Binder, pole piece, secondary battery and electric device

CN118922963APending Publication Date: 2024-11-08CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280093882.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-11-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the cell design of lithium-ion batteries, the expansion force is too large due to the rebound of the pole pieces, which affects the service life. The existing polymer binders cannot meet the needs in terms of conductivity, adhesion and flexibility.

Method used

Modified polyacrylic polymer materials are used to polymerize acrylic acid, alkaline metal salts, polyethylene glycol acrylic acid monoester and acrylonitrile to enhance the dispersion and flexibility of the binder, reduce hydrogen bonding, and improve the performance of the pole piece. Ductility and cyclic performance.

Benefits of technology

It effectively reduces the expansion force of the battery core, improves the flexibility and dynamic performance of the pole piece, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922963A_ABST
    Figure CN118922963A_ABST
Patent Text Reader

Abstract

The invention relates to a binder, a pole piece, a secondary battery and an electric device. The modified polyacrylic acid high polymer material has the structural characteristics as shown in the formula (I). According to the modified polyacrylic acid high polymer material, four monomers of acrylic acid, alkaline metal salt of acrylic acid, polyethylene glycol acrylic monoester and acrylonitrile are polymerized and can be used as a binder, the active material is fully coated in the process of mixing with the active material, the rebound of a pole piece under limit design is reduced, and the service life of the pole piece is prolonged. The expansive force in the battery cell circulation process is reduced and the service life of the battery cell is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive, electrode, secondary battery and electrical device Technical Field

[0001] The present application relates to the technical field of lithium batteries, and in particular to an adhesive, a pole piece, a secondary battery and an electrical device. Background Art

[0002] In recent years, as the application scope of lithium-ion batteries has become increasingly wider, lithium-ion batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields.

[0003] The tremendous development of lithium-ion batteries has led to higher demands for energy density, cycle performance, and safety, bringing with it an increasing number of technical challenges. For example, the increasing energy density of lithium-ion battery cells requires that the pole pieces possess high coating area density and high compaction density in cell design. Simultaneously, materials such as silicon are gradually being introduced into active material selection. These measures lead to the accumulation of pole piece rebound in the Z direction, which in the short term affects the amount of active material inserted into the battery shell. In the long term, the pole piece rebound causes excessive expansion force in the battery cell, shortening its service life.

[0004] Summary of the Invention

[0005] The present application is made in view of the above-mentioned problems, and its purpose is to provide a modified polyacrylic acid polymer material, which can be used as a binder in lithium-ion batteries to improve the problems of easy expansion during battery cell cycling and low battery life.

[0006] In order to achieve the above-mentioned object, the first aspect of the present application provides a modified polyacrylic acid polymer material having the following structural characteristics:

[0007]

[0008] Wherein, m=2500~20000, p=50~200, q=1000~15000, l=1000~15000;

[0009] n=500-5000, M is selected from alkaline metal ions.

[0010] The second aspect of the present application provides a method for preparing a modified polyacrylic acid polymer material, comprising the following steps:

[0011] The basic metal salt of acrylic acid, polyethylene glycol monoacrylate, acrylic acid and acrylonitrile are polymerized.

[0012] The third aspect of the present application provides a binder comprising the modified polyacrylic acid polymer material described in the first aspect and one or more of the modified polyacrylic acid polymer materials prepared by the preparation method described in the second aspect.

[0013] The fourth aspect of the present application provides a pole piece, characterized in that it includes a current collector and an active material layer arranged on at least one surface of the current collector, and the material of the active material layer includes an active material and the binder described in the third aspect.

[0014] The fifth aspect of the present application provides a secondary battery, comprising the electrode described in the fourth aspect.

[0015] A sixth aspect of the present application provides an electrical device comprising at least one of the secondary batteries described in the fifth aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] FIG1 is a schematic diagram of a secondary battery according to an embodiment of the present application;

[0017] FIG2 is an exploded view of the secondary battery according to one embodiment of the present application shown in FIG1 ;

[0018] FIG3 is a schematic diagram of a battery module according to an embodiment of the present application;

[0019] FIG4 is a schematic diagram of a battery pack according to an embodiment of the present application;

[0020] FIG5 is an exploded view of the battery pack according to an embodiment of the present application shown in FIG4 ;

[0021] 6 is a schematic diagram of an electrical device using a secondary battery as a power source according to an embodiment of the present application;

[0022] FIG7 is an infrared spectrum of a modified polyacrylic acid polymer material (binder) prepared in one embodiment of the present application;

[0023] Description of reference numerals:

[0024] 1. Battery pack; 2. Upper case; 3. Lower case; 4. Battery module; 5. Secondary battery; 51. Housing; 52. Electrode assembly; 53. Cover; 6. Electrical device. DETAILED DESCRIPTION

[0025] Below, the embodiments of the adhesive, electrode, secondary battery and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0026] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0027] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0028] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0029] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0030] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0031] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0032] The room temperature in this application generally refers to 4°C to 30°C, preferably 20±5°C.

[0033] Currently, a large number of organic polymers are used as binders in lithium-ion batteries, but they still struggle to meet the required conductivity, adhesion, and electrode flexibility. Therefore, research into polymer modification is needed. Polyacrylic acid polymers are widely used in lithium-ion batteries due to their high adhesion and chemical stability. While overall, polyacrylic acid polymers outperform other similar water-based binders, batteries prepared using traditional polyacrylic acid polymers as binders still suffer from excessive cell expansion, which can affect their service life.

[0034] An example of the present application provides a modified polyacrylic acid polymer material having the following structural characteristics:

[0035]

[0036] Wherein, m=2500~20000, p=50~200, q=1000~15000, l=1000~15000;

[0037] n=500-5000, M is selected from alkaline metal ions.

[0038] The above-mentioned modified polyacrylic acid polymer material uses the polymerization of four monomers: acrylic acid, alkaline metal salt of acrylic acid, polyethylene glycol acrylate monomer and acrylonitrile. It can be used as a binder. During the mixing process with the active material, it can fully cover the active material, reduce the rebound of the electrode under the extreme design, reduce the expansion force during the battery cell cycle, and improve the battery cell life.

[0039] At the same time, the modified polyacrylic acid polymer material also has the following advantages:

[0040] (1) During the use of traditional polyacrylic acid polymers, hydrogen bonding on long-chain molecules causes the polymer chains to agglomerate with each other, making it difficult for the binder in the slurry to be effectively dispersed, ultimately leading to an increase in electrode resistance and deterioration of the battery cell dynamics. The modified polyacrylic acid polymer material of the present application can also partially salt the carboxylic acid functional groups on the long chains of polyacrylic acid, thereby eliminating some hydrogen bonding between the polymer long chains, reducing hydrogen bonding during use, avoiding agglomeration of polymer chains, and enabling the binder to be effectively dispersed in the electrode material, thereby improving the battery cell dynamics.

[0041] (2) Although traditional polyacrylic acid polymers also have excellent bonding properties, they are generally brittle. Such substances often contact the particulate matter in the coating in the form of a mesh surface. Due to the linear structure of the molecular chain, the electrode is not flexible enough. After high compaction density cold pressing, the electrode has insufficient elongation, and the stress is easily concentrated at the edge of the coating area, causing edge overpressure. The electrode under high density is prone to brittle fracture during subsequent processing. The modified polyacrylic acid polymer material of the present application can enhance the flexibility of the electrode due to the addition of specific side chains to the linear structure of the molecular chain. After high compaction density cold pressing, the elongation of the electrode is improved, avoiding edge overpressure, and improving the problem of brittle fracture of the electrode under high density in subsequent processing.

[0042] (3) When the modified polyacrylic acid polymer material is used as a binder in the preparation of negative electrode sheets for lithium-ion batteries, it can also improve the dispersion effect of the slurry, increase the cold pressing window after the sheet is dried, improve the processing performance, and inhibit the rebound of the anode sheet during the cycle, reduce the growth of the expansion force of the battery cell, and improve the cycle performance.

[0043] Specifically, the value of m includes but is not limited to: 2500, 3500, 4500, 5500, 6500, 7500, 8500, 9000, 9500, 10500, 11000, 11500, 12500, 13500, 15500, 17500, 18500, 19500, and 20000. In one example, m=7500-12500.

[0044] Specifically, the value of p includes but is not limited to: 50, 55, 60, 80, 100, 115, 125, 135, 140, 145, 150, 155, 160, 165, 175, 185, 195, 200. In one example, p=125-175.

[0045] Specifically, the value of q includes but is not limited to: 1000, 1500, 2000, 2000, 4000, 6000, 8000, 8500, 9000, 9500, 10000, 10500, 11000, 11500, 12000, 13000, 14000, 14500, and 15000. In one example, q=8000-12000.

[0046] Specifically, the value of l includes but is not limited to: 1000, 1500, 2000, 2000, 4000, 6000, 8000, 8500, 9000, 9500, 10000, 10500, 11000, 11500, 12000, 13000, 14000, 14500, and 15000. In one example, l = 8000-12000.

[0047] Specifically, the value of n includes, but is not limited to, 500, 600, 800, 1000, 1500, 2000, 2200, 2300, 2400, 2500, 2600, 2700, 3000, 4000, 4500, 4800, and 5000. In one example, n=2200-2700.

[0048] In one example, M is selected from one or more of sodium ions, lithium ions, potassium ions, and magnesium ions. It is understood that M can be a monovalent ion or a divalent ion. When it is a divalent ion, 1 mole of M can bind to 2 moles of monomers.

[0049] Furthermore, M is selected from sodium ion.

[0050] Another example of the present invention provides a method for preparing a modified polyacrylic acid polymer material, comprising the following steps:

[0051] The basic metal salt of acrylic acid, polyethylene glycol monoacrylate, acrylic acid and acrylonitrile are polymerized.

[0052] In one example, the polymerization reaction is carried out in the presence of a polymerization aid and / or an initiator. Further, the polymerization reaction is carried out in the presence of a polymerization aid and an initiator.

[0053] In one example, the polymerization aid includes sodium dodecyl sulfate.

[0054] In one example, the polymerization aid is added in an amount of 2% to 5% based on the total weight of the alkaline metal salt of acrylic acid, polyethylene glycol monoacrylate, acrylic acid, and acrylonitrile. Specifically, the amount of the polymerization aid includes, but is not limited to, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, and 5%. Furthermore, the amount of the polymerization aid is 3% to 4.5%.

[0055] In one example, the initiator includes one or more of potassium sulfate, potassium persulfate, sodium persulfate, and ammonium persulfate.

[0056] In one example, the initiator is added in an amount of 1% to 3% based on the total weight of the alkaline metal salt of acrylic acid, polyethylene glycol monoacrylate, acrylic acid, and acrylonitrile. Specifically, the initiator addition amount includes, but is not limited to, 1%, 1.5%, 2%, 2.5%, and 3%. Furthermore, the initiator addition amount is 1% to 1.5%.

[0057] In one example, the polymerization reaction temperature is 65° C. to 75° C., and the polymerization time is 2 h to 3 h.

[0058] In one example, the steps of preparing the alkaline metal salt of acrylic acid include:

[0059] Acrylic acid, an alkaline metal hydroxide and a first solvent are mixed to carry out a first reaction until the pH of the reaction solution is neutral, and then distilled and dried to prepare the alkaline metal salt of acrylic acid; wherein the alkaline metal in the alkaline metal hydroxide is selected from one or more of sodium, lithium, potassium and magnesium.

[0060] In one example, the alkaline metal hydroxide is sodium hydroxide.

[0061] In one example, the first solvent includes water.

[0062] In one example, the first reaction is carried out at room temperature.

[0063] In one example, the preparation steps of the polyethylene glycol monoacrylate include:

[0064] Polyethylene glycol, acrylic acid and a second solvent are mixed and subjected to a second reaction to prepare the polyethylene glycol monoacrylate.

[0065] In one example, the second reaction is carried out in the presence of a catalyst and an inhibitor;

[0066] In one example, the catalyst includes one or more of p-toluenesulfonic acid, sulfuric acid, and aluminum chloride.

[0067] In one example, the catalyst is added in an amount of 3% to 10% based on the total weight of the polyethylene glycol and acrylic acid. Specifically, the catalyst addition amount includes, but is not limited to, 3%, 4%, 4.5%, 5%, 5.5%, 6%, 7%, 8%, 9%, and 10%. Furthermore, the catalyst addition amount is 5% to 9%.

[0068] In one example, the polymerization inhibitor includes one or more of hydroquinone, p-hydroxyanisole, and 2,6-di-tert-butyl-p-cresol.

[0069] In one example, the amount of the polymerization inhibitor added is 1% to 5% based on the total weight of the polyethylene glycol and acrylic acid. Specifically, the amount of the polymerization inhibitor added includes, but is not limited to, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, and 5%. Furthermore, the amount of the polymerization inhibitor added is 3% to 4.5%.

[0070] In one example, the molar ratio of polyethylene glycol to acrylic acid is 1:(0.8-1.2).

[0071] In one example, the temperature of the second reaction is 65° C. to 75° C., and the time is 20 min to 3 h.

[0072] In one example, the second solvent includes water.

[0073] In one example, the degree of polymerization of the polyethylene glycol is n=500-5000. Specifically, the value of n includes but is not limited to: 500, 600, 800, 1000, 1500, 2000, 2200, 2300, 2400, 2500, 2600, 2700, 3000, 4000, 4500, 4800, 5000. In one example, n=2200-2700.

[0074] In one example, the molar ratio of acrylic acid, acrylonitrile, alkaline metal salt of acrylic acid and polyethylene glycol monoacrylate is 2500-20000:50-200:1000-15000:1000-15000. Specifically, the molar ratio of acrylic acid, acrylonitrile, alkaline metal salt of acrylic acid and polyethylene glycol monoacrylate includes but is not limited to: 10000:150:10000:10000, 2500:150:10000:10000, 20000:150:10000:10000, 10000:50:10000:10000, 10000:200 In one example, the molar ratio of acrylic acid, acrylonitrile, alkaline metal salt of acrylic acid and polyethylene glycol monoacrylate is 7500-12500:125-175:8000-12000:8000-12000. Furthermore, the molar ratio of acrylic acid, acrylonitrile, alkaline metal salt of acrylic acid and polyethylene glycol monoacrylate is 9500-10500:140-160:9500-10500:9500-10500.

[0075] Another example of the present application further provides an adhesive, comprising the modified polyacrylic acid polymer material as described above and one or more of the modified polyacrylic acid polymer materials prepared by the preparation method as described above.

[0076] Another example of the present application further provides a pole piece, comprising a current collector and an active material layer disposed on at least one surface of the current collector, wherein the material of the active material layer comprises an active material and the binder as described above.

[0077] Another example of the present application provides a secondary battery, comprising the electrode as described above.

[0078] Another example of the present application further provides an electric device comprising at least one selected from the secondary batteries described above.

[0079] The secondary battery, battery module, battery pack, and electric device of the present application are described below with reference to the accompanying drawings as appropriate.

[0080] In one embodiment of the present application, a secondary battery is provided.

[0081] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During the battery's charge and discharge processes, active ions are inserted and removed between the positive and negative electrodes. The electrolyte conducts ions between the positive and negative electrodes. The separator, located between the positive and negative electrodes, primarily prevents short circuits between the positive and negative electrodes while allowing ions to pass through.

[0082] Positive electrode

[0083] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes the positive electrode active material of the first aspect of the present application.

[0084] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0085] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material on a polymer material substrate. Among them, the metal material includes but is not limited to aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc. Polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0086] In some embodiments, the positive electrode active material may include a positive electrode active material for a battery that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon. The weight ratio of the positive electrode active material in the positive electrode film layer is 80-100 weight%, based on the total weight of the positive electrode film layer.

[0087] In some embodiments, the positive electrode film layer also needs to include a binder. The binder in the present application can be used alone, or the binder in the present application can be mixed with other binders. When used alone, the binder in the present invention can account for 0.5-1.5 weight% of the total weight of the positive electrode film layer; when mixed, other binders can include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. At least one of the binders is mixed, and the total binder accounts for 0.5-1.5 weight%, and other binders account for 10-50 weight% in the mixed binder.

[0088] In some embodiments, the positive electrode film layer may further optionally include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The weight ratio of the conductive agent in the positive electrode film layer is 0-10% by weight, based on the total weight of the positive electrode film layer.

[0089] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry, wherein the positive electrode slurry has a solid content of 40-80 wt %, and the viscosity at room temperature is adjusted to 5000-25000 mPa·s, the positive electrode slurry is coated on the surface of the positive electrode current collector, and after drying, the positive electrode sheet is formed by cold rolling; the positive electrode powder coating unit area density is 120-210 g / m 2 The compaction density of the positive electrode is 3.0-3.8g / cm 3 , optional 3.3-3.7g / cm 3 The calculation formula of the compacted density is

[0090] Compaction density = coating surface density / (thickness of the electrode after extrusion - thickness of the current collector).

[0091] Negative electrode

[0092] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.

[0093] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0094] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material on a polymer material substrate. Among them, the metal material includes but is not limited to copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver and silver alloys, etc., and the polymer material substrate includes but is not limited to polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE) and other substrates.

[0095] In some embodiments, the negative electrode active material may adopt the negative electrode active material for batteries that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials and lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more. The weight ratio of the negative electrode active material in the negative electrode film layer is 70-100 weight%, based on the total weight of the negative electrode film layer.

[0096] In some embodiments, the negative electrode film layer also needs to include a binder. The binder in the present application can be used alone, or the binder in the present application can be mixed with other binders. When used alone, the binder in the present application can account for 1-2 weight% of the total weight of the negative electrode film layer. When mixed, other binders can include at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS), and the total binder accounts for 1-2 weight%, and other binders account for 10-50 weight% in the mixed binder.

[0097] In some embodiments, the negative electrode film layer may further include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The weight ratio of the conductive agent in the negative electrode film layer is 0-2 weight percent based on the total weight of the negative electrode film layer.

[0098] In some embodiments, the negative electrode film layer may further optionally include other additives, such as a thickener (e.g., sodium carboxymethyl cellulose (CMC-Na)). The weight ratio of the other additives in the negative electrode film layer is 0-3 weight %, based on the total weight of the negative electrode film layer.

[0099] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry, wherein the negative electrode slurry has a solid content of 30-70 wt% and a viscosity at room temperature adjusted to 2000-15000 mPa·s; the obtained negative electrode slurry is coated on the negative electrode current collector, and after a drying process, cold pressing, such as with a roller, is performed to obtain the negative electrode sheet. The negative electrode powder coating unit area density is 65-165 g / m2 , the compaction density of the negative electrode is 1.2-2.0g / m 3 .

[0100] electrolytes

[0101] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.

[0102] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.

[0103] In some embodiments, the electrolyte salt may be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium bis(oxalatoborate) (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP), and lithium tetrafluorooxalatophosphate (LiTFOP). The concentration of the electrolyte salt is typically 0.5-5 mol / L.

[0104] In some embodiments, the solvent can be selected from one or more of fluoroethylene carbonate (FEC), ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS) and diethyl sulfone (ESE).

[0105] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.

[0106] Isolation film

[0107] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0108] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0109] In some embodiments, the isolation film has a thickness of 3-40 μm, and optionally 5-15 μm.

[0110] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.

[0111] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0112] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0113] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG1 shows a secondary battery 5 with a square structure as an example.

[0114] In some embodiments, referring to Figure 2, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0115] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0116] Figure 3 shows an example battery module 4. Referring to Figure 3 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.

[0117] Optionally, the battery module 4 may further include a housing having an accommodation space, and the plurality of secondary batteries 5 are accommodated in the accommodation space.

[0118] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0119] Figures 4 and 5 illustrate an example battery pack 1. Referring to Figures 4 and 5 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0120] In addition, the present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0121] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0122] Figure 6 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.

[0123] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.

[0124] Example

[0125] In order to make the technical problems, technical solutions and beneficial effects solved by this application clearer, the application will be further described in detail below with reference to the embodiments and drawings. Obviously, the described embodiments are only a part of the embodiments of this application, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is in no way intended to limit the present application and its applications. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0126] If no specific techniques or conditions are specified in the examples, the experiments were carried out according to the techniques or conditions described in the literature in the field or according to the product instructions. All reagents or instruments used without specifying the manufacturer are commercially available conventional products.

[0127] 1. Preparation Example

[0128] Preparation of binder

[0129] Preparation Example 1

[0130] 1) slowly adding a sodium hydroxide aqueous solution dropwise to an acrylic acid aqueous solution at room temperature, stirring the solution during the addition until the pH value of the solution becomes neutral, and then distilling and drying to obtain sodium acrylate particles;

[0131] 2) adding polyethylene glycol and acrylic acid in a molar ratio of 2:1 to distilled water to a total mass concentration of 20%; then adding 5% of a catalyst (p-toluenesulfonic acid) and 3% of a polymerization inhibitor (hydroquinone), based on the total mass of the polyethylene glycol and acrylic acid; stirring uniformly; and heating to 70° C. for 30 minutes to obtain an aqueous solution of polyethylene glycol monoacrylate;

[0132] 3) Purify the product in 2) as follows:

[0133] The product in 2) is mixed with dichloromethane, washed with a 5% sodium hydroxide aqueous solution, separated to remove the aqueous solution, then washed with a saturated sodium chloride solution, separated to remove excess polyether substances, and finally distilled to remove the solvent to obtain polyethylene glycol acrylate monomer;

[0134] 4) preparing the following ingredients: the molar ratio of acrylic acid, acrylonitrile, sodium acrylate particles, and polyethylene glycol monoacrylate is 1000:150:10000:10000; the amount of polymerization aid (sodium lauryl sulfate) added is 3%, and the amount of polymerization initiator (potassium sulfate) added is 2%, based on the total weight of the sodium acrylate particles, polyethylene glycol monoacrylate, acrylic acid, and acrylonitrile;

[0135] 5) A polymerization aid (sodium dodecyl sulfate), acrylic acid, and the sodium acrylate particles from 1) were added to distilled water to a total mass concentration of 20%. The mixture was stirred evenly and heated to 70°C. A polymerization initiator (potassium sulfate), polyethylene glycol acrylate monoester, and acrylonitrile were then added. The mixture was simultaneously heated to 70°C and stirred for 2.5 hours. The supernatant was removed by centrifugation to obtain the target product, the infrared spectrum of which is shown in Figure 7.

[0136] The preparation methods of the adhesives of Examples 2 to 11 and Comparative Examples 1 to 2 are similar to the adhesive of Example 1, but the feeding amount and monomer type of each monomer are changed. The different product parameters are detailed in Table 1.

[0137]

[0138] Table 1

[0139]

[0140]

[0141] 2. Application Examples

[0142] Example 1

[0143] 1) Preparation of positive electrode sheet

[0144] The positive electrode active material NCM, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) are dissolved in the solvent N-methylpyrrolidone (NMP) in a weight ratio of 96.5:1.5:2, and the mixture is thoroughly stirred and mixed to obtain a positive electrode slurry; the positive electrode slurry is then evenly coated on the positive electrode collector, and then dried, cold pressed, and cut to obtain a positive electrode sheet.

[0145] 2) Preparation of negative electrode sheet

[0146] The active material graphite, silicon, conductive agent acetylene black, the above-mentioned binder, and thickener sodium carboxymethyl cellulose (CMC) are dissolved in a solvent deionized water in a weight ratio of 90:5:2:2:1, and the mixture is uniformly mixed with the solvent deionized water to prepare a negative electrode slurry. The slurry is coated on a copper foil, dried, and then cold-pressed and cut to obtain an anode electrode sheet.

[0147] 3) Isolation film

[0148] A 12μm thick polypropylene isolation film was selected.

[0149] 4) Preparation of electrolyte

[0150] The organic solvent is a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC), with a volume ratio of 1:1:1. In an argon atmosphere glove box with a water content of <10 ppm, fully dried lithium salt LiPF6 is dissolved in the organic solvent and mixed thoroughly to obtain an electrolyte solution. The concentration of the lithium salt is 1 mol / L.

[0151] 5) Preparation of batteries

[0152] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrode sheets to serve as an isolation. After winding into a square bare cell, the tabs are welded to the bare cell and filled with aluminum-plastic film. After baking at 80°C to remove water, the corresponding non-aqueous electrolyte is injected at an injection coefficient of 2.15ml / Ah and sealed. After standing, hot and cold pressing, formation, shaping, capacity testing and other processes, the finished battery is obtained.

[0153] The secondary batteries of Examples 2-11 and Comparative Examples 1-2 were prepared in a similar manner to the secondary battery of Example 1, but using the binders of the corresponding preparation examples.

[0154] 3. Battery performance test

[0155] 1. Adhesion test

[0156] Take the electrode to be tested and use a razor blade to cut a sample of appropriate length and width. Apply special double-sided tape to a steel plate, keeping the tape width constant. Place the cut electrode sample on the double-sided tape with the test surface facing down. After compacting with a roller, use a tensile testing machine to test the force corresponding to the maximum peel strength. Convert the force to N / m based on the tape width.

[0157] 2. Slurry stability

[0158] Use a beaker to take an appropriate amount of stirred slurry, seal it with plastic wrap, and let it stand for 24 hours before checking the slurry sedimentation / gelation: open the plastic wrap, gently move the slurry surface with a steel ruler, and check if there is any abnormality on the slurry surface; slowly extend the steel ruler vertically along the edge of the beaker to the bottom of the beaker, scrape the slurry at the bottom, then pull out the steel ruler and check the sedimentation brought out by the steel ruler.

[0159] 3. Expansion force

[0160] After the battery cell is fixed in the fixture of the pressure sensor, a full DOD cycle test is performed at a rate of 0.5C within the designed voltage window. The change in expansion force is monitored during the cycle. The ratio of the expansion force increment when the capacity decays to 80% to the initial expansion force is the expansion force change.

[0161] 4. Resilience

[0162] Take an appropriate amount of cold-pressed electrode sample, fold the sample in half along the TD direction, place it on the flat surface of the laboratory table, roll it once with a 2kg cylindrical roller, and then fold it again by the same operation to check whether there is any light transmittance or breakage at the crease. If so, it is NG, otherwise repeat the above test. Add 1 to the toughness each time it is folded, and record the maximum number of folds that are not NG.

[0163] 3. Test results of various embodiments and comparative examples

[0164] The electrodes and batteries of the embodiments and comparative examples were prepared according to the above methods, and various performance parameters were measured. The results are shown in Table 2 below.

[0165] Table 2

[0166]

[0167]

[0168] As can be seen, compared with Comparative Example 1, Examples 1 to 11 of the present application all have better slurry stability and adhesion, and also have an expansion force suppression effect; compared with Comparative Example 2, Examples 1 to 11 of the present application all have better adhesion and toughness. In summary, Examples 1 to 11 of the present application have better overall performance, among which Example 1 is the best.

[0169] At the same time, through the comparison between Example 1 and Examples 2 to 3, it can be seen that the proportion of acrylic acid segments in the polymer has a certain influence on adhesion, toughness and expansion force inhibition effect. When the proportion is low, the adhesion and expansion force inhibition effect decreases. When the proportion is high, the adhesion and expansion force inhibition effect increase to a certain extent, but the toughness decreases.

[0170] By comparing Example 1 with Examples 4 to 5, it can be seen that the proportion of acrylonitrile segments in the polymer has a certain influence on adhesion, toughness and expansion force inhibition effect. When the proportion is low, the adhesion and expansion force inhibition effect decrease. When the proportion is high, the adhesion and expansion force inhibition effect increase to a certain extent, but the toughness decreases.

[0171] A comparison between Example 1 and Examples 6-7 shows that the proportion of sodium acrylate segments in the polymer has a certain impact on slurry stability, adhesion, toughness, and expansion force inhibition. When the proportion is low, the slurry stability decreases, while when the proportion is high, the adhesion and expansion force inhibition effect decrease, and the toughness decreases. Furthermore, toughness decreases at both low and high proportions.

[0172] By comparing Example 1 with Examples 8 to 9, it can be seen that the proportion of polyethylene glycol monoacrylate chain segments in the polymer has a certain influence on adhesion, toughness and expansion force inhibition effect. When the proportion is low, the expansion force inhibition effect increases to a certain extent, but the toughness decreases. When the proportion is high, the toughness increases to a certain extent, but the adhesion and expansion force inhibition effects decrease.

[0173] By comparing Example 1 with Examples 10 to 11, it can be seen that the polyethylene glycol polymer in the polyethylene glycol monoacrylate segment has a certain influence on the toughness and expansion force inhibition effect. When the proportion is low or high, the expansion force inhibition effect decreases, and when the proportion is low, the toughness also decreases.

[0174] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A modified polyacrylic acid polymer material having the following structural characteristics: in, m=2500~20000, p=50~200, q=1000~15000, l=1000~15000; n=500-5000, M is selected from alkaline metal ions.

2. The modified polyacrylic acid polymer material according to claim 1, characterized in that Has at least one of the following characteristics: (1)m=7500~12500; (2)p=125~175; (3)q=8000~12000; (4)l=8000~12000。 3. The modified polyacrylic acid polymer material according to claim 1 or 2, characterized in that: n=2200~2700。 4. The modified polyacrylic acid-based polymer material according to any one of claims 1 to 3, characterized in that: M is selected from one or more of sodium ions, lithium ions, potassium ions and magnesium ions.

5. A method for preparing a modified polyacrylic acid polymer material, comprising the following steps: The basic metal salt of acrylic acid, polyethylene glycol monoacrylate, acrylic acid and acrylonitrile are polymerized.

6. The method for preparing the modified polyacrylic acid polymer material according to claim 5, wherein: The polymerization reaction is carried out in the presence of a polymerization aid and / or initiator; Optionally, the polymerization aid comprises sodium dodecylsulfonate; further optionally, the amount of the polymerization aid added is 2% to 5% based on the total mass of the alkaline metal salt of acrylic acid, polyethylene glycol monoacrylate, acrylic acid and acrylonitrile; further optionally, the amount of the polymerization aid added is 3% to 4.5%; Optionally, the initiator includes one or more of potassium sulfate, potassium persulfate, sodium persulfate and ammonium persulfate; further optionally, the added amount of the initiator is 1% to 3% based on the total mass of the alkaline metal salt of acrylic acid, polyethylene glycol monoacrylate, acrylic acid and acrylonitrile; further optionally, the added amount of the initiator is 1% to 1.5%.

7. The method for preparing the modified polyacrylic acid polymer material according to claim 5 or 6, characterized in that: The polymerization reaction temperature is 65°C to 75°C, and the time is 2h to 3h.

8. The method for preparing a modified polyacrylic acid polymer material according to any one of claims 5 to 7, characterized in that: The preparation steps of the alkaline metal salt of acrylic acid include: Mixing acrylic acid, an alkaline metal hydroxide, and a first solvent, performing a first reaction until the pH of the reaction solution is neutral, and distilling and drying to prepare the alkaline metal salt of acrylic acid; wherein the alkaline metal in the alkaline metal hydroxide is selected from one or more of sodium, lithium, potassium, and magnesium; Optionally, the first solvent comprises water; Optionally, the first reaction is carried out at room temperature.

9. The method for preparing a modified polyacrylic acid polymer material according to any one of claims 5 to 8, characterized in that: The preparation steps of the polyethylene glycol monoacrylate include: Polyethylene glycol, acrylic acid and a second solvent are mixed and subjected to a second reaction to prepare the polyethylene glycol monoacrylate.

10. The method for preparing a modified polyacrylic acid polymer material according to claim 9, wherein: The second reaction is carried out in the presence of a catalyst and a polymerization inhibitor; Optionally, the catalyst comprises one or more of p-toluenesulfonic acid, sulfuric acid and aluminum chloride; further optionally, the amount of the catalyst added is 3% to 10% based on the total mass of the polyethylene glycol and acrylic acid; further optionally, the amount of the catalyst added is 5% to 9%; Optionally, the polymerization inhibitor includes one or more of hydroquinone, p-hydroxyanisole and 2,6-di-tert-butyl-p-cresol; further optionally, the added amount of the polymerization inhibitor is 1% to 5% based on the total mass of the polyethylene glycol and acrylic acid; further optionally, the added amount of the polymerization inhibitor is 3% to 4.5%.

11. The method for preparing a modified polyacrylic acid polymer material according to claim 9 or 10, characterized in that: The second reaction has at least one of the following characteristics: (1) The molar ratio of the polyethylene glycol to the acrylic acid is 1:(0.8-1.2); (2) The temperature of the second reaction is 65°C to 75°C, and the time is 20 minutes to 3 hours; (3) The second solvent includes water.

12. The method for preparing a modified polyacrylic acid-based polymer material according to any one of claims 9 to 11, characterized in that: The degree of polymerization of the polyethylene glycol is n=500-5000; optionally, n=2200-2700.

13. The method for preparing a modified polyacrylic acid-based polymer material according to any one of claims 5 to 12, characterized in that: The molar ratio of acrylic acid, acrylonitrile, alkaline metal salt of acrylic acid and polyethylene glycol monoacrylate is 2500-20000:50-200:1000-15000:1000-15000; optionally, the molar ratio of acrylic acid, acrylonitrile, alkaline metal salt of acrylic acid and polyethylene glycol monoacrylate is 7500-12500:125-175:8000-12000:8000-12000.

14. An adhesive, characterized in that: The invention comprises one or more of the modified polyacrylic acid polymer material according to any one of claims 1 to 4 and the modified polyacrylic acid polymer material prepared by the preparation method according to any one of claims 5 to 13.

15. A pole piece, characterized in that: The device comprises a current collector and an active material layer disposed on at least one surface of the current collector, wherein the active material layer comprises an active material and the binder according to claim 14.

16. A secondary battery, characterized in that: Including the pole piece according to claim 15.

17. An electrical device, characterized in that: The invention comprises at least one selected from the group consisting of the secondary batteries according to claim 16.