Flat steel product having Al coating, method for production thereof, steel component and method for production thereof

By adding high zinc content and magnesium to the Al-based protective coating of thermoformed steel members, forming a Zn-rich layer and a thin oxide layer, the problem of liquid metal embrittlement caused by the alumina layer affecting phosphating and excessive zinc content is solved. It achieves better phosphating effect and corrosion resistance.

CN118922576APending Publication Date: 2024-11-08THYSSENKRUPP STEEL EUROPE AG PATENTE PATENT DEPARTMENT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280093587.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-04-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the phosphating process, the presence of an alumina layer in the existing thermoformed steel components leads to poor phosphating effect, which affects the aesthetics of the decorative surface, and excessive zinc content can easily lead to liquid metal embrittlement and tool adhesion problems.

Method used

Using an Al-based protective coating containing high zinc content, the Zn-rich layer is formed on the surface to improve the phosphating properties, and the thin oxide layer is formed by adding magnesium to prevent aluminum oxidation, and the zinc content is controlled within a reasonable range to avoid liquid metal brittleness. change.

Benefits of technology

It significantly improves the phosphating effect, forms a better anti-corrosion protective layer, reduces hydrogen release, avoids liquid metal embrittlement and tool adhesion problems, and improves the aesthetics and corrosion resistance of steel components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922576A_ABST
    Figure CN118922576A_ABST
Patent Text Reader

Abstract

The invention relates to a steel component consisting of a steel substrate consisting of a steel containing 0.1% to 3% by weight of Mn and optionally at most 0.01% by weight of B, and an Al-based protective coating applied to the steel substrate. The protective coating has an additional alloying composition at most 30% by mass, not in terms of iron and manganese. The mass ratio of iron to manganese of Si as an additional alloy component in the protective coating is 3% Si to 15% Si. In addition, the mass ratio of Mg as an additional alloy component, excluding iron and manganese, in the protective coating is at most 1.0% Mg. In addition, the mass ratio of Zn, which is an additional alloy component, of iron and manganese in the protective coating is 0.4% Zn to 25.0% Zn. Further, the protective coating has a near-surface first Zn-rich layer having a Zn content higher than the average Zn content of the protective coating. Wherein the Zn content of the first Zn-rich layer is greater than 5% by weight.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a flat steel product for hot forming, which consists of a steel substrate and an Al-based protective coating applied to the steel substrate, wherein the steel substrate consists of a steel containing 0.1 to 3 wt. % Mn and optionally up to 0.01 wt. % B, and the Al-based protective coating optionally contains a total of up to 30 wt. % of other alloying elements.

[0002] The invention also relates to a steel component and to a method for producing such a steel component.

[0003] The expression "flat steel products" here includes all rolled products whose length is much greater than their thickness. These products include steel strips and steel plates, as well as (pre-cut) billets obtained therefrom.

[0004] In hot forming (also called press hardening or hot press hardening), the steel blanks cut from the cold-rolled or hot-rolled steel strip are heated to a deformation temperature which is usually above the austenitizing temperature (Ac3) of the corresponding steel and placed in the mold of the forming press in the heated state. In the subsequent forming process, the metal blank or the component formed therefrom cools rapidly due to contact with the cold mold. The cooling rate is adjusted here so that a hardness microstructure is formed in the steel matrix. The microstructure transforms into a martensitic microstructure, which is called a hardness microstructure.

[0005] Typical steels suitable for hot press hardening are A steel to E steel, whose chemical compositions are listed in Table 10.

[0006] For hot-rolled MnB steel sheets provided with an Al coating and used for hot forming steel components, EP 0971044 B1 specifically describes an alloying method by which, in addition to iron and unavoidable impurities, the carbon content of the MnB steel should be greater than 0.20% but less than 0.5%, the manganese content is greater than 0.5% but less than 3%, the silicon content is greater than 0.1% but less than 0.5%, the chromium content is greater than 0.01% but less than 1%, the titanium content is less than 0.2%, the aluminum content is less than 0.1%, the phosphorus content is less than 0.1%, the sulfur content is less than 0.05%, and the boron content is greater than 0.001% but less than 0.08%. The Al coating, the so-called AlSi coating, consists of 9% to 10% by weight of Si, 2% to 3.5% by weight of iron and the remainder of aluminum. The coated flat steel product having the above-mentioned properties is heated to a heating temperature of more than 700° C. and maintained at the heating temperature for a certain holding time. During the heating and holding process, the protective coating melts and alloying is carried out by the protective coating. The iron in the steel matrix diffuses into the protective coating, thereby forming a more thermally stable phase. The molten protective coating solidifies as a result. The solidified, thermally stable protective coating is a prerequisite for the subsequent forming step. In the forming step, the flat steel product is placed in a die, where it is hot-formed into a steel component, during which the flat steel product is cooled sufficiently quickly that a hard microstructure is formed in the steel matrix of the flat steel product.

[0007] The disadvantage of the AlSi coating is that during the hot forming process, due to the temperature, very strong oxidation of the aluminum-rich surface occurs. This aluminum oxide layer in turn prevents the subsequent phosphating step from being fully effective. Since the process parameters in the phosphating process are usually not sufficient to destroy the aluminum oxide layer, the aluminum oxide layer prevents the formation of firmly adhering metal phosphates in the phosphating process. In this case, the resulting steel component is very susceptible to decorative surface corrosion. Although this does not affect the structural stability of the steel component, it reduces the aesthetics of the steel component, which is not what the end customer wants.

[0008] DE 102009007909A1 discloses a method for producing a high-strength steel component, wherein, on the one hand, an optimized forming property of the coating is ensured during the hot forming of the corresponding flat steel product, and on the other hand, the resulting steel component has an optimized cathodic corrosion protection. The steel component of the invention has a zinc alloyed surface with a zinc content of at least 60% by weight, in particular at least 80% by weight. This results in a cathodic corrosion protection that can be clearly detected by electrochemical methods.

[0009] EP 2045360A1 discloses a method for producing a high-strength steel component which has excellent corrosion protection and is particularly suitable for automobile bodies. After hot forming, the steel component of the invention has a zinc alloyed surface with a zinc content of at least 60% by weight, in particular at least 80% by weight. This results in a cathodic corrosion protection which can be clearly detected by electrochemical methods. Its corrosion resistance is at least equivalent to that of a pure zinc coating.

[0010] Zn contents above 25 wt. % increase the risk of liquid metal embrittlement. Zinc in protective coatings has the disadvantage of a relatively low melting point. During the production of steel components by hot forming, liquid Zn phases can form. These phases can firstly penetrate into the steel matrix and cause cracking (liquid metal embrittlement) and secondly adhere to the forming tools or furnace rollers, causing contamination and layer detachment.

[0011] The object of the present invention is to provide a steel component which can be produced by hot forming and has improved phosphating properties.

[0012] This object can be achieved by the following steel component, which consists of a steel substrate and an Al-based protective coating applied on the steel substrate, the steel substrate is composed of a steel containing 0.1% by weight to 3% by weight of Mn and optionally up to 0.01% by weight of B, and the Al-based protective coating optionally has an additional alloy component of up to 30% by weight, excluding iron and manganese. The mass ratio of Si as an additional alloy component in the protective coating excluding iron and manganese is 3% Si to 15% Si, especially 6% Si to 12% Si. In addition, the mass ratio of Mg as an additional alloy component in the protective coating excluding iron and manganese is up to 1.0%, and the mass ratio of Zn as an additional alloy component in the protective coating excluding iron and manganese is 0.4% Zn to 25.0% Zn. In addition, the protective coating has a first Zn-rich layer near the surface, whose Zn content is higher than the average Zn content of the protective coating. In addition, the Zn content of the first Zn-rich layer is greater than 5% by weight. The protective coating is especially an AlSi coating.

[0013] In the context of this application, the mass ratio of an alloying component in a protective coating excluding iron and manganese is taken to mean the proportion of the total mass of the alloying component to the total mass of all elements in the protective coating except iron and manganese. The advantage of using the mass ratio excluding iron and manganese to characterize the protective coating is that the values ​​are not changed by diffusion of iron and manganese out of the steel matrix. The mass ratio excluding iron and manganese is given in [%]. In contrast, the content of an element calculated on the total mass is given in the usual manner in [% by weight].

[0014] Therefore, the protective coating contains up to 30%, preferably 20%, of other alloying elements, of which Si accounts for 3% to 15%, Mg for up to 1.0% and Zn for 0.4% to 25%, based on the total mass excluding iron and manganese.

[0015] Specifically, the mass ratio of Mn is greater than 0.1 wt% and less than 2.5 wt%, preferably greater than 0.2 wt% and less than 2.0 wt%, more preferably greater than 0.4 wt% and less than 1.8 wt%. During the hot forming operation, a certain proportion of manganese will diffuse from the steel matrix into the protective coating to form an additional alloy component in the protective coating.

[0016] In addition to Fe, Si, Mg, Zn and optionally in addition to Mn, the protective coating preferably consists only of Al and unavoidable impurities. In the context of this application, an element is an unavoidable impurity in the protective coating when its mass ratio excluding iron and manganese is less than 0.5%. This definition only relates to unavoidable impurities in the protective coating. Standard technical limits apply to unavoidable impurities in the steel matrix mentioned later.

[0017] The near-surface layer in the context of this application refers to a layer extending to a 500 nm thick region adjacent to the protective coating surface. Thus, the first Zn-rich layer extends into a 500 nm thick region adjacent to the protective coating surface. In other words, the first Zn-rich layer is located within the uppermost 500 nm of the protective coating.

[0018] It has been found that an increased Zn content in the near-surface region allows reliable phosphating. During the phosphating process, the near-surface zinc is converted into zinc phosphate. The zinc phosphate layer also provides better corrosion protection than the iron phosphate layer that would otherwise form. In addition, zinc phosphate is a good base for paint adhesion.

[0019] The weight ratio of Zn in the protective coating as an additional alloying component, excluding iron and manganese, is preferably at least 0.6%, more preferably at least 1.0%, in particular at least 1.5%.

[0020] Furthermore, it is preferred that the zinc content of the first Zn-rich layer is greater than 10.0 wt. %, more preferably greater than 18.0 wt. %.

[0021] The higher the zinc content of the first Zn-rich layer, the better the phosphating properties, since more zinc phosphate and less iron phosphate are formed. The higher the mass ratio of Zn in the protective coating, excluding iron and manganese, the easier it is to achieve a high Zn content in the first Zn-rich layer in a procedurally reliable manner. Therefore, the higher the mass ratio of Zn in the protective coating, excluding iron and manganese, the better.

[0022] However, zinc in the protective coating has the disadvantage of a relatively low melting point. During the production of steel components by hot forming, liquid Zn phases may form. These liquid Zn phases firstly penetrate into the steel matrix and cause cracking (liquid metal embrittlement), and secondly adhere to the forming tools or furnace rollers and cause dirt and layer detachment. Therefore, the selected zinc content should not be too high. In experiments, it was found that in flat steel products it is particularly advantageous if the mass proportion of Zn in the protective coating, excluding iron and manganese, does not exceed 5.0%, in particular less than 5%, preferably does not exceed 2.3%, and more preferably does not exceed 1.8%.

[0023] It has been found that an advantageous additional alloying component in the protective coating is magnesium, which has good alloying properties with Al protective coatings of the type discussed herein. The amount of Mg added should be adjusted to a mass ratio of at least 0.10%, preferably at least 0.15%, of magnesium, excluding iron and manganese. In particular, it has been found in practice that a mass ratio of magnesium, excluding iron and manganese, of less than 0.50%, or less than 0.4%, or less than 0.35% is particularly advantageous. Magnesium added in small amounts to the protective coating has a higher affinity for oxygen than the main component of the protective coating, aluminum. Even in the case of small amounts of magnesium, a thin oxide layer forms on the surface of the protective coating, covering the aluminum between this oxide layer and the steel substrate. During the heating process required for hot forming of the flat steel product, this thin oxide layer prevents the aluminum from reacting with the moisture present in the furnace atmosphere used to heat the flat steel product. In this way, oxidation of the aluminum in the coating and the associated release of hydrogen (which can diffuse into the coating and the steel substrate of the flat steel product) can be effectively prevented. Surprisingly, this is the case even if the Al-based coating partially melts due to heating and its surface breaks up, resulting in contact between the molten coating material and the furnace atmosphere. In particular, in the case of relatively long annealing times, the hydrogen concentration in the component hot-formed from the flat steel product is lower in the case of the flat steel product according to the invention than in conventional flat steel products with an Al coating.

[0024] Alloying with magnesium therefore has the advantage of reducing the ingress of hydrogen into the steel matrix. If the local hydrogen concentration is very high, this can weaken the bonding at the grain boundaries of the steel matrix microstructure, causing cracks along the grain boundaries during use due to the stresses generated.

[0025] The element content in the protective coating can be determined in particular by glow discharge optical emission spectroscopy (GD-OES). In addition, wet chemical leaching with the use of ICP-OES (inductively coupled plasma-optical emission spectroscopy) can also be used to determine the element content.

[0026] The thickness of the protective coating is generally in the range of at least 5 μm and at most 35 μm, in particular at least 10 μm and at most 25 μm.

[0027] The steel matrix consists of a steel having 0.1 wt. % to 3 wt. % Mn and optionally up to 0.01 wt. % B. In particular, the microstructure of the steel can be converted into a martensitic microstructure or a partially martensitic microstructure by hot forming. Therefore, the microstructure of the steel matrix of the steel component is preferably a martensitic microstructure or at least a partially martensitic microstructure, since such a microstructure has a particularly high hardness.

[0028] More preferably, the steel matrix is ​​a steel consisting of the following together with iron and unavoidable impurities (in wt. %):

[0029] C: 0.04 wt% to 0.45 wt%,

[0030] Si: 0.02 wt% to 1.2 wt%,

[0031] Mn: 0.5 wt% to 2.6 wt%,

[0032] Al: 0.02 wt% to 1.0 wt%,

[0033] P: ≤0.05% by weight

[0034] S: ≤0.02% by weight

[0035] N: ≤0.02% by weight

[0036] Sn: ≤0.03% by weight

[0037] As: ≤0.01% by weight

[0038] Ca: ≤0.005% by weight

[0039] And optionally one or more elements "Cr, B, Mo, Ni, Cu, Nb, Ti, V" in the following contents:

[0040] Cr: 0.08 wt% to 1.0 wt%,

[0041] B: 0.001 wt% to 0.005 wt%,

[0042] Mo: ≤ 0.5 wt%,

[0043] Ni: ≤ 0.5 wt%,

[0044] Cu: ≤ 0.2 wt%,

[0045] Nb: 0.02 wt% to 0.08 wt%,

[0046] Ti: 0.01 wt% to 0.08 wt%,

[0047] V: ≤ 0.1 wt%.

[0048] The elements P, S, N, Sn, As, and Ca are impurities that cannot be completely avoided during the production of steel. In addition to these elements, other elements may also be present in the steel as impurities. These other elements are collectively referred to as "inevitable impurities". Preferably, the total content of the inevitable impurities added together does not exceed 0.2% by weight, preferably not more than 0.1% by weight. The optional alloying elements Cr, B, Nb, and Ti, for which lower limits have been specified, may also appear in the steel matrix as inevitable impurities in a content below the corresponding lower limit. In this case, they are also counted as inevitable impurities, and their total content is limited to not more than 0.2% by weight, preferably not more than 0.1% by weight. The upper limits of the corresponding impurities of these elements are preferably as follows:

[0049] Cr: ≤0.050% by weight

[0050] B: ≤0.0005% by weight

[0051] Nb: ≤ 0.005 wt%,

[0052] Ti: ≤ 0.005 wt%.

[0053] These preferred upper limits should be considered as alternatives or general options. Therefore, preferred steel variants meet one or more of the above four conditions.

[0054] In a preferred embodiment, the C content in the steel is not more than 0.37 wt. % and / or at least 0.06 wt. %. In particularly preferred variants, the C content is 0.06 wt. % to 0.09 wt. %, or 0.12 wt. % to 0.25 wt. %, or 0.33 wt. % to 0.37 wt. %.

[0055] In a preferred embodiment of the present invention, the Si content in the steel is not more than 1.00 wt. % and / or at least 0.06 wt. %.

[0056] In a preferred embodiment, the Mn content in the steel is not more than 2.4 wt.-% and / or at least 0.75 wt.-%. In a particularly preferred embodiment, the Mn content is 0.75 wt.-% to 0.85 wt.-%, or 1.0 wt.-% to 1.6 wt.-%.

[0057] In a preferred variant, the Al content in the steel is not more than 0.75 wt. %, in particular not more than 0.5 wt. %, preferably not more than 0.25 wt. %. Alternatively or in addition, the Al content is preferably at least 0.02%.

[0058] Furthermore, it has been found that limiting the total content of silicon and aluminum is beneficial. Therefore, in a preferred variant, the total content of Si and Al (usually referred to as Si+Al) does not exceed 1.5% by weight, preferably does not exceed 1.2% by weight. In addition or alternatively, the total content of Si and Al is at least 0.06% by weight, preferably at least 0.08% by weight.

[0059] P, S, N are typical impurities that cannot be completely avoided during steel production. In a preferred variant, the P content is no more than 0.03% by weight. Independently of this, the S content is preferably no more than 0.012%. Additionally or as a supplement, the N content is preferably no more than 0.009% by weight.

[0060] Optionally, the steel also contains 0.08% to 1.0% by weight of chromium. The Cr content preferably does not exceed 0.75% by weight, in particular does not exceed 0.5% by weight.

[0061] In the case of optional addition of chromium to the alloy, the total content of chromium and manganese is preferably limited. The total content preferably does not exceed 3.3% by weight, in particular does not exceed 3.15% by weight. In addition, the total content is at least 0.5% by weight, preferably at least 0.75% by weight.

[0062] Preferably, the steel optionally additionally contains boron in an amount of 0.001 wt. % to 0.005 wt. %. In particular, the B content does not exceed 0.004 wt. %.

[0063] Optionally, the steel may contain not more than 0.5% by weight of molybdenum, in particular not more than 0.1% by weight of molybdenum.

[0064] Furthermore, the steel may optionally contain not more than 0.5% by weight of nickel, preferably not more than 0.15% by weight of nickel.

[0065] Furthermore, the steel may optionally contain not more than 0.2% by weight of copper, preferably not more than 0.15% by weight of copper.

[0066] Furthermore, the steel may optionally contain one or more of the microalloying elements Nb, Ti and V. The optional Nb content is at least 0.02 wt.-% and at most 0.08 wt.-%, preferably at most 0.04 wt.-%. The optional Ti content is at least 0.01 wt.-% and at most 0.08 wt.-%, preferably at most 0.04 wt.-%. The optional V content is at most 0.1 wt.-%, preferably at most 0.05 wt.-%.

[0067] In the case of multiple additions of Nb, Ti and V elements in the alloy, the total content of Nb, Ti and V is preferably limited. The total content is preferably not more than 0.1% by weight, in particular not more than 0.068% by weight. In addition, the total content is preferably at least 0.015% by weight.

[0068] More preferably, the steel matrix is ​​a steel from the group of steels A to E, the chemical composition of which is shown in Table 10. Table 10 is to be understood as the element content of each steel of the group of steels A to E expressed in weight percentages. Minimum and maximum weight proportions are given here. For example, steel A thus contains a carbon content C of: 0.05 wt. % to 0.10 wt. %.

[0069] The above statements regarding the preferred steel base body also apply to the steel base body of the flat steel product described below, as well as to the described production method.

[0070] In a preferred variant of the steel component, the protective coating surface is mainly formed by Zn aggregates in metallic form and / or oxidized form. In the present application, when the protective coating surface has more than 50% (area percentage), preferably more than 70% of the area, the protective coating surface is mainly formed by Zn aggregates in metallic form and / or oxidized form. For example, this ratio can be determined by electron micrographs and subsequent image analysis. For each point, Al and Zn can be recorded based on the signal intensity, so that the zinc aggregates become obvious.

[0071] In a preferred variant of the steel component, the protective coating comprises a low silicon phase and a silicon-rich phase, wherein the silicon-rich phase is distributed in the low silicon phase in an island shape. The Zn content in the silicon-rich phase is less than 90%, preferably less than 80%, of the average Zn content of the protective coating. At the same time, the Zn content of the low silicon phase exceeds 105%, preferably exceeds 110%, of the average Zn content of the protective coating.

[0072] In other words, the ratio of the mass ratio of Zn in the silicon-rich phase (expressed in weight %) to the mass ratio of Zn in the entire protective coating (expressed in weight %) is less than 90%, preferably less than 80%. Similarly, the ratio of the mass ratio of Zn in the low-silicon phase (expressed in weight %) to the mass ratio of Zn in the entire protective coating (expressed in weight %) is greater than 105%, preferably greater than 110%.

[0073] Therefore, zinc enrichment occurs in the low-silicon phase, while the zinc content in the silicon-rich phase is below average.

[0074] In a specific configuration, the Si content in the low-silicon phase is less than 10 wt %, preferably less than 7 wt %, more preferably less than 5 wt %.

[0075] Another specific configuration is that the Si content in the silicon-rich phase is greater than 10 wt %, preferably greater than 12 wt %.

[0076] In the context of this application, the meaning of "island" refers to the arrangement of discrete incoherent areas surrounded by another material, that is, there are "islands" of a specific material in another material. In a vertical metallographic section, the aspect ratio of the length to the width of the "island" may be around 1:1. The length here is measured parallel to the surface, and the width is measured at right angles to the surface. Therefore, the "island" has a similar length and width. However, a larger aspect ratio may also occur, that is, the length is much greater than the width. The "island" therefore appears striped.

[0077] The object of the invention is also achieved by a flat steel product for hot forming, which consists of a steel substrate and an Al-based protective coating applied to the steel substrate, the steel substrate consisting of a steel containing 0.1% by weight to 3% by weight of Mn and optionally up to 0.01% by weight of B, the Al-based protective coating optionally having additional alloying components in a total weight ratio of up to 30% excluding iron and manganese. Furthermore, the weight ratio of Si in the protective coating as an additional alloying component excluding iron and manganese is 3% Si to 15% Si, in particular 6% Si to 12% Si, and the weight ratio of Mg in the protective coating as an additional alloying component excluding iron and manganese is 0.10% Mg to 0.50% Mg, preferably 0.1% Mg to 0.35% Mg. Furthermore, the weight ratio of Zn in the protective coating as an additional alloying component excluding iron and manganese is 0.4% Zn to 5% Zn, preferably 0.4% Zn to 2.3% Zn.

[0078] The protective coating therefore contains additional alloying elements in a proportion of up to 30%, preferably 20%, based on the total mass excluding iron and manganese, of which Si accounts for 3% to 15%, Mg for 0.10% to 0.50% and Zn for 0.4% to 2.3%.

[0079] In particular, the mass ratio of Mn is greater than 0.1 wt% and less than 2.5 wt%, preferably 0.2 wt% to 2.0 wt%, more preferably 0.4 wt% to 1.8 wt%. Even when applying a protective coating, a certain proportion of manganese may diffuse from the steel substrate into the protective coating to form an additional alloy component in the protective coating. This is the case in hot dip coating due to the high molten pool temperature.

[0080] In addition to Fe, Si, Mg, Zn and optionally Mn, the protective coating of the flat steel product preferably consists only of Al and unavoidable impurities. In the context of this application, an element is an unavoidable impurity in the protective coating if its mass fraction, excluding iron and manganese, is less than 0.5%. This definition only relates to unavoidable impurities in the protective coating. Standard technical limit values ​​apply to unavoidable impurities in the steel matrix mentioned later.

[0081] It was found that after hot forming, in addition to a Zn mass ratio of 0.4% excluding iron and manganese, the Zn content in the near-surface area is high enough to allow reliable phosphating. During the phosphating process, the zinc near the surface combines to form zinc phosphide, which provides better corrosion protection than the iron phosphate layer formed in other cases. In addition, zinc phosphate is a good base for paint adhesion.

[0082] The weight ratio of Zn in the protective coating as an additional alloying component, excluding iron and manganese, is preferably at least 0.6%, more preferably at least 1.0%, in particular at least 1.5%.

[0083] The higher the mass ratio of zinc excluding iron and manganese, the higher the zinc content in the near-surface area after hot forming and the better the phosphating properties, since more zinc phosphide and less iron phosphide are formed.

[0084] Therefore, a high Zn content of the first Zn-rich layer may be achieved in a procedurally reliable manner with a higher mass ratio of Zn excluding iron and manganese in the protective coating. Therefore, a higher mass ratio of Zn excluding iron and manganese in the protective coating is preferred.

[0085] However, zinc in the protective coating has the disadvantage of a relatively low melting point. During the production of steel components by hot forming, liquid Zn phases may form. These can firstly penetrate into the steel matrix, leading to cracking (liquid metal embrittlement), and secondly adhere to the forming tools or furnace rollers, leading to soiling and layer detachment. Therefore, the selected zinc content should not be too high. In experiments, it was found to be particularly advantageous if the mass proportion of Zn in the protective coating, excluding iron and manganese, does not exceed 2.3%, preferably not more than 1.8%.

[0086] An advantageous additional alloying component in the protective coating has been found to be magnesium, which has good alloying properties with Al protective coatings of the type discussed herein. The amount of Mg added should be adjusted to a magnesium mass ratio of at least 0.10%, preferably at least 0.15%, excluding iron and manganese. In particular, a magnesium mass ratio of less than 0.50%, less than 0.4%, or less than 0.35%, excluding iron and manganese, has been found in practice to be particularly advantageous. Magnesium added in small amounts to the protective coating has a higher affinity for oxygen than the main aluminum component of the protective coating. Even in the case of small amounts of magnesium, a thin oxide layer forms on the surface of the protective coating, which covers the aluminum between it and the steel substrate. During the heating process required for hot forming of the flat steel product, this thin oxide layer prevents the aluminum from reacting with the moisture present in the furnace atmosphere used to heat the flat steel product. In this way, oxidation of the aluminum in the coating and the associated release of hydrogen (which can diffuse into the coating and the steel substrate of the flat steel product) can be effectively prevented. Surprisingly, this is the case even if the Al-based coating partially melts due to heating and its surface breaks up, so that the molten coating material comes into contact with the furnace atmosphere. In particular, in the case of relatively long annealing times, the hydrogen concentration in the component hot-formed from the flat steel product is lower in the case of the flat steel product according to the invention than in conventional flat steel products with an aluminum coating.

[0087] Alloying with magnesium therefore has the advantage of reducing the ingress of hydrogen into the steel matrix. If the local hydrogen concentration is very high, this can weaken the bonding at the grain boundaries of the steel matrix microstructure, causing cracks along the grain boundaries during use due to the stresses generated.

[0088] In a particularly preferred flat steel product, the protective coating is applied by hot-dip coating. Hot-dip coating (also known in the technical term "hot-dip aluminizing") is a particularly economical method for applying the protective coating.

[0089] The thickness of the protective coating is generally at least 5 μm and at most 35 μm, in particular at least 10 μm and at most 25 μm.

[0090] The object of the present invention is also achieved by a method for producing a phosphating steel component, the method comprising the following steps:

[0091] - heating the above-mentioned flat steel product to the heating temperature of the hot forming operation and keeping it at this heating temperature so that diffusion leads to Zn enrichment in the near-surface region of the protective coating, in particular the formation of metallic Zn and oxidic Zn aggregates;

[0092] - hot forming the coated steel substrate into a steel component;

[0093] -Phosphating of hot-formed steel components.

[0094] Heating the above-mentioned flat steel product to the heating temperature of the hot forming operation and keeping it at the heating temperature leads to the accumulation of Zn in the near-surface region. In particular, this forms a first Zn-rich layer, as has already been explained in the case of steel components, and forms Zn oxide and / or metallic Zn accumulations on the surface of the protective coating, as has also been explained in the case of steel components. The enrichment of zinc in the near-surface region significantly improves the phosphating properties, in particular the formation of zinc phosphate instead of iron phosphate.

[0095] Preferably, the heating temperature is 830° C. to 980° C., preferably 830° C. to 910° C. Furthermore, the holding time of the flat steel product at the heating temperature is at least 1 minute and at most 18 minutes. The heating and holding are carried out in a furnace.

[0096] Thermoforming specifically includes the following two steps:

[0097] - taking the flat steel product out of the furnace and placing it into a forming tool;

[0098] - Forming the flat steel product into a steel component in a forming tool.

[0099] To avoid significant heat losses, the transfer time between the furnace and the forming tool is usually no more than 10 seconds.

[0100] During the forming operation, the flat steel product can optionally be cooled in the forming tool at a cooling rate of 20 K / s to 1000 K / s, preferably 25 K / s to 500 K / s, in order to harden the steel matrix.

[0101] Optionally, the flat steel product in the forming tool can first be formed into a steel component, and then the steel component can be cooled at a cooling rate of 20 K / s to 1000 K / s, preferably 25 K / s to 500 K / s, in order to harden the steel matrix.

[0102] In addition, the object of the present invention is also achieved by a method for producing a phosphating steel component, the method comprising the following steps:

[0103] - providing a steel matrix consisting of a steel having 0.1 wt.-% to 3 wt.-% Mn and optionally up to 0.01 wt.-% B;

[0104] - hot-dip coating of a steel substrate by melt with an Al-based protective coating having an additional alloy component of up to 30% by weight, excluding iron and manganese, wherein the Si as an additional alloy component in the protective coating has a weight ratio of 3% Si to 15% Si, in particular 6% Si to 12% Si, excluding iron and manganese

[0105] Si, wherein the mass ratio of Mg in the protective coating as an additional alloying component, excluding iron and manganese, is at most 1%, and wherein the mass ratio of Zn in the protective coating as an additional alloying component, excluding iron and manganese, is from 0.4% Zn to 25.0% Zn,

[0106] - heating the coated steel substrate to the heating temperature of the hot forming operation and keeping it at this heating temperature so that diffusion leads to Zn enrichment at the surface of the protective coating, in particular forming agglomerates of metallic Zn and oxidized Zn;

[0107] - hot forming the coated steel substrate into a steel component;

[0108] -Phosphating of hot-formed steel components.

[0109] The mass ratios here, excluding iron and manganese, have preferred minimum and maximum values, the advantages of which have already been explained above in relation to the steel components.

[0110] In particular, a steel substrate is hot-dip coated from a melt to have an Al-based protective coating having an additional alloy component in a mass ratio of up to 30% excluding iron and manganese, wherein the additional alloy component comprises Si, Mg, and Zn, wherein the mass ratio of Si in the protective coating as an additional alloy component excluding iron and manganese is 3% Si to 15% Si, specifically 6% Si to 12% Si; the mass ratio of Mg in the protective coating as an additional alloy component excluding iron and manganese is 0.10% Mg to 0.50% Mg, preferably 0.1% Mg to 0.35% Mg, and the mass ratio of Zn in the protective coating as an additional alloy component excluding iron and manganese is 0.4% Zn to 5% Zn, preferably 0.4% Zn to 2.3% Zn.

[0111] Heating the above-mentioned flat steel products to the heating temperature of the hot forming operation and keeping them at the heating temperature leads to the accumulation of Zn in the near-surface region. In particular, this forms a first Zn-rich layer, as has already been explained in the case of steel components, and leads to the formation of accumulations of oxidized Zn and metallic Zn on the surface of the protective coating, as has also been explained in the case of steel components. This enrichment of zinc in the near-surface region significantly improves the phosphating properties, in particular the formation of zinc phosphate instead of iron phosphate.

[0112] Preferably, the heating temperature is 830° C. to 980° C., preferably 830° C. to 910° C. In addition, the holding time of the flat steel product at the heating temperature is at least 1 minute and at most 18 minutes. The heating and holding are carried out in a furnace. The hot forming operation comprises in particular the following two partial steps:

[0113] - taking the flat steel product out of the furnace and placing it into a forming tool;

[0114] - Forming the flat steel product into a steel component in a forming tool.

[0115] To avoid significant heat losses, the transfer time between the furnace and the forming tool is usually no more than 10 seconds.

[0116] During the forming operation, the flat steel product can optionally be cooled in the forming tool at a cooling rate of 20 K / s to 1000 K / s, preferably 25 K / s to 500 K / s, in order to harden the steel matrix.

[0117] Furthermore, the flat steel product in the forming tool can first be formed into a steel component, and then the steel component can be cooled at a cooling rate of 20 K / s to 1000 K / s, preferably 25 K / s to 500 K / s, to harden the steel matrix.

[0118] Phosphating refers to the full-area phosphating of steel components, depositing a phosphating layer with a thickness of, for example, 0.5 μm to 3.0 μm on the steel components. The phosphating layer can increase the adhesion of the paint and reduce the corrosion of the steel substrate when the paint is damaged.

[0119] In a specific configuration of the above-mentioned phosphating steel component production method, during the heating and holding process, diffusion leads to the formation of a low-silicon phase and a silicon-rich phase, wherein the silicon-rich phase is distributed in the low-silicon phase in an island shape. The zinc content in the low-silicon phase accounts for 25% to 60% of the zinc content in the melt, preferably 30% to 50%.

[0120] In another specific configuration of the above-mentioned method for producing a phosphated steel component, the heating temperature is higher than the Ac3 temperature, so that the microstructure of the steel matrix is ​​in the form of austenite. In addition, the coated steel matrix is ​​quenched after or during hot forming, so that a hardness microstructure is formed in the steel matrix microstructure of the flat steel product.

[0121] The present invention will be described in detail below through the following embodiments in conjunction with the accompanying drawings. The accompanying drawings show:

[0122] Figure 1 Scanning electron micrograph of the surface of a hot-formed steel component before phosphating;

[0123] Figure 2 Scanning electron micrograph of the surface of a hot-formed steel component after phosphating;

[0124] Figure 3 Schematic cross section.

[0125] The steel substrate used is a steel plate having a thickness of 1.5 mm, which is composed of steel having the composition of Table 1 and the remainder being iron and inevitable impurities. Therefore, this steel belongs to Group D steel in Table 10.

[0126] Table 1: Steel composition of steel matrix (weight %)

[0127] C Si Mn P S Al Ti Cr B 0.22 0.25 1.25 0.016 0.004 0.043 0.029 0.20 0.003

[0128] On the basis of this steel substrate, four different variants were investigated in detail. For this purpose, an aluminum-based protective coating was first applied to the steel substrate by hot-dip coating. The thickness of the protective coating was 20 μm in each case. Table 2 below lists the target composition of the corresponding melt, the remainder consisting of iron and unavoidable impurities:

[0129] Table 2: Melt composition

[0130]

[0131] For the steel substrates coated in this way, GD-OES (Glow Discharge Optical Emission Spectroscopy) was then used to determine the element content in the protective coating. In this way, the mass ratios of the individual elements, excluding iron and manganese, could be determined. The results are shown in Table 3.

[0132] Table 3: Mass ratios of iron and manganese in the protective coating of the coated steel substrate (flat steel product)

[0133] Variants Zn Al Si Mg A 0.2% 88.4% 11.4% 0.0%* B 1.0% 87.5% 11.2% 0.3% C 1.7% 87.7% 10.3% 0.3% D 0.3% 93.8% 5.8% 0.1%

[0134] *Content below detection limit

[0135] Therefore, variant A does not conform to the present invention because the weight ratio of zinc excluding iron and manganese is 0.2%, which is beyond the scope of the present invention. This variant can be used as a comparative sample.

[0136] In addition to the element content of the entire protective coating, GD-OES can also be used to determine the element content of the near-surface area (i.e., the uppermost 500nm). The results are shown in Table 4 below:

[0137] Table 4: Element contents of protective coatings on applied steel substrates in the near-surface region

[0138]

[0139] *Content below detection limit

[0140] The flat steel product thus prepared (i.e. the coated steel substrate) is then heated to a heating temperature of 920°C, which is higher than Ac3. The holding time is 5 to 10 minutes at this heating temperature and then hot formed into a steel component. Heating and holding are carried out in a roller hearth furnace with closed-loop dew point control. The dew point is set to 15°C. The entire process is carried out in an ambient atmosphere. Subsequently, the flat steel product is formed in a tool to obtain a steel component and quenched to room temperature. The cooling rate exceeds 50°C per second. The process parameters of the heat treatment are summarized again in Table 5 below:

[0141] Table 5: Heat treatment process parameters

[0142]

[0143] The next step will be to reanalyze the steel components thus produced. This involves first determining the elemental content of the protective coating by GD-OES and then determining the mass ratio excluding iron and manganese.

[0144] Table 6: Mass ratio of protective coating on steel components excluding iron and manganese

[0145] Variants Zn Al Si Mg A 0.1% 90.2% 9.7% 0.0%* B 1.6% 89.0% 9.2% 0.2% C 1.5% 88.9% 9.3% 0.3% D 0.6% 89.0% 10.2% 0.2%

[0146] *Content below detection limit

[0147] Here, it is obvious that variant A also does not conform to the present invention, because the mass ratio of zinc excluding iron and manganese is 0.1%, which is beyond the scope of the present invention.

[0148] In addition to the element content in the entire protective coating, GD-OES was also used to determine the element content in the near-surface region (i.e., the uppermost 500 nm). The results are shown in Table 7 below:

[0149] Table 7: Element contents of protective coatings on steel components in the near-surface area

[0150]

[0151] It is clear that variants B, C and D have a first Zn-rich layer with a Zn content that is higher than the average Zn content of the protective coating. In any case, the average Zn content of the protective coating is lower than the zinc content of the melt and, in variants B and C, for example, the Zn content is therefore below 2.26% by weight. As a result of diffusion processes, the average Zn content can only fall further, since there is no supply of Zn. Furthermore, in all three variants B, C and D, the zinc content of the first Zn-rich layer is above 5%. Zinc is significantly enriched in the near-surface region. Figure 1 An electron micrograph of the protective coating surface is shown, taking variant B as an example. It can be clearly seen that the surface is mainly formed by Zn aggregates in metallic and / or oxidized form, which are distributed on the surface in the form of small crystals. By image analysis, the area ratio of zinc aggregates in variant B is 56%, while variants C and D are 58% and 16%, respectively.

[0152] Figure 2 An electron micrograph of the surface of the protective coating after phosphate treatment is shown for example in variant B. The homogeneous, continuous phosphate layer is clearly visible.

[0153] Figure 3A schematic cross-sectional view of variant B that can be recorded by scanning electron microscopy is shown. The steel component 11 shown is composed of a steel substrate 13 and a protective coating 15. The protective coating 15 contains a low silicon phase A and a silicon-rich phase R, and the silicon-rich phase R is distributed in the low silicon phase A in an island shape. The Zn content of the two phases was determined by energy dispersive X-ray spectroscopy (EDX). It was found that zinc was also enriched in the low silicon phase. The results are shown in Table 8 below.

[0154] Table 8: Zinc and silicon contents of silicon-rich and low-silicon phases

[0155]

[0156] It is clear that the Zn content of the low silicon phase is 25% to 60% of the Zn content of the melt. In variant B, the ratio of the Zn content of the low silicon phase to the melt is 30.1%, in variant C it is 26.5% and in variant D it is 46.1%.

[0157] The hot-formed steel components are then phosphated in the next step. For this purpose, the samples are subjected to a standard industrial phosphating process. This includes the following steps:

[0158] - Degreasing in a degreasing tank at 60°C for 150 seconds. The degreasing agent used was Chemetall Gardoclean S5176.

[0159] - The surface was activated for 30 seconds using Chemetall Gardolene ZL 6. The activator concentration was 6 g / l.

[0160] - Phosphating in a phosphating bath at 60°C for 150 seconds. The phosphating agent used is Chemetall Gardobond24.

[0162] After phosphating, the element content in the near-surface area (i.e., the uppermost 500 nm) was measured again. The results are shown in Table 9 below:

[0163] Table 9: Element contents in the near-surface area of ​​phosphated steel component protective coatings

[0164]

[0165] It is also clear that the zinc content of the first Zn-rich layer near the surface of variants B, C and D is higher than the average zinc content of the protective coating listed in Table 6. In addition, the zinc content of the first Zn-rich layer of variants B, C and D is above 5%. These values ​​are even higher than before phosphating. However, this is because the material used during the phosphating process makes the measurement range of 500nm thickness more biased towards the area with extremely high zinc content.

[0166] Furthermore, it is clearly seen that variants B, C and D have better phosphatization properties. The near-surface phosphorus content is more than 5 times higher than that of comparative sample A.

[0167] Table 10: Steel composition

Claims

1. A steel component (11), comprising a steel substrate (13) and an Al-based protective coating (15) applied on the steel substrate (13); the steel substrate (13) is composed of a steel containing 0.1 wt. % to 3 wt. % Mn and optionally up to 0.01 wt. % B; the protective coating (15) has additional alloy components with a total weight ratio of up to 30% excluding iron and manganese, wherein the additional alloy components include Si, Mg and Zn; wherein the weight ratio of Si as an additional alloy component in the protective coating, excluding iron and manganese, is 3% Si to 15% Si, in particular 6% Si to 12% Si; wherein the weight ratio of Mg as an additional alloy component in the protective coating, excluding iron and manganese, is up to 1.0%; wherein the mass ratio of Zn as an additional alloying component in the protective coating is 0.4% Zn to 25.0% Zn excluding iron and manganese; The protective coating (15) has a first Zn-rich layer near the surface, the Zn content of the first Zn-rich layer is higher than the average Zn content of the protective coating, and the Zn content of the first Zn-rich layer is greater than 5 wt %; Wherein the layer thickness of the protective coating is at least 5 μm, the near-surface layer extends over a 500 nm thick region adjacent to the surface of the protective coating.

2. The steel member according to claim 1, characterized in that The mass ratio of Mg as an additional alloying component in the protective coating, excluding iron and manganese, in total is at least 0.10%, preferably at least 0.15%, and / or the mass ratio of Mg as an additional alloying component in the protective coating, excluding iron and manganese, in total is at most 0.50%, preferably at most 0.35%, and / or the mass ratio of Zn as an additional alloying component in the protective coating, excluding iron and manganese, in total is at least 0.6%, preferably at least 1.0%, and / or the mass ratio of Zn as an additional alloying component in the protective coating, excluding iron and manganese, in total is at most 5.0%, preferably at most 2.3%, and / or the Zn content of the first Zn-rich layer is more than 10.0 wt.-%, preferably more than 18 wt.-%.

3. The steel member according to claim 1 or 2, characterized in that: The surface of the protective coating is mainly formed by Zn aggregates in metallic and / or oxidized form.

4. The steel member according to any one of claims 1 to 3, characterized in that The protective coating (15) comprises a low silicon phase (A) and a silicon-rich phase (R), wherein the silicon-rich phase is distributed in the low silicon phase in an island shape, wherein the Zn content of the silicon-rich phase is lower than 90% of the average Zn content of the protective coating, and the Zn content of the low silicon phase is higher than 105% of the average Zn content of the protective coating.

5. The steel member according to claim 4, characterized in that The Si content in the low-silicon phase is less than 10 wt %, preferably less than 7 wt %, and more preferably less than 5 wt %.

6. The steel member according to claim 4 or 5, characterized in that: The Si content in the silicon-rich phase is greater than 10 wt %, preferably greater than 12 wt %.

7. A flat steel product for hot forming, comprising a steel substrate (13) and an Al-based protective coating (15) applied to the steel substrate (13), wherein the steel substrate (13) consists of a steel containing 0.1% to 3% by weight of Mn and optionally up to 0.01% by weight of B, wherein the Al-based protective coating (15) has additional alloy components with a total mass ratio of up to 30% excluding iron and manganese, wherein the additional alloy components include Si, Mg, and Zn; wherein the mass ratio of Si as an additional alloy component in the protective coating excluding iron and manganese is 3% Si to 15% Si, in particular 6% Si to 12% Si; wherein the mass ratio of Mg as an additional alloy component in the protective coating excluding iron and manganese is 0.10% Mg to 0.50% Mg, preferably 0.1% Mg to 0.35% Mg; characterized in that The weight ratio of Zn as an additional alloying component in the protective coating, excluding iron and manganese, is 0.4% Zn to 5% Zn, preferably 0.4% Zn to 2.3% Zn.

8. The flat steel product according to claim 7, characterized in that The protective coating (15) is applied by hot dip coating.

9. A method for producing a phosphating steel component, comprising the following steps: - heating the flat steel product according to claim 7 to a heating temperature of at least 700° C. for a hot forming operation and keeping it at said heating temperature so that diffusion leads to Zn enrichment and formation of accumulations of metallic Zn and oxidized Zn in the near-surface region of said protective coating; - hot forming the coated steel substrate into a steel component; -Phosphating of hot formed steel components.

10. A method for producing a phosphating steel component, comprising the following steps: - providing a steel matrix consisting of a steel having 0.1 wt.-% to 3 wt.-% Mn and optionally up to 0.01 wt.-% B; - hot-dip coating of a steel substrate by melt with an Al-based protective coating (15), the Al-based protective coating (15) having additional alloying components in a total mass ratio of up to 30% excluding iron and manganese, wherein the additional alloying components include Si, Mg and Zn; wherein the mass ratio of Si in the protective coating as an additional alloying component excluding iron and manganese is 3% Si to 15% Si, in particular 6% Si to 12% Si; wherein the mass ratio of Mg in the protective coating as an additional alloying component excluding iron and manganese is up to 1%; wherein the mass ratio of Zn as an additional alloying component in the protective coating, excluding iron and manganese, is 0.4% Zn to 25.0% Zn, in particular 0.4% Zn to 5% Zn, - heating the coated steel substrate to a heating temperature of at least 700° C. for a hot forming operation and maintaining it at said heating temperature so that diffusion leads to Zn enrichment at the surface of said protective coating and formation of accumulations of metallic Zn and oxidized Zn; - hot forming the coated steel substrate into a steel component; -Phosphating of hot formed steel components.

11. The method according to claim 9 or 10, characterized in that During the heating and holding process, diffusion results in the formation of a low silicon phase (A) and a silicon rich phase (R), wherein the silicon rich phase is distributed in the low silicon phase in an island shape, and wherein the Zn content of the low silicon phase is 25% to 60% of the Zn content of the melt.

12. The method according to any one of claims 9 to 11, characterized in that The heating temperature is higher than the Ac3 temperature, so that the microstructure of the steel matrix is ​​austenitic, and the coated steel matrix (13) is quenched after or during hot forming, so that a hardness microstructure is formed in the microstructure of the steel matrix of the flat steel product.