agents comprising imidazole rings, imidazoline rings or imidazolidine rings. More preferably, the curing agent present in the granular coating composition comprises an imidazoline ring. The imidazoline ring may be 2-imidazoline, 3-imidazoline or 4-imidazoline. Preferably, the imidazoline ring is 2-imidazoline.

[0337] The imidazole ring, imidazoline ring or imidazolidine ring present in the curing agent present can be unsubstituted or substituted. Preferably, the imidazole ring, imidazoline ring or imidazolidine ring is substituted. Any number of substituents can be present, more preferably one or two substituents, and still more preferably one substituent.

[0338] When substituted, the imidazole ring, imidazoline ring or imidazolidinyl ring may be substituted at any position. Preferably, the imidazole ring, imidazoline ring or imidazolidinyl ring is substituted at the 2-position, for example, a preferred curing agent comprises an imidazoline ring substituted at the 2-position. Optionally, the imidazole ring, imidazoline ring or imidazolidinyl ring present in the curing agent present in the granular coating composition of the present invention is a dimer, for example, the dimer is connected by an alkylene linker between the two 2-positions of the imidazole ring, imidazoline ring or imidazolidinyl ring.

[0339] Examples of suitable substituents that may be present on the imidazole, imidazoline or imidazolidine rings include aromatic substituents, C1-C 12 Alkyl substituents, C1-C6 alkylene substituents, alcohols, amines, halides, C1-C6 alkoxy groups, and nitriles. Preferred substituents include aromatic substituents (e.g., phenyl or benzyl) and C1-C 12 Alkyl substituents (such as methyl). More preferred substituents include aromatic substituents (such as phenyl or benzyl) and C2-C 12 Alkyl substituents. Still more preferably, the imidazole ring, imidazoline ring or imidazolidine ring has an aromatic substituent. Examples of suitable aromatic substituents include phenyl and heterocycles such as pyridine, imidazole, furan and thiophene. A preferred aromatic substituent is phenyl, especially unsubstituted phenyl.

[0340] The imidazole ring, imidazoline ring or nitrogen atom of the imidazoline ring may be substituted or unsubstituted. Examples of suitable substituents include C1-C 12 Alkyl groups, alkyl alcohols and alkyl amines. The nitrogen atom is preferably unsubstituted.

[0341] When a phenyl group is present as a substituent on an imidazole ring, an imidazoline ring or an imidazoline ring, the phenyl group may be unsubstituted or substituted. Examples of suitable substituents include C1-C6 alkyl, C1-C6 alkoxy, nitrile, hydroxyl, halide, thiol and amine. The phenyl substituent may have one or more substituents located at any position on the aromatic ring. Preferably, the phenyl group present as a substituent is unsubstituted.

[0342] Particularly preferred granular coating compositions comprise a curing agent comprising an imidazoline ring, and still more preferably a 2-imidazoline ring.

[0343] Particularly preferred curing agents present in the coating composition comprise a 2-imidazoline ring substituted at the 2 position (e.g., consist of a 2-imidazoline ring substituted at the 2 position). Still more preferably, the substituent is an aromatic substituent (e.g., phenyl) or a C1-C 12 More preferably, the substituent is an aromatic substituent (e.g., phenyl or benzyl) or a C2-C 12 Alkyl substituents.

[0344] Particularly preferably, the curing agent present comprises (eg consists of) 2-phenyl-2-imidazoline (Cas number: 936-49-2).

[0345]

[0346] The curing agent preferably comprises 2-phenyl-2-imidazoline, for example in an amount of >50 wt %, more preferably >75 wt %, still more preferably >90 wt % and still more preferably >95 wt % of the curing agent.

[0347] The purity of 2-phenyl-2-imidazoline preferably present in the granular coating composition is preferably 98% or more, more preferably 99% or more.

[0348] As described above, suitable curing agents containing an imidazole ring, an imidazoline ring or an imidazolidine ring are commercially available.

[0349] It will be appreciated that the curing agent and epoxy resin need to react in order to cure the coating. The appropriate amounts of curing agent and epoxy resin depend on the relative amounts of reactive groups, i.e., the epoxide in the epoxy resin and the amine in the curing agent. Generally speaking, the amount of curing agent present (in wt%) is preferably 1-35 wt%, more preferably 1.5-20 wt%, and still more preferably 2-15 wt%, based on the amount of epoxy resin present (in wt%).

[0350] It is preferred that these components be mixed in a ratio such that the curing agent is present in a stoichiometric amount of 80-120%, more preferably 90-115%, and still more preferably 100-110%, based on the number of reactive groups present in the curing agent relative to the number of reactive groups present in the epoxy resin.

[0351] Preferably, the coating composition is as described above with respect to the coating composition itself.

[0352] The invention will now be described with reference to the following non-limiting examples.

[0353] Example

[0354] Material

[0355] The polymers and compounds used in the examples are all commercially available. The polymers and compounds used are summarized in the following table.

[0356]

[0357]

[0358]

[0359] Preparation of powder coating samples

[0360] Powder coatings are prepared using the following procedure:

[0361] (1) The raw materials are placed in a mixing tank according to the corresponding weight percentages for premixing shown in the following table, wherein the amount of each component is indicated in weight % unless otherwise specified. Blending is performed in two stages in the mixing tank. The first blending time is 3-5 minutes, the rotation speed is 700 r / min, and the operating temperature is 20-30° C. The second blending time is 3-5 minutes, the rotation speed is 900 r / min, and the operating temperature is 20-30° C.

[0362] (2) The premixed raw materials are uniformly melted, mixed, dispersed and extruded using a twin-screw extruder. The temperature of the extruder is 90-110°C, and the screw frequency is controlled to 30-50 Hz. The extruded mixture is then made into sheets and crushed.

[0363] (3) The crushed material is classified and crushed by an ACM mill. The frequency of the disc is 25-35 Hz, and the frequency of the classifier is 25-35 Hz.

[0364] (4) The finely pulverized material is classified into a powder coating having a particle size D50 of 30-50 microns.

[0365] (5) The compositions of the powder coatings prepared for the tests are summarized in the following table, wherein the amounts specified are in % by weight unless otherwise stated.

[0366] Preparation of samples for testing

[0367] Follow these steps to prepare the panels for testing:

[0368] 1. The panels are aluminum panels, model AL 6036, and the panel size is 50*30*0.8mm. The panels are pre-treated in the following ways: soaking in alkaline or acidic solution, cleaning bath, pickling bath, cleaning bath, and then treated to ensure that the panels are chromium-free, and then they are dried in an oven with a maximum target temperature of 100°C.

[0369] 2. Apply protective tape to the bottom edge of the back of each panel (approximately 0.5 x 2 cm) to avoid coating this area.

[0370] 3. In the cleaned spray booth, clean the spray gun thoroughly with compressed air. Check the gun's spray pattern to ensure it deposits an even layer of powder on the test panel.

[0371] 4. Each panel is sprayed individually for the time required to achieve the specified target thickness of 100-130μm.

[0372] 5. Hang the panel inside the curing oven and cure using a target temperature of 200°C / 10min.

[0373] 6. Remove the protective tape after the panel has cooled.

[0374] 7. Measure the coating thickness. The thickness of the panel used for the test was 100-130 μm.

[0375] 8. For adhesion testing, panels were tested prior to any exposure to electrolyte.

[0376] 9. For insulation and voltage testing, test the panels before any exposure to electrolyte and after immersion in electrolyte.

[0377] 10. For the discoloration test, test the panels after exposure to the electrolyte.

[0378] Soaking in electrolyte

[0379] Prepare 0.5 liters of electrolyte. The composition of the electrolyte is:

[0380] Ethylene carbonate (EC), diethyl carbonate (DEC) and dimethyl carbonate (DMC) mixed in a weight ratio or volume ratio of EC / DEC / DMC=2 / 1 / 7; lithium hexafluorophosphate (1.1 mol); additives, vinylene carbonate (VC)=2%, 1,3-propane sultone=1%

[0381] Half of the coated panel was immersed in the electrolyte, and the other half of the panel was left in the air. The container was sealed and left for 7 days. After 7 days, the panel was removed from the electrolyte, dried, and then tested as described below. These test conditions represent extreme conditions and are much worse than the conditions that the coating will be exposed to in a battery assembly, where the coating contacts the electrolyte due to spillage.

[0382] Test Method

[0383] Adhesion test

[0384] The samples were tested according to the cross cut test as described in ISO 2409:2013(E). In the results, Gt0 is the best and Gt5 is the worst. / = Not tested

[0385] Insulation test

[0386] The samples were tested according to the following procedure. Three parallel samples were tested for each composition:

[0387] 1. Make connections: Plug in the power supply and turn on the power of the device. Place the coated panel on a thick rubber pad to ensure no electrical leakage when voltage is applied. In step 3, a clamp is connected to the bottom of the back side of the bare metal (previously covered by protective tape), and the test electrode in the device is connected to the top coated part of the panel through a profiling checker.

[0388] 2. Parameter setting: Set DC 1000V, test time = 60 seconds, lower limit of resistance is 500MΩ. Voltage rises from zero to 1000V within 1 second.

[0389] 3. Place the profiler, a conductive metal panel of the same shape as the coated panel but slightly smaller in size (about 5 mm shorter in all directions), over the coated panel to be tested. Press the profiler with a force of ≥1.5 kgf to ensure that the potential breakdown point (of the coated panel) is in the non-edge area (the area covered by the profiler) when voltage is applied, and test the insulation resistance using the test electrodes through the profiler.

[0390] Insulation test pass standard:

[0391] The sample can withstand 1000V DC and has a resistance of >500MΩ:

[0392] O = Pass test criteria

[0393] θ=The sample has no breakdown, but the resistance is below the limit of 500MΩ

[0394] X=Withstand voltage test failed, insulation resistance not tested

[0395] Voltage test

[0396] The samples were tested according to the following procedure. Three parallel samples were tested for each composition:

[0397] 1. Make connections: Plug in the power supply and turn on the power of the device. Place the coated panel on a thick rubber pad to ensure there is no electrical leakage when voltage is applied. In step 3, a clamp is connected to the back bottom of the bare metal (previously covered by protective tape) and the test electrode in the device is connected to the top coated part of the panel through the profiling inspector.

[0398] 2. Parameter setting: Set DC 2700V, test time = 60 seconds, maximum leakage current does not exceed 1mA. The voltage rises from zero to 2700V within 1s.

[0399] 3. Place the profiler on top of the coated panel to be tested. Press the profiler with a force of ≥1.5kgf to ensure that when voltage is applied, the potential breakdown point (of the coated panel) is in the non-edge area (the area covered by the profiler), and test the leakage current using the test electrodes through the profiler.

[0400] Pass voltage test criteria:

[0401] The sample withstands 2700V and the maximum leakage current does not exceed 0.1mA

[0402] O = Pass test criteria

[0403] θ = small current leakage above 1 mA limit at voltages below 2.7 kV X = breakdown of coating film

[0404] The voltage test and then the insulation test are typically performed on the same panel, because the steps are the same except for the parameter setting. In the event that the coating film breaks down during the voltage test, the insulation test cannot be performed on the same panel.

[0405] Discoloration after soaking

[0406] Visually inspect the coating for discoloration after immersion. This is done before the insulation test and voltage test. The evaluation criteria applied are as follows:

[0407] O = Slight discoloration of the coating film after immersion

[0408] θ=Severe discoloration of the immersed coating film

[0409] X = Severe discoloration of the entire coating film

[0410] Example 1 - Effect of Curing Agent

[0411] The powder coatings described in the following Table 1 were prepared along with 7 comparative examples. The comparative examples employed various curing agents different from the curing agent containing an imidazole ring, an imidazoline ring or an imidazolidine ring. The test results are also shown in Table 1. All examples passed the insulation test and the voltage test before immersion in the electrolyte.

[0412] The result in Table 1 shows that when the curing agent present in the granular coating composition comprises imidazole ring, imidazoline ring or imidazolidine ring (for example 2-phenyl-2-imidazoline), the resulting coating adheres to substrate well, and can withstand exposure to electrolyte. After soaking in electrolyte for 7 days (this is extreme test condition), the coating made of the composition comprising 2-phenyl-2-imidazoline still passes through voltage test, and does not break down in insulation test. In contrast, after soaking in electrolyte, the coating made of the composition comprising various other curing agents does not pass through voltage test, therefore can not carry out insulation test. In the coating comprising the curing agent that is different from 2-phenyl-2-imidazoline, the degree of discoloration is also more serious.

[0413] The results in Table 1 (specifically Examples 1-5) also show that a range of different types of epoxy resins can be successfully used in the granular coating compositions of the present invention.

[0414] Examples 9 and 10 in Table 1 show particularly strong performance. In these examples, the ratio of 2-phenyl-2-imidazoline to epoxy resin is higher than in some other examples. It is believed that the relatively high ratio of curing agent may result in a higher crosslink density in the final coating, thus resulting in the improved performance results observed.

[0415] Table 1

[0416]

[0417]

[0418] Example 2 - Effect of the Total Amount of Epoxy Resin in the Coating Composition

[0419] The powder coatings described in Table 2 below were prepared. All examples passed the insulation test and the voltage test before immersion in the electrolyte. The samples were not tested for adhesion before immersion.

[0420] Table 2

[0421]

[0422] The results in Table 2 show that the granular coating compositions of the present invention can contain a wide range of combinations of epoxy resins and curing agents. These examples show that granular coating compositions containing 38-85.5 wt. % epoxy resin and 2-5 wt. % curing agent all produce coatings that pass the insulation test and the voltage test even after exposure to an electrolyte for 7 days. The examples also show that the granular compositions of the present invention can contain a range of fillers, specifically 0.2-50.2 wt. %, and still produce coatings that pass the insulation test and the voltage test even after exposure to an electrolyte.

[0423] Example 3 - Effect of fillers in coating compositions

[0424] The powder coatings described in the following Table 3 were prepared. The test results are also shown in Table 3. All examples passed the insulation test and the voltage test before immersion in the electrolyte. All coating films had an adhesion of Gt0 before immersion.

[0425] The results in Table 3 show that a wide range of fillers can be used in the granular coating compositions of the present invention. Compositions containing single fillers as well as mixtures of fillers performed well. When fillers were present, coatings produced from the granular coating compositions of the present invention passed insulation tests and voltage tests even after exposure to electrolytes.

[0426] Example 4 - Effect of Filler Combination and Pigment in Coating Compositions

[0427] The powder coatings described in the following Table 4 were prepared. The test results are also shown in Table 4. All examples passed the insulation test and the voltage test before immersion in the electrolyte.

[0428] The results in Table 4 show that both organic and inorganic pigments can be used in the granular composition of the present invention.

[0429] Table 3

[0430]

[0431]

[0432] Table 4

[0433]

Claims

1. A granular coating composition, preferably a powder coating composition, comprising: (i) epoxy resin, (ii) a curing agent, wherein the curing agent comprises an imidazoline ring; (iii) fillers; and (iv) a degassing agent, preferably benzoin, The total amount of the epoxy binder system is 40-99 wt % based on the total weight of the granular coating composition, wherein the system comprises the epoxy resin and the curing agent.

2. The composition of claim 1, wherein the curing agent comprises, or more preferably consists of, 2-phenyl-2-imidazoline.

3. The composition according to claim 1 or 2, wherein the epoxy equivalent weight (EEW) of the epoxy resin is 200-1950 g / eq, preferably 200-1300 g / eq, and more preferably 400-1300 g / eq.

4. The composition according to any preceding claim, wherein the epoxy resin is selected from bisphenol A based epoxy resins, novolac-modified bisphenol A based epoxy resins, bisphenol F epoxy resins, isocyanate-modified bisphenol A epoxy resins, and various mixtures thereof, preferably selected from bisphenol A based epoxy resins, novolac-modified bisphenol A based epoxy resins, and various mixtures thereof, and more preferably is a bisphenol A based epoxy resin.

5. A composition according to any preceding claim, wherein the total amount of epoxy binder system comprising the epoxy resin and the curing agent is 50-95 wt. %, and still more preferably 60-90 wt. %, based on the total weight of the granular coating composition.

6. A composition according to any preceding claim, comprising 38-99 wt.-%, preferably 40-99 wt.-%, more preferably 50-95 wt.-%, still more preferably 55-95 wt.-% and still more preferably 60-90 wt.-% of epoxy resin, based on the total weight of the granular coating composition, and / or 1-35 wt.-%, more preferably 1.5-20 wt.-% and still more preferably 2-15 wt.-% of curing agent, based on the amount of epoxy resin.

7. A composition according to any preceding claim, wherein the filler is selected from barium sulfate, preferably precipitated barium sulfate, mica, talc, wollastonite (calcium metasilicate), glass flakes, nepheline, kaolin, dolomite, diatomaceous earth, boron nitride, alumina, aluminum hydroxide and various mixtures thereof, and more preferably selected from barium sulfate, preferably precipitated barium sulfate, kaolin and various mixtures thereof.

8. A composition according to any preceding claim comprising 0.01-60 wt%, more preferably 1.5-50 wt% and still more preferably 10-38 wt% filler based on the total weight of the granular coating composition.

9. A composition according to any preceding claim comprising 0.15-0.45 wt%, more preferably 0.17-0.4 wt% and still more preferably 0.2-0.35 wt% of degassing agent based on the total weight of the granular coating composition.

10. A container containing a granular coating composition according to any one of claims 1 to 9.

11. A method for preparing a granular coating composition according to any one of claims 1 to 9, the method comprising: (i) blending an epoxy resin, a curing agent, a filler and a degassing agent to form a mixture, wherein the curing agent contains an imidazoline ring; as well as (ii) extruding the mixture to form granules.

12. Use of a granular coating composition according to any one of claims 1 to 9 for coating a substrate, preferably a metal substrate, such as aluminium.

13. A method for coating a substrate, preferably a metal substrate, such as aluminum, with a granular coating composition according to any one of claims 1 to 9, the method comprising: (i) applying the granular coating composition to the substrate; as well as (ii) curing the granular coating composition.

14. A coating, preferably a cured coating, comprising the granular coating composition according to any one of claims 1 to 9.

15. A substrate, preferably a metal substrate such as aluminium, coated with a granular coating composition according to any one of claims 1 to 9 or a coating according to claim 14.

16. A battery assembly comprising at least one battery cell, wherein the at least one battery cell has a coating formed on at least one surface, and the coating is formed from a composition comprising: (i) epoxy resin, (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring; (iii) fillers; and (iv) a degassing agent, preferably benzoin.

17. The battery assembly according to claim 15, wherein the composition is as described in any one of claims 1 to 9.

18. Use of a granular coating composition comprising the following components for forming an electrolyte-resistant coating on at least one surface of a substrate, preferably a battery cell: (i) epoxy resin, (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring; (iii) fillers; and (iv) a degassing agent, preferably benzoin.

19. Use of a granular coating composition comprising the following components for protecting a substrate, in particular a battery cell, from electrolytes: (i) epoxy resin, (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring; (iii) fillers; and (iv) a degassing agent, preferably benzoin.

20. Use of a granular coating composition comprising the following components for coating at least one aluminum surface of a battery cell: (i) epoxy resin, (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring; (iii) fillers; and (iv) a degassing agent, preferably benzoin.

21. Use of a granular coating composition comprising the following components for forming at least a base layer on a battery cell: (i) epoxy resin, (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring; (iii) fillers; and (iv) a degassing agent, preferably benzoin.

22. Use of a granular coating composition comprising the following components for coating a battery cell: (i) epoxy resin, (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring; (iii) fillers; and (iv) a degassing agent, preferably benzoin.

23. The use according to any one of claims 17 to 21, wherein the composition is as described in any one of claims 1 to 9.

24. A method for protecting a surface from damage by an electrolyte, the method comprising: (a) applying a particulate coating composition to the surface; as well as (b) curing the coating composition to obtain a coating, The granular coating composition comprises: (i) epoxy resin, (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring; (iii) fillers; and (iv) a degassing agent, preferably benzoin.

25. A method of retaining electrical insulation of a coating on a substrate after the coating has been exposed to (e.g., contacted with) an electrolyte, the method comprising: (a) applying a particulate coating composition to the surface; as well as (b) curing the coating composition to obtain a coating, The granular coating composition comprises: (i) epoxy resin, (ii) a curing agent, wherein the curing agent comprises an imidazole ring, an imidazoline ring or an imidazolidine ring, and preferably comprises an imidazoline ring; (iii) fillers; and (iv) a degassing agent, preferably benzoin.

26. The method of claim 21 or 22, wherein the composition is as described in any one of claims 1-9.

Citation Information

Patent Citations

  • Process for the preparation of powder coatings on heat-sensitive substrates

    CN101415743A

  • Low-temperature fast-curing epoxide powder paint and preparation method thereof

    CN103666203A

  • Epoxy resin powder coating composition

    CN1067441A

  • Method for improving chargeability of powder coating composition

    CN1189519A

  • Epoxy resin curing compositions and resin compositions including same

    CN1798785A