Flame-retardant and thermal insulation material
By using a laminate of flame retardant layer and aerogel layer in the battery system of electric vehicles, the problem that traditional insulation materials cannot be effectively insulated in high temperature environments is solved, and efficient heat insulation and safety protection in narrow spaces is achieved .
Patent Information
- Application Number
- CN202380029589.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-21
- Filing Date
- 2023-01-23
- Publication Date
- 2024-11-08
AI Technical Summary
Existing electric vehicle battery systems are prone to explosions and fires in high-temperature environments. Traditional insulation materials cannot provide sufficient insulation protection, and space limitations lead to limited material use.
Using a laminate including a flame retardant layer and an aerogel layer, the combination of a flame retardant layer and an aerogel layer can effectively delay heat transfer at high temperatures and keep the substrate temperature at 500°C or below. Application in small spaces.
The laminate can effectively insulate heat in high temperature environments, extend the use time of the battery system, reduce the risks of explosion and fire, and is suitable for small spaces such as battery systems for electric vehicles.
Smart Images

Figure CN118922514A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. Provisional Patent Application No. 63 / 301,897 filed on January 21, 2022 and U.S. Provisional Patent Application No. 63 / 481,124 filed on January 23, 2023, the entire contents of which are incorporated herein by reference. Background of the Invention A. Technical field
[0004] The present invention generally relates to a laminate of flame retardant and / or thermal insulation materials that can be used for all types of articles. In some aspects, the laminate can be used to protect articles (e.g., batteries, electronic devices, and / or non-conductive protective materials) from the effects of high temperature (e.g., greater than 500° C.) environments that the articles may be subjected to for a given period of time (e.g., 1 minute to 90 minutes).
[0005] B. Related technical description
[0006] The electrification of society is becoming more and more common today. An example of this is the rapid electrification of the transportation sector. In particular, vehicles such as cars, trains, and airplanes are moving away from internal combustion engine technology and toward electric motors that rely on battery systems. These battery systems can be complex systems that rely on chemicals, chemical reactions, electronic components, and other materials to store and release electricity for electric motors.
[0007] One problem associated with battery systems used in electric vehicles is that they are larger and store and release more energy than battery systems used in typical vehicles that rely primarily on internal combustion engine technology. A particular problem is that if batteries used in electric vehicles are mechanically damaged (e.g., automobile accidents, wiring or electronic system failures, etc.), exposed to temperatures outside their operating window, or subjected to rapid charging and / or discharging events, they can result in relatively larger explosions, larger fires, and / or release of larger amounts of corrosive chemical fumes than batteries used in vehicles that rely on internal combustion engines. Lithium-ion batteries used in electric vehicles can catch fire and / or explode at temperatures exceeding 500°C. In contrast, vehicle fires caused by, for example, traffic accidents can generate heat of more than 1500°F (815°C). When an electric vehicle has an accident and a fire occurs, there is a certain amount of time to extinguish the fire and / or leave and clean up the vehicle before the battery catches fire and / or explodes. With the increasing electrification of society, especially the increasing electrification of transportation infrastructure, and the increasing energy density of batteries, the risk of electric vehicle fires and battery fires and explosions may increase.
[0008] Traditional thermal insulation materials, such as foams, polymers and elastomers, have been used to provide some insulation for electric vehicle battery systems. Unfortunately, these traditional materials still face limitations. For example, although polymer foam has a lower thermal conductivity to mitigate heat transfer, its thermal diffusivity (i.e., the thermal conductivity of the material divided by its density and specific heat capacity) is often higher than other insulating materials. Due to the higher thermal diffusivity (meaning that the thermal conductivity is higher relative to the specific heat capacity and density of the material), the temperature of this polymer foam may tend to rise faster, so that as the heating continues, the heat spreads faster through it. Other polymers and elastic materials may have lower thermal diffusivity than polymer foam, but tend to have higher thermal conductivity. In addition, the heat concentrated on a part of this traditional thermal insulation material may not be distributed on its surface, thereby accelerating the heat transfer through the thickness of the material to the surface of the element it is designed to protect. Therefore, traditional thermal insulation materials may not provide the desired insulation level in certain applications.
[0009] Additionally, in some systems, insulation materials may be limited by tight spaces. Because traditional insulation materials are often relatively thick and / or stiff, this limitation may limit the amount of traditional insulation materials that can be included in a system—further limiting the insulation provided by the material, or possibly making such a material unusable in a system. In addition to these limitations, polymers, elastomers, and foams often have relatively high coefficients of thermal expansion, making space limitations for these materials even more severe when heated. Summary of the invention
[0010] The present invention provides a solution to at least one or more than one of the aforementioned problems, which are related to providing thermal insulation to an article, substrate or system (e.g., a battery system). In one aspect, it is found that a laminate comprising a flame retardant layer and an aerogel layer having a flammability rating that complies with at least one flammability standard (e.g., UL94 5VB or UL94 5VA rating) can provide good thermal insulation performance for an article, substrate or system (articles, substrates or systems can be used interchangeably in this specification). In such a laminate, the synergy between the flame retardant layer and the aerogel layer can provide thermal insulation to the substrate - in terms of the heating rate and / or equilibrium temperature of the substrate - more than the expected protection of the sum of those parts, especially when the thickness of the aerogel layer is low (e.g., less than 0.5 mm). Without wishing to be bound by any particular theory, it is believed that the aerogel layer has low thermal conductivity and low thermal diffusivity, effectively delaying heat transfer from the flame retardant layer to the substrate.
[0011] For example, when the laminate of the present invention is attached to the surface of a substrate, when the laminate is exposed to a temperature above 500°C, preferably 500°C to 1500°C or more preferably 700°C to 1200°C, the laminate is capable of maintaining the temperature of the substrate (e.g., the surface temperature of the substrate) at or below 500°C for 1 minute to 90 minutes, preferably at least 5 minutes. This is advantageous because it provides more time before the substrate (e.g., an electric vehicle battery system) reaches a temperature at which the substrate may fail. When used to protect an electric vehicle battery system, this can be particularly advantageous because it can provide more time for the occupants of the vehicle to leave the vehicle after an accident and before the electric vehicle battery catches fire, explodes, and / or releases toxic chemicals. This can also provide more time for initial responders (e.g., a fire department) to extinguish the fire before the electric vehicle battery catches fire, explodes, and / or releases toxic chemicals. Notably, the laminates of the present invention can be relatively thin (e.g., equal to or less than 25.4 millimeters (mm), 20 mm, 15 mm, 10 mm, 5 mm, 3 mm, 2 mm, 1 mm, 0.5 mm, 0.4 mm, 0.3 mm, 0.2 mm, 0.1 mm, or less than 0.1 mm) and / or can be relatively flexible (e.g., can be rolled up (see, e.g., Figure 5 )) and / or having a bending radius. The flexibility of the laminate of the present invention is advantageous in that it can be used in applications with narrow space constraints (eg, electric vehicle battery systems and battery packs).
[0012] In one aspect of the invention, a laminate comprising a flame retardant layer and a porous material layer (e.g., a foam layer or an aerogel layer, preferably an aerogel layer) is disclosed. The laminate may have a relative front surface and a rear surface, wherein the flame retardant layer defines at least a majority of the front surface. The laminate may have a thickness equal to or less than 25.4 millimeters (mm), 24 mm, 23 mm, 22 mm, 21 mm, 20 mm, 19 mm, 18 mm, 17 mm, 16 mm, 15 mm, 14 mm, 13 mm, 12 mm, 11 mm, 10 mm, 9 mm, 8 mm, 7 mm, 6 mm, 5 mm, 4 mm, 3 mm, 2 mm, 1 mm, 0.9 mm, 0.8 mm, 0.7 mm, 0.6 mm, 0.5 mm, 0.4 mm, 0.3 mm, 0.2 mm, 0.1 mm, or any range thereof. In other aspects, the laminate can have a thickness greater than 25.4 mm (e.g., 26 mm, 27 mm, 28 mm, 29 mm, 30 mm, 35 mm, 40 mm, 45 mm, 50 mm, 55 mm, 60 mm, 65 mm, 70 mm, 75 mm, 80 mm, 85 mm, 90 mm, 95 mm, or 100 mm or greater than 100 mm or any range therein). In some preferred aspects, the laminate has a thickness of 0.3 mm to 10 mm, 0.3 mm to 5 mm, or 0.3 mm to 3 mm. In some aspects, the flame retardant layer has a thickness of 0.05 mm to 0.8 mm. In some aspects, the porous layer (e.g., an aerogel layer) has a thickness of 0.05 mm to 1.0 mm (or any value or range therein, such as 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm), preferably 0.05 mm and 0.254 mm.
[0013] In some aspects, the flame retardant layer is not electrically insulating. In other aspects, the flame retardant layer is electrically insulating. In some aspects, the flame retardant layer and / or the entire laminate conform to the plastic flammability standard. In some specific aspects, the plastic flammability standard is UL945VA or UL94 5VB. In particular aspects, the flame retardant layer comprises fibers (e.g., woven fibers and / or non-woven fibers) and / or one or more than one metal hydroxide, organic phosphate / ester, aluminum hydroxide, inorganic filler and / or metal oxide. In some aspects, the flame retardant layer may be halogen-free. In some aspects, the flame retardant layer may include silicates (e.g., layered silicates). In some specific aspects, silicates may include mica. Based on the gross weight of the flame retardant layer, the flame retardant layer may include at least 90% by weight of silicates, preferably mica. In some aspects, the flame retardant layer comprises ceramics. Ceramics may include inorganic and / or non-metallic materials (e.g., clay, kaolin, aluminum oxide, silicon carbide, tungsten carbide, etc.) that can withstand high temperatures. In some aspects, the ceramic can include a metal oxide or a non-metal oxide or a combination thereof. In some aspects, the ceramic can include aluminum oxide, beryllium oxide, cerium oxide, zirconium oxide, carbide, boride, nitride or silicide or any combination thereof. In some aspects, the flame retardant layer can include at least 90 weight percent ceramic based on the total weight of the flame retardant layer.
[0014] In some aspects, the porous layer is an aerogel layer. In some aspects, the aerogel layer comprises an organic polymer. In some aspects, the organic polymer is a thermoplastic polymer. In some aspects, the thermoplastic polymer is a polyimide, polystyrene, polyester, polyamide, polyether, polyurethane, acrylic polymer, polyurea, polypyrrole, polythiophene, polyaniline, acrylic polymer, vinyl polymer, polysiloxane, polysulfide, polycarbonate, or its copolymer, or its mixture. In a preferred embodiment, the thermoplastic polymer is a polyimide, polyamide amide or its mixture or copolymer. In a particular aspect, the aerogel layer comprises at least 50%, 60%, 70%, 80%, 90% or 95% of a thermoplastic polymer, preferably a polyimide or polyamide amide. In other aspects, the polymer aerogel layer comprises less than 50%, 40%, 30%, 20%, 10%, 5% or less than 5% of a thermoplastic polymer, preferably a polyimide or polyamide amide. In some aspects, the decomposition temperature of the aerogel layer is equal to or higher than 400°C, preferably 400°C to 600°C.
[0015] The laminate of the present invention may include one or more adhesive layers. One or more adhesive layers may be bonded to the aerogel layer. In one aspect, the first adhesive layer is disposed between the flame retardant layer and the aerogel layer. The first adhesive layer may have a melting temperature or a decomposition temperature higher than 500°C, preferably higher than 600°C. On the other hand, the second adhesive layer may be disposed on the rear surface of the aerogel layer (the surface away from the flame retardant layer). The first adhesive layer and / or the second adhesive layer may be a pressure-sensitive adhesive layer that can adhere the rear surface of the aerogel layer to a substrate. Prior to use, a releasable or peelable liner layer may be disposed on the second adhesive layer. In some aspects, the second adhesive layer may have a melting temperature or a decomposition temperature higher than 500°C, preferably higher than 600°C. In particular aspects, the adhesive layer may contain a silicone adhesive compound and / or an epoxy compound.
[0016] The laminate of the present invention may include one or more heat dissipation layers. In some aspects, one or more heat dissipation layers may have a thermal conductivity of at least 15 W / m·K, preferably 15 W / m·K to 2500 W / m·K. In some aspects, one or more heat dissipation layers may include metal or graphite or a combination thereof. The metal or graphite may have a thermal conductivity of at least 15 W / m·K, preferably 15 W / m·K to 2500 W / m·K. In some aspects, the metal may include copper, aluminum, molybdenum, tungsten, rhenium, tantalum, niobium, stainless steel, nickel, or an alloy thereof. In some aspects, based on the total weight of the heat dissipation layer, one or more heat dissipation layers may include at least 30 wt%, 40 wt%, 50 wt%, 60 wt%, 70 wt%, 80 wt%, 90 wt%, 95 wt%, 96 wt%, 97 wt%, 98 wt%, 99 wt% or more than 99 wt% of metal and / or graphite. In some aspects, one or more heat dissipation layers can have a thickness of 0.001 mm to 0.4 mm, preferably 0.01 mm to 0.05 mm, or any range or value therein (e.g., 0.02 mm, 0.03 mm, 0.04 mm, 0.05 mm, 0.06 mm, 0.07 mm, 0.08 mm, 0.09 mm, 0.1 mm, 0.2 mm, or 0.25 mm).
[0017] In some aspects, one or more heat dissipation layers may be bonded to the flame retardant layer and / or the aerogel layer. In some aspects, one or more heat dissipation layers may be disposed between the flame retardant layer and the aerogel layer. In some aspects, the first adhesive layer may be disposed between the flame retardant layer and the heat dissipation layer, and / or the second adhesive layer may be disposed between the heat dissipation layer and the aerogel layer. In some aspects, the adhesive layer is not disposed between the flame retardant layer and the aerogel layer. In some aspects, the first adhesive layer may be in direct contact with the flame retardant layer and the heat dissipation layer, and the second adhesive layer may be in direct contact with the heat dissipation layer and the aerogel layer. In some aspects, a third adhesive layer and an optional backing layer may be used, wherein the third adhesive layer is disposed between the aerogel layer and the optional backing layer. In some aspects, the third adhesive layer may be in direct contact with the aerogel layer and the optional backing layer. In some aspects, the first adhesive layer, the second adhesive layer, and / or the third adhesive layer can each: (1) have a melting temperature or decomposition temperature greater than 500° C.; (2) contain a pressure-sensitive adhesive; and / or (3) contain a silicone adhesive compound and / or an epoxy compound. In some aspects, any one, any combination, or all of the flame retardant layer, the heat dissipation layer, the aerogel layer, and / or the first adhesive layer, the second adhesive layer, and / or the third adhesive layer can be perforated. In some aspects, the perforations can help remove any gas from the laminate (e.g., from evaporation or boiling of the adhesive layer).
[0018] The laminate of the present invention may include one or more reinforcing layers. In some aspects, one or more reinforcing layers may be attached to at least a portion of the flame retardant layer and / or be included in at least a portion of the volume of the flame retardant layer. In some aspects, one or more reinforcing layers may include fibers. Non-limiting examples of fibers include glass fibers, carbon fibers, aramid fibers, thermoplastic fibers, thermosetting fibers, ceramic fibers, basalt fibers, rock wool fibers, steel fibers or cellulose fibers or any combination thereof. In some aspects, fibers are nonwoven fibers or woven fibers.
[0019] In some aspects of the invention, any one, any combination or all of the flame retardant layer, porous layer (e.g., aerogel layer), adhesive layer, heat dissipation layer and / or reinforcement layer are perforated. The size and pattern of the perforations can be modified as needed. In some aspects, the size of the perforations is nanometers, micrometers or millimeters. In some aspects, the pattern of the perforations can be random, grid-like, circular, etc. In some specific embodiments, the pattern is grid-like. Without wishing to be bound by theory, it is believed that perforations may be helpful in the case of waste gas generated when the adhesive layer is subjected to high temperature or reduced pressure. Allowing the release of gas helps to avoid bubbling and / or delamination of the aerogel and / or flame retardant layer.
[0020] Also disclosed in the context of the present invention is a device comprising one or more laminates of the present invention. The laminate can be bonded to the device so that the front surface of the first laminate in the laminate is disposed farther from the device than the rear surface of the first laminate. The device can be any type of device. In a preferred aspect, the device is a device that may potentially be subjected to high temperatures (e.g., greater than 500° C.) during use. An example is a battery. In a preferred aspect, the battery can be an electric vehicle battery system or battery pack. The battery can be a secondary battery / rechargeable battery (e.g., a lithium-ion battery or a nickel-metal hydride battery). The vehicle can include one or more wheels and one or more motors, each motor being configured to rotate at least one wheel. The battery can be electrically connected to at least one motor. In another example, the device can be a busbar of a battery. The busbar can be electrically connected to the battery. The laminate of the present invention can be bonded to the busbar so that the front surface of the laminate is disposed farther from the busbar than the rear surface of the laminate.
[0021] In some aspects, the device can be a compression pad, a battery cell, a battery module, a battery pack, or a battery box. The compression pad, which may also be referred to as a battery gasket, can be located between the battery cells to help withstand dimensional changes in the battery cells during charging and / or use of the battery cells. The compression pad can allow sufficient pressure to be applied to the battery pack to maintain thermal and / or electrical connections while also allowing for tolerance and / or expansion when the battery cells are charged or exposed to extreme temperatures. In some aspects, the compression pad may include a compressible material. In some aspects, the compressible material may be a foam (e.g., a polyurethane foam or a silicone foam). In some aspects, the compression pad is located between the first battery cell and the second battery cell. The laminate of the present invention may cover a portion, a majority, or all of the outer surface of the compression pad.
[0022] In some aspects, the device can be a battery cell. The battery cell can be charged to provide electrical energy (e.g., to supply electrical energy to an electric motor), and can be discharged when in use or exposed to extreme temperatures or maintained in a latent state. Multiple battery cells can be arranged adjacent to each other, and compression pads can be arranged between each battery cell. The laminate of the present invention can cover a portion, a majority, or all of the outer surface of the battery cell.
[0023] In some aspects, the device may be a battery module. The battery module may include a plurality of battery cells. The laminate of the present invention may cover a portion, a majority, or all of the outer surface of the battery module.
[0024] In some aspects, the device may be a battery pack. The battery pack may include a plurality of battery modules. The laminate of the present invention may be located between the battery modules of the battery pack. The laminate of the present invention may cover a portion, a majority, or all of the outer surface of the battery pack.
[0025] In some aspects, the device may be a battery box or battery housing or container. The battery box or container may enclose a portion, most or all of the battery pack. The battery box may include an outer surface, an inner surface, and an internal volume. The laminate of the present invention may cover at least a portion, most or all of the outer surface of the battery box, at least a portion, most or all of the inner surface, or both. In some preferred aspects, at least a portion, most or all of the inner surface of the battery box is covered with one or more than one laminate of the present invention. In some aspects, the internal volume of the battery box includes a compression pad, a battery cell, a battery module or a battery pack or any combination thereof. In some aspects, the compression pad, the battery cell, the battery module, the battery pack and / or the battery box are contained in a vehicle, which includes one or more than one electric motor. In some aspects, the vehicle may be a car, an aircraft, a train, a ship or a spacecraft.
[0026] In some aspects, the device can be a cable. The cable can have a length and a width. The length can be longer than the width. In some aspects, the cable can be conductive. In some aspects, the cable can have a conductive portion and an electrically insulating portion. In some aspects, the electrically insulating portion can surround a portion, a majority, or all of the conductive portion. In some aspects, the conductive portion can include a conductive metal (e.g., copper, gold, platinum, aluminum, steel, etc.). In some aspects, the cable can include a diameter of 0.0001 inch to 10 inches, preferably 0.001 inch to 1 inch, or any range or number therein (e.g., 0.0001 inch, 0.0002 inch, 0.0003 inch, 0.0004 inch, 0.0005 inch, 0.0006 inch, 0.0007 inch, 0.0008 inch, 0.0009 inch, 0.001 inch, 0.002 inch, 0.003 inch, 0.004 inch, 0.005 inch, 0.006 inch, In some aspects, the cable can be included in a missile, rocket, artillery, manned aircraft, unmanned aircraft, land vehicle, or marine vehicle. In some aspects, the vehicle can be a spacecraft or an aircraft.
[0027] Also disclosed in the context of the present invention is a method of using any of the laminate insulation devices of the present invention. The method may include bonding the laminate to a surface of the device. Such bonding may be achieved by an adhesive. The laminate may be positioned relative to the device such that a front surface of the laminate is disposed further from the device than a rear surface of the laminate. When the front surface of the laminate is exposed to a temperature above 500°C, preferably 500°C to 1500°C (or 600°C, 700°C, 800°C, 900°C, 1000°C, 1200°C, 1300°C, 1400°C or any range therein), or more preferably 700°C to 1200°C (or 800°C, 900°C, 1000°C, or 1100°C or any range therein), the laminate of the present invention is capable of maintaining the temperature of the device at or below 500°C for 1 minute to 90 minutes (or 2 minutes, 3 minutes, 4 minutes, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 60 minutes, 70 minutes, 80 minutes or 90 minutes or any range therein), preferably at least 5 minutes.
[0028] The term "aerogel" refers to a class of materials that are typically produced by forming a gel, removing a mobile interstitial solvent phase from the pores, and then replacing it with a gas or gas-like material. By controlling the gel and evaporation system, density, shrinkage, and pore collapse can be minimized. The aerogels of the present invention can contain macropores, mesopores, and / or micropores. In preferred aspects, a majority (e.g., greater than 50%) of the pore volume of the aerogel can be composed of macropores. In other alternative aspects, a majority of the pore volume of the aerogel can be composed of mesopores and / or micropores, such that less than 50% of the pore volume of the aerogel is composed of macropores. In some embodiments, the aerogels of the present invention can have a low bulk density (about 0.75 g / cm 3 or less than 0.75g / cm 3 , preferably about 0.01 g / cm 3 To about 0.5g / cm 3 ), high surface area (usually about 10m 2 / g to 1000m 2 / g and greater than 1000m 2 / g, preferably about 50m 2 / g to about 1000m 2 / g), high porosity (about 20% and above, preferably above about 85%), and / or relatively large pore volume (greater than about 0.3 mL / g, preferably about 1.2 mL / g or above).
[0029] The presence of macropores, mesopores and / or micropores in the aerogels of the present invention can be determined by mercury intrusion porosimetry (MIP) and / or gas physical adsorption experiments. MIP testing can be used to measure mesopores and macropores (i.e., American Standard Test Method (ASTM) D4404-10, Standard Test Method for Pore Volume and Pore Volume Distribution of Soil and Rock by Mercury Intrusion Porosimetry). Gas physical adsorption experiments can be used to measure micropores (i.e., ASTM D1993-03 (2008) Standard Test Method for Precipitated Silica—Surface Area by Multipoint BET Nitrogen Measurement).
[0030] The "decomposition temperature" of a material is the temperature at which a sample of the material decomposes by 2%, 5%, or 10% when heated in an environment raised to that temperature. The decomposition temperature can be measured by placing the sample in a thermogravimetric analyzer (TGA), heating the sample from ambient temperature in the TGA (e.g., at a rate of 10°C / minute), and recording the temperature at which the sample mass is 2%, 5%, or 10% less than its initial mass as its decomposition temperature.
[0031] The term "coupled" is defined as connected, although not necessarily directly, and not necessarily mechanically. The two items "coupled" may be integral with one another or connected to one another via one or more intermediate components or elements.
[0032] Unless the disclosure clearly requires otherwise, non-use of quantifiers includes plural references.
[0033] As understood by those of ordinary skill in the art, the term "substantially" is defined as most but not necessarily all of what is specified (and includes what is specified; for example, substantially 90 degrees includes 90 degrees, substantially parallel includes parallel). In any disclosed embodiment, the terms "substantially", "approximately" and "about" may be replaced with "within a specified [percentage]", where the percentage is 1%, 1%, 5% or 10%.
[0034] The phrase "and / or" means "and" or "or". For example, A, B, and / or C includes: A alone, B alone, C alone, a combination of A and B, a combination of A and C, a combination of B and C, or a combination of A, B, and C. In other words, "and / or" serves as an inclusive "or".
[0035] The terms "comprises," "has," "includes," and "contains" are open-ended linking verbs. Thus, a device that "comprises," "has," "includes," or "contains" one or more elements possesses those one or more elements, but is not limited to possessing only those one or more elements. Likewise, a method that "comprises," "has," "includes," or "contains" one or more steps possesses those one or more steps, but is not limited to possessing only those one or more steps.
[0036] The laminates of the present invention may "comprise," "consist essentially of," or "consist of" the specific ingredients, components, compositions, etc. disclosed throughout the specification. With respect to the transitional phrase "consist essentially of," in one non-limiting aspect, the basic and novel feature of the laminates of the present invention is their ability to thermally insulate a substrate for an extended period of time when the substrate is subjected to temperatures that may cause the substrate to fail (e.g., ignite, explode, rupture, deform, etc.).
[0037] Even if not described or illustrated, one or more features of one embodiment may be applied to other embodiments, unless expressly prohibited by the disclosure or the nature of the embodiments.
[0038] Some details associated with the above-mentioned embodiments and others will be described below.
[0039] BRIEF DESCRIPTION OF THE DRAWINGS
[0040] The following figures are shown by way of example and not limitation. For the sake of brevity and clarity, every feature of a given structure is not always labeled in every figure in which the structure appears. The same reference numerals do not necessarily represent the same structure. Instead, the same reference numerals may be used to indicate similar features or features having similar functions, as may non-identical reference numerals.
[0041] Figure 1A and Figure 1B is a cross-sectional view of an embodiment of a laminate of the present invention having a flame retardant layer and a single aerogel layer ( Figure 1A ) or a flame retardant layer and two aerogel layers ( Figure 1B ).
[0042] Figure 2 is a cross-sectional view of another embodiment of a laminate of the present invention having a backing layer removably disposed on an adhesive layer of the laminate, the backing layer defining at least a portion of a back surface of the laminate.
[0043] Figure 3 is a cross-sectional view of another embodiment of a laminate of the present invention having a reinforcement layer attached to the flame retardant layer of the laminate.
[0044] Figure 4 is a cross-sectional view of another embodiment of the laminate of the present invention having a heat dissipation layer disposed between the flame retardant layer of the laminate and the aerogel layer of the laminate.
[0045] Figure 5 is a perspective view of a roll of an embodiment of a laminate of the present invention.
[0046] Figure 6 is a schematic diagram of a vehicle having a battery comprising one or more embodiments of the laminate of the present invention.
[0047] Fig. 7A is a schematic diagram of a cable comprising one or more embodiments of the laminate of the present invention.
[0048] Figure 7B It is along Fig. 7A The line 7B-7B is intercepted Fig. 7A Schematic diagram of the cross-section of the cable.
[0049] Figure 8 Schematic diagram of an apparatus for testing the thermal and combustion properties of the laminate of the present invention.
[0050] Fig. 9 is Figure 8 Schematic diagram of the laminate used in the testing apparatus.
[0051] Fig.10 Thermal curves of a control (no barrier on a copper substrate), a flame retardant barrier (layer) on a copper substrate, a thermal insulation layer on a copper substrate, a laminate of the present invention on a copper substrate (one thermal insulation layer and one flame retardant layer), and another laminate of the present invention on a copper substrate (two thermal insulation layers and one flame retardant layer).
[0052] Fig.11 is another schematic diagram of an apparatus for testing the thermal and combustion performance of laminates of the present invention.
[0053] Figures 12 to 15 are thermal profiles of laminates of the present invention bonded to a substrate, in some cases, compared to an unprotected substrate.
[0054] Fig.16 is a rear view of a carbon fiber composite panel, the front side of which was protected by one of the inventive laminates during exposure to a 1000° C. flame for 25 minutes.
[0055] Fig.17 is a thermal profile of one of the laminates of the present invention bonded to an aluminum sheet substrate.
[0056] Fig.18 is a rear view of an aluminum sheet substrate, the front side of which was protected by one of the laminates of the present invention during exposure to a 1000°C flame for 25 minutes. DETAILED DESCRIPTION OF THE INVENTION
[0058] The electrification of today's society has provided technological advances that offer alternatives to the internal combustion engine. However, with these advances come new challenges. For example, the use of electric vehicle battery systems in the transportation industry can reduce reliance on gasoline as a fuel. However, these battery systems can result in a greater risk of explosion, fire, and / or release of toxic fumes, for example, if the battery system is exposed to excessive heat (e.g., in excess of 500°C).
[0059] The present invention provides a solution to at least one of these problems. The solution is a laminate material that can provide good thermal insulation and flexibility, both of which are desirable properties for certain applications (e.g., electric vehicle battery systems). In one aspect, the present invention provides a laminate comprising a flame retardant layer having a flammability rating that complies with at least one plastic flammability standard (e.g., UL94 5VB or UL94 5VA rating) and an aerogel layer. The laminate of the present invention, when attached to the surface of a substrate, is capable of maintaining the temperature of the substrate (e.g., the surface temperature of the substrate) at or below 500°C for 1 minute to 90 minutes, preferably at least 5 minutes, when the laminate is exposed to a temperature above 500°C, preferably 500°C to 1500°C or more preferably 700°C to 1200°C. The laminates of the present invention are also thin (e.g., having a thickness equal to or less than 25.4 millimeters (mm), 20 mm, 15 mm, 10 mm, 5 mm, 3 mm, 2 mm, 1 mm, 0.5 mm, 0.4 mm, 0.3 mm, 0.2 mm, 0.1 mm, or any range therein) and flexible (e.g., they can be rolled up (see, e.g., Figure 5 ) and / or having a bending radius. The good thermal insulation performance of the laminate of the present invention and its thin and flexible characteristics allow the laminate to be used as a covering or protective layer for batteries (e.g., electric vehicle batteries and battery systems with multiple batteries), battery bus bars, and various other articles in places restricted by small spaces.
[0060] A. Thermal insulation and flame retardant protective laminate
[0061] Figure 1A and Figure 1BA laminate 100 is shown. The laminate 100 may be attached to a surface of a substrate 10, the laminate having opposite front and rear surfaces 12 and 14, respectively. The laminate 100 may include one or more thermally insulating porous layers (e.g., aerogel layers) 16, a flame retardant layer 18 defining at least a portion (e.g., at least a majority, up to all and including all) of the front surface 12, and one or more adhesive layers 20, 22, and 24. The thermally insulating layer (e.g., aerogel layer) may also include greater than or equal to any one of the following or between any two of the following thermally insulating layers: 1, 2, 3, 4, 5, 6, 7, 8, or 9. The adhesive layers 20, 22, and 24 may be the same or different materials (e.g., silicone adhesive compounds, acrylic adhesive compounds, rubber adhesive compounds, phenolic compounds, cyanate ester compounds, epoxy resin compounds, etc.). In certain aspects, the adhesive layer can be an adhesive that maintains adhesion at high temperatures (e.g., 500° C. or above), non-limiting examples of which include FLEXcon Silicone Adhesive SA6000SA 9000D Series (FLEXcon Company, Inc., Spencer, Massachusetts), Alamo Tapes Epoxy Adhesives (Alamotape, San Antonio, Texas), Avery FT 3010 (Avery Dennison Corporation, Painesville, Ohio), and Adhesive Applications S1001-01 (Adhesive Applications, Inc., Easthampton, Massachusetts). The number of adhesive layers 20, 22, and 24 can be greater than or equal to any one of the following or between any two of the following: 1, 2, 3, 4, 5, 6, 7, 8, or 9, depending on, for example, the number of thermal insulation layers. The second adhesive layer 22 can define at least a portion of the rear surface 14 (e.g., at least a majority, up to and including the entirety), such that the laminate 100 can be adhered to the surface 14 when the second adhesive layer is disposed on the surface. The third adhesive layer 24 can adhere the thermal insulation layer 16 together. As shown in the figure, the laminate 100 includes a ( Figure 1A ) or two ( Figure 1B) thermal insulation layer 16, flame retardant layer 18 and adhesive layers 20, 22, 24, substantially all of the front surface 12 is defined by the flame retardant layer, and substantially all of the rear surface 14 is defined by the second adhesive layer. In addition, in some embodiments, the laminate 100 does not need to have a first adhesive layer 20 and / or a second adhesive layer 22. In one embodiment, the laminate 100 may include a single thermal insulation layer (aerogel layer) 16, a flame retardant layer 18, an adhesive layer 20 and an adhesive layer 22.
[0062] The combination of the heat-insulating layer 16 and the flame-retardant layer 18 can slow down the spread of heat and flames, and is used to provide heat insulation and flame retardant protection for the surface of the substrate 10. For example, the flame-retardant layer 18 can include flame-retardant materials, as well as optional nonwoven fibers, paper and fillers. Flame-retardant materials include metal hydroxides, organic phosphates, metal phosphates, nitrogen-containing polymers, nitrogen-phosphorus compounds, talc, sulfonates or their salts, silicon dioxide, silicates (such as mica), hydrated oxides, organic polymers, nanoclays (nanoclays), organic clays, organic polymers, silicon phosphorus nitrogen compounds, metal oxides, ceramics (such as metals and / or non-metallic oxides, aluminum oxide, beryllium oxide, cerium oxide, zirconium oxide, carbides, borides, nitrides and / or silicides) and mixtures thereof. Non-limiting examples of metal hydroxides include trihydrate aluminum oxide, magnesium oxide, etc. Non-limiting examples of metal oxides include titanium oxide, aluminum oxide, zinc oxide, iron oxide, magnesium oxide, calcium oxide, etc. Non-limiting examples of phosphate esters include trimethyl phosphate, triethyl phosphate, tributyl phosphate, tri(2-ethylhexyl) phosphate, tributoxyethyl phosphate, isodecyl phosphate, 2-acryloyloxyethyl phosphate, tri(xylene) phosphate, tri(2-phenylphenyl) phosphate, triconaphthyl phosphate, cresyl diphenyl phosphate, diphenyl diphenyl phosphate, diphenyl-2-methacryloyloxyethyl phosphate, resorcinol bis(diphenyl phosphate), resorcinol bis(xylene phosphate), resorcinol bis(dimethyl In some embodiments, the flame retardant layer (e.g., 18) may include at least 90% by weight of a flame retardant material, such as at least 90% by weight of a silicate or at least 90% by weight of a ceramic.
[0063] Non-limiting examples of fillers include kaolin clay, talc, mica, calcium carbonate, alumina trihydrate, montmorillonite, smectite, bentonite, illite, chlorite, sepiolite, attapulgite, kaolin, vermiculite, latrodectes, rectorite, perlite, aluminum nitride, silicon carbide, boron nitride, and combinations thereof.
[0064] The flame retardant layer can be reinforced. For example, the flame retardant layer can include woven fibers and / or nonwoven fibers. Non-limiting examples of fibers include aramid fibers, organic fibers, glass fibers, carbon fibers, thermoplastic fibers, thermosetting fibers, basalt fibers, ceramic fibers, rock wool fibers, steel fibers, cellulose fibers and / or the like. In embodiments where the flame retardant layer is fiber-reinforced, the fibers can be included in at least a portion of the volume of the flame retardant layer in the form of, for example, a reinforcement layer.
[0065] Additionally or alternatively, reference Figure 3 Some laminates, such as laminate 300, include a reinforcement layer 60 that is separate from the flame retardant layer 18, which may include woven fibers and / or nonwoven fibers as described above. More specifically, the reinforcement layer 60 may be attached to at least a portion of the flame retardant layer 18, for example, by an adhesive layer 20. Other laminates may include any suitable number of reinforcement layers (e.g., 60), each of which may be disposed at any suitable location within the laminate.
[0066] The flame retardant layer 18 can be electrically insulating or non-electrically insulating and meet plastic flammability standards (e.g., UL94 V-0, V-1, V-2, HB, 5VA, 5VB, etc.). The thickness of the flame retardant layer can be 0.05mm to 1.0mm, 0.1mm to 0.6mm, 0.2mm to 0.5mm, 0.05mm, 0.1mm, 0.15mm, 0.2mm, 0.25mm, 0.3mm, 0.35mm, 0.4mm, 0.45mm, 0.5mm or any range or value therebetween. In one example, the thickness of the flame retardant layer is 0.145mm to 0.225mm and has a flammability rating of UL94 5VA or UL94 5VB, preferably UL94 5VA. The flame retardant layer 18 can be a commercially available product that can be bonded to the thermal insulation layer 16. The flame retardant layer can include an adhesive layer (e.g., a pressure-sensitive adhesive) to facilitate the bonding of the two layers. Non-limiting examples of commercially available flame retardant tapes or papers are Unifrax brands (e.g., FyreWrap LiB papers and films), Brand (e.g. 3MVHB tape, 3M FRB paper), Brand, U-Line brand, etc. In some specific embodiments, Unifrax brand FyreWrap LiB paper (such as FX70 and IN70), Unifrax brand FyreWrap LiB film (such as C1554), Flame retardant FRB-WT series, Flame retardant FRB-NT series (eg, FRB-BK, FRB-NT laminate, FRB-NC laminate or FRB-NC series) (3M, St. Paul, Minnesota).
[0067] Each thermal insulation layer 16 may have a thermal conductivity equal to or less than any one of 0.05 W / m·K, 0.045 W / m·K, 0.040 W / m·K, 0.035 W / m·K, 0.030 W / m·K, 0.025 W / m·K, 0.020 W / m·K, 0.015 W / m·K, and 0.010 Watt / meter-Kelvin (W / m·K) or between any two (e.g., equal to or less than 0.025 W / m·K) and / or be equal to or less than 0.30 mm 2 / s, 0.20mm 2 / s, 0.15mm 2 / s, 0.125mm 2 / s、0.10mm 2 / s, 0.09mm 2 / s、0.08mm 2 / s, 0.07mm 2 / s, 0.06mm 2 / s and 0.05 square millimeters per second (mm 2 / s) or between any two items (e.g. less than or equal to 0.15 mm 2 / s or less than or equal to 0.10mm 2 As used herein, thermal conductivity and thermal diffusivity are measured at 25° C. In addition, each thermal insulation layer 16 can be heat resistant and / or have a low coefficient of thermal expansion so that the laminate 100 can withstand heating when used and resist expansion in applications where the laminate is restricted by small spaces. For example, each thermal insulation layer 16 may have a decomposition temperature higher than or equal to any one of 400°C, 425°C, 450°C, 475°C, 500°C, 525°C, 550°C, 575°C or 600°C, or between any two of them (e.g., higher than 450°C or equal to 450°C) and / or a thermal expansion coefficient (e.g., at least in one direction) equal to or less than any one of 40μm / m·K, 35μm / m·K, 30μm / m·K, 25μm / m·K, 20μm / m·K, 15μm / m·K, 10μm / m·K or 5μm / m·K, or between any two of them (e.g., equal to 35μm / m·K or less than 35μm / m·K).
[0068] To achieve such performance, at least one - up to each and including each - thermal insulation layer 16 may include a polymer aerogel layer. The amount of polymer aerogel may be at least 90% by weight of an organic polymer such as polyimide, polyaramid, polyurethane, polyurea and / or polyester (e.g., polyimide). Each polymer aerogel layer may have micropores, mesopores and / or macropores. Greater than or equal to any one of the following or between any two of the following: 10%, 25%, 50%, 75% or 95% of the pore volume of each aerogel layer may be composed of micropores, mesopores and / or macropores (e.g., micropores, mesopores, micropores and mesopores or macropores). The average pore size and / or median pore size of each aerogel layer can be greater than or equal to any one of the following or between any two of the following: 50nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm, 800nm, 1000nm, 2000nm, 3000nm, 4000nm or 5000nm (e.g., the average pore size can be 100nm to 500nm, and the median pore size can be 250nm to 600nm). The materials and processes used to make the polymer aerogel layers will be explained in further detail below.
[0069] In some embodiments, for at least one (e.g., each) insulating layer 16, the aerogel layer may include reinforcing fibers, which may be dispersed (e.g., as ordered (e.g., woven) or chopped or discontinuous fibers that are not arranged in a sheet) or embedded (e.g., as a woven, non-woven or unidirectional fiber sheet) in the aerogel layer, optionally with a volume of fibers greater than or equal to any one of 0.1%, 10%, 20%, 30%, 40%, or 50% of the volume of the aerogel layer or between any two. However, the aerogel layer need not include fibers (e.g., to promote flexibility).
[0070] Suitable fibers include glass fibers, carbon fibers, polyaramid fibers, thermoplastic fibers, thermosetting fibers, ceramic fibers, basalt fibers, rock wool fibers, steel fibers, cellulose fibers, and / or the like. The average filament cross-sectional area of the fibers used for reinforcement is greater than or equal to any of the following, or between any two of the following: 7 μm 2 , 15μm 2 、30μm 2 、60μm 2 , 100μm 2 , 200μm 2 、300μm 2 , 400μm 2 , 500μm 2 、600μm 2 、700μm 2 or 800μm2 ; For example, for fibers having a circular cross-section, the average diameter of the fibers is greater than, or equal to, any of the following, or between any two of the following: 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 21μm, 22μm, 23μm, 24μm, 25μm, 26μm, 27μm, 28μm, 29μm or 30μm (for example, 5μm to 24μm, such as 10μm to 20μm or 12μm to 15μm).
[0071] Non-limiting examples of thermoplastic polymers that can be used to polymerize the reinforcing fibers include polyethylene terephthalate (PET), polycarbonate (PC), polybutylene terephthalate (PBT), poly(1,4-cyclohexanedimethanol 1,4-cyclohexanedicarboxylate) (PCCD), glycol-modified polycyclohexyl terephthalate (PCTG), poly(phenylene oxide) (PPO), polypropylene (PP), polyethylene (PE), polyvinyl chloride (PVC), polystyrene (PS), polymethyl methacrylate (PMMA), polyethylene Polyetherimide (PEI) and its derivatives, thermoplastic elastomers (TPE), terephthalic acid (TPA) elastomers, poly(cyclohexane dimethyl terephthalate) (PCT), polyethylene naphthalate (PEN), polyamide (PA), polysulfone sulfonate (PSS), sulfonate of polysulfone, polyetheretherketone (PEEK), polyetherketoneketone (PEKK), acrylonitrile butadiene styrene (ABS), polyphenylene sulfide (PPS), copolymers thereof, polyesters or their derivatives, polyamides or their derivatives (e.g., nylon), or blends thereof.
[0072] Non-limiting examples of thermoplastic polymers that can be used to polymerize the reinforcing fibers include unsaturated polyester resins, polyurethanes, polyoxybenzyl methylene glycol anhydrides (e.g., phenolic resins), urea-formaldehyde, diallyl phthalate, epoxy resins, epoxy vinyl esters, polyimides, polycyanurate esters, dicyclopentadiene, phenolics, benzophenones, and polyisocyanates. Oxazine, its copolymer or its blend.
[0073] Although each insulation layer 16 may include a polymer aerogel layer, in other embodiments, at least one (up to each and including each) insulation layer may include any suitable insulation material, such as a fiber layer. At least one (up to each and including each) of the insulation layers 16 may also include a fiber layer laminated to the polymer aerogel layer, optionally such that the fiber layer is disposed closer to the front surface 12 of the laminate 100 than the aerogel layer. The fibers in the fiber layer may be any of the fibers described above for aerogel fiber reinforcement (e.g., glass fibers and / or basalt fibers), and may be arranged in various fiber structures. For example, the fibers may form a fiber matrix, such as felt, cotton batting, thick and resilient cotton batting, mats, woven fabrics, nonwoven fabrics, and the like. The fibers may be unidirectional or omnidirectional.
[0074] In some embodiments, the fibers used as reinforcement in the aerogel layer or fiber layer may have a diameter of 5 μm. 2 Up to 40000μm 2 The average filament cross-sectional area and / or the average length of 20mm to 100mm.
[0075] To allow the laminate 100 to be used in applications with limited space constraints, each insulation layer 16 (e.g., aerogel layer) can be relatively thin. For example, at least one (e.g., each) insulation layer 16 has a thickness 26 ( Figure 1A ) can be equal to or less than any of the following, or between any two of the following: 50mm, 25mm, 20mm, 15mm, 10mm, 5mm, 4mm, 3mm, 2mm, 1mm, 0.9mm, 0.8mm, 0.7mm, 0.6mm, 0.5mm, 0.4mm, 0.3mm, 0.2mm, 0.15mm, 0.1mm or 0.05mm (for example, 0.10mm to 0.20mm, for example 0.165mm).
[0076] When the laminate 100 includes multiple thermal insulation layers 16 and / or flame retardant layers 18, the laminate may include multiple adhesive layers (e.g., adhesive layers 20, 22, and 24), wherein the second adhesive layer 22 defines at least a portion of the second surface 14 to allow adhesion to the surface 10 (e.g., a substrate), as described above. The remaining adhesive layers (e.g., adhesive layer 24) can bond the thermal insulation layers 16, the flame retardant layers 18, or a combination of thermal insulation layers and flame retardant layers. To this end, each adhesive layer may be disposed between and in contact with the other adjacent layers (e.g., between two thermal insulation layers 16 and / or between one of the thermal insulation layers and the flame retardant layer). As an example, two thermal insulation layers can be bonded together and bonded to the flame retardant layer. In another example, a stack of a first flame retardant layer (e.g., 18), a first thermal insulation layer (e.g., 16), a second flame retardant layer, and a second thermal insulation layer can be bonded together with adhesive layers. As Figure 1BAs shown, an adhesive layer 20 is disposed between and in contact with the flame retardant layer 18 and one of the thermal insulation layers 16, and an adhesive layer 24 is disposed between and in contact with the two thermal insulation layers. In order to promote adhesion without adding a large amount of thickness to the laminate 100, the thickness 34 of at least one (e.g., each) adhesive layer (e.g., adhesive layers 20, 22, and 24) may be equal to or less than any one of the following, or between any two of the following: 5.0 mm, 4.5 mm, 4.0 mm, 3.5 mm, 3.0 mm, 2.5 mm, 2.0 mm, 1.5 mm, or 1.0 mm (e.g., 1.5 mm to 3.5 mm).
[0077] At least one - up to and including each - adhesive layer may include a pressure sensitive adhesive, such as adhesives including silicones, epoxies, acrylates, phenolics, cyanates, epoxy resins, and / or rubbers. Such pressure sensitive adhesives, when used in the second adhesive layer 22, can allow the laminate 100 to be immediately applied to the surface 10 for thermal insulation (e.g., by simply pressing the laminate 100 onto the surface). However, at least one of the adhesive layers may include a different type of adhesive, such as a fluoropolymer film, a polyimide film, and a B-stage epoxy resin; for example, commercially available adhesives such as DuPont TM FEP film, HT and GPL and TSU510S-A of Toyochem Co., LTD. (Tokyo, Japan). Using such other adhesives, bonding can be achieved by stacking the layers of laminate 100 (e.g., 16 and 24, optionally flame retardant layer 18) and applying heat and / or pressure (e.g., using a press) to the stack, optionally to a temperature exceeding the glass transition temperature of the adhesive layer. In some embodiments having multiple adhesive layers, some adhesive layers (e.g., the second adhesive layer) may include a pressure-sensitive adhesive, while others (e.g., adhesive layers other than the second adhesive layer) may include another type of adhesive, such as those listed above.
[0078] The combination of adhesive layers 20, 22 or 24 can mitigate the risk of delamination, for example, through heat resistance. For example, the melting temperature or decomposition temperature of at least one (e.g., each) adhesive layer 20, 22 and 24 is greater than or equal to any one of the following, or between any two of the following: 350°C, 375°C, 400°C, 425°C, 450°C, 500°C, 550°C or 600°C. In addition, the glass transition temperature or melting point of at least one (e.g., each) adhesive layer 20, 22 and 24 is greater than or equal to any one of the following, or between any two of the following: 100°C, 150°C, 170°C, 200°C, 225°C, 250°C or 257°C.
[0079] By the above configuration, the laminate 100 can provide thermal insulation and flame retardant protection in high temperature and flammable environments. For example, the thermal diffusivity of the laminate 100 can be equal to or less than any one of the following, or between any two of the following: 0.15 mm 2 / s, 0.125mm 2 / s、0.10mm 2 / s, 0.09mm 2 / s、0.08mm 2 / s, 0.07mm 2 / s, 0.06mm 2 / s, 0.05mm 2 / s or 0.04mm 2 / s (e.g., equal to 0.10 mm 2 / s or less than 0.10mm 2 / s, for example, equal to 0.075mm 2 / s or less than 0.075mm 2 / s), thereby mitigating the spread of heat therethrough. The flammability rating of the laminate 100 may meet UL 94 requirements. For example, the laminate may inhibit the spread of flames for at least 5 minutes at a temperature above 500°C, thereby resisting combustion. The laminate may have a UL945VB or UL94 5VA rating.
[0080] In addition, although the total thickness of the laminate 100 (shown as 30 in Figures 1a and 1B) can be equal to or less than 25.4 mm, as described above, the laminate can be advantageously relatively thin, such as equal to or less than any of the following, or between any two of the following: 25.4 mm, 20 mm, 15 mm, 10 mm, 5 mm, 4 mm, 3 mm, or 2 mm (e.g., equal to or less than 10 mm or equal to or less than 0.3 mm). Such a thin thickness can allow the laminate 100 to be used in small spaces, such as spaces typically found in vehicles such as electric or hybrid vehicles and / or electronic components, while still providing the above-mentioned thermal insulation and flame retardant protection. Therefore, compared to traditional insulation / flame retardant materials, the laminate 100 can provide better thermal insulation and flame retardant protection in size-constrained applications, which may not be able to meet the thermal insulation or flame retardant protection or may sacrifice thermal insulation or flame retardant protection to meet the size constraints.
[0081] refer to Figure 2, shown is a second laminate 200 substantially similar to laminate 100, with the primary exception that laminate 200 includes a backing layer 32. As shown, laminate 200 is not yet attached to substrate surface 10. To protect second adhesive layer 22 (e.g., from contaminants that may impair its adhesion) prior to attachment to substrate surface 10, backing layer 32 may be removably disposed on second adhesive layer such that at least a portion (e.g., at least a majority, up to all, and including all) of back surface 14 of laminate 200 is defined by backing layer. Backing layer 32 may include, for example, a polymer film or paper, and may be removed from second adhesive layer 22 by, for example, peeling it off laminate 200.
[0082] refer to Figure 4 , shown is a laminate 400 substantially similar to laminate 100, with the primary exception that laminate 400 includes a heat dissipation layer 62. Laminate 400 includes a heat dissipation layer 62 disposed between flame retardant layer 18 and aerogel layer 16. However, other laminates of the present invention may include any suitable number of heat dissipation layers (e.g., 62), which may be disposed at any suitable position within the laminate. In addition, in laminate 400, heat dissipation layer 62 is attached to flame retardant layer 18 and aerogel layer 16 by adhesive layers 20 and 22, respectively, but neither adhesive layer is required. And like any laminate of the present invention, laminate 400 may include an adhesive layer 24 for adhering the laminate to a substrate, which may optionally be protected by a backing layer (e.g., 32) prior to adhering as described above.
[0083] The heat dissipation layer 62 may include a thermally conductive material, such as a metal (e.g., copper, aluminum, molybdenum, tungsten, rhenium, tantalum, niobium, stainless steel, nickel, or alloys thereof), graphite, and / or the like. More specifically, the heat dissipation layer 62 may include at least 90% by weight of a thermally conductive material, such as at least 90% by weight of a metal or at least 90% by weight of graphite. The heat dissipation layer 60 may have a thermal conductivity of at least 15 W / m·K, preferably 15 W / m·K to 2500 W / m·K. The heat dissipation layer may also have a melting point or decomposition temperature of at least 500°C, preferably a melting temperature of at least 1300°C, at least 1600°C, at least 1900°C, at least 2200°C, at least 2400°C, at least 2700°C, at least 3000°C, or at least 3300°C (e.g., less than 3800°C or less than 3600°C). Generally, such a heat dissipation layer can mitigate the development of hot spots along lower layers in the laminate and the subsequent burning or charring of the lower layers by spreading heat from the environment along the laminate. The thickness of the heat dissipation layer can be greater than any one of the following or between any two of the following: 0.001mm, 0.002mm, 0.004mm, 0.006mm, 0.008mm, 0.01mm, 0.02mm, 0.04mm, 0.06mm, 0.08mm, 0.10mm, 0.12mm, 0.14mm, 0.16mm, 0.18mm, 0.20mm, 0.22mm, 0.24mm, 0.26mm, 0.28mm, 0.30mm, 0.32mm, 0.34mm, 0.36mm, 0.38mm and 0.40mm (e.g., 0.001mm to 4mm or 0.01mm to 0.05mm).
[0084] Reference now Figure 5 , the laminate (e.g., 100, 200, 300 or 400) can be flexible. For illustration, such a laminate can be arranged in a roll 34 having an inner diameter 36 equal to or less than any one of 10cm, 8cm, 5cm, 4cm, 2cm, 1cm, 8mm, 5mm, 4mm, 2mm or 1mm, or between any two, without suffering from permanent deformation. This flexibility, even if not reaching the level of this example, can be provided by the material of the insulating layer, flame retardant adhesive layer and other layers (if present) of the laminate and / or the relatively small thickness of these layers (e.g., those discussed above). When in roll 34, a portion of the front surface 12 of the laminate can face a portion of its rear surface 14.
[0085] In some embodiments, the laminate can protect the device or substrate from temperatures above 500°C. For example, the laminates 100 to 400 can be positioned relative to the device so that the front surface having the flame retardant layer is disposed farther from the device than the rear surface of the laminate (e.g., rear surface 14). When exposed to a temperature above 500°C to 1500°C for 1 minute to 90 minutes (preferably at least 5 minutes), the temperature of the device does not exceed 500°C during this time period. The exposure temperature can be 500°C to 1500°C or 700°C to 1200°C, or 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C, or any range or value therebetween. Of course, the laminates of the present invention are also suitable for applications exposed to lower temperatures (e.g., equal to or less than 100°C, 200°C, 300°C or 400°C) and / or exposed to any of the above temperatures for shorter times (e.g., equal to or less than 1 second, 2 seconds, 3 seconds, 4 seconds, 5 seconds, 10 seconds, 15 seconds, 20 seconds, 25 seconds, 30 seconds, 40 seconds, 50 seconds or 60 seconds).
[0086] Devices in which such thermal insulation is beneficial include, for example, batteries (e.g., lithium-ion batteries), busbars, particularly electric or hybrid vehicles or electrical components, including batteries and motors that are subject to high temperature environments. The surface 10 to which the laminate 100 is attached can be the surface of a battery such as a lithium-ion battery. The surface 10 can also be a busbar or a non-conductive material.
[0087] For example, refer to Figure 6 , shown is a battery 66 including a battery cell 68. The battery cells 68 can be combined into battery modules 70, and these modules can be assembled into a battery pack 72. The battery 66 can also include a battery housing or box 74. In order to protect the battery cells 68, the battery modules 70 and / or the battery pack 72 from vibration and / or expansion / contraction of the battery cells, battery modules and / or battery packs, the battery 66 can also include one or more compression pads 76, which can be arranged between the battery cells, between the battery modules, between the battery pack and the battery box 74 and / or in a similar manner. The compression pad 76 can include, for example, a compressible material, such as foam. The battery 66 can be contained in a vehicle 78, such as the car shown. The vehicle 78 can also be, for example, a motor vehicle (e.g., an internal combustion engine vehicle, an electric vehicle, a hybrid electric vehicle), an aircraft (e.g., an airplane, a jet, a helicopter, an unmanned aerial vehicle or an electric vertical take-off and landing (eVTOL) aircraft), a train, a motorcycle, a ship, a spacecraft, etc.
[0088] However, such a battery 66 may be susceptible to thermal runaway events and / or exposure to other high temperature environments. In order to protect the battery 66, the vehicle 78 in which the battery is disposed, and / or the occupants of the vehicle, one or more of the laminates of the present invention may be implemented. For illustration, one of the laminates of the present invention may be disposed on the inner and / or outer surfaces of at least one of the battery cell 68, the battery module 70, the battery pack 72, the compression pad 76, and / or the battery box 74.
[0089] As another example, refer to Fig. 7A and Figure 7B , shown is a cable 80. Cable 80 has a length 82 and a width or diameter 84, wherein the length is greater than the width (e.g., the length is 10 times or greater than 10 times the width). More specifically, diameter 84 can be from 0.0003 inches to 10 inches, preferably from 0.001 inches to 1 inch. Cable 80 can be conductive, but not necessarily conductive. The cable can be contained in a vehicle (e.g., the above-mentioned vehicles), a missile, a rocket, an artillery, a manned aircraft, an unmanned aircraft, a land vehicle, a sea vehicle, or a spacecraft. Such a cable can be exposed to high temperatures, and the laminates of the present invention can be used to mitigate high temperatures. For example, cable 80 can include one or more than one of the laminates of the present invention that constitute at least a portion of the outer surface of the cable (e.g., in Figure 7B denoted as 100).
[0090] Non-limiting examples of articles that may include the laminates of the present invention include, in addition to the above, vehicles, trucks, trailers, trains, rail vehicles, aircraft, spacecraft, panels or components for any of the above, bridges, pipelines, ducts, pipes, ships, ships, storage containers, tanks, furniture, windows, doors, railings, functional or decorative architectural parts, pipe railings, electrical components, conduits, beverage containers, food containers, foils, batteries (such as electric vehicle batteries, battery systems, battery housings) and battery bus bars.
[0091] B. Materials of polymer aerogel layer
[0092] The polymer aerogel layer may include organic materials, inorganic materials, or mixtures thereof. The organic aerogel may be made of polyacrylate, polystyrene, polyacrylonitrile, polyurethane, polyurea, polyimide, polyamide, polyaramid, polyfurfuryl alcohol, phenol furfuryl alcohol, melamine formaldehyde, resorcinol formaldehyde, cresol formaldehyde, phenol formaldehyde, polyvinyl alcohol dialdehyde, polycyanurate, polyacrylamide, various epoxy resins, agar, agarose, etc. In a specific embodiment, the aerogel is a polyimide aerogel.
[0093] Polyimide is a polymer with many desirable properties. Polyimide polymers include nitrogen atoms in the polymer backbone, wherein the nitrogen atoms are connected to two carbonyl carbons so that the nitrogen atoms are stabilized to some extent by adjacent carbonyl groups. The carbonyl group includes a carbon double-bonded to an oxygen atom, referred to as a carbonyl carbon. Polyimide is generally considered to be an AA-BB type polymer because two different types of monomers are generally used to produce polyimide polymers. Polyimide can also be prepared from AB type monomers. For example, aminodicarboxylic acid monomers can be polymerized to form AB type polyimide. If desired, monoamines and / or monoanhydrides can be used as end-capping agents.
[0094] A class of polyimide monomers is usually diamine or diamine monomer. Diamine monomers can also be diisocyanates, and it should be understood that in this specification, amines can be appropriately replaced with isocyanates. As known to those skilled in the art, other types of monomers can be used to replace diamine monomers. Other types of monomers are called acid monomers, which are usually present in the form of dianhydrides. In this specification, the term "diacid monomer" is defined as including dianhydrides, tetraesters, diester acids, tetracarboxylic acids or trimethylsilyl esters, all of which can react with diamines to form polyimide polymers. Dianhydrides should be understood as tetraesters, diester acids, tetracarboxylic acids or trimethylsilyl esters, which can be appropriately substituted. As known to those skilled in the art, other types of monomers can also be used to replace diacid monomers.
[0095] Because a diacid monomer has two anhydride groups, a different diamine monomer can react with each anhydride group, so the diacid monomer can be located between two different diamine monomers. Diamine monomers contain two amine functional groups; therefore, after the first amine functional group is attached to a diacid monomer, the second amine functional group can still be attached to another diacid monomer, which is then attached to another diamine monomer, and so on. In this way, a polymer backbone is formed. The resulting polycondensation reaction forms polyamic acid.
[0096] Polyimide polymers are typically formed from two different types of monomers, and different species of each type of monomer can be mixed. Thus, one, two, or more than two diacid monomers can be included in the reaction vessel, along with one, two, or more than two diamine monomers. If long polymer chains are desired, the total molar amount of the diacid monomers remains approximately the same as the total molar amount of the diamine monomers. Because more than one type of diamine or diacid can be used, the various monomer components of each polymer chain can be varied to produce polyimides with different properties. For example, a single diamine monomer AA can be reacted with two diacid comonomers B1B1 and B2B2 to form a polymer having the general formula (AA-B1B1) x -(AA-B2B2) yAlternatively, diamine comonomers A1A1 and A2A2 can be reacted with a single diacid monomer BB to form a polymer chain of the general formula (A1A1-BB) x -(A2A2-BB) y In addition, the two diamine comonomers A1A 1 and A2A2 can react with two diacid comonomers B1B1 and B2B2 to form a general formula (A1A1-B1B1) w -(A1A1-B2B2) x -(A2A2-B1B1) y -(A2A2-B2B2) z A polymer chain of wherein w, x, y and z are determined by the relative amounts of A1A1-B1B1, A1A1-B2B2, A2A2-B1B1 and A2A2-B2B2 incorporated into the polymer backbone. More than two diacid comonomers and / or more than two diamine comonomers may also be used. Thus, one or more than one diamine monomer may be polymerized with one or more than one diacid, and the general formula of the polymer is determined by varying the amounts and types of monomers used.
[0097] There are many examples of monomers that can be used to prepare polymer aerogels containing polyamideamide polymers. In some embodiments, the diamine monomer is a substituted or unsubstituted aromatic diamine, a substituted or unsubstituted alkyl diamine, or a diamine that can contain both aromatic and alkyl functional groups. A non-limiting list of possible diamine monomers includes 4,4'-diaminodiphenyl ether (ODA), 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, p-phenylenediamine, m-phenylenediamine, o-phenylenediamine, diaminobenzanilide, 3,5-diaminobenzoic acid, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 1,3-bis-(4-aminophenoxy)benzene, 1,3-bis-(3-aminophenoxy)benzene, 1,4-bis-(4-aminophenoxy)benzene, 1,4-bis-(3-aminophenoxy)benzene, 2,2-bis[4-(4-aminophenoxy)phenyl]-hexafluoropropane, 2,2-bis(3-aminophenyl) -1,1,1,3,3,3-hexafluoropropane, 4,4'-isopropylenediphenylamine, 1-(4-aminophenoxy)-3-(3-aminophenoxy)benzene, 1-(4-aminophenoxy)-4-(3-aminophenoxy)benzene, bis-[4-(4-aminophenoxy)phenyl]sulfone, 2,2-bis[4-(3-aminophenoxy)phenyl]sulfone, bis(4-[4-aminophenoxy]phenyl)ether, 2,2'-bis-(4-aminophenyl)-hexafluoropropane (6F-diamine), 2,2'-bis-(4-phenoxyaniline)isopropylenediamine, m-phenylenediamine, p-phenylenediamine, 1,2-diaminobenzene, 4,4'-diaminodiphenylmethane, 2, 2-Bis(4-aminophenyl)propane, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 2,6-diaminopyridine, bis(3-aminophenyl)diethylsilane, 4,4'-diaminodiphenyldiethylsilane, benzidine, dichlorobenzidine, 3,3'-dimethoxybenzidine, 4,4'-diaminobenzophenone, N,N-bis(4-aminophenyl)-n-butylamine, N,N-bis(4-aminophenyl)methylamine, 1,5-diaminonaphthalene, 3,3'-dimethyl-4,4'-diaminobiphenyl, 4-aminophenyl -3-aminobenzoate, N,N-bis(4-aminophenyl)aniline, bis(p-β-aminotert-butylphenyl)ether, p-bis-2-(2-methyl-4-aminopentyl)benzene, p-bis(1,1-dimethyl-5-aminopentyl)benzene, 1,3-bis(4-aminophenoxy)benzene, m-xylene diamine, p-xylene diamine, 4,4'-diaminodiphenyl ether phosphine oxide, 4,4'-diaminodiphenyl N-methylamine, 4,4'-diaminodiphenyl N-phenylamine, amino-terminated polydimethylsiloxane, amino-terminated polypropylene oxide, amino-terminated polybutylene oxide, 4,4'-methylenebis(2-methylcyclohexylamine), 1,2-diaminoethane, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane and 4,4'-methylenedianiline, 2,2'-dimethylbenzidine (also known as 4,4'-diamino-2,2'-dimethylbiphenyl (DMB)), dianiline-p-xylidine, 4,4'-bis(4-aminophenoxy)biphenyl, 3,3'-bis(4-aminophenoxy)biphenyl, 4,4'-(1,4-phenylene diisopropylidene)dianiline and 4,4'-(1,3-phenylene diisopropylidene)dianiline, or a combination thereof. In a specific embodiment, the diamine monomer is ODA, 2,2'-dimethylbenzidine, or both. ,
[0098] A non-limiting list of possible dianhydride ("diacid") monomers include hydroquinone dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 4,4'-oxydiphthalic anhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 4,4'-(4,4'-isopropylidenediphenoxy)bis(phthalic anhydride), 2,2-bis(3,4-dicarboxyphenyl)tetracarboxylic anhydride, and 1,2-bis(1,2-diphenyl)bis(1,2-dicarboxyphenyl)tetracarboxylic anhydride. ) propane dianhydride, 4,4'-(hexafluoroisopropylidene) diphthalic anhydride, bis(3,4-dicarboxyphenyl) sulfoxide dianhydride, polysilicone-containing dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 2,3,2',3'-benzophenonetetracarboxylic dianhydride, naphthalene-2,3,6,7-tetracarboxylic dianhydride, naphthalene-1,4,5,8-tetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, 3,3',4,4'-biphenylsulfonetetracarboxylic dianhydride, 3,4,9,10- Tetracarboxylic acid dianhydride, bis(3,4-dicarboxyphenyl)sulfurized dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane, 2,6-dichloronaphthalene-1,4,5,8-tetracarboxylic acid dianhydride, 2,7-dichloronaphthalene-1,4,5,8-tetracarboxylic acid dianhydride, 2,3,6,7-tetrachloronaphthalene-1,4,5,8-tetracarboxylic acid dianhydride, phenanthrene, 8,9,10-tetracarboxylic acid dianhydride, pyrazine-2,3,5,6-tetracarboxylic acid dianhydride, benzene-1,2,3,4-tetracarboxylic acid dianhydride and thiophene-2,3,4,5-tetracarboxylic acid dianhydride. In a specific embodiment, the dianhydride monomer is BPDA, PMDA or both.
[0099] In some aspects, the molar ratio of anhydride to total diamine is 0.4: 1 to 1.6: 1, 0.5: 1 to 1.5: 1, 0.6: 1 to 1.4: 1, 0.7: 1 to 1.3: 1, or specifically 0.8: 1 to 1.2: 1. In further aspects, the molar ratio of dianhydride to multifunctional amine (e.g., triamine) is 2: 1 to 140: 1, 3: 1 to 130: 1, 4: 1 to 120: 1, 5: 1 to 110: 1, 6: 1 to 100: 1, 7: 1 to 90: 1, or specifically 8: 1 to 80: 1. Monoanhydride groups can also be used. Non-limiting examples of monoanhydride groups include 4-amino-1,8-naphthoic anhydride, endobicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, citraconic anhydride, trans-1,2-cyclohexanedicarboxylic anhydride, 3,6-dichlorophthalic anhydride, 4,5-dichlorophthalic anhydride, tetrachlorophthalic anhydride, tetrafluorophthalic anhydride, maleic anhydride, 1-cyclopentene-1,2-dicarboxylic anhydride, 2,2-dimethylglutaric anhydride, 3,3-dimethylglutaric anhydride, 2,3-dimethylmaleic anhydride, 2,2-dimethylsuccinic anhydride, 2,3-diphenylmaleic anhydride, phthalic anhydride, 3-methylglutaric anhydride, methylsuccinic anhydride, 3-nitrophthalic anhydride, 4-nitrophthalic anhydride, 2,3-pyrazinedicarboxylic anhydride, or 3,4-pyridinedicarboxylic anhydride. Specifically, the monoanhydride group may be phthalic anhydride.
[0100] In another embodiment, the polymer composition for preparing the polymer aerogel layer comprises a polyfunctional amine monomer having at least three primary amine functional groups. The polyfunctional amine can be a substituted or unsubstituted aliphatic polyfunctional amine, a substituted or unsubstituted aromatic polyfunctional amine, or a polyfunctional amine comprising a combination of aliphatic and two aromatic groups, or a combination of aromatic and two aliphatic groups. A non-limiting list of possible polyfunctional amines includes propane-1,2,3-triamine, 2-aminomethylpropane-1,3-diamine, 3-(2-aminoethyl)pentane-1,5-diamine, bis(hexamethylene)triamine, N',N'-bis(2-aminoethyl)ethane-1,2-diamine, N',N'-bis(3-aminopropyl)propane-1,3-diamine, 4-(3-aminopropyl)heptane-1,7-diamine, N', N'-bis(6-aminohexyl)hexane-1,6-diamine, benzene-1,3,5-triamine, cyclohexane-1,3,5-triamine, melamine, N-2-dimethyl-1,2,3-propanetriamine, diethylenetriamine, 1-methyl or 1-ethyl or 1-propyl or 1-benzyl substituted diethylenetriamine, 1,2-dibenzyldiethylenetriamine, lauryldiethylenetriamine, N-(2-hydroxypropyl)diethylenetriamine, N, N-bis(1-methylheptyl)-N-2-dimethyl-1,2,3-propanetriamine, 2,4,6-tris(4-(4-aminophenoxy)phenyl)pyridine, N,N-dibutyl-N-2-dimethyl-1,2,3-propanetriamine, 4,4'-(2-(4-aminobenzyl)propane-1,3-diyl)diphenylamine, 4-((bis(4-aminobenzyl)amino)methyl)aniline, 4-(2-(bis(4-aminophenethyl) )amino)ethyl)aniline, 4,4'-(3-(4-aminophenethyl)pentane-1,5-diyl)diphenylamine, 1,3,5-tris(4-aminophenoxy)benzene (TAPOB), 4,4',4"-methanetriyltriphenylamine, N,N,N',N'-tetrakis(4-aminophenyl)-1,4-phenylenediamine, polyoxypropylenetriamine, octa(aminophenyl)cage polysilsesquione, or a combination thereof. Specific examples of polyoxypropylenetriamine are T-403 from Huntsman Corporation, The Woodlands, TX USA. In a specific embodiment, the aromatic multifunctional amine can be 1,3,5-tris(4-aminophenoxy)benzene or 4,4',4"-methanetriyltriphenylamine. In some embodiments, the multifunctional amine comprises three primary amine groups and one or more than one secondary and / or tertiary amine groups, for example, N',N'-bis(4-aminophenyl)benzene-1,4-diamine.
[0101] Non-limiting examples of capping agents or capping groups include amines, maleimides, nadic imides, acetylene, biphenyl, norbornene, cycloalkyl and N-propargyl groups, particularly those derived from agents including 5-norbornene-2,3-dicarboxylic anhydride (nadic anhydride, NA), methyl-nadic anhydride, hexachloro-nadic anhydride, cis-4-cyclohexene-1,2-dicarboxylic anhydride, 4-amino-N-propargylphthalimide, 4-ethynylphthalic anhydride and maleic anhydride.
[0102] The characteristics or properties of the final polymer are significantly affected by the choice of monomers used to produce the polymer. Factors to consider when selecting monomers include properties of the final polymer, such as flexibility, thermal stability, coefficient of thermal expansion (CTE), coefficient of hygroscopic expansion (CHE), and any other particularly desirable properties, as well as cost. Often, certain important properties of a polymer can be determined for a particular application. Other properties of the polymer may be less important, or may have a wider range of acceptable values; many different combinations of monomers may be used.
[0103] In some cases, the main chain of polymer can include substituents.Substituents (e.g., oligomers, functional groups, etc.) can be directly bonded to the main chain or connected to the main chain by a linking group (e.g., a connecting chain or a flexible connecting chain). In other embodiments, compounds or particles can be incorporated (e.g., mixed and / or encapsulated) into the polyimide structure, and are not covalently bound to the polyimide structure. In some cases, the incorporation of compounds or particles can be carried out in the polyamide reaction process. In some cases, particles can gather, thereby producing polyimides with non-covalently bound compounds or particle domains of different concentrations.
[0104] Specific properties of polyimides can be affected by incorporating certain compounds into the polyimide. The choice of monomers is one way to influence specific properties. Another way to influence properties is to add compounds or property modifying moieties to the polyimide.
[0105] C. Preparation of polymer aerogel layers
[0106] Polymer aerogel films that can be used in at least some of the laminates of the present invention are commercially available. Non-limiting examples of such films include Blueshift Rolled film (available from Blueshift Materials, Inc., Spencer, Massachusetts) and membrane (available from Aerogel Technologies, LLC), in some aspects, Blueshift Rolled films are preferred.
[0107] In addition, in addition to the process described below, polymer aerogels (films, raw material shapes or blocks, etc.) can be manufactured using the methods described in patent application publication No. WO 2014 / 189560 to Rodman et al., US2017 / 0355829 to Sakaguchi et al., US2018 / 078512 to Yang et al., US2018 / 140804 to Sakaguchi et al., and US2019 / 006184 to Irvin et al., international patent application No. PCT / US2019 / 029191 to Ejaz et al., U.S. patent application publication No. 2017 / 0121483 to Poe et al., and / or U.S. Patent No. 9,963,571 to Sakaguchi et al., the entire contents of which are incorporated herein by reference in their entirety.
[0108] The following provides non-limiting processes that can be used to make polymer aerogel layers suitable for use in the laminates of the present invention. These processes include: 1) preparing a polymer gel; 2) optionally exchanging solvents; 3) drying the polymer solution to form an aerogel; and (4) attaching the polymer aerogel film to a substrate.
[0109] 1. Formation of polymer gel
[0110] The first stage of aerogel synthesis can be the synthesis of a polymerized gel. For example, if a polyimide aerogel is desired, at least one acid monomer can react with at least one diamine monomer in a reaction solvent to form a polyamic acid. As described above, many acid monomers and diamine monomers can be used to synthesize polyamic acid. On the one hand, the polyamic acid is contacted with an imidization catalyst in the presence of a chemical dehydrating agent to form a polymerized polyimide gel by an imidization reaction. "Imidization" is defined as the conversion of a polyimide precursor into an imide. Any imidization catalyst suitable for driving a polyimide precursor into a polyimide state is suitable. Non-limiting examples of chemical imidization catalysts include pyridine, picoline, quinoline, isoquinoline, 1,8-diazabicyclo [5.4.0] undec-7-ene (DBU), triethylenediamine, lutidine, N-methylmorpholine, triethylamine, tripropylamine, tributylamine, other trialkylamines, 2-methylimidazole, 2-ethyl-4-methylimidazole, imidazole, other imidazoles and combinations thereof. Any dehydrating agent suitable for forming an imide ring from an amic acid precursor is suitable for the method of the present invention. Preferred dehydrating agents include at least one compound selected from acetic anhydride, propionic anhydride, n-butyric anhydride, benzoic anhydride, trifluoroacetic anhydride, phosphorus trichloride and dicyclohexylcarbodiimide.
[0111] In one aspect of the invention, one or more diamine monomers and one or more multifunctional amine monomers are premixed in one or more solvents and then treated with one or more small amounts of dianhydrides (e.g., diacid monomers) added sequentially in predetermined time increments while monitoring viscosity. The desired viscosity of the polymerized solution can be 50 cP to 20,000 cP, or specifically 500 cP to 5,000 cP. Non-crosslinked aerogels can be prepared by reacting using incremental additions of dianhydrides while monitoring viscosity. For example, a triamine monomer (23 equivalents) can be added to a solvent to obtain a 0.0081 molar solution. A first diamine monomer (280 equivalents) can be added to the solution, followed by a second diamine monomer (280 equivalents). Next, smaller amounts of dianhydrides (552 total equivalents) can be added sequentially in predetermined time increments while monitoring viscosity. Dianhydrides can be added until the viscosity reaches 1000 cP to 1500 cP. For example, a first portion of the dianhydride can be added, the reaction can be stirred (e.g., 20 minutes), a second portion of the dianhydride can be added, and then a sample of the reaction mixture can be analyzed for viscosity. After stirring for an additional time (e.g., 20 minutes), a third portion of the dianhydride can be added and a sample can be taken for viscosity analysis. After further stirring for a desired period of time (e.g., 10 to 12 hours), a monoanhydride (96 equivalents) can be added. After reaching the target viscosity, the reaction mixture can be stirred for a desired time (e.g., 10 to 12 hours) or the reaction can be considered complete.
[0112] The reaction temperature for gel formation can be determined by routine experiments based on the raw materials. In a preferred embodiment, the temperature can be higher than or equal to any one of the following, or between any two of the following: 15°C, 20°C, 30°C, 35°C, 40°C and 45°C. After the desired amount of time (e.g., about 2 hours), the product can be isolated (e.g., filtered), after which nitrogen-containing hydrocarbons (828 equivalents) and dehydrating agents (1214 equivalents) can be added. The addition of nitrogen-containing hydrocarbons and / or dehydrating agents can be carried out at any temperature. In some embodiments, nitrogen-containing hydrocarbons and / or dehydrating agents are added to the solution at 20°C to 28°C (e.g., room temperature) and stirred at room temperature for the desired time. In some cases, after adding nitrogen-containing hydrocarbons and / or dehydrating agents, the solution temperature is raised to 150°C.
[0113] The reaction solvent may include dimethyl sulfoxide (DMSO), diethyl sulfoxide, N,N-dimethylformamide (DMF), N,N-diethylformamide, N,N-dimethylacetamide (DMAc), N,N-diethylacetamide, N-methyl-2-pyrrolidone (NMP), 1-methyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, 1,13-dimethyl-2-imidazolidinone, diethylene glycol dimethoxy ether, o-dichlorobenzene, phenol, cresol, xylenol, catechol, butyrolactone, hexamethylphosphoramide, and mixtures thereof. The reaction solvent and other reactants may be selected based on compatibility with the materials and methods applied; that is, if the polymerized polyamide amide gel is cast onto a support film, injected into a moldable element, or cast into a shape for further processing into a workpiece. In a specific embodiment, the reaction solvent is DMSO.
[0114] In a non-limiting manner, the formation of macropores relative to smaller mesopores and micropores can be controlled mainly by controlling the polymer / solvent dynamics during gel formation. By doing so, the pore structure can be controlled, and the number and volume of macropores, mesopores and micropores can be controlled. For example, compared with another curing additive that improves the solubility of the resulting polymer, such as triethylamine, a curing additive that reduces the solubility of the polymer formed during the polymerization process, such as 1,4-diazabicyclo [2.2.2] octane, can prepare a polymer gel containing more macropores. In another specific non-limiting example, when forming a polyimide aerogel, increasing the ratio of rigid amines (such as p-phenylenediamine (p-PDA)) incorporated into the polymer backbone to a more flexible diamine (such as -ODA) can be conducive to the formation of macropores rather than smaller mesopores and micropores.
[0115] The polymer solution can be optionally cast on the casting sheet covered by the support film for a period of time. Casting can include casting spin, gravure coating, three-roll coating, roller blade coating, slot extrusion coating, dip coating, Meyer rod coating or other technologies. In one embodiment, the casting sheet is polyethylene terephthalate (PET) casting sheet. After a period of time, the enhanced gel through polymerization is removed from the casting sheet, and is prepared for solvent exchange process. In some embodiments, the casting film can be heated to high temperature in stages to remove solvent, and the amic acid functional group in the polyamic acid is converted into imide by dehydration cyclization reaction, also referred to as imidization. In some cases, polyamic acid can be converted into polyimide in solution by adding chemical dehydrating agent, catalyst and / or heating.
[0116] In some embodiments, the polyimide polymer may be produced by preparing a polyamic acid polymer in a reaction vessel. The polyamic acid is then formed into a sheet or film and subsequently treated with a catalyst or heat and a catalyst to convert the polyamic acid into a polyimide.
[0117] Wet gels used to prepare aerogels can be prepared by any known gel-forming technique, such as adjusting the pH and / or temperature of a dilute metal oxide sol to a point where gelation occurs.
[0118] 2. Optional solvent exchange
[0119] After the polymer gel is synthesized, it may be necessary in some cases to perform a solvent exchange, wherein the reaction solvent is exchanged for a more desirable second solvent. Thus, in one embodiment, a solvent exchange may be performed, wherein the polymerized gel is placed in a pressure vessel and immersed in a mixture comprising a reaction solvent and a second solvent. A high pressure atmosphere is then generated in the pressure vessel, thereby forcing the second solvent to enter the polymerized gel and displace a portion of the reaction solvent. Alternatively, the solvent exchange step may be performed without using a high pressure environment. Multiple rounds of solvent exchange may be required. In some embodiments, no solvent exchange is required.
[0120] The time required for solvent exchange will change according to the type of the polymer exchanged and the reaction solvent used and the second solvent. In one embodiment, the time of each solvent exchange can be 1 hour to 168 hours or any time period therebetween, including 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, or 23 hours, 24 hours, 25 hours, 50 hours, 75 hours, 100 hours, 125 hours, 150 hours, 155 hours, 160 hours, 165 hours, 166 hours, 167 hours or 168 hours. In another embodiment, each solvent exchange can be about 1 minute to 60 minutes, or about 30 minutes. Exemplary second solvent includes methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutanol, the tert-butyl alcohol, 3-methyl-2-butanol, 3,3-dimethyl-2-butanol, 2-pentanol, 3-pentanol, 2,2-dimethyl propan-1-ol, cyclohexanol, diethylene glycol, cyclohexanone, acetone, acetylacetone, 1,4-dioxane, ether, methylene chloride, trichloroethylene, chloroform, carbon tetrachloride, water, and mixture thereof. In some non-limiting embodiments, the second solvent can have a suitable freezing point for carrying out supercritical or subcritical drying steps. For example, at an atmospheric pressure, the freezing point of the tert-butyl alcohol is 25.5°C, and the freezing point of water is 0°C. However, or, as described below, it is possible to dry without using supercritical or subcritical drying steps, for example, by evaporative drying technology.
[0121] The temperature and pressure used in the solvent exchange process can vary. The duration of the solvent exchange process can be adjusted by performing the solvent exchange under varying temperatures or atmospheric pressures, or both, provided that the pressure and temperature within the pressure vessel do not cause the first solvent or the second solvent to leave the liquid phase and become a gas phase, a vapor phase, a solid phase, or a supercritical fluid. Generally, higher pressures and / or temperatures will reduce the time required to perform the solvent exchange, while lower temperatures and / or pressures will increase the time required to perform the solvent exchange.
[0122] 3. Cooling and drying
[0123] In one embodiment, after solvent exchange, the polymerized gel can be exposed to supercritical drying. In this case, the solvent in the gel can be removed by supercritical CO2 extraction.
[0124] In another embodiment, after solvent exchange, the polymerized gel can be exposed to subcritical drying. In this case, the gel can be cooled to below the freezing point of the second solvent and subjected to a freeze drying or lyophilization process to produce an aerogel. For example, if the second solvent is water, the polymerized gel is cooled to below 0°C. After cooling, the polymerized gel can be subjected to a vacuum for a period of time to allow the second solvent to sublime.
[0125] In yet another embodiment, after solvent exchange, after most of the second solvent has been removed by sublimation, the polymerized gel can be exposed to subcritical drying, with optional heating. In this case, the partially dried gel material is heated to a temperature close to or above the boiling point of the second solvent for a period of time. The period of time can range from a few hours to a few days, although a typical period of time is about 4 hours. During the sublimation process, a portion of the second solvent present in the polymerized gel is removed, leaving a gel that can have macropores, mesopores, or micropores, or any combination thereof, or all of these pore sizes. After the sublimation process is complete or nearly complete, an aerogel is formed.
[0126] In another embodiment after solvent exchange, the polymerized gel can be dried under ambient conditions, for example, by removing the solvent under a gas flow, such as air, anhydrous gas, an inert gas such as nitrogen (N2), etc. In addition, passive drying techniques can be used, such as simply exposing the gel to ambient conditions without the use of a gas flow.
[0127] Once cooled or dried, the film and raw material shapes can be configured for the laminate of the present invention. For example, the film or raw material shape can be processed (e.g., by cutting or grinding) into a desired shape, such as a square, rectangle, circle, triangle, irregular shape, random shape, etc. In addition, as described above, the film or raw material shape can be fixed to the support material, for example, with an adhesive. In an alternative embodiment, the support material can be incorporated into the matrix of the polymer aerogel, which will be discussed below.
[0128] 4. Incorporation of reinforcement layers into the polymer aerogel matrix
[0129] In addition to the methods discussed above regarding the use of adhesives to attach polymer aerogels to support materials, optional embodiments of the present invention may include incorporating support materials into polymer matrices to produce reinforced polymer aerogels without the use of adhesives. It is noteworthy that in the manufacture of non-reinforced polymer aerogels, a reinforced support film can be used as a carrier to support the gelled film during processing. During the rewinding process, the gelled film can be irreversibly pressed into the carrier film. Pressing the gelled film into the base film can significantly improve durability. In another case, in the above-mentioned solvent casting step, the polymer solution can be cast into the reinforcing material or the support material.
[0130] Substrate selection and direct casting can optimize (e.g., minimize) the thickness of the resulting reinforced aerogel material. This process can also be extended to produce fiber-reinforced polymer aerogels—internal reinforced polyimide aerogels are examples. The process can include: (a) forming a polyamic acid solution from a mixture of dianhydride and diamine monomers in a polar solvent such as DMSO, DMAc, NMP, or DMF; (b) contacting the polyamic acid solution with the chemical curing agent and chemical dehydrating agent listed above to initiate chemical imidization; (c) casting the polyamic acid solution onto a fiber support and allowing it to penetrate before gelation; (d) gelling the catalyzed polyamic acid solution around and inside the fiber support during chemical imidization; (e) performing an optional solvent exchange, which can facilitate drying; and (f) removing the transient liquid phase contained in the gel by supercritical, subcritical, or room temperature drying to obtain an internally reinforced aerogel.
[0131] D. Non-Limiting Aspects of the Invention
[0132] The present invention may include the following non-limiting aspects.
[0133] Aspect 1: A laminate comprising: a flame retardant layer having a flammability rating that complies with at least one plastic flammability standard; and an aerogel layer; wherein: the laminate has opposing front and rear surfaces; the flame retardant layer defines at least a majority of the front surface; and the thickness of the laminate is equal to or less than 25.4 millimeters (mm).
[0134] Aspect 2: The laminate according to aspect 1, wherein the thickness of the laminate is equal to or less than 10 mm, preferably equal to or less than 5 mm, more preferably equal to or less than 2 mm, or even more preferably 0.3 mm to 2 mm.
[0135] Aspect 3: The laminate according to aspect 1 or 2, wherein the flame retardant layer has a thickness of 0.05 mm to 0.8 mm.
[0136] Aspect 4: The laminate according to any one of aspects 1 to 3, wherein the flame retardant layer is not electrically insulating.
[0137] Aspect 5: The laminate according to any one of aspects 1 to 3, wherein the flame retardant layer is electrically insulating.
[0138] Aspect 6: The laminate according to any one of aspects 1 to 5, wherein the plastic flammability standard is UL94 5VA or UL94 5VB, and wherein the flammability rating of the flame retardant layer complies with UL94 5VA or UL94 5VB.
[0139] Aspect 7: The laminate according to any one of aspects 1 to 6, wherein the flammability rating of the laminate complies with the plastic flammability standard, preferably UL94 5VB, more preferably UL94 5VA.
[0140] Aspect 8: The laminate according to any one of aspects 1 to 7, wherein the flame retardant layer comprises fibers.
[0141] Aspect 9: The laminate of aspect 8, wherein the fibers are nonwoven.
[0142] Aspect 10: The laminate of aspect 8, wherein the fibers are woven.
[0143] Aspect 11: The laminate according to any one of aspects 1 to 10, wherein the flame retardant layer comprises one or more than one metal hydroxide, organic phosphate, aluminum hydroxide, inorganic filler and / or metal oxide.
[0144] Aspect 12: The laminate according to any one of aspects 1 to 11, wherein the flame retardant layer comprises a silicate.
[0145] Aspect 13: The laminate of aspect 12, wherein the silicate comprises mica, and wherein the flame retardant layer preferably comprises at least 90 wt% mica.
[0146] Aspect 14: The laminate according to any one of aspects 1 to 13, wherein the flame retardant layer comprises ceramic, and wherein the flame retardant layer preferably comprises at least 90 wt% ceramic.
[0147] Aspect 15: The laminate according to aspect 14, wherein the ceramic comprises a metal oxide or a non-metal oxide or a combination thereof.
[0148] Aspect 16: The laminate according to aspect 15, wherein the ceramic comprises aluminum oxide, beryllium oxide, cerium oxide, zirconium oxide, carbide, boride, nitride or silicide, or any combination thereof.
[0149] Aspect 17: The laminate according to any one of aspects 1 to 16, wherein the flame retardant layer is halogen-free.
[0150] Aspect 18: The laminate according to any one of aspects 1 to 17, wherein the thickness of the aerogel layer is 0.05 mm to 0.254 mm.
[0151] Aspect 19: The laminate according to any one of aspects 1 to 18, wherein the aerogel layer is a polymer aerogel layer.
[0152] Aspect 20: The laminate according to any one of aspects 1 to 19, wherein the polymer aerogel layer comprises at least 50 wt%, preferably at least 80 wt%, or more preferably at least 90 wt% of the polyimide.
[0153] Aspect 21: The laminate according to any one of aspects 1 to 20, wherein the aerogel layer has a decomposition temperature higher than or equal to 400°C, preferably 400°C to 600°C.
[0154] Aspect 22: The laminate according to any one of aspects 1 to 21, comprising one or more adhesive layers bonded to the aerogel layer.
[0155] Aspect 23: The laminate according to aspect 22, wherein among the adhesive layers, a first adhesive layer is disposed between the flame retardant layer and the aerogel layer.
[0156] Aspect 24: The laminate according to aspect 23, wherein the first adhesive layer has a melting temperature or a decomposition temperature greater than 500°C.
[0157] Aspect 25: The laminate according to aspect 23 or 24, wherein at least a portion of the back surface is defined by: a second adhesive layer in the adhesive layer; or a backing layer removably disposed on the second adhesive layer.
[0158] Aspect 26: The laminate of any one of Aspects 22 to 25, wherein each of the adhesive layers comprises a pressure sensitive adhesive.
[0159] Aspect 27: The laminate according to any one of aspects 22 to 26, wherein each of the adhesive layers comprises a silicone adhesive compound and / or an epoxy compound.
[0160] Aspect 28: The laminate according to any one of aspects 1 to 27, wherein any one, any combination, or all of the flame retardant layer, the aerogel layer, and the adhesive layer are perforated.
[0161] Aspect 29: A laminate according to any one of Aspects 1 to 28, wherein, when the laminate is attached to a substrate, when the front surface of the laminate is exposed to a temperature above 500°C, preferably 500°C to 1500°C or more preferably 700°C to 1200°C, the laminate is capable of maintaining the temperature of the substrate at or below 500°C for 1 minute to 90 minutes, preferably at least 5 minutes.
[0162] Aspect 30: The laminate according to any one of aspects 1 to 29, wherein the laminate is provided in a roll such that a portion of a front surface of the laminate faces a portion of a back surface of the laminate.
[0163] Aspect 31: The laminate according to any one of aspects 1 to 30, further comprising a heat dissipation layer.
[0164] Aspect 32: The laminate according to Aspect 31, wherein the heat dissipation layer comprises a metal having a thermal conductivity of at least 15 W / m·K, preferably 15 W / m·K to 2500 W / m·K.
[0165] Aspect 33: The laminate according to aspect 32, wherein the metal comprises copper, aluminum, molybdenum, tungsten, rhenium, tantalum, niobium, stainless steel, nickel, or alloys thereof.
[0166] Aspect 34: The laminate according to aspect 32 or 33, wherein the heat dissipation layer comprises at least 90 wt % metal.
[0167] Aspect 35: The laminate according to Aspect 31, wherein the heat dissipation layer comprises graphite.
[0168] Aspect 36: The laminate of aspect 35, wherein the heat dissipation layer comprises at least 90 wt% graphite.
[0169] Aspect 37: The laminate according to any one of Aspects 31 to 36, wherein the heat dissipation layer has a thickness of 0.001 mm to 0.4 mm, preferably 0.01 mm to 0.05 mm.
[0170] Aspect 38: The laminate according to any one of aspects 31 to 37, wherein the heat dissipation layer is disposed between the flame retardant layer and the aerogel layer.
[0171] Aspect 39: The laminate according to aspect 38, comprising a first adhesive layer disposed between the flame retardant layer and the heat dissipation layer and a second adhesive layer disposed between the heat dissipation layer and the aerogel layer.
[0172] Aspect 40: The laminate of aspect 39, wherein the first adhesive layer is in direct contact with the flame retardant layer and the heat dissipating layer, and the second adhesive layer is in direct contact with the heat dissipating layer and the aerogel layer.
[0173] Aspect 41: The laminate according to aspect 39 or 40, further comprising a third adhesive layer and a backing layer, wherein the third adhesive layer is disposed between the aerogel layer and the backing layer.
[0174] Aspect 42: The laminate of aspect 41, wherein the third adhesive layer is in direct contact with the aerogel layer and the backing layer.
[0175] Aspect 43: A laminate according to any one of Aspects 39 to 42, wherein the first adhesive layer, the second adhesive layer and / or the third adhesive layer: have a melting temperature or decomposition temperature greater than 500°C; contain a pressure-sensitive adhesive; and / or contain a silicone adhesive compound and / or an epoxy compound.
[0176] Aspect 44: The laminate according to any one of aspects 31 to 43, wherein any one, any combination or all of the flame retardant layer, the heat dissipation layer, the aerogel layer, and the first adhesive layer, the second adhesive layer and the third adhesive layer are perforated.
[0177] Aspect 45: The laminate according to any one of aspects 1 to 44, further comprising a reinforcement layer.
[0178] Aspect 46: The laminate of aspect 45, wherein the reinforcement layer is attached to at least a portion of the flame retardant layer.
[0179] Aspect 47: The laminate of aspect 45 or 46, wherein the reinforcing layer is contained within at least a portion of the volume of the flame retardant layer.
[0180] Aspect 48: The laminate of any one of Aspects 45 to 47, wherein the reinforcement layer comprises fibers.
[0181] Aspect 49: The laminate according to aspect 48, wherein the fibers include glass fibers, carbon fibers, polyaramid fibers, thermoplastic fibers, thermoset fibers, ceramic fibers, basalt fibers, rock wool fibers, steel fibers, cellulose fibers, or any combination thereof.
[0182] Aspect 50: The laminate according to aspect 48 or 49, wherein the fibers are nonwoven fibers or woven fibers.
[0183] Aspect 51: A device comprising one or more laminates according to any one of Aspects 1 to 50, wherein a first laminate in the one or more laminates is joined to the device such that a front surface of the first laminate is disposed farther from the device than a rear surface of the first laminate.
[0184] Aspect 52: The device of aspect 51, wherein the device is a battery.
[0185] Aspect 53: An apparatus according to Aspect 52, wherein the battery is contained in a vehicle, the vehicle comprising: one or more wheels; and one or more electric motors, each motor configured to rotate at least one wheel; wherein the battery is electrically connected to at least one electric motor.
[0186] Aspect 54: The device according to Aspect 52 or 53 further includes: a busbar electrically connected to the battery; wherein one or more laminates include two or more laminates, wherein the second laminate is joined to the busbar so that the front surface of the second laminate is arranged farther from the busbar than the rear surface of the second laminate.
[0187] Aspect 55: The device according to any one of aspects 52 to 54, wherein the battery is a lithium-ion battery.
[0188] Aspect 56: The device according to Aspect 51, wherein the device is a busbar.
[0189] Aspect 57: The device according to aspect 51, wherein the device is a compression pad, a battery cell, a battery module, a battery pack or a battery box.
[0190] Aspect 58: The device of aspect 57, wherein the device is a compression pad, and wherein the compression pad comprises a compressible material.
[0191] Aspect 59: The device of aspect 58, wherein the compressible material comprises foam.
[0192] Aspect 60: The device of aspect 58 or 59, wherein the compression pad is located between the first battery cell and the second battery cell.
[0193] Aspect 61: The device of aspect 57, wherein the device is a battery cell.
[0194] Aspect 62: The device of aspect 57, wherein the device is a battery module comprising at least two battery cells, and wherein the one or more laminates are located between the two battery cells.
[0195] Aspect 63: The device of aspect 57, wherein the device is a battery pack comprising at least two battery modules, and wherein the one or more laminates are located between the two battery modules.
[0196] Aspect 64: The device of aspect 57, wherein the device is a battery case comprising an outer surface, an inner surface, and an inner volume.
[0197] Aspect 65: The device of Aspect 64, wherein one or more laminates cover at least a portion of the exterior surface, at least a portion of the interior surface, or both.
[0198] Aspect 66: The device of Aspect 64 or 65, wherein the internal volume is configured to enclose a compression pad, a battery cell, a battery module, or a battery pack.
[0199] Aspect 67: The device according to Aspect 66, wherein the internal volume includes a compression pad, a battery cell, a battery module, a battery pack, or any combination thereof.
[0200] Aspect 68: The device of any one of Aspects 57 to 67, wherein the compression pad, battery cell, battery module, battery pack or battery box is contained in a vehicle, the vehicle comprising one or more electric motors.
[0201] Aspect 69: The apparatus according to Aspect 68, wherein the vehicle is a car, an aircraft, a train, a motorcycle, a ship or a spacecraft.
[0202] Aspect 70: The device of aspect 51, wherein the device is a cable.
[0203] Aspect 71: The apparatus of aspect 70, wherein the cable has a length and a width, and wherein the length is longer than the width.
[0204] Aspect 72: The apparatus of Aspect 70 or 71, wherein the cable is conductive.
[0205] Aspect 73: The device according to any one of aspects 70 to 72, wherein the cable comprises a diameter of 0.0003 inches to 10 inches, preferably 0.001 inches to 1 inch.
[0206] Aspect 74: The apparatus of any one of Aspects 70 to 73, wherein the cable is contained in a missile, a rocket, an artillery piece, a manned aircraft, an unmanned aircraft, a land vehicle, a sea vehicle, or a spacecraft.
[0207] Aspect 75: The apparatus according to Aspect 74, wherein the vehicle is a spacecraft or an aircraft.
[0208] Aspect 76: An apparatus according to any one of Aspects 51 to 75, wherein one or more laminates are capable of maintaining the temperature of the apparatus at 500°C or less for 1 minute to 90 minutes, preferably at least 5 minutes, when the front surface of the laminate is exposed to a temperature above 500°C, preferably 500°C to 1500°C or more preferably 700°C to 1200°C.
[0209] Aspect 77: A method of insulating a device according to any one of aspects 51 to 76, the method comprising bonding a laminate according to any one of aspects 1 to 50 to the device.
[0210] Aspect 78: The method of aspect 77, wherein the laminate is positioned relative to the device such that a front surface of the laminate is disposed farther from the device than a back surface of the laminate.
[0211] Aspect 79: The method according to aspect 78, wherein when the front surface of the laminate is subjected to a temperature above 500°C to 1500°C for a period of 1 minute to 90 minutes, preferably at least 5 minutes, the temperature of the device does not exceed 500°C during this period.
[0212] Aspect 80: The method according to aspect 78, wherein when the front surface of the laminate is subjected to a temperature above 700°C to 1200°C for a period of 1 minute to 90 minutes, preferably at least 5 minutes, the temperature of the device does not exceed 500°C during this period.
[0213] Aspect 81: The laminate according to any one of aspects 1 to 50, wherein the flame retardant layer includes a first flame retardant layer and a second flame retardant layer, and the first flame retardant layer and the second flame retardant layer are disposed on opposite sides of the aerogel layer. Example
[0214] The present invention will be described in more detail by specific examples. The following examples are provided for illustrative purposes only and are not intended to limit the present invention in any way. Those of ordinary skill in the art will readily recognize that various non-critical parameters that may be changed or modified produce substantially the same results.
[0215] Example 1
[0216] (Testing of flame retardant and thermal insulation laminates)
[0217] Materials: 12" x 1.6" x 0.2" copper rods were obtained from McMaster Carr. AeroZero (AZ) film (6.5 mil) was manufactured by Blueshift Materials Inc. and the flame retardant barrier material used was 3M FRBWT145 (5.8 mil) manufactured by 3M. Laminate test samples were assembled using pressure sensitive silicone adhesive SA6101LR produced by FLEXcon.
[0218] Test Setup: The flame retardant and thermal insulation samples were tested for their effectiveness using a bare copper bar as the test substrate. The copper bar was fixed to a support frame in a horizontal position and a thermocouple was fixed to the center of the copper bar using Kapton tape. The test sample was wrapped around the copper bar before exposure to flame.
[0219] The test sample was wrapped about 2 inches around a 12-inch copper rod, with the tip of the thermocouple directly below the test sample and in direct contact with the copper rod. The test sample was bonded to the copper rod using a silicone pressure sensitive adhesive. A flame source (Bunsen burner) with a flame temperature set at 700°C was placed 1.5 inches from the test sample so that the flame was in direct contact with the horizontally placed test sample. The temperature of the thermocouple was recorded at 30 second intervals for 10 minutes.
[0220] Test configuration such as Figure 8 As shown, the test setup 400 includes a copper rod 40 , test samples 42 , 44 , a thermocouple 46 , and a flame source 48 . Fig. 9 The layup of the flame retardant and thermal insulation test samples 42, 44 is shown. Each sample includes one or more AeroZero aerogel layers as the thermal insulation layer 16, adhesive layers 20, 22 directly attaching the aerogel layers to the copper rod 40 and the flame retardant layer 18. The flame retardant layer 18 faces the flame source 48. Several samples were tested, and their specific layups are provided in Table 1.
[0221] Table 1: Lamination of flame retardant and thermal insulation test samples
[0222]
[0223] The thermal curve of the test sample is as follows: Fig.10 For each sample, the temperature of the copper bar after 5 and 10 minutes of exposure to the flame is shown in Table 2. These temperatures are compared to the control sample (i.e., the copper bar without a barrier). The tests show that when one or both of the thermal insulation layers (here, AeroZero membrane) are combined with the flame retardant layer (here, FRM WT-145), the temperature of the copper bar is significantly reduced, resulting in an unexpected synergy between the thermal insulation layer and the flame retardant layer.
[0224] Table 2: Temperature of the copper rod when the sample was exposed to flame
[0225]
[0226] Examples 2 to 7
[0227] (Testing of flame retardant and thermal insulation laminates)
[0228] 1000°C flame test setup: Further testing of flame retardant and thermal insulation samples was performed using Fig.11The test setup 500 shown was performed. Test setup 500 is substantially similar to test setup 400, with the following exceptions. Here, the flame is 3 inches high, 2 inches wide, the temperature is 1000°C ± 30°C, and the bottom of the flame is 2.5 inches from the test sample 44. In addition, some tests were performed without using a test substrate, while other tests used test substrates including 8-inch x 8-inch aluminum, steel, and carbon fiber composite panels. In the tests using the test substrate, instead of two samples 42 and 44, only one sample 44 was adhered to the side of the test substrate facing the flame. Finally, two thermocouples 46a and 46b were used. Thermocouple 46a was in direct contact with the flame to measure the flame temperature, and thermocouple 46b was set on the side of the laminate test sample (if no test substrate was used) or the test substrate that was not facing the flame (i.e., "cold"). All thermal curves described in Examples 2 to 7 are based on the temperature recorded by thermocouple 46b.
[0229] Example 2
[0230] Flame retardant and thermal insulation laminate test samples having the laminates shown in Table 3 were exposed to a 1000°C flame for 600 seconds (10 minutes). The laminate test samples did not adhere to the test substrate. In this example, a laminate having only a flame retardant layer ("FRB") was compared to a laminate in which the FRB and thermal insulation layer were combined. The FRB tested was FRB NT381 produced by 3M Company.
[0231] Table 3: Lamination of flame retardant and thermal insulation test samples
[0232]
[0233] Table 3 Thermal curves of samples Fig.12 As shown in the figure, the laminate including the FRB and the thermal insulation layer has a lower primary heating rate and temperature after 5 minutes (312°C vs 341°C) compared to the laminate including only the FRB.
[0234] Example 3
[0235] Flame retardant and thermal insulation laminate test samples with the layup shown in Table 4 were exposed to a 1000°C flame for 25 minutes. The laminate test samples did not adhere to the test substrate. In this example, one of the samples included an additional heat dissipation layer - a 0.05 mm thick graphite layer - disposed between the FRB facing the flame and the thermal insulation layer.
[0236] Table 4: Lamination of flame retardant and thermal insulation test samples
[0237]
[0238] Table 4 Thermal curves of samples Fig.13The data show that adding a heat sink between the FRB facing the flame and the insulation can further reduce the cold side temperature of the laminate. For the first 3 minutes or so, the one-shot heating rate of the laminate including the heat sink is similar to the one-shot heating rate of the laminate not including the heat sink. But after 3 minutes, the laminate including the heat sink performs better than the laminate not including the heat sink, including in terms of heating rate. These improvements are quantified in Table 5, which provides the cold side temperature of the laminate when the samples were exposed to the flame for 5 minutes, 10 minutes, and 25 minutes.
[0239] Table 5: Laminate Cold Side Temperatures When Samples Were Exposed to Flame
[0240]
[0241] Example 4
[0242] Flame retardant and thermal insulation laminate test samples of three different thicknesses (0.57 mm, 0.70 mm, and 1.17 mm) were adhered to 8" x 8" mild steel panels with a thickness of 0.7 mm and exposed to a 1000°C flame for 600 seconds (10 minutes). The layup of the laminate test samples is provided in Table 6.
[0243] Table 6: Lamination of flame retardant and thermal insulation test samples
[0244] sample FRB Type FRB thickness(mm) Laminate thickness (mm) FRB / AeroZero NT-381 0.38 0.57 FRB / AeroZero / AeroZero / FRB WT-145 0.13 0.70 FRB / AeroZero / AeroZero / FRB NT-381 0.38 1.17
[0245] Table 6 Thermal profiles of the samples, and thermal profiles of a control consisting of a steel plate without an adhered laminate ("no FRB") Fig.14 The data show that as the thickness of the laminate increases, both the primary heating rate (measured within the first 200 seconds) and the maximum temperature (measured at 600 seconds) of the cold side of the substrate decrease. Notably, during the 600 seconds (10 minutes) of flame exposure, the maximum temperature of the cold side of the substrate for the 0.70 mm thick and 1.17 mm thick laminates remained below 350°C.
[0246] Example 5
[0247] Flame retardant and thermal insulation laminate test samples, including one sample with a 0.05 mm thick graphite layer and one sample without such a heat dissipation layer, were adhered to an 8 inch x 8 inch carbon fiber composite plate with a thickness of 1.0 mm and exposed to a 1000°C flame for 25 minutes. The layup of the laminate test samples is provided in Table 7.
[0248] Table 7: Lamination of flame retardant and thermal insulation test samples
[0249]
[0250] Table 7 Thermal profiles of the laminate and the control consisting of a carbon fiber composite panel without an adhered laminate ("No FRB") Fig.15 As shown. Without a protective laminate, the carbon fiber composite panel began to burn and produce heavy smoke within 10 seconds of contact with the flame. The temperature of the cold side of the carbon fiber composite panel rose rapidly, reaching 200°C within 40 seconds. The test was stopped due to high smoke volume and decomposition of the carbon fiber composite panel. When protected by a flame retardant and thermal insulation laminate that does not include a heat dissipation layer, the primary heating rate is significantly reduced: it takes about 2 minutes for the cold side of the carbon fiber composite panel to reach 200°C. After 10 minutes of flame exposure, the maximum temperature on the cold side of the carbon fiber composite panel was 355°C and did not increase further during the 25-minute test.
[0251] The flame retardant and thermal insulation laminate including the heat dissipation layer exhibits enhanced performance in terms of the primary heating rate and the maximum temperature of the cold side of the carbon fiber composite panel, especially the primary heating rate shifts slightly to the right, reaching 200°C after 2.8 minutes, and the maximum temperature of the cold side of the carbon fiber composite panel during the 25-minute flame exposure is 333°C. These improvements are further quantified in Table 8, which provides the substrate cold side temperature when the sample is exposed to the flame for 5 minutes, 10 minutes, and 25 minutes.
[0252] Table 8: Cold side temperatures of substrates during flame exposure of samples
[0253]
[0254] In addition, if Fig.16 As shown, for the laminates of Table 7, there was no burn through of the carbon fiber composite panel during the test.
[0255] Example 6
[0256] The 1.17 mm thick FRB / AeroZero / AeroZero / FRB flame retardant and thermal insulation laminate of Table 3 was adhered to an 8 inch x 8 inch aluminum plate having a thickness of 0.025 mm (1 mil) and exposed to a 1000°C flame for 25 minutes. The thermal curve of the laminate is shown in FIG. Fig.17 As shown in the figure, this thermal profile includes a gradual increase in the temperature of the aluminum plate, reaching a maximum of 325°C during the 25-minute test: well below the melting point of aluminum. Fig.18 As shown, no burn-through of the aluminum plate was observed during the test.
[0257] Example 7
[0258] The thermal conductivity of several flame retardant and thermal insulation laminates was tested according to the ASTM C518 test method "Standard Test Method for Steady-State Thermal Transmission Properties by Means of the Heat Flow Meter Apparatus." The instrument used was a Fox 50 heat flow meter manufactured by TA Instruments. Table 9 provides the layup, thermal conductivity, and density of the tested laminates.
[0259] Table 9: Properties of flame retardant and thermal insulation test samples
[0260]
[0261] The above description and examples provide a complete description of the structure and use of the illustrative embodiments. Although certain embodiments have been described above to some extent in particular or with reference to one or more than one separate embodiment, a person of ordinary skill in the art may make various changes to the disclosed embodiments without departing from the scope of the present invention. Therefore, the various illustrative embodiments of the apparatus and method are not intended to be limited to the specific forms disclosed. Instead, they include all modifications and substitutions that fall within the scope of the claims, and embodiments other than the illustrated embodiments may include some or all of the features of the depicted embodiments. For example, elements may be omitted or combined into a single structure and / or connections may be replaced. In addition, where appropriate, aspects of any of the above embodiments may be combined with aspects of any other embodiments described to form other embodiments with comparable or different properties and / or functions, and to solve the same or different problems. Similarly, it should be understood that the above advantages and advantages may relate to one embodiment, or may relate to multiple embodiments.
[0262] The claims are not intended to include, nor should they be interpreted as including, means-plus- or step-plus-function limitations, unless such limitations are explicitly recited in a given claim using the phrases "means for" or "step for," respectively.
Claims
1. A laminate, wherein include: A flame retardant layer having a flammability rating that complies with at least one flammability standard for plastics; and Aerogel layer; in: The laminate has opposing front and rear surfaces; The flame retardant layer defines at least a majority of the front surface; and The laminate has a thickness equal to or less than 25.4 millimeters (mm).
2. The laminate according to claim 1, wherein the thickness of the laminate is equal to 10 mm or less, preferably equal to 5 mm or less, more preferably equal to 2 mm or less, or even more preferably 0.3 mm to 2 mm. 3 . The laminate according to claim 1 , wherein the flame retardant layer has a thickness of 0.05 mm to 0.8 mm.
4. The laminate according to any one of claims 1 to 3, wherein the plastic flammability standard is UL94 5VA or UL94 5VB, and wherein the flammability rating of the flame retardant layer complies with UL94 5VA or UL94 5VB.
5. The laminate according to any one of claims 1 to 4, wherein the flammability rating of the laminate complies with the plastic flammability standard, preferably UL94 5VB, more preferably UL94 5VA.
6. The laminate according to any one of claims 1 to 5, wherein the flame retardant layer comprises one or more than one metal hydroxide, organic phosphate, aluminum hydroxide, inorganic filler and / or metal oxide.
7. The laminate according to any one of claims 1 to 6, wherein the flame retardant layer comprises a silicate, and wherein the flame retardant layer preferably comprises at least 90% by weight of a silicate.
8. The laminate according to any one of claims 1 to 7, wherein the flame retardant layer comprises ceramic, and wherein the flame retardant layer preferably comprises at least 90% by weight of ceramic.
9. The laminate according to any one of claims 1 to 8, wherein the aerogel layer comprises at least 50 wt.-%, preferably at least 80 wt.-% or more preferably at least 90 wt.-% of polyimide.
10. The laminate according to any one of claims 1 to 9, comprising one or more adhesive layers joined to the aerogel layer, the adhesive layers comprising a first adhesive layer disposed between the flame retardant layer and the aerogel layer.
11. The laminate of claim 10, wherein at least a first adhesive layer of the adhesive layers comprises a pressure sensitive adhesive.
12. The laminate according to any one of claims 1 to 11, in, When the laminate is attached to a substrate, when the front surface of the laminate is exposed to a temperature above 500°C, preferably 500°C to 1500°C or more preferably 700°C to 1200°C, the laminate is capable of maintaining the temperature of the substrate at or below 500°C for 1 minute to 90 minutes, preferably at least 5 minutes.
13. The laminate according to any one of claims 1 to 12, further comprising a heat dissipation layer. 14 . The laminate according to claim 13 , wherein the heat dissipation layer comprises a metal having a thermal conductivity of at least 15 W / m·K, preferably 15 W / m·K to 2500 W / m·K.
15. The laminate of claim 14, wherein the metal comprises copper, aluminum, molybdenum, tungsten, rhenium, tantalum, niobium, stainless steel, nickel, or alloys thereof.
16. The laminate according to claim 14 or 15, wherein the heat dissipation layer comprises at least 90 wt% metal.
17. The laminate according to claim 13, wherein the heat dissipation layer comprises graphite, preferably at least 90 wt% graphite.
18. The laminate according to any one of claims 14 to 17, wherein the heat dissipation layer is provided between the flame retardant layer and the aerogel layer.
19. A device comprising one or more than one laminate according to any one of claims 1 to 18, wherein a first laminate of the laminates is joined to the device such that a front surface of the first laminate is disposed further away from the device than a rear surface of the first laminate.
20. The device of claim 19, wherein the device is a compression pad, a battery cell, a battery module, a battery pack, or a battery case.
21. The device of claim 19, wherein the device is a conductive cable.
22. The laminate according to any one of claims 1 to 18, wherein the flame retardant layer comprises a first flame retardant layer and a second flame retardant layer, and the first flame retardant layer and the second flame retardant layer are disposed on opposite sides of the aerogel layer.
Citation Information
Cited By
Preparation method and application of plant fiber flame-retardant heat-insulating foam material
CN122277281A