Method for stabilizing perovskite ink and perovskite ink formulation according to method
By adding additives such as elemental sulfur to perovskite inks, the amine-water proton exchange is inhibited, and the problem of unstable perovskite inks in ambient air is solved, and the long-term stability of inks and the performance of perovskite solar cells is achieved. Maintaining, supporting large-scale and commercial production.
Patent Information
- Application Number
- CN202280071676.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2021-08-25
- Filing Date
- 2022-08-25
- Publication Date
- 2024-11-08
AI Technical Summary
Conventional perovskite inks are unstable in ambient air, resulting in a decline in the performance of perovskite solar cells, especially due to the influence of moisture accelerates their degradation, limiting the feasibility of large-area and commercial production.
By adding elemental sulfur or other additives, such as triethyl borate, 18-crown-6, ITIC-Th and L-α-phosphatidylcholine to the perovskite ink, to inhibit amine-water proton exchange and reduce cationic Reactivity, thereby improving the stability of the ink.
The long-term stability of ink at room temperature is achieved, the half-life of ink is extended, the performance of perovskite solar cells is maintained, and the feasibility of large-area and commercial production is supported.
Smart Images

Figure CN118922513A_ABST
Abstract
Description
Technical Field
[0001] Described herein are methods for stabilizing perovskite inks so they can be used in applications such as the fabrication of perovskite solar cells, and perovskite ink formulations according to the methods. Background Art
[0002] Perovskite inks can be used in different fields, including but not limited to solar cells, displays, and sensors. Unfortunately, conventional perovskite inks are unstable. This problem and proposed solutions will now be described in the context of solar cells.
[0003] One advantage of perovskite solar cells (PSCs) is that it is cost-effective and simple to deposit the solar absorbing layer from a perovskite ink using a solution-processable method. The ink consists of a precursor salt dissolved in a solvent, which is deposited as a thin film and crystallized to form a perovskite structure with an "ABX3" composition. "A" is a monovalent cation (methylammonium (MA+), formamidine (FA+), or Cs+), "B" is a divalent cation (Pb2+ or Sn2+), and "X" is a halogen (I-, Br-, or Cl-). Given the high efficiency demonstrated by small-area PSCs, significant efforts are being invested to make commercially viable, large-area, stable, and efficient devices. One of the remaining obstacles is the instability of conventional perovskite inks, especially in ambient air: the performance of PSCs depends on the aging of the ink in hours.
[0004] In aged perovskite inks, detrimental oxidation of I- to I210 and reactions of organic components including MA+, FA+, and solvents are the main factors for decomposition. Processing outside of an inert environment in ambient air increases the water content of the ink, accelerating its degradation. In some cases, this is due to the hydrolysis of the N,N-dimethylformamide (DMF) solvent to produce dimethylamine and formic acid; however, degradation of perovskite inks containing FA+ or MA+ / FA+ in dimethyl sulfoxide (DMSO) and DMF co-solvents (not involving DMF hydrolysis) is also accelerated by water. The deleterious effects of humidity on perovskite inks are a major concern for scaling up PSC fabrication; a goal is to develop water-stable inks. Summary of the invention
[0005] This article provides a method for stabilizing perovskite inks. The method involves adding an additive to the perovskite ink that can interact with the amino groups in the perovskite ink to inhibit amine-water proton exchange. When the additive is elemental sulfur, beneficial results have been obtained.
[0006] A variety of solvents may be used, including but not limited to one or more solvents selected from the group consisting of: N-methyl-2-pyrrolidone (NMP), alkyl-2-pyrrolidone, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), dialkylformamide, γ-butyrolactone (GBL), 2-methylpyrazine (2-MB), 1-pentanol (1-P), 2-methoxyethanol (2-ME), and N,N'-dimethylpropyleneurea (DMPU). The weight percentage of the selected one or combination of solvents may be in the range of 10-30% to achieve the final concentration of the perovskite ink required for forming the perovskite film. We have determined that a scalable perovskite ink containing mixed cations (3FA+:1MA+) in NMP and DMF (abbreviated as "MC-NMP") degrades within hours through the reaction of MA with FA+; water increases the reactivity of MA+ by accelerating the proton exchange between MA+ and MA. However, the addition of elemental sulfur (S8) slows down the proton exchange process through sulfur-amine interactions, reducing the reactivity of MA+.
[0007] In addition to elemental sulfur, other additives such as L-α-phosphatidylcholine may also be used.
[0008] The best performance occurred when the ratio of NMP to DMF solvent was 30 to 70.
[0009] The perovskite ink preferably includes one or more additives selected from the group consisting of sulfur or sulfur-based compounds, which may be added for stabilization of the ink. Examples of other additives for stabilizing the ink are triethyl borate, 18-crown-6, ITIC-Th, and phenylboronic acid. The additives may be added at a concentration of about 0.001 M to about 0.1 M. The sulfur-stabilized MC-NMP ink (abbreviated as "MC-NMP-S8") shows minimal degradation of the organic components after aging for a minimum of three months at room temperature in ambient air.
[0010] PSCs made from MC-NMP-S8 ink aged for more than one month have comparable performance to those made from fresh MC-NMP ink and demonstrate the feasibility of using MC-NMP-S8 ink to fabricate large-area PSCs by doctor blade coating.
[0011] The degradation of the MC-NMP ink showed minimal degradation in the temperature range of -10°C to +85°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] These and other features will become more apparent from the following description, in which reference is made to the accompanying drawings, which are for purposes of illustration only and are not intended to be limiting in any way, and in which:
[0013] FIG. 1A is a photographic image of a film made from MC-NMP ink aged for 0 and 28 hours.
[0014] FIG1B and FIG1C are XRD and HNMR spectra of MC-NMP ink aged in dimethyl sulfoxide-d6 (DMSO-d6) for 0 and 28 hours.
[0015] FIG. 1D is a reaction scheme disclosing a proposed mechanism for the reaction of MA with FA+ and MFA+.
[0016] Figure 1E is a graph disclosing the percentage of MA+ remaining after aging at ~20-30% relative humidity (RH) and ~40% RH relative to the MA+ in fresh MC-NMP ink (~20-30% RH), calculated from the MA+CH3 resonance. The half-life of MA+ at ~20-30% and ~40% RH is approximately 14 hours and 9 hours, respectively.
[0017] 2A is a graph showing amine-water proton exchange, with the 1H NMR H2O resonance being broader in solutions containing MA+ and / or FA+ (inset), and narrower in the spectrum of solutions without MA+ or FA+ (black line).
[0018] Figure 2B is a diagram showing the amine-water proton exchange process - protons are transferred from alkylammonium to water, and from water to alkylamine.
[0019] FIG. 3 is a photographic image of stabilized films made from MC-NMP-S8 ink aged at 0 and 124 days.
[0020] FIG. 3B is an XRD pattern (normalized intensity) of films made from MC-NMP-S8 ink aged between 0 and 124 days.
[0021] FIG3C is the 1H NMR spectra of MC-NMP-S8 ink after aging in DMSO-d6 for 0 and 124 days.
[0022] Figure 3D is a plot of the percentage of initial MA+ remaining as a function of ink age, calculated from the integration of the MA+CH3 resonance.
[0023] FIG. 4A is a graph of the interaction of the S8 additive with amines in MC-NMP ink before and after aging for 6 hours: images of the ink, and the corresponding shapes of the NH and H2O 1H NMR resonances.
[0024] FIG. 4B is a graph of the change in the chemical shift of the NH resonance as a function of ink aging.
[0025] Figure 4CThe chemical formula of the amine-sulfur complex in the aged MC-NMP-S8 ink is disclosed (top), in contrast to the degradation of the aged MC-NMP ink (bottom).
[0026] FIG. 5A is a graph of current density-voltage (JV) of a perovskite solar cell (PSC) fabricated by spin coating MC-NMP-S8 ink aged in ambient air for 5 days, showing the photovoltaic parameters for reverse sweeps.
[0027] FIG5B is a graph of the power conversion efficiency (PCE) for an pore area of 0.4 cm2 as a function of the aging of the ink used to make the PSC (by spin coating) (Note: the non-perovskite film was obtained from aged MC-NMP, as shown in FIG1).
[0028] FIG5C is a JV curve plot of a PSC fabricated by doctor blade coating of fresh MC-NMP-S8 ink, showing the photovoltaic parameters for the reverse scan.
[0029] Figure 5D is a plot of PCE as a function of pore area measured for devices fabricated by doctor blade coating of fresh MC-NMP-S8 ink.
[0030] Figure 6 Shown are images of films made from MC-NMP inks containing different weight ratios of NMP to DMF and annealed at 150°C for 1, 3, or 5 minutes.
[0031] Figure 7 Shows Figure 6 XRD of the films shown in .
[0032] Figure 8 XRD of films made from MC-NMP ink aged at -20-30% RH for 0, 1 and 2 days are shown (the XRD of films from MC-NMP aged at 40% RH is shown in FIG. 1B ).
[0033] Fig. 9 The XRD of a film made from fresh MC-NMP ink is shown after aging the film in ambient air for 8 days. The film had partially transformed from black to yellow before XRD analysis.
[0034] Fig.10 The 1H NMR of fresh MC-NMP ink is shown.
[0035] Fig.11 Shown is the 1H NMR of MC-NMP ink aged at -20-30% RH for 24 hours.
[0036] Fig.12The 1H NMR of the MC-NMP ink aged for 5 days (121 hours) at -20-30% RH is shown.
[0037] Fig.13 The 1H NMR of the MC-NMP ink aged for 6 hours at -40% RH is shown.
[0038] Fig.14 The 1H NMR of the MC-NMP ink aged at -40% RH for 28 hours is shown.
[0039] Fig.15 Shown is the 1H NMR of a 16% dimethylamine in H2O solution in solutions of PbI2, PbBr2, NMP, and DMF.
[0040] Fig.16 1H NMR of N-methylformamide in PbI2, PbBr2, NMP and DMF is shown.
[0041] Fig.17 1H NMR of PbI2, PbBr2, NMP and DMF are shown.
[0042] Fig.18 1H NMR of FAI in DMF is shown.
[0043] Fig.19 1H NMR of MABr in DMF is shown.
[0044] Fig. 20 1H NMR of MACl in DMF is shown.
[0045] Fig.21 Shown are the XRDs of films made from MC-NMP inks aged 0 and 1 day with 0.001 M NH4Cl additive.
[0046] Fig. 22 Shown is the 1H NMR of the MC-NMP ink aged for 85 days with 0.001 M NH4Cl additive.
[0047] Fig.23 Shown are the XRDs of films made from MC-NMP inks aged 0 and 1 day with 0.001 M CH3COONH4 additive.
[0048] Fig.24 Shown is the 1H NMR of the MC-NMP ink aged for 84 days containing 0.001 M CH3COONH4 additive.
[0049] Fig.25Shown are the XRDs of films made from MC-NMP inks aged 0 and 1 day with 0.001 M dibenzo-18-crown-6 additive.
[0050] Fig.26 Shown is the 1H NMR of a MC-NMP ink containing 0.001 M dibenzo-18-crown-6 aged for 1 day.
[0051] Fig. 27 1H NMR of fresh MC-NMP-S8 ink is shown.
[0052] Fig.28 Shown is the 1H NMR of MC-NMP-S8 ink aged for 1 day at -20% RH.
[0053] Fig.29 The 1H NMR of MC-NMP-S8 ink aged for 6 hours at -40% RH is shown.
[0054] Fig.30 Shown is the 1H NMR of MC-NMP-S8 ink aged for 31 days at -20-30% RH.
[0055] Fig.31 Shown is the 1H NMR of MC-NMP-S8 ink aged for 124 days at -20-55% RH.
[0056] Fig.32 Shown is the 1H NMR of fresh MC-NMP-S8 ink containing 1 M H2O.
[0057] Fig.33 Shown is the 1H NMR of MC-NMP-S8 ink containing 1M H2O aged for 1 day.
[0058] Fig.34 Shown is the 1H NMR of MC-NMP-S8 ink containing 1M H2O aged for 25 days.
[0059] Fig.35 XRD of films made from aged MC-NMP-S8 are shown, with actual peak intensities (normalized peak intensities are shown in FIG. 3 ).
[0060] Fig.36 Shown is the XRD (starting from 5°) of a film made from MC-NMP-S8 aged for 124 days.
[0061] Fig.37 J-V curves of PSCs fabricated by spin-coating fresh MC-NMP ink are shown, showing the photovoltaic parameters for the reverse sweep.
[0062] Fig.38Shown is the absorbance of a fresh film made from MC-NMP-S8 ink after 3 aging cycles.
[0063] Fig.39 Shown is the PL of a fresh film made from MC-NMP-S8 ink after 3 aging cycles. DETAILED DESCRIPTION
[0064] Now we will refer to Figure 1 Figure 5D To describe the method to stabilize the perovskite ink, Figure 6 to Figure 39 and Supplementary Tables S1 to S3 have also been provided as support.
[0065] Study on the causes of degradation of perovskite ink:
[0066] Before addressing the degradation problem of perovskite inks, we must first understand the mechanisms that cause the degradation.
[0067] The proposed ink degradation mechanism involving MA+, FA+, and solvent begins with the deprotonation of MA+ or FA+ to generate reactive methylamine (MA) or formamidine (FA). Although inhibition of deprotonation with sulfur, triethyl borate, or phenylboronic acid significantly improves the stability of DMSO / DMF inks, the nature of the additives required to confer stability to water remains to be explored.
[0068] Furthermore, degradation and stabilization studies have previously focused only on perovskite inks containing DMSO and DMF co-solvents, a composition optimized for laboratory-scale spin coating of MA+-based perovskites; however, spin coating and simultaneous removal of excess ink solvent by antisolvent dripping cannot be used to make uniform large-area perovskite films. For scalable fabrication of PSCs, deposition methods such as doctor blade, slot die, and spray coating are highly desirable. The subsequent perovskite processing window should be as long as possible to make reproducible, high-performance PSCs, where rapid removal of excess ink solvent leads to the formation of high-quality perovskite films. Using DMF as a co-solvent but replacing DMSO with N-methyl-2-pyrrolidone (NMP) significantly extends the processing window from seconds to minutes or longer. Furthermore, in wet precursor films, the interaction between NMP and FAI is stronger than that between DMSO and FAI, resulting in improved film quality when NMP is used as a co-solvent for FA-based perovskite compositions used in record-breaking small-area devices. These properties of FA+-based NMP / DMF inks have led to their use in the fabrication of high-performance PSCs via a scalable deposition method.
[0069] As PSC production moves from research labs to industry, an understanding of the role of water in promoting ink degradation and how to prevent water from participating in these reactions is needed. In particular, the degradation process should be explored in perovskite ink compositions that are compatible with scalable deposition to explain any potential impact on the degradation mechanism.
[0070] Here, we use 1H NMR spectroscopy to show that: a scalable perovskite ink containing a mixture of NMP and organic cations (3FA+:1MA+) in DMF (abbreviated as "MC-NMP") degrades via the reaction of MA with FA+ within hours; water increases the reactivity of MA+ by accelerating proton exchange between MA+ and MA; and the addition of elemental sulfur (S8) slows this proton exchange process via a sulfur-amine reaction, reducing the reactivity of MA+. Sulfur-stabilized MC-NMP ink (abbreviated as "MC-NMP-S8") shows minimal degradation of the organic components over more than three months of aging in ambient air at room temperature. We report that PSCs made from MC-NMP-S8 ink aged for more than one month have comparable performance to PSCs made from fresh MC-NMP ink, and demonstrate the use of MC-NMP-S8 ink to fabricate large-area PSCs by doctor blade coating.
[0071] Films made from fresh MC-NMP ink turned black upon annealing due to the formation of perovskite, as indicated by characteristic X-ray diffraction (XRD) peaks. When the same ink was aged for one day, it formed a yellow non-perovskite film with an XRD peak located at 11.7° (Figure 1A, B). Although the δ(2H) phase has a characteristic peak at 11.8° ( Fig. 9 ), but the peak at 11.7° is not from the δ phase, as heating it would cause a partial conversion to the α phase. The peak at 11.7° is most likely the result of the incorporation of organic degradation products from the aged ink, which is consistent with previous reports. Both films contain some PbI2, as evidenced by the low-intensity XRD peak at 12.7°. In addition, the film from the fresh ink has a peak at 12.2° due to the formation of the "6H" polytype initiated by phase separation, while the film from the aged ink has peaks at 11.5° and 12.9° from the "4H" polytype. Because the polytype formed by phase separation depends on the ratio of FA+ to MA+ in the film, the observation of different polytypes indicates that the organic components of MC-NMP undergo compositional changes upon aging.
[0072] We investigated the precise role of organic components in the degradation of MC-NMP by 1H NMR spectroscopy. The intensities of the peaks for the MA+CH3 resonance (2.37 ppm) and the FA+CH resonance (7.87 ppm) decreased over time in an approximate 3:1 ratio, indicating an equimolar decrease in the concentrations of MA+ and FA+. Accompanying the consumption of MA+ and FA+, new resonances appeared at 2.80, 2.96, and 7.96 ppm (Figure 1C). The signals at 2.80 ppm and 7.96 ppm appeared in a 3:1 ratio of peak areas and are derived from the CH3 and CH protons of the N-methylformamidine isomer (“MFA+”), respectively. The 2.96 ppm resonance is from the CH3 group in the N,N-dimethylformamidine isomer (“DMFA+”). In the 1H NMR spectrum of the aged MC-NMP ink, we did not observe any resonances from dimethylamine (at 2.54 ppm, Fig.15 ), N-methylformamide (at 2.56 ppm, Fig.16 ) or s-triazine (at 9.3 ppm), which are caused by the degradation of single organic cation inks containing MA+ or FA+. Therefore, these reaction pathways are not involved in the degradation of mixed MA+ and FA+ inks. The lack of dimethylamine, a product of DMF hydrolysis, also indicates that this reaction does not contribute to the degradation of MC-NMP inks.
[0073] Figure 1. Degradation of MC-NMP ink in ambient air. (A) Images of corresponding films made from MC-NMP ink aged at -40% relative humidity (RH) for 0 and 28 hours, and (B) XRD (XRD of films from ink aged at low RH see Figure 8 (C) Simplified 1H NMR spectra of MC-NMP ink aged for 0 and 28 h in dimethyl sulfoxide-d6 (DMSO-d6), showing only key resonances (for full spectrum see Fig.10 and 14 , including solvent peaks). (D) Proposed mechanism for the reaction of MA with FA+ and MFA+. (E) Calculated by MA+CH3 resonance, the percentage of MA+ remaining after aging at ~20-30% RH and ~40% RH relative to that in fresh MC-NMP ink (~20-30% RH) ( Figure 10-14 ).
[0074] After most of the MA+ is consumed, the resonances from the MFA+ and DMFA+ CH3 groups exhibit a peak area ratio of 9:1, indicating a 9:1 molar ratio of MFA+ to DMFA+. Aging the MA+ / FA+ ink in a DMSO / DMF co-solvent results in the formation of similar proportions of MFA+ and DMFA+, indicating that using NMP instead of DMSO does not affect the degradation mechanism. The formation of these degradation products is believed to be triggered by neutral MA, which affects the aminolysis of FA+ to produce MFA+ and ammonia, followed by a second aminolysis reaction between MA and MFA+ to produce DMFA+ and ammonia (Figure 1D). MA and FA, both of which are able to participate in these reactions, are always present in the perovskite ink at low concentrations as conjugate bases in their respective acid-base equilibrium (Equations 1, 2). Fresh MC-NMP ink contained 0.38 M MA+ and 1.2 M FA+; based on the aqueous pKa values of these cations (Equations 1, 2), which are strongly associated with each other and have similar pKa values in polar aprotic solvents such as DMSO, NMP, and DMF, the approximate initial concentrations of MA and FA in the MC-NMP ink were 3 × 10 -6 and 2×10 -6 M.
[0075]
[0076] We found that ink degradation accelerated significantly with increasing humidity: the half-life of MA+ was ∼14 hours at ∼20-30% relative humidity (RH), compared to ∼9 hours at ∼40% RH ( Figure 1E ). Given that the ink solvents are very hygroscopic, it is clear that higher concentrations of dissolved water (from a humid atmosphere) would accelerate the degradation reactions. Water is not a reactant in the formation of MFA+ and DMFA+ (Figure 1D), and we did not observe any hydrolysis products; therefore, we assume that water plays an indirect role in promoting the reaction of MA+ and FA+.
[0077] Figure 2. Amine-water proton exchange. (A) The resonance of 1H NMR HO is broad in solutions containing MA+ and / or FA+ (inset), and narrow in the spectrum of solutions without MA+ or FA+ (black line). (B) Amine-water proton exchange process: protons are transferred from alkylammonium to water, and from water to alkylamine. This process broadens the resonance of 1H NMR HO.
[0078] To investigate the role of water in ink degradation, we compared the 1H NMR spectra of solutions containing water with and without MA+ and FA+. In the 1H NMR spectra of MC-NMP ink, MABr and MACl solutions, the resonance of water is broad, each with a half-maximum width (FWHM) of ~50 Hz, and the FAI solution is ~20 Hz ( Figure 17-19 ). On the other hand, water protons in the solution containing all components of the MC-NMP ink except MA+ and FA+ produce a very narrow resonance of ~1 Hz (Figures 2A, 20). During the acquisition of the NMR signal, a broad peak of protons undergoing chemical exchange was observed: the FWHM of the resonance of the exchanged proton population is directly related to its exchange rate. Therefore, the broadening of the resonance of water in the presence of MA+ and FA+ indicates an increase in the water proton exchange rate. This can be attributed to the transfer of protons between water and the amino groups of MA+ and FA+.
[0079] In the acid-base equilibrium of MA+ and FA+, the protonated forms and their conjugate bases are interconvertible. In aqueous solution, the main mechanism of this process involves water ( Figure 2B ); interconversion via direct proton transfer between the protonated species and their conjugate bases contributes to a lesser extent and at a slower rate. The exchange of water and NH protons in the MC-NMP ink indicates the involvement of water, suggesting that high water content leads to an increased rate of interconversion. This leads to an accelerated rate of ink degradation, as MA+ and FA+ cations can be rapidly converted to MA and FA, which then participate in the aminolysis reaction.
[0080] Stabilization of ink
[0081] To stabilize the ink, the rate of interconversion between the weak acid and its conjugate base should be slowed by inhibiting amine-water proton exchange. The reduction in exchange rate can be observed by the narrowing of the 1H NMR water peak: it becomes easily distinguishable from the baseline, and further slowed proton exchange narrows the water peak until it looks similar to that of an amine-free solution (Figure 2A). In highly acidic solutions, the amine-water proton exchange rate is slowed and the acid dissociation equilibrium is shifted, allowing lower concentrations of reactive MA and FA to form; however, the acid will induce alternative ink degradation pathways, such as acid-catalyzed DMF hydrolysis ( Figure 21-26 ). Therefore, we explored neutral additives that can interact with the amino group. The rate of amine proton exchange decreases with increasing alkyl substitution, suggesting that the steric hindrance of the amino group can effectively improve stability.
[0082] Figure 3. Stabilization of MC-NMP ink using S8 additive. (A) Images of films made from MC-NMP-S8 ink aged between 0 and 124 days, and (B) XRD (normalized intensity - actual intensity see Figure 27-28(C) Simplified 1H NMR spectra of MC-NMP-S8 ink after aging for 0 and 124 days in DMSO-d6 (at 18-21 °C, 15-50% RH), showing only the key resonances (for the full spectrum see Fig.29 and 33 , including solvent peak). (D) Percent of initial MA+ remaining as a function of ink aging, calculated from the integration of the MA+CH3 resonance ( Figure 29-33 ).
[0083] It has been shown that the addition of elemental sulfur (S8) to inks containing FA+ and MA+ in DMSO / DMF co-solvents improves their stability due to the sulfur-methylamine reaction; however, the exact stabilization mechanism remains to be explored. The addition of 0.001M S8 to MC-NMP ink ("MC-NMP-S8") resulted in a highly stable ink: films made from MC-NMP-S8 aged for 124 days formed only the perovskite phase (Figures 3A, B). In the 1H NMR spectrum of the aged MC-NMP-S8 ink, the integrals of the MA+ (2.37 ppm) and FA+ (7.87 ppm) resonances decreased slightly over a period of more than 3.5 months (Figures 3C, D). The minimal change in the MA+ content inferred in MC-NMP-S8 suggests a MA+ half-life of ~6300 hours ( Figure 3D ). Sulfur slows down the water-amine proton exchange, as evidenced by the narrowing of the 1H NMR water resonance within the first day of aging (Figure 4A). Suppression of acid / base interconversion by slowing down the water-amine proton exchange results in a highly stable ink.
[0084] Sulfur must interact with water, amino groups, or both to inhibit their proton exchange. To investigate the role of sulfur-water interaction, we prepared MC-NMP-S8 ink using 1 M water. Despite the water concentration being 100 times higher than atomic sulfur (S), water-amine proton exchange was still inhibited, stabilizing MA+ and FA+ in the ink for at least 25 days ( Figure 34-36 ). Given the stability of this ink and the weakness of the sulfur-water interaction, we conclude that the sulfur-water interaction does not play a role in inhibiting the water-amine proton exchange and therefore does not contribute to the stabilization of the ink.
[0085] We also noticed that the orange color of MC-NMP remained unchanged during the first day of aging, while MC-NMP-S8 changed from orange to yellow after aging for ~1 day (Figure 4A). The color change suggests the formation of open-chain polysulfide anions and free radicals, which has been shown to result from the dissolution of S8 in aliphatic primary amine solutions at room temperature. The opening of the S8 ring to form these polysulfide species begins with the nucleophilic attack of the amine on the S8 ring to form N-polysulfide salts with a single NS bond (Scheme 3) or N,N'-polysulfide diamines with two NS bonds (Scheme 4). Subsequent cleavage of the SS bond generates polysulfide ions and free radicals, as well as N-polysulfide amines with shorter polysulfide chains. The weakly acidic H2S (pKa = 7) formed in reaction 4 can protonate the amine, directing the ionic interaction of the generated alkylammonium cation with the polysulfide anion to form "alkylammonium polysulfide" (Scheme 5).
[0086]
[0087] 2RNH2+S x →(RNH)2S x-1 +H2S (4)
[0088] 2RNH2+H2S+S x →(RNH3 + )2S x+1 2- (5)
[0089] Figure 4. Interaction of the S8 additive with amines in MC-NMP inks. (A) MC-NMP and MC-NMP-S8 inks before and after aging for 6 hours: images of the inks, and the corresponding appearance of the NH and H2O 1H NMR resonances. (B) Changes in the chemical shifts of the NH resonances as a function of ink aging. (C) Amine-sulfur complexes in the aged MC-NMP-S8 ink (top), in contrast to the degradation of the aged MC-NMP ink (bottom).
[0090] The color change of the MC-NMP-S8 ink correlates with the shift and broadening of the NH resonance in the 1H NMR spectrum, indicating that the environment of the NH protons changes as the polysulfide forms. In the fresh, orange MC-NMP-S8 ink, the NH peak is similar to that of MC-NMP at 8.57 ppm with a FWHM of 25 Hz; in the one-day aged, yellow MC-NMP-S8, the NH resonance shifts to 8.71 ppm and broadens significantly to 170 Hz, which is only observed when S8 is added (Figure 4A, B). The shift of the NH proton peak to a higher chemical shift is most likely due to the formation of NS-containing species, as shown previously by the direct relationship between the NH chemical shift of the aliphatic primary amine and the concentration of S8. The shift and broadening of the NH resonance, in contrast to the appearance of the new peak, indicates that the amine-sulfur complex is exchanging with the amine. These NS-containing species can be N-polysulfamines and N,N'-polysulfodiamines (Equations 3 and 4) because their NS bond formation is a reversible process, or alkylammonium polysulfides (Equation 5) because polysulfides are reactive and rapid exchange between alkylammonium polysulfides and amines is possible ( Figure 4C The reaction of sulfur with the amino groups of MA and FA can stabilize them and inhibit the water-accelerated interconversion of MA / MA+ and FA / FA+, reducing the reactivity of MA+ and FA+ to the aminolysis reaction that degrades the MC-NMP ink.
[0091] Solar Cells
[0092] We fabricated PSCs with an indium tin oxide (ITO) / SnO2 / (FAPbI3)0.95(MAPbBr3)0.05 / Spiro-OMeTAD / gold (Au) structure. Fresh MC-NMP produced PSCs with an average efficiency of ∼16%, −21 mA / cm2 Jsc, 1.10 V Voc, and 68% FF (Table S1, Fig.37 ). MC-NMP aged for one day formed a yellow non-perovskite film (Figure 1), which could not be used to make PSCs. On the other hand, devices made with MC-NMP-S8 ink throughout 38 days of aging consistently delivered an average of ∼14% efficiency, −20 mA / cm2 Jsc, 1.05 V Voc, and 64% FF (Figure 5A, B; Table S2).
[0093] Figure 5. PSCs. (A) Current density-voltage (JV) curves of PSCs made by spin coating of MC-NMP-S8 ink aged for 5 days in ambient air. (B) Power conversion efficiency (PCE) with an pore area of 0.4 cm2 as a function of ink age used to make PSCs (by spin coating) (Note: non-perovskite films were obtained from aged MC-NMP, as shown in Figure 1). (C) JV curves of PSCs made by doctor blade coating of fresh MC-NMP-S8 ink, showing the photovoltaic parameters for the reverse scan. (D) PCE as a function of pore area measured for devices made by doctor blade coating of fresh MC-NMP-S8 ink (Table S3).
[0094] PSCs fabricated by blade coating of MC-NMP-S8 demonstrated comparable efficiencies to those of devices fabricated by spin coating (Fig. 5C; Table S3), indicating the compatibility of the ink for scalable fabrication of solar cells. As the aperture area increased, the blade-coated devices showed decreased efficiencies (primarily due to decreased fill factor) ( Figure 5D ). This well-known trend of efficiency loss with scaling is inevitable in all types of solar cells, as the series resistance (Rs) from the sheet resistance of the transparent electrode (e.g., ITO) increases approximately linearly with the aperture area. Further optimization of electrode conductivity and absorber thickness should increase fill factor and photocurrent (Jsc values of 25 mA / cm2 are achievable for similar perovskite compositions), thereby improving the overall efficiency of scalable PSCs.
[0095] Material
[0096] Tin(IV) oxide (15% aqueous solution, Alfa Aesar). Formamidine iodide (FAI) (>99.99%, GreatcellSolar); Lead(II) iodide (99.99%, TCI); Methylammonium bromide (MABr) (>99.99%, Greatcell Solar); Lead(II) bromide (≥98%, Sigma-Aldrich); Methylammonium chloride (MACl) (>99%, Greatcell Solar); 1-methyl-2-pyrrolidone (NMP) (>99.0%, Sigma-Aldrich); N,N-dimethylformamide (DMF) (anhydrous, 99.8%, Sigma-Aldrich); Sulfur (sublimed, BDH); L-α-phosphatidylcholine (egg yolk, Type XVI-E, ≥99% (TLC), lyophilized powder, Sigma-Aldrich); Phenethylammonium iodide (PEAI) (98%, Sigma-Aldrich). 2,2',7,7'-Tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (spiro-OMeTAD) (Xi'an Polymer Optical Technology Co., Ltd.);
[0097] Lithium bis(trifluoromethane)sulfonyl imide salt (Li-TFSI) (99.95%, Sigma-Aldrich); 4-tert-butylpyridine (tBP) (96%, Sigma-Aldrich); FK 209 Co(III) TFSI salt (Co-TFSI) (Sigma-Aldrich). Dimethyl sulfoxide-d6 (DMSO-d6) (99.9 atomic % D, Sigma-Aldrich).
[0098] instrument
[0099] XRD measurements were performed at PANalytical TM Empyrean system using Cu(Kα, ) source completed. 1 HNMR spectra were obtained using Bruker AVANCE TM -III 300 MHz spectrometer, with chemical shifts calibrated to residual DMSO-d5 signal. Doctor blade coating was done with a Zehntner Proceq ZAA 2300 automatic film coater, and photovoltaic parameters were measured with a Newport Oriel sol-3A (class AAA) solar simulator.
[0100] Perovskite ink
[0101] All inks contain 1.23M FA + , 0.382M MA+ , 1.29M Pb 2+ 、3.69MI - , 0.186M Br - and 0.32M Cl - , the weight ratio of NMP to DMF is 30:70 (the optimization of solvent composition is as follows Figure 6 and 7 The sulfur-containing ink was prepared by making a stock solution of S8, which was then used to make a final concentration of 0.001 M S8 in the ink. In addition to 0.001 M S8, the ink used for blade coating also contained 0.206 mg / mL L-α-phosphatidylcholine. In order to obtain all 1 For H NMR spectra, 100 μL of ink was mixed with 500 μL of DMSO-d6 immediately before analysis. 1 The H NMR signal was integrated relative to the residual DMSO-d5 signal at 2.49 ppm (calibrated to 1.00). The exponential and linear regression analysis equations for the NMR data were calculated using the SciPy library (Optimization and Statistics modules) ( Figure 1E , 3D , 4B) are as follows:
[0102] Figure 1E
[0103] y=100e -0.05x +0.2(20-30%RH)
[0104] y=100e -0.08x -1(40%RH)
[0105] Figure 3D :y=-0.2x+93
[0106] Figure 4B:
[0107] y=-0.2e -0.09x +9(MC-NMP-S8)
[0108] y=0.2e -0.04x +8(MC-NMP)
[0109] Solar cell manufacturing
[0110] The indium tin oxide patterned glass substrate was cleaned by sonication for 15 min each in additional aqueous solutions, water, acetone, and isopropyl alcohol (IPA), followed by 30 min UV / O3 treatment. The electron transport layer was made from a solution containing a volume ratio of 6:1 of H2O to 15% SnO2 aqueous solution, which was sonicated for 30 s (twice) before spin coating 100 μL of deposition at 3000 rpm. Water was used to wipe off the SnO2 solution on the edge of the substrate before annealing at 150°C for 30 min. After another 30 min UV / O3 treatment, the perovskite ink (filtered with 0.22 μm PTFE) was deposited by spin coating (75 μL ink at 4000 rpm for 25 s) or doctor blade coating (20 μL ink, 120 μm gap height, 7 mm / s), followed by a 1 min ether bath and annealing at 150°C for 3 min. The interfacial modification of the perovskite layer deposited by doctor blade coating was accomplished by immersion in a 1 mg / mL PEAI solution in IPA for 1 min, followed by rinsing the film with IPA for 5-10 sec and annealing at 100°C for 1 min. The hole transport layer was made from a mixture of 0.07 M spiro-OMeTAD in chlorobenzene, 1.88 M Li-TFSI in acetonitrile, 0.25 M Co-TFSI in acetonitrile and tBP in a volume ratio of 110:2.3:1:3.9 (filtered with 0.22 μm PTFE) and deposited by dynamic spin coating of 70 μL at 2000 rpm for 30 sec. The perovskite layer and HTL were wiped off the substrate edges with 2-ethoxyethanol before thermal volatilization of the gold on the HTL. The samples for XRD analysis were prepared from cleaned ITO-glass substrates and SnO2 and perovskite layers were deposited by spin coating as described above. All ink and film preparation and storage were done at room temperature (18-22°C) in ambient air.
[0111]
[0112] Table S1. Photovoltaic parameters of solar cells made by spin coating fresh MC-NMP ink. Values are from an aperture area of 0.3996 cm 2 The average of 35 pixels was measured after aging the device for 3 days in a box with desiccant. Figure 5B includes data from the reverse scan.
[0113]
[0114]
[0115] Table S2. Photovoltaic parameters of solar cells made by spin coating aged MC-NMP-S8 ink; for each set of devices, data for the forward and then reverse scan directions are shown. Devices were aged for 6-7 days in a box with desiccant at 0.3996 cm 2 The pore area was measured. Figure 5A includes data from ink aged for 5 days, and Figure 5B includes data from the reverse scan.
[0116]
[0117] Table S3. Photovoltaic parameters of solar cells fabricated by doctor blade coating of fresh MC-NMP-S8 ink; for each set of devices, data for the forward and then reverse scan directions are shown. The devices were measured on the day they were fabricated. Figure 5D The linear regression equation in , back-scan PCE vs pore area, is y = -3.8x + 18.3.
[0118] With the help of supplement Figures 6 to 39 Further understanding can be gained by reviewing the Supplementary Tables S1, S2, and S3.
[0119] FIG3B shows the XRD (normalized intensity—actual intensity see Figure 27-28 3C is a simplified 1H NMR spectrum of MC-NMP-S8 ink after 0 and 124 days of aging (at 18-21°C, 15-50% RH) in DMSO-d6, showing only the key resonances (for the full spectrum see Fig.29 and 33 , including the solvent peak). ( Figure 3D ) is the percentage of initial MA+ remaining as a function of ink aging, calculated from the integration of the MA+CH3 resonance ( Figure 29-33 ).
[0120] Sulfur must interact with water, amino groups, or both to inhibit their proton exchange. To investigate the role of sulfur-water interaction, we prepared MC-NMP-S8 ink using 1 M water. Despite the water concentration being 100 times higher than atomic sulfur (S), water-amine proton exchange was still inhibited, stabilizing MA+ and FA+ in the ink for at least 25 days ( Figure 34-36 ). Given the stability of this ink and the weakness of the sulfur-water interaction, we conclude that the sulfur-water interaction does not play a role in inhibiting the water-amine proton exchange and therefore does not contribute to the stabilization of the ink.
[0121] Figure 8 and 9 : shows the degradation of perovskite without additive (sulfur) in the presence of humidity. Figure 21-26 : Stabilize the ink by using additives.
[0122] In highly acidic solutions, the amine-water proton exchange rate slows down and the acid dissociation equilibrium shifts, resulting in the formation of lower concentrations of reactive MA and FA; however, the acid induces alternative ink degradation pathways, such as acid-catalyzed DMF hydrolysis ( Figure 21-26 ). Therefore, we explored neutral additives that can interact with the amino group. The rate of amine proton exchange decreases with increasing alkyl substitution, suggesting that the steric hindrance of the amino group can effectively improve stability.
[0123] Figures 10 to 14 The degradation of the perovskite film due to the amine-water proton exchange reaction is shown when additives such as sulfur are not added. FIG3B shows the XRD of films made from MC-NMP-S8 ink aged between 0 and 124 days (normalized intensity - actual intensity see Figure 27-28 ).
[0124] FIG3C is a simplified 1H NMR spectrum of MC-NMP-S8 ink after 0 and 124 days of aging (at 18-21° C., 15-50% RH) in DMSO-d6, showing only the key resonances (see Fig.29 and 33 , including the solvent peak). ( Figure 3D ) is the percentage of initial MA+ remaining as a function of ink aging, calculated from the integration of the MA+CH3 resonance ( Figure 29-33 ). Sulfur must interact with water, amino groups, or both to inhibit their proton exchange. To investigate the role of sulfur-water interaction, we prepared MC-NMP-S8 ink using 1 M water. Despite the water concentration being 100 times higher than atomic sulfur (S), water-amine proton exchange was still inhibited, stabilizing MA+ and FA+ in the ink for at least 25 days ( Figure 34-36 ). Given the stability of this ink and the weakness of the sulfur-water interaction, we conclude that the sulfur-water interaction does not play a role in inhibiting the water-amine proton exchange and therefore does not contribute to the stabilization of the ink.
[0125] Fig.15 and 16 : Shows that the degradation pathway in the mixed MA+ and FA+ inks is different from the other inks: In the 1H NMR spectrum of the aged MC-NMP ink, we do not observe any degradation from dimethylamine (at 2.54 ppm, Fig.15 ), N-methylformamide (at 2.56 ppm, Fig.16) or s-triazine (at 9.3 ppm), which are caused by the degradation of single organic cation inks containing MA+ or FA+. Therefore, these reaction pathways are not involved in the degradation of mixed MA+ and FA+ inks.
[0126] Fig.17 , 18 and 19: Role of water in ink degradation, 1H NMR spectra of solutions containing water with and without MA+ and FA+. Fig. 20 On the other hand, water protons in solutions containing all components of the MC-NMP ink except MA+ and FA+ produce a very narrow resonance of ~1 Hz (Figures 2A, 20). During the acquisition of the NMR signal, a broad peak of protons undergoing chemical exchange was observed: the FWHM of the resonance of the exchanged proton population is directly related to its exchange rate.
[0127] In summary, a major obstacle limiting the commercialization of perovskite solar cells is the degradation of the perovskite inks routinely used to make solar cells via scalable processes: decomposition of organic cations in perovskite inks has been observed within hours in ambient air. We provide evidence that water accelerates the aminolysis of FA+ by MA by promoting a fast proton transfer process, and that low concentrations of additives that can interact with amine groups to inhibit amine-water proton exchange, such as elemental sulfur, stabilize the ink for up to months. These findings provide a mechanistic understanding of the role of water in ink degradation, give tools to overcome the instability of perovskite inks and pave the way for the commercialization of perovskite solar cells.
[0128] Ambient air processing is desirable for industrial fabrication of perovskite solar cells. Here we show that a perovskite ink containing methylammonium and formamidine in N-methyl-2-pyrrolidone and N,N-dimethylformamide, a co-solvent composition that meets the prerequisites for scaling up solar cell fabrication, has a half-life of only 9 hours in ambient air. From 1H NMR spectroscopy analysis, we find that the presence of water in the ink accelerates the methylammonium-methylamine proton exchange, promoting the aminolysis of formamidine by methylamine. Addition of elemental sulfur inhibits this proton exchange process via the sulfur-amine reaction, leading to the formation of a stable perovskite ink with a half-life of 6,300 hours. A control ink aged for one day did not form a perovskite film for solar cell fabrication, while the sulfur-stabilized ink could be repeatedly used to make devices with >15% efficiency when aged for more than one month. The stabilized ink is suitable for scaling up perovskite solar cell fabrication, with efficiencies as high as 17% for blade-coated devices.
[0129] The present invention provides a method for stabilizing perovskite ink, comprising adding an additive to the perovskite ink, wherein the additive is capable of interacting with amine groups in the perovskite ink to inhibit amine-water proton exchange. In some embodiments, the additive is elemental sulfur.
[0130] Provided herein is a perovskite ink formulation comprising a precursor salt dissolved in a solvent, which is deposited as a thin film and crystallized to form the perovskite structure having an "ABX3" composition, wherein: "A" is a monovalent cation, such as methylammonium (MA+), formamidine (FA+) or cesium (Cs+), "B" is a divalent cation (Pb2+ or Sn2+), and "X" is a halogen (F-, I-, Br- or Cl-); and wherein the additive interacts with the amine groups in the perovskite ink to inhibit amine-water proton exchange. The ink may further comprise a combination of one or more salts from Group-A, Group-B, added in a molar ratio of 1:1:3 to form the perovskite precursor salt, which will later form a thin film of perovskite.
[0131] The perovskite ink formulation may be added for stabilization of the ink, wherein the perovskite ink comprises one or more additives selected from the group consisting of sulfur or sulfur-based compounds. Examples of other additives for stabilizing the ink are triethyl borate, 18-crown-6, ITIC-Th, L-α-phosphatidylcholine, and phenylboronic acid. The additives are added at a concentration of about 0.001 M to about 0.1 M. The ink containing the additives may have a stabilization temperature of 10 -4 The molar concentration of the additive varies between 1 M and 1 M. In some embodiments, the perovskite ink formulation may contain 0.001 M sulfur.
[0132] The "A" in the perovskite ink formulation can be a mixture of methylammonium (MA+) and formamidine (FA+). The ratio of MA+ to FA+ can vary from 1:19 to 1:1. The ratio of MA+ to FA+ can be 1 to 3.
[0133] The perovskite ink precursor may contain one or more solvents selected from: N-methyl-2-pyrrolidone (NMP), alkyl-2-pyrrolidone, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), dialkylformamide, γ-butyrolactone (GBL), 2-methylpyrazine (2-MB), 1-pentanol (1-P), 2-methoxyethanol (2-ME) or N,N'-dimethylpropyleneurea (DMPU). The weight percentage of the selected one or combination of solvents may be in the range of 10-30% to achieve the final concentration of the perovskite ink required for forming a perovskite film.
[0134] The solvent in the formation of the perovskite ink can be a mixture of NMP and DMF. The ratio of NMP to DMF can vary from 5:95 to 50:50. The ratio of NMP to DMF solvent is 30 to 70.
[0135] In some embodiments, "B" in the perovskite ink formulation can be a divalent cation, which includes one or more metals selected from: Be, Mg, Ca, Sr, Ba, Fe, Cd, Co, Ni, Cu, Ag, Au, Hg, Sn, Ge, Ga, Pb, In, Tl, Sb, Bi, Ti, Zn, Cd, Hg, and Zr.
[0136] In this patent document, the word "comprising" is used in its non-limiting sense, meaning that the items following the word are included, but items not specifically mentioned are not excluded. Reference to an element by the indefinite article "a" does not exclude the possibility that more than one element is present, unless the context clearly requires that there be and only one element.
[0137] The scope of the claims should not be limited by the illustrative embodiments listed as examples, but should be given the broadest interpretation consistent with the intended construction of the claims in light of the entire specification.
Claims
1. A method for stabilizing perovskite ink, comprising the following steps: preparing a perovskite ink using one or more solvents selected from N-methyl-2-pyrrolidone (NMP), alkyl-2-pyrrolidone, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), dialkylformamide, gamma-butyrolactone (GBL), 2-methylpyrazine (2-MB), 1-pentanol (1-P), 2-methoxyethanol (2-ME) or N,N'-dimethylpropyleneurea (DMPU); and Sulfur or a sulfur-based compound is added to the perovskite ink, and the sulfur or the sulfur-based compound interacts with amine groups in the perovskite ink to inhibit amine-water proton exchange.
2. The method of claim 1, wherein the sulfur or sulfur-based compound is elemental sulfur.
3. The process of any one of claims 1 and 2, wherein the one or more solvents comprise a mixture of NMP and DMF.
4. The method of claim 3, wherein the volume ratio of NMP to DMF is in the range of 5:95 to 50:
50.
5. method as claimed in claim 3, wherein the volume ratio of NMP and DMF solvent is 30 to 70.
6. A perovskite ink comprising: A precursor salt dissolved in one or more solvents which, when deposited as a thin film, crystallizes to form a perovskite structure having a composition of "ABX3", wherein: "A" is a monovalent cation, which is one or more of methylammonium (MA+) and formamidine (FA+); "B" is a divalent cation; "X" is a halogen, which is one or more of F-, I-, Br- and Cl-; and an additive selected from the group consisting of elemental sulfur and sulfur-based compounds that interact with amine groups in the perovskite ink to inhibit amine-water proton exchange; and The one or more solvents are selected from: N-methyl-2-pyrrolidone (NMP), alkyl-2-pyrrolidone, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), dialkylformamide, γ-butyrolactone (GBL), 2-methylpyrazine (2-MB), 1-pentanol (1-P), 2-methoxyethanol (2-ME) or N,N'-dimethylpropyleneurea (DMPU).
7. The perovskite ink of claim 6, wherein "B" is a divalent cation selected from one or more of Pb2+, Sn2+ or Bi2+.
8. The perovskite ink of claim 6, wherein "B" is a divalent cation selected from one or more of Pb2+ or Sn2+.
9. The perovskite ink according to any one of claims 6-8, wherein "A", "B" and "X" form a perovskite precursor salt in a molar ratio of 1:1:
3.
10. The perovskite ink according to any one of claims 6 to 9, wherein the concentration of the additive is 0.0001M to 1M.
11. The perovskite ink of any one of claims 6-9 comprising 0.001 M sulfur.
12. The perovskite ink according to any one of claims 6-11, wherein the "A" is a mixture of methylammonium (MA+) and formamidine (FA+).
13. The perovskite ink according to claim 12, wherein the molar ratio of MA+ to FA+ is in the range of 1:19 to 1:
1.
14. The perovskite ink according to claim 12, wherein the molar ratio of MA+ to FA+ is 1 to 3.
15. The perovskite ink according to any one of claims 6 to 14, wherein the weight percentage of the one or more solvents is in the range of 10-30% to achieve the desired final concentration of the perovskite ink for forming a perovskite film.
16. The perovskite ink according to any one of claims 6-15, wherein the solvent comprises a mixture of NMP and DMF.
17. The perovskite ink according to claim 16, wherein the volume ratio of NMP to DMF is in the range of 5:95 to 50:
50.
18. The perovskite ink according to claim 16, wherein the volume ratio of NMP to DMF solvent is 30 to 70.
19. The perovskite ink of claim 7, wherein the divalent cation "B" comprises one or more metals selected from Be, Mg, Ca, Sr, Ba, Fe, Cd, Co, Ni, Cu, Ag, Au, Hg, Sn, Ge, Ga, Pb, In, Tl, Sb, Bi, Ti, Zn, Cd, Hg, or Zr.
Citation Information
Cited By
Methylamino perovskite single crystal, preparation method and X-ray detector thereof
CN119710934A