Thin film masking agent, thin film forming method using same, semiconductor substrate manufactured by method, and semiconductor device

By using film shielding agents and precursor compounds of specific electronegative elements on semiconductor substrates, combined with physical adsorption or chemical adsorption technology, the uniformity and impurities of film formation on complex structural substrates at high temperatures are solved, and high-step coverage is achieved Improved properties and membrane quality.

CN118922582APending Publication Date: 2024-11-08SOULBRAIN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026980.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-10-25
Filing Date
2023-03-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Under high temperature conditions, it is difficult for the prior art to form a uniform thickness and seamless film on a semiconductor substrate with complex structures, and impurities are prone to residual, affecting the step coverage and film quality.

Method used

Using thin film shielding agents containing specific electronegative elements, improves the deposition of metal oxide films or non-metal oxide films by providing strong and stable physical adsorption or chemical adsorption on the surface of the substrate, combining compounds of specific chemical formulas and precursor compounds. The step coverage and thickness uniformity of the deposition layer and reduce process by-products by-products through specific process steps and vapor deposition methods.

Benefits of technology

A seamless film with high step coverage and thickness uniformity is achieved under high temperature conditions, reducing impurity residues, improving film quality and electrical characteristics, and improving the density and dielectric characteristics of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922582A_ABST
    Figure CN118922582A_ABST
Patent Text Reader

Abstract

The present invention relates to a thin film masking agent, a composition for forming a thin film comprising the same, a method for forming a thin film using the same, a semiconductor substrate manufactured by the method, and a semiconductor device, in which the thin film masking agent is applied to improve the reaction speed and appropriately reduce the growth rate of the thin film. Therefore, even if a thin film is formed on a substrate with a complex structure under a high-temperature condition, the step coverage and the thickness uniformity of the thin film can be greatly improved to form a seamless thin film, impurities are reduced, and the film quality is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thin film shielding agent, a thin film forming method using the same, a semiconductor substrate manufactured by the method, and a semiconductor device, and more specifically to a thin film shielding agent, a thin film forming method using the same, and a semiconductor substrate manufactured by the method, wherein strong and stable physical adsorption or chemical adsorption is provided to the surface of a deposited layer on the surface of the substrate, so that even when a thin film is formed on a substrate with a complex structure under high temperature conditions, a seamless thin film with greatly improved step coverage and thickness uniformity of the thin film can be provided, and impurities can be greatly reduced and film quality can be improved. Background Art

[0002] As the integration of memory and non-memory semiconductor devices increases, the fine structure of the substrate becomes increasingly complex.

[0003] As an example, the ratio of the width to the depth of the fine structure (hereinafter also referred to as the "aspect ratio") increases to above 20:1 or above 100:1. The larger the aspect ratio, the more difficult it is to form a deposition layer of uniform thickness along the surface of the complex fine structure.

[0004] Therefore, the step coverage (step coverage) that defines the thickness ratio of the deposited layers formed on the upper and lower parts in the depth direction of the fine structure has remained at around 90%, making it increasingly difficult to express the electrical characteristics of the component, and therefore its importance is gradually increasing. The above-mentioned step coverage of 100% means that the thickness of the deposited layers formed on the upper and lower parts of the fine structure is the same, so it is necessary to develop a technology that makes the step coverage as close to 100% as possible.

[0005] Taking a NAND word line made of metal as an example, when filling a very narrow gap (trench), if the metal content deposited at the upper and lower parts of the gap is different and mainly deposited at the upper part, a seam defect with a void inside the gap may be caused.

[0006] In order to produce a step coverage (step coverage) close to 100%, that is, as a variable to determine whether the thickness of the atomic layer deposited on the upper and lower parts of the pattern is the same, it is necessary to induce a difference in the adsorption density of the masking agent to the precursor compound so that the precursor compound occupies more positions to be adsorbed in the upper part of the pattern and occupies less as it goes down.

[0007] On the other hand, in order to achieve excellent film quality, it is also necessary to overcome the problem that the masking agent is difficult to adsorb onto the substrate as the deposition temperature increases.

[0008] As a specific example, according to Korean Patent Publication No. 2021-0059332, which uses ether as a shielding material, although a thin film shielding effect can be provided, the problem of residual oxygen or carbon impurities in the deposited layer may occur due to hydrogen (a representative reactant for forming a metal layer) or ammonia (a representative reactant for forming a metal nitride layer).

[0009] Therefore, it is necessary to develop a method for forming a seamless thin film that can effectively form a thin film with a complex structure even at high temperatures, has low residual impurities, and significantly improves step coverage and thickness uniformity of the thin film, and a semiconductor substrate manufactured thereby. Summary of the invention

[0010] Problem that the invention aims to solve

[0011] In order to solve the problems in the prior art as described above, the object of the present invention is to provide a thin film shielding agent and a thin film forming composition containing the same, which is not affected by the deposition temperature and provides strong and stable physical adsorption or chemical adsorption to the surface of the deposited layer on the surface of the substrate, so that even when a thin film is formed on a substrate with a complex structure under high temperature conditions, the step coverage and the thickness uniformity of the thin film can be greatly improved to form a seamless thin film, and impurities can be reduced, thereby improving the film quality.

[0012] An object of the present invention is to provide a thin film forming method and a semiconductor substrate manufactured thereby, which improve the crystallinity and oxidation fraction of the thin film, thereby improving the density, electrical properties and dielectric properties of the thin film.

[0013] The above-mentioned object and other multiple objects of the present invention can be fully achieved by the present invention described below.

[0014] Means used to solve problems

[0015] In order to achieve the above-mentioned purpose, the present invention provides a thin film shielding agent, which is used when depositing a metal oxide film or a non-metal oxide film on a substrate, and contains at least one element whose electronegativity is between the electronegativity of the metal or non-metal constituting the above-mentioned oxide film and the electronegativity of oxygen, and is used to shield the above-mentioned deposition.

[0016] The above-mentioned metal or non-metal can be one or more selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd.

[0017] The film shielding agent may be a compound containing four or more elements having an electronegativity ranging from 2.1 to 3.1.

[0018] The film shielding agent may be one or more selected from compounds having a structure represented by the following Chemical Formula 1,

[0019] [Chemical formula 1]

[0020]

[0021] (In the above chemical formula 1, R1 is H, OH, CH3, OCH3, OCH2CH3, OCH2CH2CH3, or an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 1 to 5 carbon atoms, or an alkynyl group having 1 to 5 carbon atoms, and X is m is an integer from 0 to 4.)

[0022] The refractive index of the thin film shielding agent may be 1.4 to 1.5, 1.41 to 1.48, or 1.41 to 1.47.

[0023] The film shielding agent may be one or more compounds selected from the group consisting of the following chemical formulas 1-1 to 1-9:

[0024] [Chemical Formula 1-1] to [Chemical Formula 1-9]

[0025]

[0026] In addition, the present invention provides a thin film shielding agent, comprising a precursor compound constituting a thin film deposition layer and a thin film shielding agent, wherein the thin film shielding agent is the thin film shielding agent, and the precursor compound is a compound represented by the following Chemical Formula 2.

[0027] [Chemical formula 2]

[0028]

[0029] (In the above chemical formula 2, M is one or more selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd, L 1 , L 2 , L 3 and L 4 As -H, -X, -R, -OR, -NR or Cp (cyclopentadienyl), they may be the same or different, wherein -X is F, Cl, Br or I, -R is C1-C10 alkyl, C1-C10 alkenyl or C1-C10 alkynyl, which may be linear or cyclic, and the above L 1, L 2 , L 3 and L 4 It can be formed into 2 to 6 according to the oxidation valence of the central metal (M).

[0030] For example, when the central metal is divalent, L 1 and L 2 It can act as a ligand to bind to the central metal. When the central metal is hexavalent, L 1 , L 2 , L 3 , L 4 , L 5 , L 6 Can be combined with the central metal, equivalent to L 1 ~L 6 The ligands may be the same as or different from each other.

[0031] The thin film shielding agent provides a shielding area for the oxide film, nitride film, metal film or their selective thin films, and the shielding area can be formed on the entire substrate or a part of the substrate on which the oxide film, nitride film, metal film or their selective thin films are formed.

[0032] When the total area of ​​the entire substrate or a portion of the substrate is set to 100%, the shielded area occupies 10 to 95% of the area, and the unshielded area may occupy the remaining area.

[0033] The above-mentioned thin film can improve the step coverage during the formation of a stacked film of one or more selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd.

[0034] The above-mentioned thin film can be used as an anti-diffusion film, an etching stopper film, an electrode film, a dielectric film, a gate insulating film, a blocking oxide film, or a charge trap.

[0035] In addition, the present invention provides a thin film forming method, which includes the following steps: injecting one or more thin film shielding agents selected from compounds having a structure represented by the following Chemical Formula 1 and a precursor compound into a chamber to form a deposition layer on a loading substrate.

[0036] [Chemical formula 1]

[0037]

[0038] (In the above chemical formula 1, R1 is H, OH, CH3, OCH3, OCH2CH3, OCH2CH2CH3, or an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 1 to 5 carbon atoms, or an alkynyl group having 1 to 5 carbon atoms, and X is m is an integer from 0 to 4.

[0039] The above chamber may be an ALD chamber, a CVD chamber, a PEALD chamber or a PECVD chamber.

[0040] The precursor compound and the film masking agent may be independently delivered into the chamber by vapor flow control (VFC), direct liquid injection (DLI) or liquid delivery system (LDS).

[0041] The above-mentioned thin film can be a silicon nitride film, a silicon oxide film, a titanium nitride film, a titanium oxide film, a tungsten nitride film, a molybdenum nitride film, a hafnium oxide film, a zirconium oxide film, a tungsten oxide film or an aluminum oxide film.

[0042] The deposition rate reduction rate of the thin film shielding agent represented by the following Mathematical Formula 1 may be 20% or more.

[0043] [Mathematical formula 1]

[0044] Deposition rate (DR) reduction rate = [{(DR i )-(DR f )} / (DR i )]×100

[0045] (In the above mathematical formula, DR (Deposition rate, ) is the rate of film deposition. When depositing a film formed from a precursor and a reactant, DR i Initial deposition rate is the deposition rate of a thin film without the use of a film shielding agent. r The final deposition rate is the deposition rate of the film formed by adding the oxide film shielding agent during the above process. The deposition rate (DR) is the value measured by an ellipsometer at room temperature and pressure for a film with a thickness of 3 to 30 nm. The unit used is )

[0046] The above-mentioned thin film masking agent can provide a replacement region for an oxide film, a nitride film, a metal film, or a selective thin film thereof.

[0047] The replacement region is formed on the entire substrate or a portion of the substrate on which the oxide film, nitride film, metal film or a selective thin film thereof is formed.

[0048] When the total area of ​​the entire substrate or a part of the substrate is set to 100%, the ligand adsorbed region occupies 10 to 95% of the area, and the ligand non-adsorbed region may occupy the remaining area.

[0049] When the total area of ​​the entire substrate or a part of the substrate is set to 100%, the first ligand adsorption area occupies 10-95% of the area, the second ligand adsorption area occupies 10-95% of the residual area, and the ligand non-adsorbed area can occupy the remaining area.

[0050] The above-mentioned thin film can be a stacked film of one or more selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd.

[0051] The above-mentioned thin film is used as an anti-diffusion film, an etching stopper film, an electrode film, a dielectric film, a gate insulating film, a blocking oxide film or a charge trap, and can improve the step coverage during its formation.

[0052] The precursor compound used in the above-mentioned thin film forming method may be a compound represented by Chemical Formula 2 below.

[0053] [Chemical formula 2]

[0054]

[0055] (In the above chemical formula 2, M is one or more selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd, L 1 , L 2 , L 3 and L 4 -H, -X, -R, -Cp, -OR, -NR or Cp (cyclopentadienyl) may be the same or different, wherein -X is F, Cl, Br or I, -R is C1-C10 alkyl, C1-C10 alkenyl or C1-C10 alkynyl, and may be linear or cyclic, and the above L 1 , L 2 , L 3 and L 4 It can be formed into 2 to 6 according to the oxidation valence of the central metal (M).

[0056] In the above chemical formula 2, L 1 , L 2 , L 3 and L 4-H, -Cp or -R may be the same as or different from each other, wherein -R may be a C1-C10 alkyl, a C1-C10 alkenyl or a C1-C10 alkynyl, and may be linear or cyclic.

[0057] In the above chemical formula 2, L 1 , L 2 , L 3 and L 4 -H, -Cp, -OR, -NR or Cp (cyclopentadienyl) may be the same as or different from each other, wherein -R may be H, C1-C10 alkyl, C1-C10 alkenyl or C1-C10 alkynyl, iPr or TBu.

[0058] In the above chemical formula 2, L 1 , L 2 , L 3 and L 4 -H, -Cp or -X may be the same as or different from each other, wherein -X may be F, Cl, Br or I.

[0059] In addition, the present invention provides a thin film forming method, which includes: step i), vaporizing the above-mentioned thin film masking agent to mask the surface of the substrate loaded in the chamber; step ii), using a purge gas to perform a first purge on the inside of the above-mentioned chamber; step iii), vaporizing the precursor compound and adsorbing it in an area away from the masking area; step iv), using a purge gas to perform a second purge on the inside of the above-mentioned chamber; step v), supplying a reaction gas to the inside of the above-mentioned chamber; and step vi), using a purge gas to perform a third purge on the inside of the above-mentioned chamber.

[0060] The above-mentioned precursor compound, as a molecule formed by one or more selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd, can be a precursor having a vapor pressure greater than 0.01mTorr and less than or equal to 100Torr under a temperature condition of 25°C.

[0061] The chamber may be an atomic layer deposition (ALD) chamber, a chemical vapor deposition (CVD) chamber, a plasma enhanced atomic layer deposition (PEALD) chamber or a plasma enhanced chemical vapor deposition (PECVD) chamber.

[0062] The above-mentioned thin film forming method may include the following steps: after vaporizing and injecting the thin film shielding agent or precursor compound, performing plasma post-treatment.

[0063] The amount of the purge gas introduced into the chamber in the above step ii) and the above step iv) may be 10 to 100,000 times the volume of the thin film shielding agent introduced.

[0064] The reaction gas may be an oxidizing agent, a nitriding agent or a reducing agent. The reaction gas, the thin film shielding agent and the precursor compound may be delivered into the chamber by a VFC method, a DLI method or a LDS method.

[0065] The above-mentioned thin film can be a silicon nitride film, a silicon oxide film, a titanium nitride film, a titanium oxide film, a tungsten nitride film, a molybdenum nitride film, a hafnium oxide film, a zirconium oxide film, a tungsten oxide film or an aluminum oxide film.

[0066] The substrate loaded in the chamber is heated to 100-800° C., and the ratio of the amount (mg / cycle) of the thin film shielding agent to the amount of the precursor compound fed into the chamber may be 1:1-1:20.

[0067] In addition, the present invention provides a semiconductor substrate including a thin film manufactured by the above-mentioned thin film forming method.

[0068] The above-mentioned film can be a multi-layer structure of two layers or three layers or more.

[0069] In addition, the present invention provides a semiconductor device, which includes the semiconductor substrate mentioned above.

[0070] The semiconductor substrate may be low resistive metal gate interconnects, high aspect ratio 3D metal-insulator-metal (MIM) capacitors, DRAM trench capacitors, 3D gate-all-around (GAA) or 3D NAND flash memory.

[0071] Effects of the Invention

[0072] The present invention provides a thin film shielding agent which can effectively shield the adsorption on the substrate surface to improve the reaction speed and appropriately reduce the film growth rate, thereby improving the step coverage even when a thin film is formed on a substrate with a complex structure under high temperature conditions.

[0073] In addition, when forming a thin film, process byproducts can be more effectively reduced, corrosion and degradation can be prevented, and the film quality can be modified to improve the crystallinity of the thin film, thereby improving the electrical properties of the thin film.

[0074] In addition, the step coverage and density of the thin film can be improved, and further, a thin film forming method using the thin film and a semiconductor substrate manufactured thereby are provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0075] Figure 1 This is a diagram schematically showing the deposition process sequence of the present invention mainly in one cycle.

[0076] Figure 2 TEM photographs are taken of the thickness of the upper part (100 nm downward from the top) and the lower part (100 nm upward from the bottom) of the cross section of the oxide film deposited according to Comparative Example 1 without using a thin film shielding agent, as well as the thickness of the upper part (100 nm downward from the top) and the lower part (100 nm upward from the bottom) of the cross section of the oxide film deposited using a thin film shielding agent.

[0077] Figure 3 The TEM photographs are taken of the thickness of the upper part (100 nm downward from the top) and the lower part (100 nm upward from the bottom) of the cross section of the oxide film deposited by using a thin film shielding agent according to Example 1, as well as the thickness of the upper part (100 nm downward from the top) and the lower part (100 nm upward from the bottom) of the cross section of the oxide film deposited by using a thin film shielding agent.

[0078] Figure 4 The TEM photographs are taken of the thickness of the upper part (100 nm downward from the top) and the lower part (100 nm upward from the bottom) of the cross section of the oxide film deposited by using a thin film shielding agent according to Example 2, as well as the thickness of the upper part (100 nm downward from the top) and the lower part (100 nm upward from the bottom) of the cross section of the oxide film deposited by using a thin film shielding agent. DETAILED DESCRIPTION

[0079] Hereinafter, the thin film shielding agent of the present invention, the thin film forming method using the same, and the semiconductor substrate produced thereby will be described in detail.

[0080] Unless otherwise specifically defined, the term "shielding" in the present invention means reducing, preventing or blocking not only the adsorption of precursor compounds for forming a thin film on the substrate but also reducing, preventing or blocking the adsorption of process byproducts on the substrate.

[0081] Unless otherwise specifically defined, the terms "physical adsorption" and "chemical adsorption" in the present invention can be divided into adsorption that can be removed by purging and adsorption that is not removed but remains even after purging, and the former and the latter can be respectively referred to as physical adsorption and chemical adsorption.

[0082] The inventors of the present invention have confirmed that by using a thin film shielding agent that can effectively shield the adsorption of a precursor compound (provided to form a thin film on the surface of a substrate loaded inside a chamber), the thin film shielding agent provides a strong and stable physical adsorption or chemical adsorption mechanism on the surface of the deposited layer of the substrate, thereby improving the reaction rate, so that even if high temperature conditions are applied to a substrate with a complex structure, the uniformity of the thin film can be ensured by improving the film quality, thereby greatly improving the step coverage, and in particular, it is possible to deposit with a thinner thickness and improve the amount of O, Si, metals, metal oxides and residual carbon that are difficult to reduce as process byproducts. Based on this, the inventors have devoted themselves to the study of thin film shielding agents, and completed the present invention.

[0083] As an example, the above-mentioned thin film can be provided by one or more precursors selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd, and can provide an oxide film, a nitride film or a metal film. At this time, the effect to be achieved by the present invention can be fully obtained.

[0084] As a specific example, the thin film may have a film composition of a silicon nitride film, a silicon oxide film, a titanium nitride film, a titanium oxide film, a tungsten nitride film, a molybdenum nitride film, a hafnium oxide film, a zirconium oxide film, a tungsten oxide film, or an aluminum oxide film.

[0085] The thin film may include the above-mentioned film composition alone or in a selective area, but is not limited thereto and may also include SiH and SiOH.

[0086] The above-mentioned thin film can be used not only as a generally used anti-diffusion film in a semiconductor device but also as an etching stopper film, an electrode film, a dielectric film, a gate insulating film, a blocking oxide film or a charge trap.

[0087] In the present invention, the precursor compound used to form the thin film is a molecule with Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd as the central metal atom (M) and one or more ligands described below. In the case of a precursor with a vapor pressure of 1mTorr to 100Torr at a temperature of 25°C, the effect of being replaced by a thin film shielding agent can be maximized.

[0088] As an example, the precursor compound may be a compound represented by the following Chemical Formula 2.

[0089] [Chemical formula 2]

[0090]

[0091] In the above chemical formula 2, M is one or more selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd, and L 1 , L 2 , L 3 and L 4 -H, -X, -R, -Cp (cyclopentadienyl), -OR, NR or Cp (cyclopentadienyl) may be the same or different, wherein -X is F, Cl, Br or I, -R is C1-C10 alkyl, C1-C10 alkenyl or C1-C10 alkynyl, and may be linear or cyclic, and the above L 1 , L 2 , L 3 and L 4 It can be formed into 2 to 6 according to the oxidation valence of the central metal (M).

[0092] For example, when the central metal is divalent, L 1 and L 2 It can act as a ligand to bind to the central metal. When the central metal is hexavalent, L 1 , L 2 , L 3 , L 4 , L 5 , L 6 Can be combined with the central metal, equivalent to L 1 ~L 6 The ligands may be the same as or different from each other.

[0093] In the above chemical formula 2, the above M is hafnium (Hf), silicon (Si), zirconium (Zr) or aluminum (Al), preferably hafnium (Hf) or silicon (Si). In this case, the process by-product reduction effect is significant, the step coverage is excellent, and it has the advantages of improving the film density, and the electrical properties, insulation and dielectric properties of the film are better.

[0094] The above L 1 , L 2 , L 3 and L 4 -H, -Cp or -R may be the same as or different from each other, wherein -R may be a C1-C10 alkyl group, a C1-C10 alkenyl group or a C1-C10 alkynyl group, and may have a linear or cyclic structure.

[0095] In addition, the above L 1 , L 2, L 3 and L 4 -H, Cp, -OR, NR or Cp (cyclopentadienyl) may be the same as or different from each other, wherein -R may be H, C1-C10 alkyl, C1-C10 alkenyl or C1-C10 alkynyl, iPr or tBu.

[0096] In addition, in the above chemical formula 1, L 1 , L 2 , L 3 and L 4 -H, -Cp or -X may be the same as or different from each other.

[0097] Specifically, for example, the hafnium precursor compound may use tris(dimethylamido)cyclopentadienylhafnium (CpHf(NMe2)3)) and (methyl-3-cyclopentadienylpropylamino)bis(dimethylamino)hafnium (Cp(CH2)3NM3Hf(NMe2)2).

[0098] In addition, for example, the silicon precursor compound can be selected from SiH4, SiHCl3, SiH2Cl2, SiCl4, Si2Cl6, Si3Cl8, Si4Cl 10 , SiH2[NH(C4H9)]2, Si2(NHC2H5)4, Si3NH4(CH3)3, SiH3[N(CH3)2], SiH2[N(CH3)2]2, SiH[N(CH3)2]3 and one or more of Si[N(CH3)2]4.

[0099] In addition, the aluminum precursor compound may include trimethyl aluminum (TMA), tris(dimethylamido)aluminum (TDMAA), and aluminum chloride (AlCl 3 ).

[0100] The above-mentioned thin film shielding agent can be used to deposit a metal oxide film or a non-metal oxide film on a substrate.

[0101] The thin film shielding agent contains at least one element having an electronegativity between the electronegativity of the metal or non-metal constituting the oxide film and the electronegativity of oxygen, and is used to deposit a metal oxide film or a non-metal oxide film.

[0102] As an example, the above-mentioned metal or non-metal can shield the surface of a thin film formed by one or more precursor compounds selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd.

[0103] When the above-mentioned film shielding agent is a compound containing 4 or more elements with electronegativity ranging from 2.1 to 3.1, the process by-product reduction effect is significant, the step coverage is excellent, and the film density improvement effect and the electrical properties of the film can be more outstanding.

[0104] Preferably, the above-mentioned thin film shielding agent can be a compound containing sulfur, phosphorus or nitrogen. In this case, when forming a thin film, side reactions can be suppressed and the film growth rate can be adjusted to reduce process by-products in the thin film, thereby reducing corrosion and degradation, and improving film quality, such as improving the crystallinity of the thin film. Even if the thin film is formed on a substrate with a complex structure, the step coverage and thickness uniformity of the thin film can be greatly improved.

[0105] Preferably, the above-mentioned thin film shielding agent is a compound containing more than 4 elements with an electronegativity range of 2.1 to 3.1, and the deposition rate reduction rate represented by the following mathematical formula 1 can be more than 20%, as a specific example, more than 35%. At this time, based on the difference in adsorption distribution of the shielding agent having the above-mentioned structure, a deposition layer with uniform thickness is formed as a shielding area that will not remain in the thin film, thereby forming a relatively sparse thin film while greatly reducing the growth rate of the formed thin film. Therefore, even if applied to a substrate with a complex structure, the uniformity of the thin film can be ensured, thereby greatly improving the step coverage. In particular, it can be deposited with a thinner thickness and improve the amount of O, Si, metals, metal oxides remaining as process by-products and the residual carbon that was previously difficult to reduce.

[0106] [Mathematical formula 1]

[0107] Deposition rate (DR) reduction rate = [{(DR i )-(DR f )} / (DR i )]×100

[0108] (In the above mathematical formula, DR (Deposition rate, ) is the rate of film deposition. When depositing a film formed from a precursor and a reactant, DR i Initial deposition rate is the deposition rate of a thin film without the use of a film shielding agent. r The final deposition rate is the deposition rate of the film formed by adding the oxide film shielding agent during the above process. The deposition rate (DR) is the value measured by an ellipsometer at room temperature and pressure for a film with a thickness of 3 to 30 nm. The unit used is )

[0109] In the above mathematical formula 1, when a film shielding agent is used or not, the film growth rate per cycle represents the film deposition thickness per cycle. That is, the deposition rate may be, for example, an average deposition rate obtained by measuring the final thickness of a thin film having a thickness of 3 to 30 nm using an ellipsometer under normal temperature and pressure conditions and dividing the result by the total number of cycles.

[0110] In the above mathematical formula 1, "when a thin film shielding agent is not used" means a case where a thin film is manufactured by adsorbing only a precursor compound on a substrate in a thin film deposition process. As a specific example, it means a case where a thin film is formed by omitting the step of adsorbing a thin film shielding agent and the step of purging the non-adsorbed thin film shielding agent in the above-mentioned thin film forming method.

[0111] The above-mentioned thin film shielding agent includes a linear or cyclic saturated or unsaturated hydrocarbon containing two or more nitrogen (N), oxygen (O), phosphorus (P) or sulfur (S) and having 3 to 15 carbon atoms. At this time, it is possible to form a shielding area that will not remain in the thin film when the thin film is formed, suppress side reactions while forming a relatively sparse thin film, and adjust the film growth rate to reduce process by-products in the thin film, thereby reducing corrosion and degradation, and improving the crystallinity of the thin film. When a metal oxide film is formed, a stoichiometric oxidation state is reached. Even if a thin film is formed on a substrate with a complex structure, the step coverage and the thickness uniformity of the thin film can be greatly improved.

[0112] The above-mentioned film shielding agent includes a central atom connected to an oxygen atom by a double bond, preferably, contains oxygen (O) or phenyl at one end or both ends of sulfur (S), phosphorus (P) or nitrogen (N), or a compound having a ring structure formed by connecting both ends, thereby significantly reducing the effect of process by-products, and has excellent step coverage, and the film density improvement effect and the electrical properties of the film can be more outstanding.

[0113] As a specific example, the above-mentioned thin film shielding agent can be one or more selected from compounds having a structure represented by the following chemical formula 1. In this case, a shielding area is formed that will not remain in the thin film when the thin film is formed, and side reactions are suppressed while forming a relatively sparse thin film. The film growth rate is adjusted to reduce process by-products in the thin film, thereby reducing corrosion and degradation, and improving the crystallinity of the thin film. Even if a thin film is formed on a substrate with a complex structure, the step coverage and the thickness uniformity of the thin film can be greatly improved, thereby forming a seamless thin film.

[0114] [Chemical formula 1]

[0115]

[0116] (In the above chemical formula 1, R1 is H, OH, CH3, OCH3, OCH2CH3, OCH2CH2CH3, or an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 1 to 5 carbon atoms, or an alkynyl group having 1 to 5 carbon atoms, and X is m is an integer from 0 to 4.

[0117] In the above chemical formula 1, the above R1 is H or CH3. In this case, the process by-product reduction effect is significant, the step coverage is excellent, the film density is improved, and the electrical properties, insulation and dielectric properties of the film are more outstanding.

[0118] The above m is an integer of 0 to 2, and is preferably 0 or 1.

[0119] As an example, the refractive index of the thin film shielding agent may be a compound in the range of 1.4 to 1.5, 1.41 to 1.48, or 1.41 to 1.47.

[0120] At this time, a thin film shielding agent having the above-mentioned structure is used for the substrate. Through the strong and stable physical adsorption or chemical adsorption mechanism of the thin film shielding agent on the surface of the deposited layer of the substrate, the adsorption of the precursor compound on the substrate is appropriately shielded, thereby improving the reaction rate. Even when a thin film is formed on a substrate with a complex structure under high temperature conditions, the step coverage and thickness uniformity of the thin film can be greatly improved, and the adsorption of the thin film precursor and the process by-products can be prevented, thereby effectively protecting the surface of the substrate, and having the advantage of effectively removing the process by-products.

[0121] As an example, when the shielding agent is a compound represented by the following Chemical Formula 1, the refractive index may be within the range of 1.4 to 1.5, 1.41 to 1.48, or 1.41 to 1.47.

[0122] At this time, on the substrate, based on the difference in adsorption distribution of the shielding agent with the above structure, a deposition layer with uniform thickness is formed as a shielding area that will not remain in the film, thereby reducing the deposition rate of the film and appropriately reducing the film growth rate. Even when a thin film is formed on a substrate with a complex structure under high temperature conditions, the step coverage and thickness uniformity of the film can be greatly improved, thereby forming a seamless film, and preventing the adsorption of film precursors and process by-products, thereby effectively protecting the surface of the substrate, and having the advantage of effectively removing process by-products.

[0123] In particular, while forming a relatively sparse film, the growth rate of the formed film is greatly reduced. Therefore, even if it is applied to a substrate with a complex structure, the uniformity of the film can be ensured, thereby greatly improving the step coverage. In particular, it can be deposited with a thin thickness and improve the amount of O, Si, metals, metal oxides remaining as process by-products, and residual carbon that was previously difficult to reduce.

[0124] The above-mentioned thin film shielding agent may include one or more compounds selected from the following chemical formulas 1-1 to 1-9. In this case, a thin film shielding area is provided, thereby significantly adjusting the film growth rate, significantly removing process by-products, and having excellent step coverage improvement and film quality improvement effects.

[0125] [Chemical formula 1-1[ to [Chemical formula 1-9]

[0126]

[0127] The thin film-forming composition including the above-mentioned thin film shielding agent may include a precursor compound constituting a thin film deposition layer and a thin film shielding agent.

[0128] The precursor compound may be a compound represented by the following Chemical Formula 2.

[0129] [Chemical formula 2]

[0130]

[0131] (In the above chemical formula 2, M is one or more selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd, L 1 , L 2 , L 3 and L 4 -H, -X, -R, -Cp, -OR, -NR or Cp (cyclopentadienyl) may be the same or different, wherein -X is F, Cl, Br or I, -R is C1-C10 alkyl, C1-C10 alkenyl or C1-C10 alkynyl, and may be linear or cyclic, and the above L 1 , L 2 , L 3 and L 4 It can be formed into 2 to 6 according to the oxidation valence of the central metal (M).

[0132] For example, when the central metal is divalent, L 1 and L 2 It can act as a ligand to bind to the central metal. When the central metal is hexavalent, L 1, L 2 , L 3 , L 4 , L 5 , L 6 Can be combined with the central metal, equivalent to L 1 ~L 6 The ligands may be the same as or different from each other.

[0133] The thin film shielding agent provides a shielding area for the oxide film, nitride film, metal film or their selective thin films, and the shielding area can be formed on the entire substrate or a part of the substrate on which the oxide film, nitride film, metal film or their selective thin films are formed.

[0134] The film shielding region does not remain on the film.

[0135] At this time, unless otherwise specifically defined, no residue means that when the components are analyzed by XPS, the C element is 0.1 atom %, the Si element is less than 0.1 atom %, the N element is less than 0.1 atom %, and the halogen element is less than 0.1 atom %. Preferably, in a secondary ion mass spectrometry (SIMS) measurement method or an X-ray photoelectron spectroscopy (XPS) measurement method that measures by digging into the substrate in the depth direction, when considering the increase and decrease rates of C, N, Si, and halogen impurities before and after using an activator under the same deposition conditions, the increase and decrease rate of the signal intensity of each element species is preferably less than 5%.

[0136] As a specific example, when the total area of ​​the entire substrate or a portion of the substrate is set to 100%, the shielded area may occupy 10% to 95% of the area, and the unshielded area may occupy the remaining area.

[0137] As an example, the content of the halogen compound in the above-mentioned film can be 100 ppm or less. For reference, when too much halogen remains, when a nitriding agent is used under the temperature condition of 200 to 300° C. as the experimental condition described later, impurities such as NH4Cl with a high boiling point are generated and remain in the film, which is not preferred.

[0138] The above-mentioned thin film can be used as an etching stopper film, an electrode film, a dielectric film, a gate insulating film, a blocking oxide film or a charge trap, and improves the step coverage during its formation process, so that it can be applied to semiconductor devices.

[0139] Preferably, the above-mentioned film shielding agent can be a compound with a purity of 99.9% or more, a compound with a purity of 99.95% or more, or a compound with a purity of 99.99% or more. For reference, when a compound with a purity of less than 99% is used, there is a possibility that impurities will remain in the film or cause side reactions with precursors or reactants. Therefore, materials with a purity of 99% or more should be used as much as possible.

[0140] Preferably, the thin film shielding agent is used in an atomic layer deposition (ALD) process. In this case, the thin film shielding agent effectively protects the surface of the substrate while not hindering the adsorption of the precursor compound, and has the advantage of effectively removing process byproducts.

[0141] Preferably, the density of the film shielding agent can be 0.8 to 2.5 g / cm 3 or 0.8~1.5g / cm 3 , the vapor pressure (20°C) can be 0.1 to 300 mmHg or 1 to 300 mmHg.

[0142] More preferably, the density of the film shielding agent can be 0.8 to 2.0 g / cm 3 or 0.8~1.3g / cm 3 , the vapor pressure (20°C) can be 1 to 260 mmHg.

[0143] In particular, while forming a relatively sparse film, the growth rate of the formed film is greatly reduced. Therefore, even if it is applied to a substrate with a complex structure, the uniformity of the film can be ensured, thereby greatly improving the step coverage. In particular, it can be deposited with a thinner thickness and improve the amount of O, Si, metals, metal oxides remaining as process by-products, and residual carbon that was previously difficult to reduce.

[0144] The thin film forming method of the present invention includes the step of injecting the above-mentioned thin film shielding agent into a chamber to form a deposition layer on a loaded substrate. At this time, the reaction rate is improved and the thin film growth rate is appropriately reduced through a physical reaction or a chemical reaction on the surface of the substrate, so that even when a thin film is formed on a substrate with a complex structure under high temperature conditions, the step coverage and the thickness uniformity of the thin film can be greatly improved.

[0145] In the step of masking the substrate surface with the above-mentioned thin film masking agent, the feeding time (Feeding Time, sec) of the thin film masking agent to the surface of the substrate per cycle is preferably 0.01 to 5 seconds, more preferably 0.02 to 3 seconds, more preferably 0.04 to 2 seconds, and further preferably 0.05 to 1 second. Within this range, it has the advantages of low thin film growth rate and excellent step coverage and economy.

[0146] In the present invention, the feeding time of the film shielding agent is based on a flow rate of 0.1 to 50 mg / cycle when the volume of the chamber is 15 to 20 L, and more specifically, based on a flow rate of 0.8 to 20 mg / cycle when the volume of the chamber is 18 L.

[0147] As a preferred embodiment, the above-mentioned thin film forming method may include: step i), vaporizing the above-mentioned thin film shielding agent to shield the surface of the substrate loaded in the chamber; step ii), using a purge gas to perform a first purge on the inside of the above-mentioned chamber; step iii), vaporizing the precursor compound and adsorbing it in an area away from the above-mentioned shielding area; step iv), using a purge gas to perform a second purge on the inside of the above-mentioned chamber; step v), providing a reaction gas into the above-mentioned chamber; and step vi), using a purge gas to perform a third purge on the inside of the above-mentioned chamber. At this time, the above-mentioned steps i) to vi) can be used as a unit cycle, and the above cycle can be repeatedly implemented until a thin film of a desired thickness is obtained (refer to Figure 1 ), and when in this way the thin film shielding agent of the present invention is added before the precursor compound in one cycle and adsorbed on the substrate, and the thin film shielding agent is added sequentially after the precursor compound to improve the film quality, even if deposition is performed at a high temperature, the thin film growth rate can be appropriately reduced, and the generated process by-products can be effectively removed to reduce the resistivity of the thin film, and it has the advantage of greatly improving the step coverage.

[0148] As a preferred example, in the thin film forming method of the present invention, the thin film shielding agent of the present invention can be added before the precursor compound and adsorbed on the substrate within one cycle. At this time, even if the thin film is deposited at a high temperature, the growth rate of the thin film can be appropriately reduced, thereby greatly reducing process by-products and greatly improving step coverage. The crystallinity of the thin film is increased to reduce the resistivity of the thin film, and even if it is applied to semiconductor devices with a large aspect ratio, the thickness uniformity of the thin film can be greatly improved, thereby ensuring the reliability of the semiconductor device.

[0149] In the above-mentioned thin film forming method, when the above-mentioned thin film shielding agent is deposited before depositing the precursor compound or after depositing the precursor compound as needed, the number of repetitions of the unit cycle implemented can be 1 to 99,999 times, preferably 10 to 10,000 times, more preferably 50 to 5,000 times, and even more preferably 100 to 2,000 times, as needed. Within this range, the desired film thickness can be obtained and the effect to be achieved by the present invention can be fully obtained.

[0150] As an example, in the present invention, the chamber may be an ALD chamber, a CVD chamber, a PEALD chamber or a PECVD chamber.

[0151] The present invention may include a step of performing plasma post-treatment after vaporizing and injecting the above-mentioned film masking agent or precursor compound, thereby improving the growth rate of the film and reducing process byproducts.

[0152] When the thin film shielding agent is alternately injected onto the substrate and the precursor compound is adsorbed therein, in the step of purging the non-adsorbed thin film shielding agent, there is no particular limitation on the amount of the purge gas injected into the chamber as long as it is an amount that can fully remove the non-adsorbed thin film shielding agent. For example, it can be 10 to 100,000 times, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times. Within this range, the non-adsorbed thin film shielding agent is fully removed, so that a thin film can be formed uniformly and the film quality can be prevented from deteriorating. The input amounts of the purge gas and the thin film shielding agent are based on one cycle, respectively, and the volume of the thin film shielding agent refers to the volume of the vaporized thin film shielding agent vapor.

[0153] As a specific example, in the step of injecting the above-mentioned thin film shielding agent at a flow rate of 1.66 mL / s and an injection time of 0.5 sec (for each cycle) and purging the unadsorbed thin film shielding agent, when the purge gas is injected (for each cycle) at a flow rate of 1.66 mL / s and an injection time of 3 sec, the injection amount of the purge gas is 602 times the injection amount of the thin film shielding agent.

[0154] In addition, in the step of purging the above-mentioned non-adsorbed precursor compound, the amount of the purge gas introduced into the interior of the above-mentioned chamber is not particularly limited, as long as it is sufficient to remove the above-mentioned non-adsorbed precursor compound. As an example, it can be 10 to 100,000 times the volume of the precursor compound introduced into the interior of the above-mentioned chamber, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times. Within this range, the non-adsorbed precursor compound can be sufficiently removed to form a uniform thin film and prevent the degradation of the film quality. The amount of the above-mentioned purge gas and precursor compound introduced is based on one cycle, and the volume of the above-mentioned precursor compound represents the volume of the vaporized precursor compound vapor.

[0155] In addition, in the purge step performed immediately after the reaction gas supply step, as an example, the amount of the purge gas introduced into the chamber may be 10 to 100,000 times, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times the volume of the reaction gas introduced into the chamber. Within this range, the desired effect can be fully obtained. The amounts of the purge gas and the reaction gas introduced are based on one cycle, respectively.

[0156] Preferably, the thin film shielding agent and precursor compound can be delivered into the chamber by VFC, DLI or LDS, and more preferably, can be delivered into the chamber by LDS.

[0157] As an example, the substrate loaded in the chamber can be heated to 50-400°C. As a specific example, it can be heated to 50-400°C. The thin film shielding agent or precursor compound can be injected into the substrate in an unheated or heated state. According to the deposition efficiency, it is also possible to heat it during the deposition process after injecting it in an unheated state. As an example, it can be injected into the substrate at 50-400°C within 1-20 seconds.

[0158] Preferably, the ratio of the amount (mg / cycle) of the thin film shielding agent to the precursor compound added into the chamber can be 1:1.5 to 1:20, more preferably 1:2 to 1:15, more preferably 1:2 to 1:12, and further preferably 1:2.5 to 1:10. Within this range, the effect of improving step coverage and reducing process by-products is significant.

[0159] As an example, in the present invention, the above-mentioned precursor compound is mixed with a non-polar solvent and then introduced into the chamber. In this case, there is an advantage that the viscosity or vapor pressure of the precursor compound can be easily adjusted.

[0160] Preferably, the non-polar solvent may be selected from at least one of alkanes and cycloalkanes. In this case, the non-polar solvent includes an organic solvent with low reactivity and solubility and easy water management, and has the advantage of improving step coverage even when the deposition temperature is increased during film formation.

[0161] As a more preferred example, the non-polar solvent may include C1-C10 alkane or C3-C10 cycloalkane, preferably C3-C10 cycloalkane. In this case, the non-polar solvent has the advantages of low reactivity and solubility and easy water management.

[0162] In the present invention, C1, C3, etc. represent the number of carbon atoms.

[0163] Preferably, the cycloalkane may be a C3-C10 monocycloalkane. Among the monocycloalkane, cyclopentane is liquid at room temperature and has the highest vapor pressure. Therefore, it is preferred in the vapor deposition process, but is not limited thereto.

[0164] As an example, the solubility of the non-polar solvent in water (25° C.) is less than 200 mg / L, preferably 50 to 400 mg / L, and more preferably 135 to 175 mg / L. Within this range, the non-polar solvent has the advantages of low reactivity to precursor compounds and easy water management.

[0165] In the present invention, the solubility is not particularly limited as long as it is based on the measurement method and standard conventionally used in the art. As an example, a saturated solution can be measured by HPLC.

[0166] Preferably, based on the total weight of the precursor compound and the non-polar solvent, the content of the non-polar solvent may be 5 to 95% by weight, more preferably 10 to 90% by weight, even more preferably 40 to 90% by weight, and most preferably 70 to 90% by weight.

[0167] If the content of the above-mentioned non-polar solvent is greater than the above-mentioned upper limit value, impurities will be induced, thereby causing an increase in the impurity values ​​in the resistor and the film. When the content of the above-mentioned organic solvent is less than the above-mentioned lower limit value, there are the disadvantages that the effect of improving the step coverage by adding the solvent and the effect of reducing impurities such as chloride (Cl) ions are not significant.

[0168] As an example, when the above-mentioned thin film forming method uses the above-mentioned thin film shielding agent, the deposition rate reduction rate represented by the following mathematical formula 1 can be greater than 30%, and a specific example is greater than 35%. At this time, based on the difference in adsorption distribution of the active agent having the above-mentioned structure, a deposition layer with uniform thickness is formed as a replacement area that will not remain in the thin film, thereby forming a relatively sparse thin film while greatly reducing the growth rate of the formed thin film. Therefore, even if applied to a substrate with a complex structure, the uniformity of the thin film can be ensured, thereby greatly improving the step coverage. In particular, it can be deposited with a thinner thickness and improve the amount of O, Si, metals, metal oxides remaining as process by-products, and residual carbon that was previously difficult to reduce.

[0169] [Mathematical formula 1]

[0170] Deposition rate (DR) reduction rate = [{(DR i )-(DR f )} / (DR i )]×100

[0171] (In the above mathematical formula, DR (Deposition rate, ) is the rate of film deposition. When depositing a film formed from a precursor and a reactant, DR i Initial deposition rate is the deposition rate of a thin film without the use of a film shielding agent. r The final deposition rate is the deposition rate of the film formed by adding the oxide film shielding agent during the above process. The deposition rate (DR) is the value measured by an ellipsometer at room temperature and pressure for a film with a thickness of 3 to 30 nm. The unit used is )

[0172] In the above-mentioned thin film forming method, the film thickness measured by SIMS is The residual halogen intensity (c / s) in the film is preferably 100,000 or less, more preferably 70,000 or less, more preferably 50,000 or less, and further preferably 10,000 or less. As a preferred embodiment, it can be 5,000 or less, more preferably 1,000 to 4,000, and further preferably 1,000 to 3,800. Within this range, the effect of preventing corrosion and degradation is excellent.

[0173] In the present invention, the purge is preferably 1,000 to 50,000 sccm (Standard Cubic Centimeter per Minute), more preferably 2,000 to 30,000 sccm, and even more preferably 2,500 to 15,000 sccm. Within this range, the film growth rate per cycle is properly controlled, and deposition is performed in an atomic mono-layer or a manner close thereto, which is advantageous in terms of film quality.

[0174] The above-mentioned ALD (atomic layer deposition process) is very beneficial for manufacturing integrated circuits (ICs) that require high aspect ratios. In particular, it has advantages such as excellent step coverage (conformality), uniform coverage (uniformity) and precise thickness control based on the self-limiting film growth mechanism.

[0175] As an example, the above-mentioned thin film forming method can be implemented at a deposition temperature in the range of 50 to 800°C, preferably in the range of 100 to 700°C, more preferably in the range of 200 to 650°C, even more preferably in the range of 220 to 400°C, and further preferably in the range of 220 to 300°C. Within this range, it has the effect of realizing the characteristics of the ALD process and growing a thin film with excellent film quality.

[0176] As an example, the above-mentioned thin film forming method can be implemented at a deposition pressure in the range of 0.01 to 20 Torr, preferably at a deposition pressure in the range of 0.1 to 20 Torr, more preferably at a deposition pressure in the range of 0.1 to 10 Torr, and most preferably at a deposition pressure in the range of 0.3 to 7 Torr. Within this range, the effect of obtaining a thin film with uniform thickness can be achieved.

[0177] In the present invention, the deposition temperature and the deposition pressure may be measured by the temperature and pressure formed in the deposition chamber or by the temperature and pressure applied to the substrate in the deposition chamber.

[0178] Preferably, the above-mentioned thin film forming method may include the following steps: before the above-mentioned thin film shielding agent is introduced into the chamber, the temperature in the chamber is increased to the deposition temperature; and / or before the above-mentioned thin film shielding agent is introduced into the chamber, an inert gas is injected into the chamber for purging.

[0179] In addition, in the present invention, a thin film manufacturing apparatus capable of implementing the above-mentioned thin film manufacturing method may include: an ALD chamber; a first vaporizer for vaporizing a thin film shielding agent; a first conveying unit for conveying the vaporized thin film shielding agent into the ALD chamber; a second vaporizer for vaporizing a thin film precursor; and a second conveying unit for conveying the vaporized thin film precursor into the ALD chamber. There are no particular limitations on the vaporizer and the conveying unit, as long as they are conventionally used in the art.

[0180] According to need, the first vaporizer for vaporizing the thin film shielding agent may be divided into at least two structures: a vaporizer for vaporizing the thin film shielding agent and a vaporizer for vaporizing the thin film shielding agent.

[0181] The above-mentioned thin film forming method will be described as a specific example. First, a substrate on which a thin film is to be formed is placed in a deposition chamber capable of performing atomic layer deposition.

[0182] The substrate may include a semiconductor substrate such as a silicon substrate or silicon oxide.

[0183] The substrate may further have a conductive layer or an insulating layer formed on an upper portion thereof.

[0184] In order to deposit a thin film on the substrate placed in the deposition chamber, the thin film shielding agent and precursor compound or a mixture thereof with a non-polar solvent are prepared respectively.

[0185] Then, after the prepared thin film shielding agent (eg, thin film shielding agent) is injected into the vaporizer, it is changed into a vapor phase to be transported to the deposition chamber and adsorbed on the substrate, and then purging is performed to remove the unadsorbed thin film shielding agent.

[0186] Next, after the prepared precursor compound or its mixture with a non-polar solvent (hereinafter referred to as a thin film forming composition) is injected into the vaporizer, it is changed into a vapor phase so as to be transported to the deposition chamber and adsorbed on the substrate, masked by a previously injected thin film masking agent, and the precursor compound or its mixture with a non-polar solution that is not adsorbed is purged.

[0187] Next, after the prepared thin film shielding agent is injected into the vaporizer, it is changed into a vapor phase so as to be transported to the deposition chamber and adsorbed, and then the non-adsorbed thin film shielding agent is purged.

[0188] In the present invention, as an example, the method of delivering a thin film masking agent and a precursor compound (thin film forming composition) to a deposition chamber can use a method of delivering a volatile gas (Vapor Flow Control, VFC) using a gas phase flow control (Mass Flow Controller, MFC) method or a method of delivering a liquid (Liquid Delivery System; LDS) using a liquid phase flow control (Liquid Mass Flow Controller, LMFC) method. Preferably, the LDS method is used.

[0189] At this time, as a carrier gas or dilution gas for transporting thin film shielding agents and precursor compounds to the substrate, one or a mixed gas selected from argon (Ar), nitrogen (N2), and helium (He) can be used, but it is not limited to this.

[0190] In the present invention, as an example, an inert gas may be used as the purge gas, and preferably, the above-mentioned carrier gas or diluent gas may be used.

[0191] Next, a reaction gas is supplied. The reaction gas is not particularly limited as long as it is a reaction gas commonly used in the art, and preferably, it may contain a nitriding agent. The nitriding agent reacts with the precursor compound adsorbed on the substrate to form a nitride film.

[0192] Preferably, the nitriding agent may be nitrogen (N2), hydrazine (N2H4) or a mixture of nitrogen and hydrogen.

[0193] Next, the unreacted residual reaction gas is purged with an inert gas, thereby removing not only the excess reaction gas but also the generated by-products.

[0194] As described above, as an example, the above-mentioned thin film forming method can take the following steps as a unit cycle and repeat the above-mentioned unit cycle to form a thin film of desired thickness, wherein the above-mentioned steps include: a step of supplying a thin film shielding agent on a substrate; a step of purging the unadsorbed thin film shielding agent; a step of adsorbing a precursor compound / thin film forming composition on a substrate; a step of purging the unadsorbed precursor compound; a step of supplying a reaction gas; and a step of purging the residual reaction gas.

[0195] As an example, the number of repetitions of the above-mentioned unit cycle may be 1 to 99,999 times, preferably 10 to 10,000 times, more preferably 50 to 5,000 times, and even more preferably 100 to 2,000 times. Within this range, the desired film properties can be well expressed.

[0196] The present invention also provides a semiconductor substrate manufactured by the thin film forming method of the present invention, in which the step coverage and thickness uniformity of the thin film are excellent, and the density and electrical characteristics of the thin film are excellent.

[0197] Preferably, the thickness of the above-mentioned thin film is less than 20nm, based on the film thickness of 10nm, the resistivity value is 50-400μΩ·cm, the halogen content is less than 10,000ppm, and the step coverage is more than 90%. Within this range, as an anti-diffusion film, it has excellent performance and the effect of reducing corrosion of metal wiring materials, but is not limited to this.

[0198] As an example, the thickness of the thin film may be 0.1 to 20 nm, preferably 1 to 20 nm, more preferably 3 to 20 nm, and even more preferably 5 to 20 nm. Within this range, the film has excellent properties.

[0199] As an example, based on a film thickness of 10 nm, the resistivity value of the above-mentioned film can be 0.1 to 400 μΩ·cm, preferably 15 to 300 μΩ·cm, more preferably 20 to 290 μΩ·cm, and even more preferably 25 to 280 μΩ·cm. Within this range, the film has excellent properties.

[0200] Preferably, the halogen content of the film may be less than 10,000 ppm or 1 to 9,000 ppm, more preferably 5 to 8,500 ppm, and even more preferably 100 to 1,000 ppm. Within this range, the film has excellent properties and has the effect of reducing the film growth rate. As an example, the residual halogen in the film may be Cl2, Cl or Cl - The lower the residual amount of halogen in the film, the better the film quality, so it is preferred.

[0201] As an example, the step coverage of the above-mentioned film can be above 90%, preferably above 92%, and more preferably above 95%. Within this range, even a thin film with a complex structure can be easily deposited on the substrate. Therefore, it has the advantage of being applicable to a new generation of semiconductor devices.

[0202] Preferably, the thickness of the above-mentioned film is less than 20nm, and the content of carbon, nitrogen and halogen is less than 10,000ppm based on the film thickness of 10nm, and the step coverage is more than 90%. Within this range, it has excellent performance as a dielectric film or barrier film, but is not limited to this.

[0203] As an example, the film may be a multilayer structure of two or more layers as required. As a specific example, the multilayer film of the two-layer structure may be a structure of a lower film-middle film, and as a specific example, the multilayer film of the three-layer structure may be a structure of a lower film-middle film-upper film.

[0204] As an example, the above-mentioned lower layer film may include one or more selected from Si, SiO2, MgO, Al2O3, CaO, ZrSiO4, ZrO2, HfSiO4, Y2O3, HfO2, LaLuO2, Si3N4, SrO, La2O3, Ta2O5, BaO, and TiO2.

[0205] As an example, the intermediate layer film may include Ti x N y The composition preferably contains TN.

[0206] As an example, the upper layer film may include one or more selected from W and Mo.

[0207] Below, in order to help understand the present invention, preferred embodiments and drawings are proposed. However, it is clear to those skilled in the art that the following embodiments and drawings are only used to illustrate the present invention, and various changes and modifications can be made within the scope of the scope of the present invention and the technical concept, and such deformation and modification undoubtedly fall within the scope of the attached invention application patent.

[0208] Example

[0209] Example 1 to Example 2, Comparative Example 1 to Comparative Example 3

[0210] Using the ingredients shown in Table 1, Figure 1 An ALD deposition process is performed.

[0211] Figure 1 This is a diagram schematically showing the deposition process sequence of the present invention mainly in one cycle.

[0212] Specifically, a compound represented by Chemical Formula 1-4 and a compound represented by Chemical Formula 3-1 were prepared as the thin film shielding agent.

[0213] [Chemical formula 1-4]

[0214]

[0215] [Chemical formula 3-1]

[0216]

[0217] In addition, tris(dimethylamido)cyclopentadienylhafnium (CpHf(NMe2)3) (denoted as CpHf in the table) and trimethylaluminum (denoted as TMA in the table) were prepared as precursors.

[0218] Argon gas was introduced into the chamber at 5000 mL / min, and the pressure in the chamber was set to 1.5 Torr using a vacuum pump, thereby forming a rarefied inert environment.

[0219] The prepared thin film shielding agent shown in Table 1 was loaded into a tank and the partial pressure and temperature were adjusted to reach the injection amount (mg / cycle), and it was injected into the deposition chamber loaded with the substrate for 1 second to coat it on the substrate, and the chamber was purged for 10 seconds.

[0220] Next, the precursor compound was loaded into a can and introduced into the deposition chamber through a vapor flow controller (VFC) in the manner shown in Table 1, and the chamber was purged for 10 seconds.

[0221] Then, as a reactive gas, the concentration of O3 in O2 was adjusted to 200 g / m 3 The substrate on which the thin film was to be formed was heated under the temperature conditions shown in Table 1.

[0222] This process was repeated 100 to 400 times to form a self-limiting atomic layer film with a thickness of 10 nm.

[0223] For each of the obtained thin films of Examples 1 to 2 and Comparative Examples 1 to 3, the deposition rate reduction rate (DR reduction rate) and SIMS C impurities and step coverage were measured in the following manner and are shown in Table 1.

[0224] *Deposition rate reduction rate (DR (dep.rate) reduction rate): It indicates the ratio of the deposition rate reduction after the addition of the shielding agent compared to the DR before the addition of the shielding agent. The percentage is calculated using the A / cycle values ​​measured respectively.

[0225] Specifically, the thickness of the film measured by an ellipsometer is divided by the number of cycles to calculate the thickness of the film deposited per cycle, thereby calculating the reduction rate of the film growth rate, wherein the ellipsometer is a device that can measure optical properties such as the thickness or refractive index of the manufactured film using the polarization properties of light. Specifically, the calculation is performed using the following mathematical formula 1.

[0226] [Mathematical formula 1]

[0227] Deposition rate (DR) reduction rate = [{(DR i )-(DR f )} / (DR i )]×100

[0228] In the above mathematical formula, DR (Deposition rate, ) is the rate of film deposition. When depositing a film formed from a precursor and a reactant, DR i Initial deposition rate is the deposition rate of a thin film without the use of a film shielding agent. r The final deposition rate is the deposition rate of the film formed by adding the oxide film shielding agent during the above process. The deposition rate (DR) is the value measured by an ellipsometer at room temperature and pressure for a film with a thickness of 3 to 30 nm. The unit used is

[0229] *Non-uniformity: The highest and lowest thicknesses were selected from the thicknesses of the thin film measured using the above-mentioned ellipsometer, and the results were calculated using the following mathematical formula 2, and the results are shown in Table 1. Specifically, the thicknesses were measured at four locations on the east, west, south, and north edges of a 300 mm wafer and at one location in the center.

[0230] [Mathematical formula 2]

[0231] Unevenness % = [{(highest thickness - lowest thickness) / 2}×average thickness]×100

[0232] *SIMS (Secondary-ion mass spectrometry) C impurities: Ion sputtering was used to dig into the film axially, and the C impurity counts were considered when the sputtering time was 50 seconds where there was less contamination on the surface layer of the substrate, and the C impurity value was confirmed in the SIMS graph.

[0233] *Step coverage (%): The TEM of the sample was measured and calculated using the following Mathematical Formula 3, wherein the sample was horizontally cut 100 nm downward from the top (left figure) and 100 nm upward from the bottom (right figure) for the thin film deposited on a complex structure substrate with an aspect ratio of 22:1 by Example 1 to Example 2 and Comparative Examples 1 to Comparative Examples 3.

[0234] [Mathematical formula 3]

[0235] Step coverage % = (thickness deposited on the lower inner wall / thickness deposited on the upper inner wall) × 100

[0236] Table 1

[0237]

[0238] In the above table, CpHf is the abbreviation of Tris(dimethylamido)cyclopentadienyl hafnium, and TMA is the abbreviation of trimethylaluminum. As shown in Table 1 above, it can be confirmed that compared with Comparative Examples 1 and 3 which do not use the thin film shielding agent of the present invention, Examples 1 and 2 which use the thin film shielding agent of the present invention not only significantly improve the deposition rate reduction rate, but also have excellent impurity reduction characteristics.

[0239] Specifically, it was confirmed that the unevenness of 1.93% in Example 1 was not only very low compared to the unevenness of 8.33% in Comparative Example 1, but also the GPC reduction effect was 45%, which was significantly improved compared to the level of 20% in Comparative Example 1.

[0240] Specifically, Figures 2 to 4 As shown, it can be confirmed that the films of Examples 1 and 2 produced using the film shielding agent of the present invention have increased thickness in both the upper and lower portions, compared with Comparative Example 1 in which the film shielding agent of the present invention is not used.

[0241] In addition, it can be confirmed that compared with Comparative Example 2 which used other species than the appropriate species such as dimethyl sulfoxide, Examples 1 and 2 using the thin film shielding agent of the present invention not only significantly improved the deposition rate reduction rate but also had significant impurity reduction characteristics.

[0242] * Specifically, the step coverage in Example 1 using the thin film shielding agent of the present invention was 45%, which was more than twice the step coverage of 20% in Comparative Example 2 using dimethyl sulfoxide.

Claims

1. A thin film shielding agent used when depositing a metal oxide film or a non-metal oxide film on a substrate, characterized in that: The thin film shielding agent includes at least one element having an electronegativity between the electronegativity of the metal or non-metal constituting the oxide film and the electronegativity of oxygen, and is used to shield the deposition.

2. The thin film shielding agent according to claim 1, characterized in that The above-mentioned metal or non-metal is one or more selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd.

3. The thin film shielding agent according to claim 1, characterized in that: The film shielding agent is a compound containing four or more elements having an electronegativity ranging from 2.1 to 3.

1.

4. The thin film shielding agent according to claim 1, characterized in that: The above-mentioned film shielding agent is a compound having a structure represented by the following chemical formula 1, [Chemical formula 1] In the above chemical formula 1, R1 is H, OH, CH3, OCH3, OCH2CH3, OCH2CH2CH3, or an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 1 to 5 carbon atoms, or an alkynyl group having 1 to 5 carbon atoms, and X is m is an integer from 0 to 4.

5. The thin film shielding agent according to claim 1, characterized in that: The film shielding agent is one or more compounds selected from the group consisting of the following chemical formulas 1-1 to 1-9. [Chemical formulas 1-1 to 1-9] 6. A thin film forming composition, characterized in that Include: Precursor compounds constituting the deposited thin film layers; and Film masking agent, The above-mentioned film shielding agent is the film shielding agent according to any one of claims 1 to 5, The above-mentioned precursor compound is a compound represented by the following chemical formula 2: [Chemical formula 2] In the above chemical formula 2, M is one or more selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd, L 1 , L 2 , L 3 and L 4 as -H, -X, -R, -OR, -NR or Cp, and are the same as or different from each other, Wherein, -X is F, Cl, Br or I, -R is a C1-C10 alkyl, C1-C10 alkenyl or C1-C10 alkynyl, and is linear or cyclic, and the above L 1 , L 2 , L 3 and L 4 The number of the ions is 2 to 6 depending on the oxidation valence of the central metal (M).

7. The thin film forming composition according to claim 6, wherein The thin film shielding agent provides a shielding area for an oxide film, a nitride film, a metal film or a selective thin film thereof, and the shielding area is formed on the entire substrate or a portion of the substrate on which the oxide film, the nitride film, the metal film or a selective thin film thereof is formed.

8. The thin film forming composition according to claim 6, wherein When the total area of ​​the entire substrate or a portion of the substrate is set to 100%, the shielded area occupies 10 to 95% of the area, and the unshielded area occupies the remaining area.

9. The thin film forming composition according to claim 6, wherein The above-mentioned thin film improves step coverage during the formation of a stacked film of one or more selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd.

10. A method for forming a thin film, characterized in that: The following steps are involved: A thin film shielding agent and a precursor compound are injected into the chamber to form a deposition layer on the loaded substrate, wherein the thin film shielding agent is selected from one or more compounds having a structure represented by the following chemical formula 1, [Chemical formula 1] In the above chemical formula 1, R1 is H, OH, CH3, OCH3, OCH2CH3, OCH2CH2CH3, or an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 1 to 5 carbon atoms, or an alkynyl group having 1 to 5 carbon atoms, and X is m is an integer from 0 to 4.

11. The thin film forming method according to claim 10, characterized in that: The precursor compound and the thin film shielding agent are independently delivered into the chamber by VFC method, DLI method or LDS method. The above-mentioned thin film is a silicon nitride film, a silicon oxide film, a titanium nitride film, a titanium oxide film, a tungsten nitride film, a molybdenum nitride film, a hafnium oxide film, a zirconium oxide film, a tungsten oxide film or an aluminum oxide film.

12. A semiconductor substrate, characterized in that: Includes a thin film manufactured according to the thin film forming method according to claim 10.

13. The semiconductor substrate according to claim 12, characterized in that The film is a multi-layer structure of two or more layers.

14. A semiconductor device, characterized in that: Comprising the semiconductor substrate according to claim 12.