Conductive film, connection structure, and method for producing same

By neatly aligning the solder particle areas in the conductive film, the short circuit and conduction instability caused by uneven particle density in the micro-light emitting diode connection are solved, which improves connection reliability and reduces manufacturing costs.

CN118922923APending Publication Date: 2024-11-08DEXERIALS CORP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380029832.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-09-28
Filing Date
2023-03-10
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the installation of microlight emitting diodes, the existing conductive films have short circuit risks and conduction instability problems caused by uneven particle density in fine pitch connections, and the grading of solder particles increases manufacturing costs.

Method used

By neatly arranging and configuring the solder particle areas in the conductive film, the average value in the plane view of 100×100μm is set to SA, and the maximum and minimum values ​​are SA±80%, ensuring uniform distribution and conduction of solder particles Pass.

Benefits of technology

It is realized that the conduction is ensured and the occurrence of short circuits is suppressed in the micro-light emitting diode connection, which improves the reliability of the connecting structure and reduces the manufacturing cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922923A_ABST
    Figure CN118922923A_ABST
Patent Text Reader

Abstract

In the conductive film (100), particle regions (30) having a predetermined area are regularly distributed and arranged in plan view, and the particle regions (30) include a projection pattern of one conductive particle (20) or a projection pattern of a conductive particle group comprising a plurality of conductive particles (20). When the area of any one of the particle regions (30) is set to be S and the average value of the area S in the field of view of at least 100 * 100 [mu] m of the conductive film (100) is set to be SA, the maximum value and the minimum value of the area S are within SA + / -80%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a conductive film, a connection structure using the conductive film, and a method for manufacturing the same. Background Art

[0002] As the next generation of displays and light sources, sub-millimeter light-emitting diodes (Mini LED) and micro LEDs using light-emitting diodes (LED: Light Emitting Diode) as optical semiconductor elements have attracted attention. Micro LEDs are in the process of research and development, and the connection method with the substrate has not been fully established. On the other hand, in the installation of electronic components such as IC chips, conductive films in which a large number of conductive particles are dispersed in an insulating resin layer are widely used. When a conductive film is used, fine pitch connection can be performed, but due to the contact connection via the conductive particles, there are reliability issues. In addition, for the installation of micro LEDs using a conductive film, high loads and high pressures are also required in order to make the conductive particles stably contact the electrodes. Usually, in the case of driver ICs (Integrated Circuits: Integrated Circuits) and FPCs (Flexible Printed Circuits: Flexible Circuits), the connection is made by pressing, but in the case of micro LEDs, the installation area becomes too large, so there are concerns that there are limitations such as the load limit of the connecting device, and if it becomes a high load, it will be excessively loaded on the substrate side.

[0003] It is also known to use solder particles as conductive particles in fine pitch connections (Patent Document 1). Solder can perform bonding based on intermetallic compounds, so the reliability of conductive connection is high, and connection under low load can also be performed. However, in the case where the solder particles are made into a dispersed conductive film that is not neatly arranged and applied to fine pitch connections, the following undesirable conditions are worried about: if the particle density is too large, undesirable agglomeration will occur during connection, and conversely, if the particle density is too small, a sufficient amount of solder particles are not clamped between the electrodes, and the amount of solder particles required for bonding is insufficient. In particular, the electrodes of micro-LEDs are extremely small, so sometimes the space between the electrodes is also extremely narrow. Therefore, in order to achieve stable connection, the conductive particles need to be dispersed at a surface density above a certain level. On the other hand, if the surface density of the conductive particles is too large, the solder particles bridge between adjacent electrodes or between electrodes of adjacent micro-LEDs, and the risk of short circuit increases.

[0004] If solder particles are arranged one by one to form a conductive film with aligned particles, the amount and arrangement of solder particles can be appropriately controlled. However, the effort of classifying solder particles with large particle size variations in advance may increase the manufacturing cost of the conductive film.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2021-68842 Summary of the invention

[0008] Problems to be solved by the invention

[0009] Therefore, it is desirable to provide a conductive film in which solder particles that are not excessively classified are arranged in a regular pattern when a plurality of micro light-emitting diodes are mounted at a fine pitch.

[0010] An object of the present invention is to provide a conductive film which can ensure conduction after conductive connection and suppress the occurrence of short circuits without excessively classifying solder particles having large variations in particle size, thereby improving the reliability of a connection structure.

[0011] Solutions for solving problems

[0012] The present inventors have found that the above-mentioned problems can be solved by arranging metal particles such as solder particles having large variations in particle size in a particle region including one or more metal particles, and have completed the present invention.

[0013] That is, the present invention provides a conductive film, comprising: an insulating resin film; and a plurality of conductive metal particles carried on the insulating resin film, wherein when the conductive film is viewed from above, a particle region of a predetermined area including a projection pattern from one or more of the metal particles is arranged in a regular pattern, and the area of ​​one of the particle regions is set to S, and the average value of the area S in a surface field of at least 100×100 μm of the conductive film is set to S. A When the area S has a maximum and minimum value, it is S A Within ±80%.

[0014] In addition, the present invention provides a connection structure and a method for manufacturing the connection structure, in which a first electronic component is conductively connected to a second electronic component, the first electronic component has a plurality of first electrodes joined to the electrodes of the second electronic component, and a resin filling layer formed of an insulating resin is formed around the first electrodes, in which conductive metal particles or aggregates thereof are dispersed in a plurality of locations, and in a cross-section of the resin filling layer parallel to a joining surface between the first electrode and the electrode of the second electronic component, the total SP of the area when a figure projected from the metal particles or aggregates thereof contained in the inter-electrode area as a circle is regarded as a proportion of less than 35% with respect to the total area SR of an inter-electrode area divided by mutually adjacent first electrodes, and in the method for manufacturing the connection structure, the electrode of the first electronic component is conductively connected to the electrode of the second electronic component by the conductive film of the present invention.

[0015] Effects of the Invention

[0016] In the conductive film of the present invention, the particle region containing one or more metal particles is neatly arranged, and since the deviation of the amount of metal particles in the particle region is small, it is possible to ensure conduction while using metal particles with large deviation in particle size without excessively classifying them, and to perform conductive connection that suppresses the occurrence of short circuits. Therefore, in the connection structure that uses the conductive film of the present invention for conductive connection, it is possible to achieve both ensuring conduction between electronic components and suppressing short circuits, and to improve reliability. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 is a cross-sectional view of a conductive film of the present invention.

[0018] Figure 2 is a top perspective view of a conductive film of the present invention.

[0019] Figure 3 It is an enlarged top perspective view of the conductive film of the present invention.

[0020] Figure 4 is a top perspective view of a conductive film of the present invention.

[0021] Figure 5 It is a cross-sectional view of the connection structure of the present invention.

[0022] Figure 6 It is an explanatory diagram of the inter-electrode region of the connection structure.

[0023] Figure 7 This is a microscope photograph of the conductive film of the present invention.

[0024] Figure 8 This is an explanatory diagram of a microchip used for evaluating resin filling properties.

[0025] Fig. 9 This is an explanatory diagram of a microchip used for evaluating resin filling properties.

[0026] Fig.10 This is a microscope photograph of the inter-electrode region observed by observing the LED chip of the mounted body of the example through the glass substrate.

[0027] Fig.11 This is a microscope photograph of the inter-electrode region observed through the glass substrate of the LED chip of the mounted body of the comparative example. DETAILED DESCRIPTION

[0028] The conductive film of the present invention is useful for mounting optical semiconductor elements such as sub-millimeter light-emitting diodes and micro-light-emitting diodes (hereinafter, although they are collectively referred to as "micro-light-emitting diodes", sub-millimeter light-emitting diodes are not excluded).

[0029] <Conductive film>

[0030] Figure 1 An arbitrary cross section in the thickness direction of the conductive film 100 according to one embodiment of the present invention is shown. Figure 2 1 is a top perspective view of the conductive film 100. Figure 1 As shown, the conductive film 100 has a plurality of conductive particles 20 as metal particles arranged on or near the surface of a single-layer insulating adhesive film (adhesive film) 10. It should be noted that the insulating adhesive film 10 may also be composed of multiple layers. In addition, the conductive film 100 may be an anisotropic conductive film (ACF: Anisotropic Conductive Film).

[0031] (Plane grid pattern and particle area)

[0032] like Figure 2 As shown, in the conductive film 100, when viewed from above (i.e., when viewed from the Z direction), Figure 2 In the X-Y plane in FIG. 1 , particle regions 30 of a predetermined area are regularly dispersed and arranged, and the particle regions 30 include a projection pattern of a conductive particle 20 or a projection pattern of a conductive particle group composed of a plurality of conductive particles 20. Here, "dispersed" refers to a state in which adjacent particle regions 30 are separated from each other without contacting each other.

[0033] The conductive particles 20 are arranged in a state of being a single conductive particle or a group of two or more conductive particles. Figure 2 The particle region 30 is a particle region 30 having a predetermined area with a lattice point P of the plane lattice pattern represented by a dotted line as the center or the center of gravity. Figure 2The dotted lines are shown in the form of intersections, and are arranged regularly corresponding to the plane lattice pattern. Therefore, the particle region 30 with the lattice point P of the plane lattice pattern as the center or the center of gravity is also arranged regularly. In this way, by making the plurality of particle regions 30 arranged regularly using the plane lattice pattern, in the connection structure using the conductive film 100 for conductive connection, it is possible to achieve both ensuring the conduction between the electronic components and suppressing the short circuit.

[0034] Figure 3 The main part of the perspective view when the conductive film 100 is viewed from above is enlarged and shown. Figure 3 For example, the particle region shown by reference numeral 30A includes the projection pattern of one conductive particle 20, the particle region shown by reference numeral 30B includes the projection patterns of two conductive particles 20, and the particle region shown by reference numeral 30C includes the projection patterns of four conductive particles 20 (here, the symbols "A, B, C" in reference numerals 30A, 30B, and 30C are marked for the convenience of explanation and for the purpose of distinction).

[0035] For example, when observing 100 particle regions 30, the conductive film 100 preferably includes more than 10 particle regions 30, more preferably includes more than 30 and less than 90 particle regions 30, and further preferably includes more than 40 and less than 80 particle regions 30, wherein the particle regions 30 include a conductive particle group consisting of three or more conductive particles 20. In the present invention, when the particle regions 30 are arranged neatly as a whole, the particle regions 30 that form a conductive particle group by aggregating or agglomerating three or more conductive particles 20 exist randomly, and the amount of conductive particles 20 required for the connection of the electrode can be ensured without excessive classification, thereby achieving both connection stability and cost increase suppression.

[0036] exist Figure 3In the embodiment, the diameter D of a particle region 30 and the shortest distance L between adjacent particle regions 30 are preferably appropriately set in consideration of the total volume of the conductive particles 20 contained in one particle region 30. In this case, it is important to set the diameter D and the shortest distance L in consideration of the viewpoint of ensuring conduction by fully capturing the conductive particles 20 through the electrodes and preventing short circuits by preventing the conductive particles 20 from crossing multiple electrodes when melted. In the installation of the micro-light-emitting diode, the diameter D and the shortest distance L can be set according to the usual electrode layout. For example, when the particle region 30 is circular, its diameter D is preferably smaller than the length of the space between the electrodes of the micro-light-emitting diode. The diameter D is preferably in the range of 1.0 μm to 10 μm, and more preferably in the range of 1.5 μm to 4.0 μm. In this case, the shortest distance L between the particle regions 30 is preferably in the range of 1.0 μm to 20 μm, and more preferably in the range of 1.5 μm to 4.0 μm.

[0037] The particle region 30 may be a square, a rectangle, a triangle, or a polygon with a pentagon or more as described below. In the case of a square, a rectangle, or a triangle, one side may be within a range of 1 μm to 10 μm.

[0038] When there are multiple conductive particles 20 in each particle region 30, the multiple conductive particles 20 may exist at different positions in the thickness direction. That is, in the particle region 30, the multiple conductive particles 20 may exist three-dimensionally in the surface direction (X-Y direction) and thickness direction (Z direction) of the conductive film 100.

[0039] In addition, the arrangement of the conductive particles 20 in the particle region 30 in the thickness direction is not particularly limited, but is preferably arranged in a range of 0.5 μm or more and 8 μm or less from the surface of the conductive film 100 in the thickness (depth) direction, and more preferably arranged in a range of 1 μm or more and 6 μm or less. From another point of view, the arrangement of the conductive particles 20 in the particle region 30 in the thickness direction is preferably in a range of 10% or more and 200% or less relative to the diameter D of the particle region 30.

[0040] In addition, in the particle region 30, it is preferred that the plurality of conductive particles 20 are gathered in a manner that is easy to become one when melted. In this case, the adjacent particles may be in contact or separated, but preferably in contact. In addition, the plurality of conductive particles 20 may exist in the particle region 30 in a coagulated state.

[0041] The shape of the particle region 30 is not particularly limited as long as it can contain the projection pattern of one or more conductive particles 20, and various shapes can be used. The shape of the particle region 30 can be, for example, a circle, a polygon such as a triangle / quadrilateral, or an amorphous shape. When the conductive particle 20 is circular (including an ellipse) when viewed from above, Figure 2 , Figure 3 As shown in the example, the shape of the particle region 30 is also preferably a circle with similarity. In the case of a circle, the particle region 30 can be assumed to be a perfect circle with the lattice point P as the center and having the outermost circumference of the projection figure of the conductive particle 20, and defined as the area surrounded by the perfect circle. Therefore, when the particle region 30 is obtained from the film, the size and shape of the particle region 30 will deviate within a certain range. In this case, the average value can be obtained from N=200 or more by observation under an optical microscope and set as the size of the particle region 30 (for example, the diameter D). In addition, in the case of a polygon, the particle region 30 can be considered as an inscribed circle with the lattice point P as the center of gravity and containing the projection figure of the conductive particle 20, which can be considered in the same way as a circle. In particular, in the case of a polygon with a shape of pentagon or more, it is preferably considered as an inscribed circle containing the polygon in the same way as a circle.

[0042] The plane lattice pattern is not limited to the hexagonal lattice. For example, Figure 4 The square grid is shown. The grid point P is Figure 4 The dotted lines are shown in the form of intersections, and are arranged regularly corresponding to the plane lattice pattern. Furthermore, the plane lattice pattern can also be a rhombus lattice, a rectangular lattice, a parallelogram lattice, etc. Figure 2 The lattice points P of the hexagonal lattice shown are arranged at equal intervals, and therefore it is most preferable from the viewpoint of achieving both ensuring conduction between electronic components and suppressing short circuits.

[0043] It should be noted that the regular arrangement of the plurality of particle regions 30 is not limited to the neat arrangement using a planar lattice pattern, and may be various regular arrangements. When the plurality of particle regions 30 are neatly arranged, the lattice axis or arrangement axis of the arrangement may be parallel to the long dimension direction Y of the conductive film 100, the short dimension direction X orthogonal to the long dimension direction Y, or may intersect with the long dimension direction Y of the conductive film 100. In addition, the neat arrangement of the plurality of particle regions 30 may be determined according to the width of the connected terminals, the terminal spacing, the layout, etc.

[0044] In order to achieve both electrode-based capture stability and short circuit suppression, the plurality of particle regions 30 are preferably arranged neatly when the conductive film 100 is viewed from above, and the positions of a conductive particle 20 or a conductive particle group consisting of a plurality of conductive particles 20 are roughly aligned in the film thickness direction Z.

[0045] (Area deviation of particle area)

[0046] For the conductive film 100, the area of ​​any particle region 30 is set to S, and the average value of the area S in the surface field of the conductive film 100 that is at least 100×100 μm and includes more than 20 particle regions 30 (referred to as "the surface field of at least 100×100 μm" in this specification) is set to S A When the area S has a maximum and minimum value, it is S A Within ±80%, preferably S A Within ±70%. The maximum and minimum values ​​of area S are S A Within ±80% means that the deviation of the total volume of one or more conductive particles 20 existing in each particle region 30 is small, which can ensure the conduction of the connection structure after mounting the micro light-emitting diode using the conductive film 100 and prevent short circuit.

[0047] On the other hand, the maximum value of area S exceeds S A When the conductive particles 20 are melted, they spread beyond the space between adjacent electrodes or adjacent micro-LEDs and may cause a short circuit. A In the case of -80%, the volume of the conductive particles 20 within the area of ​​one electrode to be connected is insufficient, and it may be difficult to ensure conduction.

[0048] It should be noted that, based on the standard of "a surface field of at least 100×100 μm", it is preferred to observe more than 5 (N=100 or more) surface fields of 100×100 μm, and more preferably to observe more than 10 (N=200 or more) surface fields of 100×100 μm and take the average.

[0049] The maximum, minimum, and average values ​​S of the area S of a particle region 30 A There is no particular limitation. As an example, if the area of ​​the electrodes of a micro-LED and the area of ​​the inter-electrode region (space) are taken into consideration, the maximum value of the area S is preferably 7.0 μm. 2 Above and 9.0μm 2 The following range, more preferably 7.5 μm 2 Above and 8.5μm 2 In addition, the minimum value of the area S is preferably 0.5 μm 2 Above and 2.5μm 2 The following range, more preferably 1.0 μm 2 Above and 2.0μm 2 In addition, the average value S of the area S is APreferably at 4.0 μm 2 Above and 6.0μm 2 The following range, more preferably 4.5 μm 2 Above and 5.5μm 2 Within the following range.

[0050] (Area ratio of particle area)

[0051] In addition, in the surface field of at least 100×100 μm of the conductive film 100, the ratio of the total area S1 of the aligned particle region 30 to the total area S2 of the pattern projected from all the conductive particles 20 is preferably 90% or more. In other words, the ratio of the area of ​​the projected pattern of the conductive particles 20 that deviates from the aligned particle region 30 to the total S2 is preferably less than 10%. The ratio of the total area S1 of the particle region 30 to the total area S2 projected from all the conductive particles 20 being 90% or more means that most of the conductive particles 20 present in the conductive film 100 are present in the aligned particle region 30. In the manufacturing process of the conductive film 100, in the stage of fixing the conductive particles 20 to the insulating adhesive film 10, most of the conductive particles 20 can be arranged in the particle region 30 by using a transfer mold. However, there is a possibility that the conductive particles 20 that inevitably deviate from the particle region 30 are generated. In this way, if the ratio of the conductive particles 20 that inevitably deviate from the particle area 30 is too large, the conductive particles 20 are close to being randomly dispersed, so sometimes the conductive particles 20 are concentrated, and a short circuit occurs between adjacent electrodes or adjacent micro-LEDs, or vice versa, it is difficult to ensure conduction in the electrodes that are connected. In contrast, when the proportion of the total area S1 relative to the total area S2 is greater than 90%, most of the conductive particles 20 or conductive particle groups are arranged in the particle area 30 with the lattice point P of the plane lattice pattern as the center or center of gravity, and become neatly arranged, which can achieve both ensuring conduction and preventing short circuits. From this point of view, the ratio of the total area S1 to the total area S2 is more preferably in the range of greater than 95% and less than 100%, and further preferably in the range of greater than 98% and less than 100%.

[0052] In addition, if Figure 2 and Figure 4 As shown in the example, by using a plane lattice pattern to neatly arrange the particle area 30, it is easy to identify the conductive particles 20 existing in the neatly arranged particle area 30 and the conductive particles 20 existing away from the neatly arranged particle area 30, and it is easy to control the ratio of the total area S1 to the total area S2, so it is preferred.

[0053] (Total area of ​​adjacent particle regions)

[0054] In the conductive film 100, the total area S3 of two particle regions 30 adjacent to each other at the shortest distance is preferably within 1 μm. 2 Above and 20μm 2 The following range, more preferably 5 μm 2 Above and 16μm 2 By making the total area S3 of two adjacent particle regions 30 at the shortest distance within 1 μm 2 Above and 20μm 2 Within the following range, it is possible to achieve both ensuring the conduction of the connection structure after mounting the micro LED using the conductive film 100 and preventing short circuits. 2 In the case of , the conductive particles 20 may spread beyond the space between adjacent electrodes or adjacent micro-LEDs when melted, and may cause a short circuit. 2 In such a case, the volume of the conductive particles 20 within the area of ​​one electrode to be connected is insufficient, and it may be difficult to ensure conduction.

[0055] (Area occupancy of particle region)

[0056] In the surface field of at least 100×100μm of the conductive film 100, the proportion (area occupancy) of the total area S1 of the particle region 30 is preferably in the range of 5% to 25%, and more preferably in the range of 10% to 20%. By making the area occupancy of the particle region 30 in the range of 5% to 25%, it is possible to achieve both ensuring the conduction of the connection structure after the micro-light-emitting diode is installed using the conductive film 100 and preventing short circuits. That is, when the area occupancy of the particle region 30 exceeds 25%, the conductive particles 20 diffuse beyond the space between adjacent electrodes or adjacent micro-light-emitting diodes when melted, and short circuits may occur. On the other hand, if the area occupancy of the particle region 30 is less than 5%, the volume of the conductive particles 20 is insufficient relative to the electrode area to be connected, and it is sometimes difficult to ensure conduction. The area occupancy of the particle region 30 can be calculated by the following formula based on the surface field of at least 100×100μm.

[0057] Area occupancy (%) = n × S A ×100

[0058] Where n is the number density of particles in the particle area 30 in a surface field of at least 100×100 μm (unit: particles / 0.01 mm 2 ), S A It refers to the average value of the area of ​​the particle region 30.

[0059] As for the conductive film 100, as long as the area occupancy is within the above range, the value of the number density n of the particle region 30 is not particularly limited. If the number density n is too small, the number of conductive particles 20 captured by the electrode is reduced, and it is difficult to conduct conductive connection of the micro-LED, etc. If the number density n is too large, a short circuit may occur. Therefore, as the number density n, the total number of the particle regions 30 arranged in a regular arrangement in the surface field of at least 100×100 μm of the conductive film 100 is preferably within the range of 100 or more and 1500 or less, and more preferably within the range of 200 or more and 1000 or less.

[0060] As shown above, a top view area S of the particle region 30 and an average area S A , the total area S1, and the number density n can be measured based on the observation image of the film surface using an electron microscope such as a metallographic microscope, SEM (scanning electron microscope), etc. As an example, the top-view area S and the number density n of the particle region 30 can be measured using the observation image obtained using the SEM for a surface field of at least 100×100 μm (preferably 5 or more, more preferably 10 or more) arbitrarily selected from the conductive film 100. In the case where the particle region 30 is circular, it is assumed that a perfect circle having the outermost circumference of the projection pattern passing through the conductive particles 20 is assumed, and the area of ​​the region surrounded by the perfect circle is taken as the top-view area S.

[0061] In addition, the total area S2 of the pattern projected from all the conductive particles 20 can also be measured based on the observation image of the film surface using a metallographic microscope, SEM or other electron microscope. For the above measurement, for example, image analysis software such as WinROOF (manufactured by Mitani Shoji Co., Ltd.) and A-image-kun (Japanese: A-image-kun) (registered trademark) (manufactured by Asahi Kasei Engineering Co., Ltd.) can be used.

[0062] (Conductive particles)

[0063] As the conductive particles 20, any conductive particles that melt due to heat may be used, for example, solder particles are preferably used. In the case where the conductive particles 20 are solder particles, the solder particles contain tin or a tin alloy, and as tin alloys, for example, Sn-In, Sn-Bi, Sn-Ag-Cu, Sn-Cu, etc. are preferred. Among them, if the bonding strength is considered, it is preferably Cu, and more preferably Sn-Ag-Cu (for example, Sn: 96.5 mass%, Ag: 3 mass%, Cu: 0.5 mass%). In addition to solder, for example, any one or more metals such as Au, Cu, Ag, Ni, Al, Sn, Ti, or alloys of these multiple metals can be listed. If the resistance value and migration are considered, Au, Cu, and Ni are preferred.

[0064] The average particle size (median particle size: D 50 ) is not particularly limited, and in the case of solder particles, for example, it is preferably in the range of 0.5 μm to 10 μm, and more preferably in the range of 1 μm to 5 μm. The average particle size can be measured using an image-type or laser-type particle size distribution meter.

[0065] (Insulating adhesive film)

[0066] As the material of the insulating adhesive film 10, a thermal polymerizable resin is preferably used. For example, a thermal free radical polymerizable resin containing an acrylate compound and a thermal free radical polymerization initiator; a thermal cationic polymerizable resin containing an epoxy compound and a thermal cationic polymerization initiator; a thermal anionic polymerizable resin containing an epoxy compound and a thermal anionic polymerization initiator, etc. can be used. In addition, the insulating adhesive film 10 can contain a silane coupling agent, a pigment, an antioxidant, an ultraviolet absorber, etc. as appropriate as needed.

[0067] When the conductive particles 20 are solder particles, the resin constituting the insulating adhesive film 10 preferably has a curing temperature higher than the melting point of the solder, and preferably has a temperature reaching the minimum melt viscosity lower than the melting point of the solder.

[0068] By setting the curing temperature of the resin constituting the insulating adhesive film 10 to be above the melting point of the solder, the solder particles can be melted while the resin is melted or softened by heating so that the solder particles are sandwiched between the electrodes. Here, the curing temperature is the exothermic peak temperature obtained by measuring a sample of 5 mg or more in an aluminum crucible, performing differential scanning calorimetry (DSC) at a temperature range of 30 to 250°C and a heating rate of 10°C / min.

[0069] In addition, the temperature at which the resin constituting the insulating adhesive film 10 reaches the minimum melt viscosity is preferably within the range of -10°C to -50°C compared to the melting point of the solder particles, and more preferably within the range of -10°C to -40°C compared to the melting point. If the temperature at which the minimum melt viscosity is reached is such that the minimum melt viscosity can be reached before the solder particles melt, the solder particles are melted after the resin melts, and then the resin is solidified, so that a good solder joint can be obtained. The temperature at which the minimum melt viscosity is reached is measured using a rotational rheometer (manufactured by TA Instruments) with a heating rate of 10°C / min, a constant measuring pressure of 5g, and a measuring plate diameter of 8mm. The measuring temperature is preferably within the measuring range of, for example, above 60°C and below 250°C. The range of the measuring temperature can be appropriately adjusted according to the material of the insulating adhesive film 10.

[0070] The minimum melt viscosity of the resin constituting the insulating adhesive film 10 is preferably less than 10000 Pa·s, more preferably 3000 Pa·s or less. If the minimum melt viscosity is too high, the resin may not melt during thermocompression bonding, and the filling property between electrodes may decrease.

[0071] In addition, it is preferable that the insulating adhesive film 10 contains a flux component. The flux component may be in a state where the surface of the conductive particles 20 is coated. As the flux component, for example, carboxylic acids such as levulinic acid, maleic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, and sebacic acid are preferably used. The flux component has the functions of removing foreign matter or oxide film on the electrode surface and anti-oxidation of the electrode surface; and has the function of reducing the surface tension of the melt of the conductive particles 20.

[0072] The insulating adhesive film 10 can be formed by forming a coating composition containing the above-mentioned resin into a film by a coating method and drying the film, or by forming the film by a known method.

[0073] The thickness of the insulating adhesive film 10 is preferably within a range of 1 / 5 or more and 3 or less of the diameter D of the particle region 30, but the conductive particles 20 may be exposed from the insulating adhesive film 10. In addition, the thickness of the insulating adhesive film 10 is preferably less than 1 / 2 of the height of the micro-LED chip, and more preferably about 1 / 3 of the height of the micro-LED chip, so that after the micro-LED chip is installed, the chip is not buried in the insulating adhesive film 10.

[0074] In addition, in order to ensure the holding force of the micro-LED chip, the insulating adhesive film 10 needs to be fully filled on the electrode surface side of the micro-LED chip. Therefore, the thickness of the insulating adhesive film 10 is preferably 1 / 2 or more relative to the electrode height of the micro-LED chip, and more preferably the same as the electrode height. From the above point of view, as an example, the thickness of the insulating adhesive film 10 can be in the range of 1 μm or more and 10 μm or less, preferably in the range of 2 μm or more and 8 μm or less.

[0075] If necessary, insulating fillers such as silica particles, alumina, and aluminum hydroxide may be added to the insulating adhesive film 10. The amount of the insulating filler is preferably within a range of 3 parts by mass to 40 parts by mass based on 100 parts by mass of the resin constituting these layers.

[0076] <Method for producing conductive film>

[0077] Next, a method for manufacturing the conductive film 100 will be described. Here, an example of manufacturing the conductive film 100 of the present invention using a transfer mold will be described. When a transfer mold is used, the conductive film 100 can be obtained by, for example, the following steps A and B.

[0078] (Process A)

[0079] First, one or more conductive particles 20 are added to the concave portions of a transfer mold having a plurality of concave portions formed therein.

[0080] As the transfer mold used, for example, a transfer mold obtained by forming openings in inorganic materials such as silicon, various ceramics, glass, stainless steel and other metals, and organic materials such as various resins by a known opening forming method such as photolithography can be used. In addition, the transfer mold can be in the form of a plate or a roll.

[0081] As the shape of the concave portion of the transfer mold, examples can be shown: cylindrical, cylindrical, quadrangular, etc., truncated cones, truncated pyramids, cones, quadrangular pyramids, etc. The arrangement of the concave portions is preferably a lattice shape corresponding to the particle region 30 of the plane lattice pattern. The depth of the concave portion can be determined in a manner such that the diameter D of the particle region 30 becomes a desired size according to the spacing, size, and space width of the electrodes to be conductively connected, and the total volume, average particle size, etc. of the conductive particles 20. The transfer mold used in step A can be made using a known method.

[0082] (Process B)

[0083] Next, a thermopolymerizable composition containing a thermopolymerizable compound, a thermopolymerization initiator, and, if necessary, an insulating filler is pressed against the conductive particles 20 in the transfer mold, thereby forming the conductive film 100 to which the conductive particles 20 are transferred.

[0084] By adjusting the pressing force in step B, the degree of embedding of the conductive particles 20 in the insulating adhesive film 10 can be changed. By increasing the degree of pressing, the degree of embedding of the conductive particles 20 in the insulating adhesive film 10 can be increased. Thus, a conductive film 100 having a structure in which the conductive particles 20 are arranged on the surface or near the surface of the insulating adhesive film 10 can be obtained.

[0085] The deviation of the total volume amount of the conductive particles 20 contained in each particle region 30 is preferably small. In order to average the total volume amount of the conductive particles 20 contained in each particle region 30, it is important to make the amount of the conductive particles 20 added to the concave portion of the transfer mold in step A close to uniform. For this purpose, for example, it is preferable to implement one or more of the following a) to c):

[0086] a) classifying the conductive particles 20 in advance to control the deviation of the particle size within a certain range;

[0087] b) determining the amount of conductive particles 20 to be added to the concave mold in consideration of the relationship between the size (diameter and depth) of the concave mold and the size (average particle size, minimum particle size, maximum particle size) of the conductive particles 20;

[0088] c) After the conductive particles 20 are added to the concave mold, a step of leveling the mold using, for example, a brush or a scraper is provided.

[0089] Here, the deviation of the particle size of the conductive particles 20 can be calculated by an image-type particle size analyzer, etc. The particle size of the conductive particles 20 as raw material particles not arranged in the conductive film 100 can be obtained using, for example, a wet flow particle size / shape analyzer FPIA-3000 (manufactured by Malvern Panalytical).

[0090] The conductive film 100 can be preferably used for conductive connections at fine pitches, such as when micro-LEDs are mounted on substrates. For example, the conductive film 100 can be preferably used for conductive connections or anisotropic conductive connections between first electronic components such as micro-LEDs, sub-millimeter LEDs, IC chips, IC modules, FPCs, and second electronic components such as FPCs, glass substrates, rigid substrates, and ceramic substrates. It should be noted that the reaction rate of the conductive film is preferably less than 25%, more preferably less than 20%, and further preferably less than 15%. Thus, the manufacturing of the connection structure can be carried out stably. The reaction rate is the ratio of the amount of reduction in the thermally polymerizable compound after the formation of the conductive film to the amount of the thermally polymerizable compound before the formation. The method for determining the reaction rate will be described below.

[0091] <Conductive film modification plan>

[0092] For example, in the case of a micro-component such as a micro-LED, the conductive film may be a single piece of a specified unit such as one pixel unit of a set of RGB. Single pieces may be provided respectively according to each electrode on the substrate side corresponding to each electrode of the micro-LED. The shape of the single piece is not particularly limited and may be appropriately set according to the size of the electronic component to be connected. In the case of forming a single piece of conductive film on a substrate film by using a laser lift-off (LLO: Laser Lift Off) device (for example, trade name: Invisi LUM-XTR, manufactured by Shin-Etsu Chemical Co., Ltd.) (refer to Japanese Patent Publication No. 2017-157724), in order to suppress the occurrence of curling and notches, the shape of the single piece is preferably selected from at least one of a polygon formed by an obtuse angle, a polygon with rounded corners, an ellipse, an oblong, and a circle. The electrodes on the substrate side may be separately provided with single pieces of at least one selected from such shapes, and the electrodes of the micro-LED may be connected by different single pieces.

[0093] The size (length x width) of a single piece of the conductive film is appropriately set according to the size of the electronic component to be connected, and the ratio of the area of ​​the single piece to the area of ​​the electronic component is preferably 2 or more, more preferably 4 or more, and further preferably 5 or more. In addition, the thickness of the single piece is the same as the thickness of the conductive film, preferably the average particle size of the conductive particles plus 1 to 4 μm, particularly preferably the average particle size of the conductive particles plus 1 to 2 μm, preferably 1 μm or more and 10 μm or less, more preferably 1 μm or more and 6 μm or less, and further preferably 2 μm or more and 4 μm or less.

[0094] In addition, the distance between the single pieces of the conductive film on the substrate film is preferably 3 μm or more, more preferably 5 μm or more, and further preferably 10 μm or more. In addition, the upper limit of the distance between the single pieces is preferably 3000 μm or less, more preferably 1000 μm or less, and further preferably 500 μm or less. When the distance between the single pieces is too small, the transfer of the single piece using the LLO device becomes difficult. When the distance between the single pieces is large, the method of attaching the single piece is preferred. The distance between the single pieces can be measured using a microscope (optical microscope, metal microscope, electron microscope, etc.).

[0095] <Method for producing a modified conductive film>

[0096] The single sheet of the conductive film can be formed by slit, half cut, or by using a laser lift-off device. When the single sheet is formed using an LLO device, the base film only needs to be transmissive to the laser, and preferably quartz glass having high transmittance over all wavelengths.

[0097] When forming a single piece of a conductive film using an LLO device, a conductive film provided on a base film is irradiated with laser light from the base film side, and the irradiated portion of the conductive film is removed, thereby forming a single piece of a conductive film in a predetermined shape on the base film.

[0098] For example, by using a mask having a quadrilateral opening window, unnecessary portions of the conductive film are removed from the base film, and a single piece of a predetermined shape can be formed from the remaining portion of the conductive film. Also, for example, by using a mask having a light shielding portion of a predetermined shape formed in the opening window, unnecessary portions of the conductive film around the single piece are removed from the base film, and a single piece of a predetermined shape can be formed from the remaining portion of the conductive film.

[0099] In addition, when a laser stripping device is used to form a single sheet, the reaction rate of the single sheet is 25% or less, preferably 20% or less, and more preferably 15% or less. In this way, excellent transferability can be obtained. It should be noted that the reaction rate of the curable resin film before laser irradiation and the single sheet obtained after laser irradiation can be determined by, for example, using FT-IR, by the reduction rate of the reactive group. For example, in the case of a curable resin film using the reaction of an epoxy compound, infrared rays can be irradiated to the sample, and the IR spectrum can be measured to determine the methyl group (2930cm -1 Nearby) and epoxy (914cm -1 The peak height of the epoxy group (near the peak height of the methyl group) is calculated as the ratio of the peak height of the epoxy group to the peak height of the methyl group before and after the reaction (for example, before and after laser irradiation) as shown in the following formula.

[0100] Reaction rate (%) = {1-(a / b) / (A / B)}×100

[0101] In the above formula, A is the peak height of the epoxy group before the reaction, B is the peak height of the methyl group before the reaction, a is the peak height of the epoxy group after the reaction, and b is the peak height of the methyl group after the reaction. It should be noted that when other peaks overlap with the peak of the epoxy group, the peak height of the fully cured sample (reaction rate 100%) can be set to 0%.

[0102] <Utilization of conductive film (connection structure, method for producing the same)>

[0103] The conductive film of the present invention can be used by being attached to an article in the same way as the conductive film of the past, and the article to be attached is not particularly limited. Therefore, a connection structure formed by connecting the first member and the second member via a conductive film, and a method for manufacturing a connection structure by arranging a conductive film between the first member and the second member for connection are also part of the present invention. For example, in the case where the conductive film is constituted as an anisotropic conductive film by using conductive particles as a filler, a thermocompression bonding tool can be used to use the anisotropic conductive film for anisotropic conductive connection between a first electronic component and a second electronic component, wherein the first electronic component is a semiconductor element using PN connection (a power generation element such as a solar cell, an imaging element such as a CCD, a sub-millimeter light-emitting diode with a side of the chip of about 50 μm to 200 μm, a light-emitting element such as a micro-light-emitting diode with a side of the chip less than 50 μm, a Peltier element), other various semiconductor elements, IC chips, IC modules, FPCs, etc., and the second electronic component is an FPC, a glass substrate, a plastic substrate, a rigid substrate, a ceramic substrate, etc., and the conductive film can also be used as a conductive film for electronic components in uses other than anisotropic conductive connection. It should be noted that the surface of the article to which the conductive film is bonded may be smooth or may have a step portion or a convex shape.

[0104] As a specific method of using the conductive film, for example, when the first electronic component is a micro-light-emitting diode, an IC chip, or an FPC containing a semiconductor element, and the second electronic component is a substrate, the first electronic component is usually placed on the side of a press tool, and the second electronic component is placed on a workbench opposite to the first electronic component. The conductive film, preferably a single piece thereof, is temporarily pasted to the second electronic component in advance by a laser lift-off method, and the first electronic component and the second electronic component are thermally pressed using a press tool. In this case, a single piece of the conductive film may be temporarily pasted to the first electronic component instead of the second electronic component in advance. In addition, the first electronic component is not limited to an IC chip or an FPC containing a semiconductor element. In particular, when the first electronic component and the second electronic component are substrates, they may have, for example, a silicone rubber layer. The silicone rubber layer may be polydimethylsiloxane (PDMS).

[0105] <Connection structure>

[0106] Figure 5 2 is a cross-sectional view showing a structural example of a connection structure obtained by using the conductive film 100. The connection structure 200 is a micro light emitting diode assembly in which a micro light emitting diode element 50 as a first electronic component and a substrate 60 as a second electronic component are conductively connected or anisotropically conductively connected using the conductive film 100. Here, the case where the conductive particles 20 in the conductive film 100 are solder particles is described.

[0107] like Figure 5 As shown, the connection structure 200 includes: a micro-LED element 50; a substrate 60; and a resin filling layer 101 filled between the micro-LED element 50 and the substrate 60. It should be noted that Figure 5 In the figure, the surface direction parallel to the bonding surface between the electrodes 51, 52 of the micro-LED element 50 and the electrodes 61, 62 of the substrate 60 is set as an X-Y plane composed of the X-axis direction and the Y-axis direction which are orthogonal to each other, and the crimping direction of the first electronic component and the second electronic component which is perpendicular to the X-Y plane is set as the Z-axis direction.

[0108] The micro-LED element 50 includes an electrode 51 and an electrode 52. When a voltage is applied between the electrode 51 and the electrode 52, carriers are concentrated in the active layer in the element and emit light by recombination. The height of the electrodes 51 and 52 can be appropriately set according to the size of the micro-LED element 50, for example, preferably in the range of 0 μm to 10 μm, more preferably in the range of 0 μm to 7 μm, and further preferably in the range of 0 μm to 5 μm.

[0109] The length of the space between the electrode 51 and the electrode 52 (the space between the electrodes) can be appropriately set according to the size of the micro-LED element 50, for example, preferably within the range of 3 μm to 15 μm, more preferably within the range of 3 μm to 12 μm, and further preferably within the range of 5 μm to 10 μm.

[0110] The substrate 60 has electrodes 61 and 62 on a base material. The electrodes 61 and 62 are respectively arranged at positions corresponding to the electrodes 51 and 52 of the micro light-emitting diode element 50. Examples of the substrate 60 include a printed circuit board, a glass substrate, a flexible substrate, a ceramic substrate, a plastic substrate, and a semiconductor substrate (IC chip).

[0111] The resin filling layer 101 is formed when the conductive film 100 is in a film shape after bonding. The resin filling layer 101 is filled between the micro-LED element 50 and the substrate 60 around the solder joint 21 where the electrodes 51, 52 of the micro-LED element 50 are bonded to the electrodes 61, 62 of the substrate 60. In the resin filling layer 101 filled between the micro-LED element 50 and the substrate 60, the conductive particles 20 that are not involved in bonding are dispersed in the form of one or more aggregates.

[0112] The electrodes 51 and 52 of the connection structure 200 as the terminals on the micro-LED element 50 side and the electrodes 61 and 62 as the terminals of the substrate 60 are respectively bonded at the solder joints 21. That is, the solder particles as the conductive particles 20 in the conductive film 100 are melted and solidified, and an alloy (intermetallic compound) is formed between the solder particles and the electrode material. Through the solder joints 21, conduction is achieved between the electrode 51 of the micro-LED element 50 and the electrode 61 of the substrate 60, and between the electrode 52 of the micro-LED element 50 and the electrode 62 of the substrate 60.

[0113] <Method for producing a connection structure>

[0114] The connection structure 200 can be manufactured by sandwiching the conductive film 100 between the micro-LED element 50 and the substrate 60 and performing thermocompression bonding. The solder particles as the conductive particles 20 in the conductive film 100 are melted and solidified by thermocompression bonding to form the solder joint 21. In addition, after sandwiching the conductive film 100 between the micro-LED element 50 and the substrate 60, the solder particles can be melted by heat treatment (reflow soldering) to manufacture the connection structure 200. The reflow soldering can be atmospheric pressure reflow soldering or vacuum reflow soldering, preferably vacuum reflow soldering.

[0115] Figure 6Represents a cross section of the resin filling layer 101 parallel to the bonding surface between the electrodes 51, 52 of the micro-LED element 50 and the electrodes 61, 62 of the substrate 60 in the connection structure 200. Here, the "cross section of the resin filling layer 101 parallel to the bonding surface" is a hypothetical surface, for example, it can be a polished cross section obtained by polishing after connection. It should be noted that the thickness (height in the Z direction) of the connection structure 200 using the micro-LED element 50 is very small, so when the electrodes 51, 52 of the micro-LED element 50 can be seen through from the substrate 60 side, the plane observed in the Z direction across the substrate 60 can also be regarded as the same as the above-mentioned cross section. In addition, the peeling surface when the micro-LED element 50 is peeled off from the substrate 60 after connection is also regarded as the same as the above-mentioned cross section. In such a cross section, with respect to the connection structure 200, the ratio (area occupancy rate) of the total SP of the area projected from the conductive particles 20 (solder particles or their aggregates) contained in the inter-electrode region R relative to the area SR of the inter-electrode region R (inter-electrode space) divided by the mutually adjacent electrodes 51 and 52 is 35% or less, preferably 30% or less. In the case where the ratio of the total area SP to the area SR exceeds 35%, a short circuit may occur between the adjacent electrodes (i.e., the electrode 51 and the electrode 52). Here, the total area SP can be obtained by summing up the areas when the figures projected from each conductive particle 20 (solder particles or their aggregates) contained in the inter-electrode region R are regarded as circles. In this case, according to the "area of ​​the figure projected from the conductive particles 20 (solder particles or their aggregates)", it is assumed that a perfect circle having the circumference of the outermost circle passing through the projected figure is summed up. The total area SP can be measured by observing the cross section (or peeling surface) of the inter-electrode region R using an observation method using a metallographic microscope or an electron microscope such as a SEM. The total area SP can be measured using any software.

[0116] It should be noted that, since the conductive film 100 in which the particle regions 30 are arranged in a neat arrangement is used, when the ratio of the total area SP to the area SR is too small, there is not a sufficient amount of solder particles between the electrodes of the connection object (electrode 51 and electrode 61, electrode 52 and electrode 62), and sufficient conduction may not be ensured. Therefore, the lower limit of the ratio of the total area SP to the area SR is preferably 0.5% or more, and more preferably 1.0% or more.

[0117] <Variations of the method for producing a connection structure>

[0118] It should be noted that, in the case of mounting a very fine first electronic component on a second electronic component such as a wiring substrate, the first electronic component can also be mounted by landing it on the second electronic component using the laser lift-off method as described above. For example, in the case where the first electronic component is a large number of micro-light-emitting diodes formed on the surface of a light-transmitting substrate, the first electronic component can be mounted by irradiating each first electronic component with a laser so that it lands on a conductive film arranged at a specified position of the second electronic component (such as each electrode of the wiring substrate) or a single piece of the conductive film transferred. The laser lift-off processing conditions can be appropriately determined according to the type of the first electronic component, the constituent material, etc. It should be noted that the conductive film is arranged at a specified position of the second electronic component (such as each electrode of the wiring substrate), or a single piece of the conductive film is transferred, which can be performed by thermal compression or laser lift-off processing.

[0119] It should be noted that when a first electronic component such as a micro-LED is landed on a conductive film arranged at a predetermined position of a second electronic component by thermal compression or a single sheet of conductive film transferred by laser lift-off processing by a laser lift-off processing method, in order to prevent the first electronic component from being shifted, deformed, damaged, or falling off, the insulating adhesive film of the conductive film preferably contains a rubber component (such as acrylic rubber, silicone rubber, butadiene rubber, polyurethane elastomer, etc.) that imparts a cushioning property for mitigating the impact of landing, and an inorganic filler (such as silica, talc, titanium oxide, calcium carbonate, etc.) that imparts mechanical strength.

[0120] The insulating adhesive film containing such a rubber component and inorganic filler has a durometer A hardness (based on JIS K6253) of preferably 20 to 40, more preferably 20 to 35, and particularly preferably 20 to 30 before laser irradiation, and a storage modulus obtained by a dynamic viscoelasticity testing device based on JIS K7244 (temperature 30°C, frequency 200 Hz; VIBRON, A&D Co., Ltd.) of preferably 60 MPa or less, more preferably 30 MPa or less, and particularly preferably 10 MPa or less.

[0121] In addition, the storage modulus at a temperature of 30°C measured in the tensile mode according to JIS K7244 after curing (after connection) of the insulating adhesive film is preferably 100 MPa or more, and more preferably 2000 MPa or more. When the storage modulus at a temperature of 30°C is too low, there is a tendency that good conductivity cannot be obtained and the connection reliability is also reduced. The storage modulus at a temperature of 30°C can be measured according to JIS K7244 under the tensile mode using a viscoelasticity tester (VIBRON), for example, under the measurement conditions of a frequency of 11 Hz and a heating rate of 3°C / min.

[0122] It should be noted that the first electronic component configuration sheet can also be obtained by transferring (landing) the first electronic component such as a micro-light-emitting diode on a specified position of a silicone rubber sheet such as polydimethylsiloxane (PDMS) (i.e., a position corresponding to the specified position of the second electronic component to which the first electronic component should be transferred) through a laser lift-off method, and placing the first electronic component side of the obtained first electronic component configuration sheet opposite to the second electronic component, aligning them, and then transferring them.

[0123] Example

[0124] Hereinafter, the present invention will be specifically described by way of examples.

[0125] [Preparation of Thermally Polymerizable Composition]

[0126] A phenoxy resin [YP-50, manufactured by Nippon Steel Chemical & Material Co., Ltd.], an epoxy resin A [YD-019 (bisphenol A type epoxy resin), manufactured by Nippon Steel Chemical & Material Co., Ltd.], an epoxy resin B [YL-980 (liquid epoxy resin), manufactured by Mitsubishi Chemical Co., Ltd.], an epoxy resin C [YX-8000 (liquid hydrogenated epoxy resin), manufactured by Mitsubishi Chemical Co., Ltd.], a flux compound [adipic acid, manufactured by Tokyo Chemical Industry Co., Ltd.], and a curing agent [Novacure HX-3941, manufactured by Asahi Kasei Corporation] were mixed to prepare a thermally polymerizable composition having the formulation composition (unit: parts by mass) shown in Table 1.

[0127] [Table 1]

[0128]

[0129] [Preparation of Adhesive Film]

[0130] The obtained thermopolymerizable composition was applied to a substrate using a bar coater, dried at 60° C. for 3 minutes, and then peeled off to form adhesive films 1 and 2 having thicknesses shown in Table 2. In addition, solder particles (composition: Sn 42 Bi 58 ; ST-3, manufactured by Mitsui Mining & Smelting Co., Ltd., particle size distribution D 10 ; 1.7μm, D 50 ; 3.1 μm, D 90; 5.0 μm) 10 parts by mass or 50 parts by mass were mixed, and adhesive films 3 and 4 having the thickness shown in Table 2 were similarly prepared. Adhesive films 3 and 4 are anisotropic conductive films (hereinafter referred to as "ACF") of a non-aligned arrangement type in which solder particles are randomly dispersed in an insulating resin film.

[0131] [Table 2]

[0132] Adhesive film 1 2 3 4 Thickness [μm] 4 8 4 4 Solder particles [parts by mass] 10 50

[0133] [Production of ACF: Examples 1 to 6, Comparative Examples 1 and 2]

[0134] A mold having an arrangement pattern of convex portions corresponding to the hexagonal lattice pattern was prepared, and a substance made by melting transparent resin particles (polycarbonate system) was poured into the mold and cooled and solidified to prepare three types of transfer molds made of resin having concave portions in a hexagonal lattice pattern. Solder particles (composition Sn 42 Bi 58 ; ST-3, manufactured by Mitsui Mining & Smelting Co., Ltd., particle size distribution D 10 ; 1.7μm, D 50 ; 3.1μm, D 90 ; 5.0μm).

[0135] Using an elastic roller, the adhesive film 1 in Table 2 was pressed against the solder particle receiving surface of each transfer mold under the conditions of a pressing temperature of 50°C and a pressing pressure of 0.5 MPa to form an adhesive film to which solder particles were transferred. The adhesive film to which solder particles were transferred was peeled off from the transfer mold, thereby making an ACF of the aligned arrangement type of Examples 1 to 4. The ACF of Examples 1 to 4 was determined by the combination of the adhesive films 1 and 2 in Table 2 and the aligned arrangement forms 1 to 3 in Table 3. In addition, as the ACF of Comparative Examples 1 and 2, the adhesive films 3 and 4 in Table 2 were used. The above summary is shown in Table 4.

[0136] [Table 3]

[0137] Neatly arranged configuration Neatly arranged configuration form 1 Neatly arranged configuration form 2 Neatly arranged configuration form 3 Diameter of particle area [μm] 3.2 2.2 1.7 <![CDATA[Density of particle region [particles / mm 2 > 28,000 58,000 100,000 arrangement Hexagonal lattice Hexagonal lattice Hexagonal lattice Distance between particle regions [μm] 3.2 2.2 1.7

[0138] [Table 4]

[0139]

[0140] The ACF obtained in Examples 1 to 4 was observed by SEM. As a result, it was confirmed that, when the area of ​​an arbitrary particle region was defined as S and the average value of the area S in a surface field of at least 100×100 μm was defined as S A When the maximum and minimum values ​​of area S are relative to the average value S A The ratio [%] (denoted as "to SA ratio") in S A Within ±80%.

[0141] As an example, the average value S of the area S of 20 particle regions in the plane field of at least 100×100 μm in Example 1 is A 5.1μm 2 , the maximum value is 8.0μm 2 , for S A The ratio is 157%, and the minimum value is 1.5μm 2 , for S A The ratio is 29%, with an average value of S A As a benchmark, within ±80%. A The results of the ratio [%] are also shown in Table 4. In addition, as a representative example, the SEM image of the ACF obtained in Example 1 is shown in Figure 7 .

[0142] In addition, it was confirmed that the ratio of the total area S of the particle region arranged in a regular pattern (S1 / S2 ratio; %) to the total area S2 projected from all solder particles in the ACF obtained in Examples 1 to 4 in a surface field of at least 100×100 μm was 90% or more. The results of the S1 / S2 ratio [%] are also shown in Table 4.

[0143] In addition, it was confirmed that in the ACF obtained in Examples 1 to 4, the total area S3 of two particle regions adjacent to each other at the shortest distance was within 1 μm. 2 Above and 20μm 2 The total area S3[μm 2 The results of ] are also shown in Table 4. It should be noted that the total area S3 in the table is the average value of 10 groups of particle regions adjacent to each other at the shortest distance.

[0144] In addition, in the ACF obtained in Examples 1 to 4, the total number of neatly arranged particle regions (the number density of the particle regions) is within the range of 100 to 1500 in a surface field of at least 100×100 μm. 2 ] The results are also shown in Table 4.

[0145] In addition, it was confirmed that in the ACF obtained in Examples 1 to 4, the ratio (area occupancy) of the total area S1 of the area S of the particle region in the surface field of at least 100×100μm was within the range of 5% to 25%. The results of the area occupancy [%] of the total area S1 are also shown in Table 4. It should be noted that the area occupancy in the table is the average value of the surface fields of 10 in total.

[0146] [Evaluation of on-resistance and insulation properties]

[0147] The ACFs of Examples 1 to 3 and Comparative Examples 1 and 2 were attached to a glass substrate having a Cr-Au electrode pattern, and an IC chip (chip size; 1.5×1.5 cm) having an electrode pattern simulating the electrodes of a micro-LED element was placed thereon, and thermocompression bonding was performed under the conditions of a maximum reaching temperature of 150°C, a pressure of 1 MPa, and 30 seconds to form a micro-LED assembly, thereby obtaining assembly bodies 1 to 6 of the examples and comparative assembly bodies 1 and 2 of the comparative examples. As IC chips, three evaluation components 1 to 3 were manufactured and used, in which electrodes were square when viewed from above and electrode patterns were formed with the electrode sizes, lengths of inter-electrode spaces, and areas of inter-electrode spaces shown in Table 5.

[0148] [Table 5]

[0149] Evaluation Components Evaluation component 1 Evaluation component 2 Evaluation component 3 <![CDATA[Electrode size [μm 2 > 20×20 15×15 10×10 Length of the space between electrodes [μm] 10 7.5 5 <![CDATA[Area of the space between electrodes [μm 2 > 200 112.5 50

[0150] The evaluation results of the on-resistance and insulation properties of the micro light emitting diode packages formed by ACF bonding of Examples 1 to 3 and Comparative Examples 1 and 2 are shown in Table 6. The evaluation criteria are as follows.

[0151] On-resistance determination criteria:

[0152] A to C were judged as passed, and D and E were judged as failed.

[0153] A: Below 30Ω.

[0154] B: 31~100Ω.

[0155] C: 101~300Ω.

[0156] D: 301Ω or more.

[0157] E: There is one or more sites that cannot be measured.

[0158] Insulation determination criteria:

[0159] Confirm the space between 100 electrodes and 3 Ω or less is considered a short circuit, A to C are judged as pass, and D is judged as fail.

[0160] A: No short circuit.

[0161] B: 1 short circuit.

[0162] C: 2 short circuits.

[0163] D: 3 short circuits.

[0164] [Table 6]

[0165]

[0166] [Evaluation of resin filling properties]

[0167] like Figure 8 , Fig. 9 As shown, a microchip 50A simulating a micro light-emitting diode element was produced (chip size; 15×30μm, chip thickness 10μm). The height of electrodes 51A and 52A was set to H, and three types of flat (0μm), 2.5μm, and 5μm were produced. After temporarily pasting the ACFs of Examples 1 and 4 on the glass substrate, the produced microchips were arranged in a range of 1.5×1.5cm in a manner equivalent to 110ppi, and then crimped under the conditions of a maximum reaching temperature of 150°C, a pressure of 1MPa, and 30 seconds, thereby obtaining the mounted bodies 7 to 12 shown in Table 7. The resin filling property of the obtained mounted bodies 7 to 12 was evaluated. The judgment criteria are as follows. The results are also shown in Table 7.

[0168] Criteria for judging resin filling properties:

[0169] As described below, the chip side surface, electrode height, and chip top surface were used as references for determination, and only A was determined to be acceptable.

[0170] A: The resin is filled to the side of the chip but not to the top of the chip.

[0171] B: The state where the electrode is not completely filled to the height.

[0172] C: The resin has flowed to the upper surface of the chip (the entire chip is buried in the resin).

[0173] It should be noted that in Figure 8 In the figure, symbols A to C indicate the range of the chip side surface (A), the range to the electrode height (B), and the range beyond the chip upper surface (C) used as the judgment standard.

[0174] [Table 7]

[0175]

[0176] [Evaluation of area occupancy after installation]

[0177] The area occupancy of solder particles in the inter-electrode space (inter-electrode region) was determined for the mounted bodies 1 to 6 and the comparative mounted bodies 1 and 2. Figure 6The inter-electrode region R surrounded by the dotted line. In each assembly, observe a section parallel to the bonding surface (here, although the IC chip of the assembly is observed from the glass substrate side through the glass substrate, it can be regarded as the same as the cross-sectional observation). For one assembly, confirm the inter-electrode spaces at any 10 locations, thereby measuring the total area SP of the solder particles, and finding the area occupancy rate (%) relative to the total area SR of the inter-electrode space. Here, the total area SP of the solder particles is found by summing up the areas when the figure projected from the solder particles or their aggregates contained in the inter-electrode space is regarded as a circle. In this case, based on the figure projected from the solder particles or their aggregates, it is assumed that there is a perfect circle with the outermost circumference of the projected figure, and the area surrounded by the perfect circle is summed. The total area SP is measured by a metallographic microscope. The results are shown in Table 8.

[0178] In addition, as a representative example, a metallographic microscope image of the inter-electrode space of the mounting body 1 is shown in FIG. Fig.10 The metallographic microscope image of the comparative mounting body 1 is shown in Fig.11 .

[0179] [Table 8]

[0180]

[0181] According to Table 8, it can be confirmed that by using the neatly arranged ACF of Examples 1 to 3, a highly reliable micro-LED assembly (connection structure) can be produced in which the area occupancy of solder particles in the inter-electrode space is 35% or less, thereby suppressing the occurrence of short circuits between adjacent electrodes.

[0182] On the other hand, in the micro-LED assembly made using the non-aligned ACF of Comparative Examples 1 and 2, the area occupancy of the solder particles in the inter-electrode space has a large deviation in Comparative Assembly 1, and in some cases exceeds 35%, so it is estimated that the distribution of the solder particles is offset, and poor conduction or short circuit may occur. For Comparative Assembly 2, the area occupancy is too high, and short circuit may occur.

[0183] In addition, according to Fig.10 In the mounted body 1, solder particles were present in the inter-electrode space, but no bridging was observed. Fig.11 It was confirmed that in Comparative Mounting Body 1, solder particles were fused in the inter-electrode space and bridges were generated.

[0184] From the above results, it was confirmed that by using the aligned arrangement type ACF of the example, it was possible to achieve both ensuring conduction and preventing short circuits in the micro LED assembly (connection structure), and the resin filling property was also good.

[0185] Industrial Applicability

[0186] The conductive film of the present invention is useful, for example, in conductive connection or anisotropic conductive connection of electronic components such as micro-LEDs to wiring substrates. It should be noted that the embodiments of the present invention are described in detail for illustrative purposes, but the present invention is not limited to the above embodiments.

[0187] Description of Reference Numerals

[0188] 10: insulating adhesive film; 20: conductive particles; 21: solder joint; 30: particle area; 50: micro light-emitting diode element; 50A: microchip; 51, 51A, 52, 52A: electrodes; 60: substrate; 61, 62: electrodes; 100: conductive film; 101: resin filling layer; 200: connecting structure; D: diameter of particle area; L: shortest distance between particle areas; H: height of electrode; P: lattice point; R: area between electrodes.

Claims

1. A conductive film, characterized in that: The invention comprises: an insulating resin film; and a plurality of conductive metal particles carried by the insulating resin film. When the conductive film is viewed from above, a particle region of a predetermined area including a projection pattern from one or more of the metal particles is arranged in a regular pattern. The area of ​​one of the particle regions is denoted as S, and the average value of the area S in a surface field of at least 100×100 μm of the conductive film is denoted as S. A When the area S has a maximum and minimum value, it is S A Within ±80%.

2. The conductive film according to claim 1, wherein In a surface field of at least 100×100 μm of the conductive film, a ratio S1 of the total area S of the aligned particle regions to a total area S2 of the pattern projected from all the metal particles is 90% or more.

3. The conductive film according to claim 1, wherein The total area of ​​two adjacent particles at the shortest distance is 1 μm 2 Above and 20μm 2 Within the following range.

4. The conductive film according to claim 1, wherein In a surface field of at least 100×100 μm of the conductive film, the total number of the particle regions arranged in a regular pattern is within a range of 100 to 1500.

5. The conductive film according to claim 1, wherein In a surface field of at least 100×100 μm of the conductive film, a ratio of the total area S1 of the area S is within a range of 5% to 25%. The conductive film according to claim 1 , wherein: The particle regions are neatly arranged to form lattice points of any planar lattice pattern among hexagonal lattices, square lattices, rhombic lattices, rectangular lattices or parallelogram lattices.

7. The conductive film according to claim 1, wherein The shape of the particle region is circular or polygonal.

8. The conductive film according to claim 1, wherein The metal particles are solder particles.

9. The conductive film according to claim 1, wherein The reaction rate of the film was less than 25%.

10. A connection structure, characterized in that: The first electronic component is conductively connected to the second electronic component, The first electronic component has a plurality of first electrodes joined to the electrodes of the second electronic component, and a resin filling layer formed of an insulating resin is formed around the first electrodes. In the resin filling layer, conductive metal particles or aggregates thereof are dispersed in a plurality of locations. In the cross-section of the resin filling layer parallel to the bonding surface of the first electrode and the electrode of the second electronic component, the ratio of the total SP of the areas when the figure projected from the metal particles or their aggregates contained in the inter-electrode area is regarded as a circle to the total area SR of the inter-electrode area divided by the first electrodes adjacent to each other is less than 35%.

11. The connection structure according to claim 10, wherein: The ratio of the total area SP of the circles to the total area SR of the inter-electrode region is 0.5% or more.

12. A method for manufacturing a connection structure, wherein: The electrode of the first electronic component and the electrode of the second electronic component are conductively connected via the conductive film according to any one of claims 1 to 9.

Citation Information

Cited By

  • Water-based copper composite conductive paste and preparation method thereof

    CN118782289A