Connection structure and method for manufacturing same

By using conductive particles with an average particle size less than 3 μm and a moderate compression hardness of 20% in high-density installation, and combining softness and insulating adhesives, the position stability of the conductive particles during the thermal pressing process is solved. The initial conduction reliability and short-circuit suppression effect of high-density installation are achieved.

CN118923005APending Publication Date: 2024-11-08DEXERIALS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028314.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-02-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the case of high-density installation, when using conductive particles with an average particle size less than 3 μm, it is difficult to maintain the position of the conductive particles during the hot pressing process, resulting in a decrease in initial conduction reliability and an increase in the risk of short circuit.

Method used

Conductive particles with an average particle size less than 3 μm are used, and the compression hardness of 20% deformation is 1500N/mm2 or more and 8000N/mm2 or less. The soft conductive particles and appropriate insulating adhesive are used to ensure thermal pressing. It is not easy to move conductive particles, and the rebound effect is achieved.

Benefits of technology

It realizes that the initial conduction reliability is not reduced under high-density installation, and the occurrence of short circuits is suppressed, while maintaining the rebound characteristics of conductive particles to ensure the stability of the connection structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118923005A_ABST
    Figure CN118923005A_ABST
Patent Text Reader

Abstract

A connection structure which connects a first electronic component and a second electronic component via conductive particles and an insulating adhesive disposed between an electrode of the first electronic component and an electrode of the second electronic component, and which is suitable for high-density mounting, conductive particles having an average particle diameter of less than 3 [mu] m and a compression hardness (20% K value) at 20% deformation of 1500 N / mm2 or more and 8000 N / mm2 or less are used.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a connection structure and a method for manufacturing the same. Background Art

[0002] There has always been a demand for fine pitch IC chips mounted on electronic devices, and there is also a demand for fine pitch LED chips. When these fine pitch electronic components such as IC chips or LED chips are mounted on a wiring substrate to manufacture a connection structure, the connection structure is usually manufactured by clamping an anisotropic conductive film or conductive film containing conductive particles between the electrodes of the electronic component and the electrodes of the wiring substrate and performing heat pressing. For such anisotropic conductive films or conductive films, in order to cope with high-density mounting (for example, mounting electronic components with electrodes (bumps) spaced about 10 μm apart on a wiring substrate), it has been proposed to use conductive particles with an average particle size of about 3 to 10 μm (for example, Patent Document 1).

[0003] However, in recent years, anisotropic conductive films or conductive films are required to cope with higher-density mounting. Therefore, conductive particles used in anisotropic conductive films or conductive films are required to be smaller, and attempts have been made to use conductive particles having an average particle size of less than 3 μm.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2003-64324. Summary of the invention

[0007] Problems to be solved by the invention

[0008] However, if the average particle size of the conductive particles to be contained in the anisotropic conductive film or the conductive film is reduced from the previous 3 to 10 μm to less than 3 μm, even if the inherent compression hardness of the conductive particles does not change, the absolute value of the deformation in the extrusion direction during the hot pressing process will become smaller than before the average particle size is reduced, the cushioning property (in other words, the susceptibility to crushing) of the conductive particles will decrease, and it will be difficult to obtain a rebound effect. Therefore, during hot pressing, it is difficult for the conductive particles located between a pair of electrodes to withstand the extrusion force without misalignment, and there is a tendency to move toward the surface direction of the electrode (bump). In particular, if Figure 3A As shown in FIG. 1 , the conductive particles 30 held near the ends of a pair of electrodes 31 and 32 opposite to each other by the insulating adhesive 33 at the beginning of the thermal compression process are as follows: Figure 3BAs shown, there is a problem of movement from the ends of a pair of electrodes 31 and 32 to the adjacent inter-electrode interval S. Therefore, it is difficult to grasp the behavior of capturing conductive particles. When the electrode area is small, there is a concern that the number of captured conductive particles is insufficient and the initial conduction reliability is reduced. When the distance between the electrodes is too close, there is a concern that the risk of short circuit increases.

[0009] The purpose of the present invention is to solve the existing problems, and the purpose is: for a connection structure in which a first electronic component and a second electronic component are connected via an insulating adhesive and conductive particles arranged between an electrode of a first electronic component such as an IC chip or an LED chip and an electrode of a second electronic component such as a wiring substrate, in order to be suitable for high-density mounting, even when conductive particles having an average particle size of less than 3μm are used as conductive particles, the initial conduction reliability is not reduced and the occurrence of short circuits is suppressed.

[0010] Means for solving problems

[0011] The inventors have found that when using conductive particles with an average particle size of less than 3 μm to manufacture a connection structure, if relatively soft conductive particles are used, it is not easy to cause the following problems during thermal compression: Figure 3B The present invention was completed based on the finding that the conductive particles have a tendency to move unexpectedly and that, if the conductive particles are too soft, a springback effect sufficient to ensure conduction cannot be obtained from the conductive particles.

[0012] That is, the present invention provides a connection structure in which a first electronic component and a second electronic component are connected via conductive particles and an insulating adhesive disposed between an electrode of the first electronic component and an electrode of the second electronic component.

[0013] The average particle size of the conductive particles is less than 3 μm.

[0014] The compression hardness of the conductive particles at 20% deformation (20% K value) is 1500N / mm 2 Above and 8000N / mm 2 the following.

[0015] In addition, the present invention provides a method for manufacturing a connection structure, wherein the connection structure is the above connection structure, that is, the first electronic component and the second electronic component are connected via conductive particles arranged between the electrodes of the first electronic component and the electrodes of the second electronic component and an insulating adhesive, the average particle size of the conductive particles is less than 3 μm, and the compression hardness (20% K value) of the conductive particles at 20% deformation is 1500 N / mm 2 Above and 8000N / mm 2 The following connection structure,

[0016] The manufacturing method is to arrange conductive particles and an insulating adhesive between an electrode of a first electronic component and an electrode of a second electronic component, and heat and pressurize the conductive particles and the insulating adhesive from either side of the first electronic component or the second electronic component, thereby connecting the first electronic component and the second electronic component. In this case, it is preferred that an anisotropic conductive film or a conductive film in which conductive particles are retained in a film-like insulating adhesive is sandwiched between the electrode of the first electronic component and the electrode of the second electronic component, thereby arranging the conductive particles and the insulating adhesive between the electrode of the first electronic component and the electrode of the second electronic component.

[0017] Effects of the Invention

[0018] The connection structure of the present invention has a structure in which the first electronic component and the second electronic component are connected via conductive particles arranged between the electrodes of the first electronic component and the electrodes of the second electronic component and an insulating adhesive, characterized in that very fine conductive particles with an average particle size of less than 3 μm are used as conductive particles. Therefore, the connection structure of the present invention is suitable for high-density installation. Moreover, as the conductive particles, a compressive hardness (20% K value) of 1500 N / mm when 20% deformation is used. 2 Above and 8000N / mm 2 Therefore, during thermal compression bonding, it is difficult to Figure 3B The problem of the movement of the conductive particles shown above can not only suppress the reduction of the initial conduction reliability, but also suppress the occurrence of short circuits. In addition, a springback effect can be obtained, and the situation where the indentation caused by the conductive particles at the connection part is not easily observed can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] [ Figure 1 ] Figure 1 This is a schematic cross-sectional view of the connection structure of the present invention.

[0020] [ Figure 2A ] Figure 2A It is a diagram for explaining the production process of the connection structure of the present invention.

[0021] [ Figure 2B ] Figure 2B It is a diagram for explaining the production process of the connection structure of the present invention.

[0022] [ Figure 3A ] Figure 3A This is an explanatory diagram of the manufacturing of a conventional connection structure immediately before thermal compression bonding.

[0023] [ Figure 3B ] Figure 3B This is an explanatory diagram of a conventional connection structure immediately after heat compression bonding during production. DETAILED DESCRIPTION

[0024] Hereinafter, the connection structure of the present invention will be described in detail with reference to the drawings.

[0025] <Overall structure of the connection structure>

[0026] like Figure 1 As shown, the connection structure 100 of the present invention has a structure in which the first electronic component 1 and the second electronic component 2 are connected via conductive particles 3 and an insulating adhesive 4 disposed between the electrode 1a of the first electronic component 1 and the electrode 2a of the second electronic component 2. Figure 1 In the example, a case where a pair of electrodes constitutes one group is illustrated, but a pair of electrodes may exist in multiple groups in the planar direction.

[0027] (Electronic Components)

[0028] Examples of the first electronic component 1 include IC chips, LED chips, IC modules, LED modules, and FPCs. Examples of the second electronic component 2 include FPCs, glass wiring substrates, plastic wiring substrates, rigid wiring substrates, and ceramic wiring substrates, but are not limited thereto.

[0029] (Electrodes of electronic components)

[0030] Regarding the electrode 1a of the first electronic component 1, its material, size, shape, arrangement pattern, etc. can be appropriately selected according to the type or purpose of the first electronic component 1. In addition, regarding the electrode 2a of the second electronic component 2, its material, size, shape, arrangement pattern, etc. can also be appropriately selected according to the type or purpose of the second electronic component 2. In particular, from the perspective of being suitable for high-density mounting and the perspective of the average particle size of the conductive particles being less than 3μm, and then from the perspective of obtaining stable conduction characteristics, it is preferred that the electrode (bump) width and the interval between electrodes are respectively greater than 5μm, preferably greater than 10μm and less than 25μm. In terms of the relationship between the electrode width and the conductive particle size, from the perspective of capturing the conductive particles, the electrode width is preferably more than twice the conductive particle size. In addition, from the perspective of high precision of the micro-LED display, the upper limit of the required electrode width is also reduced, so the electrode width is preferably less than 10 times the conductive particle size.

[0031] <Conductive particles>

[0032] (Average particle size of conductive particles)

[0033] In the present invention, from the viewpoint of high-density mounting, the average particle size of the conductive particles 3 is less than 3 μm, preferably less than 2.8 μm, and more preferably less than 2.5 μm. In addition, from the viewpoint of manufacturing conductive particles with uniform particle sizes, obtaining good resilience, and achieving clear indentations during thermal compression, it is preferably greater than 1 μm, and more preferably greater than 1.1 μm. This average particle size range of conductive particles becomes a range that deviates in the direction of being lower than the particle size range disclosed in Patent Document 1, and is a very narrow range, which is understood to be a range that is not envisioned to be actually applicable in the prior art.

[0034] The average particle size of the conductive particles can be measured using a common particle size distribution measuring device, for example, a wet flow particle size / shape analyzer specified by the trade name: FPIA-3000 (manufactured by Malvern Panalytical) can be used for measurement. During the measurement, it is desirable to set the number of samples for measuring the particle size to be 200 or more, preferably 1000 or more, and more preferably 5000 or more. In this case, the volume basis can be used, and in terms of making the pressed state uniform, the average particle size is preferably obtained on a number basis. In addition, the average particle size of the conductive particles can also be obtained by not using a common particle size distribution measuring device, but by using a metal microscope or a scanning electron microscope to observe a sample obtained by dispersing the conductive particles on a flat plate such as a glass plate, or a sample obtained by mixing with a curable resin composition to make it monodisperse and then coating it, and the particle sizes of the multiple conductive particles obtained are arithmetic averaged and obtained.

[0035] It should be noted that the particle size deviation of the conductive particles is preferably set to 30% or less, and more preferably set to 20% or less in terms of CV value (standard deviation / average). By setting the CV value to 20% or less, the conductive particles are easily uniformly squeezed during the pressing process when manufacturing the connection structure, and especially when the conductive particles are arranged, the squeezing force can be prevented from being locally concentrated, which can contribute to the stability of the connection. In addition, after the connection, the connection state caused by the indentation can be accurately evaluated.

[0036] (Compression hardness of conductive particles at 20% deformation (20% K value))

[0037] In the present invention, the hardness of the conductive particles is defined by the "compression hardness at 20% deformation" (20% K value) described below. The reason for defining the hardness of the conductive particles by the 20% K value is that, in fact, the conductive particles are compressed and deformed during hot pressing. In addition, the reason for setting the degree of deformation of the conductive particles to 20% is that, in the present invention, the conductive particles used are assumed to be small particles with an average particle size of less than 3 μm, and it is difficult to assume a situation where the deformation amount far exceeds 20%.

[0038] Here, the compression hardness at 20% deformation (20% K value) refers to the value calculated by the following formula when the particle size of the conductive particles is shortened by 20% compared with the original particle size by applying a load to the conductive particles in one direction and compressing them. The smaller the 20% K value, the softer the particles. In the following formula, "F" is the "load at 20% compression deformation of the conductive particles", "S" is the "compression displacement (mm)", and "R" is the "radius of the conductive particles (mm)". It should be noted that the 20% K value can be measured using a micro compression tester (for example, Fischer scope H-100 manufactured by Fischer Instruments).

[0039]

[0040] In the present invention, the 20% K value of the conductive particles is 1500 N / mm 2 Above, preferably 2000N / mm 2 Above, and 8000N / mm 2 Below, preferably 7000N / mm 2 The reason is that if the 20% K value of the conductive particles is less than 1500N / mm 2 If the wiring surface has oxides, it may be difficult to penetrate. If it exceeds 8000N / mm 2 , the thrust required for compression may become too large due to the smaller particle size.

[0041] (Shape of conductive particles)

[0042] The shape of the conductive particles is appropriately determined according to the type of the first electronic component or the second electronic component as a constituent element of the connection structure or the average particle size or 20% K value of the conductive particles, and is preferably spherical or approximately spherical. When a transfer mold is used to arrange the conductive particles to produce an anisotropic conductive film that can be used when manufacturing a connection structure, the conductive particles can be filled in a predetermined position on the transfer mold with high precision because the conductive particles roll smoothly on the transfer mold, so the conductive particles can be accurately transferred and arranged in the adhesive resin layer (refer to Japanese Patent Publication No. 2014-60150). It should be noted that as conductive particles, in order to easily penetrate the oxide film on the surface of the electrode, a plurality of tiny protrusions can be formed on its surface (refer to Japanese Patent Publication No. 2017-59471).

[0043] (Number density of conductive particles)

[0044] In the connection structure of the present invention, the number density of the conductive particles between the electrodes of the first electronic component and the second electronic component is appropriately determined according to the type of the first electronic component or the second electronic component as a constituent element of the connection structure, the average particle size of the conductive particles, the 20% K value, etc. If the number density of the conductive particles is too low, it is sometimes difficult to cope with the anisotropic conductive connection of the electronic components with fine pitches, and if it is too high, it may sometimes cause a short circuit. Therefore, there is no particular lower limit, but it is preferably 3000 particles / mm 2 More preferably, 12000 pieces / mm 2 More than, particularly preferably 150000 pieces / mm 2 The upper limit is preferably 500,000 pieces / mm. 2 Less than, more preferably 350000 pieces / mm 2 Below, particularly preferably 300,000 pieces / mm 2 The number density of the conductive particles can be calculated based on the electron microscope observation data of the connection part of the connection structure. In addition, it can be obtained by measuring the observation image using image analysis software (for example, WinROOF, manufactured by Mitani Shoji Co., Ltd.). It should be noted that when an anisotropic conductive film or conductive film is used in the manufacture of the connection structure, the number density of the conductive particles in the connection structure roughly reflects the number density of these conductive particles.

[0045] (Area occupancy of conductive particles)

[0046] In the connection structure of the present invention, the area occupancy of the conductive particles between the electrodes of the first electronic component and the electrodes of the second electronic component relative to each other, that is, the area occupancy of the electrodes in a top view ("the number density of the conductive particles between the relative electrodes of the connection structure" × "the average area of ​​the conductive particles" × 100) is also appropriately determined according to the type of the first electronic component or the second electronic component as a constituent element of the connection structure or the average particle size of the conductive particles or the 20% K value, etc. For the same reasons as the number density, the lower limit is preferably 0.2% or more, more preferably 1.0% or more, and the upper limit is preferably 40% or less, more preferably 25% or less. The area occupancy of the conductive particles can be calculated from the average particle size D and the number density of the conductive particles. It should be noted that when an anisotropic conductive film or conductive film is used in the manufacture of the connection structure, the area occupancy of the conductive particles in the connection structure roughly reflects the area occupancy of these conductive particles.

[0047] (Arrangement of conductive particles)

[0048] In the connection structure of the present invention, the arrangement of the conductive particles between the electrodes of the first electronic component and the electrodes of the second electronic component is not particularly limited, and can be randomly dispersed or randomly arranged without contact. From the perspective of suppressing the reduction of conduction reliability or the occurrence of short circuits, it is preferred that the conductive particles are kept in the insulating adhesive without contact with each other, and more preferably arranged regularly (preferably in a grid shape). In particular, it is preferred to arrange them regularly in a single layer. It should be noted that when an anisotropic conductive film or conductive film is used in the manufacture of the connection structure, the arrangement of the conductive particles in the connection structure roughly reflects the arrangement of these conductive particles.

[0049] Here, as a scheme of lattice arrangement, in addition to the hexagonal lattice, there can also be listed: a rectangular lattice, an oblique lattice, a square lattice, other rectangular lattices, a Thousand Island lattice and other lattice arrangements. Among them, if a hexagonal lattice, a square lattice or an oblique lattice (i.e., a diamond lattice) is formed, the configuration of each conductive particle can be made uniform, so it is preferred. It should be noted that in the present invention, the lattice-like arrangement also includes a scheme in which the conductive particle group is arranged in a lattice. The conductive particles forming the group preferably have regularity within the group. In addition, it also includes an arrangement in which a part of the conductive particles are regularly extracted from the conductive particles arranged in a lattice.

[0050] (Ratio of non-contact conductive particles)

[0051] In the connection structure of the present invention, regardless of the configuration of the conductive particles, the proportion of the conductive particles between the electrodes of the first electronic component and the electrodes of the second electronic component that do not contact each other is preferably 95% or more, more preferably 98% or more, and further preferably 99.5% or more. Thus, the slight misalignment of the conductive particles can be suppressed. It should be noted that the proportion of the conductive particles that do not contact each other can be calculated by electron microscope observation of the connection portion of the connection structure.

[0052] It should be noted that as a method of preventing conductive particles from contacting each other, when manufacturing an anisotropic conductive film or conductive film used in manufacturing a connected structure, a mold that specifies the location where the conductive particles should be arranged can be prepared in advance, conductive particles are arranged at the location, and the conductive particles are transferred to the adhesive resin layer.

[0053] (Constituent materials of conductive particles)

[0054] As conductive particles, metal particles such as nickel, cobalt, silver, copper, gold, and palladium can be listed; alloy particles such as solder; metal-coated resin particles having a metal layer formed on the surface of the resin core; metal-coated resin particles having insulating particles attached to the surface, etc. Two or more kinds can also be used in combination. Among them, metal-coated resin particles are preferred from the perspective of easy maintenance of contact with the terminal due to the repulsion of the resin particles after connection and stable conduction performance. In addition, in order to easily penetrate the oxide film on the surface of the connection object, protrusions can be formed on the surface of the conductive particles. For example, conductive particles described in Japanese Patent Publication No. 2015-8129 can be used. By forming such protrusions, the protective film provided on the terminal can be penetrated during anisotropic connection. The formation of protrusions is preferably uniformly present on the surface of the conductive particles. It should be noted that for the surface of conductive particles such as metal-coated resin particles, an insulating treatment that does not hinder the conduction characteristics can be applied according to known techniques. The occurrence of short circuits can be suppressed. As an insulating treatment, for example, an insulating film may be further formed on the surface of the metal layer of the metal-coated resin particles, or the surface of the conductive particles may be coated with insulating particles. In this case, the particle size of the conductive particles is a size excluding the insulating treatment (insulating particles). When such conductive particles with insulating particles are used, in the process of filling the conductive particles into the mold in order to arrange the conductive particles in the manufacturing process of the anisotropic conductive film, a part of the insulating particles may be missing.

[0055] <Insulating adhesive>

[0056] like Figure 1 As shown, in the connection structure 100 of the present invention, the conductive particles 3 are held in the insulating adhesive 4. Here, the insulating adhesive 4 not only holds the conductive particles 3 but also has a function of preventing the conductive particles 3 from contacting each other in the planar direction of the connection structure 100.

[0057] (Minimum melt viscosity of insulating adhesive)

[0058] The minimum melt viscosity of the insulating adhesive is appropriately determined according to the type of the first electronic component or the second electronic component as a constituent element of the connection structure of the present invention, the average particle size of the conductive particles, or the 20% K value. If the minimum melt viscosity is too low, excessive pressure may be applied to the particles, resulting in unexpected movement of the conductive particles. If it is too high, a thrust is also required for pressing the resin, so a sufficient rebound effect may not be obtained. Therefore, it is preferably 2000 Pa·s or more, more preferably 3000 Pa·s or more, preferably 15000 Pa·s or less, and more preferably 10000 Pa·s or less. In addition, when the 20% K value is between 5000 and 8000 N / mm 2range, and further, when the particle size is less than 2.8μm, the influence of the resin flow on the terminal is lower than that of about 3μm, so the effect of the invention is easily reflected in the range of higher viscosity. Therefore, the minimum melt viscosity is preferably greater than 8000Pa·s and less than 12000Pa·s. It should be noted that the minimum melt viscosity can be measured by a known method, for example, a rotational rheometer (manufactured by TA Instruments) can be used, kept constant under a measuring pressure of 5g, and a measuring plate with a diameter of 8mm can be used to obtain it. More specifically, it can be obtained by setting the heating rate to 10℃ / min, the measuring frequency to 10Hz, and the load change on the above-mentioned measuring plate to 5g within the temperature range of 30-200℃.

[0059] (Constituent materials of insulating adhesive)

[0060] The insulating adhesive 4 can be plastic or curable, and can preferably be formed from a curable composition. For example, it can be formed from a thermopolymerizable composition containing a thermopolymerizable compound and a thermopolymerization initiator. In the thermopolymerizable composition, a photopolymerization initiator can be contained as needed. In addition, it can be formed from a photopolymerizable composition containing a photopolymerizable compound and a photopolymerization initiator (or photocuring agent). In the photopolymerizable composition, a thermopolymerization initiator can be contained as needed. These can use known polymerizable compositions and polymerization initiators (curing agents). It should be noted that the insulating adhesive 4 can be formed from a cured product of a curable composition.

[0061] When a thermal polymerization initiator and a photopolymerization initiator are used together in the insulating adhesive 4, a compound that also functions as a photopolymerization compound may be used as the thermal polymerization compound, and a photopolymerization compound may be contained in addition to the thermal polymerization compound. Preferably, a photopolymerization compound is contained in addition to the thermal polymerization compound. For example, a thermal cationic polymerization initiator may be used as the thermal polymerization initiator, an epoxy compound may be used as the thermal polymerization compound, a photoradical polymerization initiator may be used as the photopolymerization initiator, and a (meth)acrylate compound may be used as the photopolymerization compound.

[0062] As a photopolymerization initiator, multiple types that react with light of different wavelengths can be used together. Thus, the wavelengths used in the photocuring treatment of the resin constituting the insulating adhesive when making the anisotropic conductive film or conductive film used in the manufacture of the connection structure and the wavelengths used in the photocuring treatment of the resin used to bond electronic components to each other when these films are used to manufacture the connection structure can be used separately. It should be noted that in the photocuring when forming the anisotropic conductive film or conductive film, all or part of the photopolymerizable compound contained in the insulating adhesive can be photocured. Through this photocuring, the configuration of the conductive particles 3 can be maintained or fixed by the insulating adhesive 4. In addition, through this photocuring, the viscosity of the insulating adhesive can be appropriately adjusted.

[0063] The amount of the photopolymerizable compound in the insulating adhesive 4 is preferably 30% by mass or less, more preferably 10% by mass or less, and more preferably less than 2% by mass. This is because if the amount of the photopolymerizable compound is too large, the thrust for pressing in during the thermal compression process when manufacturing the connection structure increases.

[0064] Examples of the thermally polymerizable composition in the insulating adhesive 4 include: a thermally free radical polymerizable acrylate composition containing a (meth)acrylate compound and a thermally free radical polymerization initiator, a thermally cationic polymerizable epoxy composition containing an epoxy compound and a thermally cationic polymerization initiator, and the like. A thermally anionic polymerizable epoxy composition containing a thermally anionic polymerization initiator can be used instead of a thermally cationic polymerizable epoxy composition containing a thermally cationic polymerization initiator. In addition, if no particular hindrance is caused, a plurality of polymerizable compositions can be used in combination. As examples of the combination, a combination of a cationic polymerizable composition and a free radical polymerizable composition can be mentioned.

[0065] Here, as the (meth)acrylate compound, a conventionally known heat-polymerizable (meth)acrylate monomer can be used, for example, a monofunctional (meth)acrylate monomer or a difunctional or higher polyfunctional (meth)acrylate monomer.

[0066] Examples of the thermal radical polymerization initiator include organic peroxides and azo compounds, etc. In particular, an organic peroxide that does not generate nitrogen that causes bubbles can be preferably used.

[0067] The amount of the thermal radical polymerization initiator used is preferably 2 to 60 parts by mass, more preferably 5 to 40 parts by mass, based on 100 parts by mass of the (meth)acrylate compound, because too little curing may result, while too much may shorten the product life.

[0068] Examples of epoxy compounds include bisphenol A epoxy resins, bisphenol F epoxy resins, novolac epoxy resins, modified epoxy resins thereof, alicyclic epoxy resins, etc., and two or more of these may be used in combination. In addition to the epoxy compounds, oxetane compounds may also be used in combination.

[0069] As the thermal cationic polymerization initiator, a substance known as a thermal cationic polymerization initiator for epoxy compounds can be used. For example, iodonium salts, sulfonium salts, phosphonium salts, ferrocenes, etc. that generate acid by heat can be used. In particular, aromatic sulfonium salts that show good potential against temperature can be preferably used.

[0070] The amount of the thermal cationic polymerization initiator used tends to be insufficient in curing if it is too small, and tends to reduce the product life if it is too large. Therefore, it is preferably 2 to 60 parts by mass, more preferably 5 to 40 parts by mass, based on 100 parts by mass of the epoxy compound.

[0071] The thermal polymerizable composition in the insulating adhesive 4 preferably contains a film-forming resin or a silane coupling agent. As the film-forming resin, phenoxy resin, epoxy resin, unsaturated polyester resin, saturated polyester resin, urethane resin, butadiene resin, polyimide resin, polyamide resin, polyolefin resin, etc. can be listed, and two or more of them can be used in combination. Among these, from the viewpoint of film forming property, processability, and connection reliability, phenoxy resin can be preferably used. The weight average molecular weight is preferably more than 10,000. In addition, as the silane coupling agent, epoxy silane coupling agent, acrylic silane coupling agent, etc. can be listed. As these silane coupling agents, mainly alkoxysilane derivatives can be listed.

[0072] In order to adjust the melt viscosity, the thermopolymerizable composition may contain an insulating filler in addition to the above-mentioned conductive particles 3. Examples thereof include silica powder and alumina powder. The insulating filler is preferably a micro filler having a particle size of 20 to 1000 nm, and the blending amount is preferably 5 to 50 parts by mass relative to 100 parts by mass of a thermopolymerizable compound (photopolymerizable composition) such as an epoxy compound.

[0073] It should be noted that the insulating adhesive 4 may contain a filler, a softener, an accelerator, an anti-aging agent, a colorant (pigment, dye), an organic solvent, an ion scavenger, and the like.

[0074] The insulating adhesive 4 may be a single-layer structure or a multi-layer structure of two or more layers. In the case of a multi-layer structure, the compositions may be the same or different.

[0075] <Method for producing a connection structure>

[0076] like Figure 2AAs shown in FIG. 1 , regarding the connection structure of the present invention, the first electronic component 21 and the second electronic component 22 are opposed to each other between a stage 25 and a thermal press head 26, and conductive particles 23 and an insulating adhesive 24 are further arranged between the electrode 21a of the first electronic component 21 and the electrode 22a of the second electronic component 22, and the first electronic component 21 or the second electronic component 22 is connected to the second electronic component 22 from either side ( Figure 2A In the embodiment, the conductive particles 23 and the insulating adhesive 24 are heated and pressed by a heat press head 26 from the first electronic component 21 side to connect the first electronic component 21 and the second electronic component 22, thereby manufacturing Figure 2B The connection structure 200 shown. In this case, it is preferred that an anisotropic conductive film or a conductive film in which conductive particles are retained in a film-like insulating adhesive is sandwiched between the electrode of the first electronic component and the electrode of the second electronic component, so that the conductive particles and the insulating adhesive are arranged between the electrode of the first electronic component and the electrode of the second electronic component.

[0077] It should be noted that as an anisotropic conductive film or conductive film for manufacturing a connection structure, a conductive film consisting of a single layer of conductive particles containing conductive particles in an insulating adhesive can be used, or a conductive film having a layer of an insulating adhesive of the same or different composition stacked on at least one side thereof can also be used.

[0078] Example

[0079] Hereinafter, the connection structure of the present invention will be specifically described by way of examples.

[0080] It should be noted that the average particle size of the conductive particles used in the examples and comparative examples is a value obtained by measuring using a wet flow particle size / shape analyzer (FPIA-3000 (manufactured by Malvern Panalytical). In addition, the compression hardness (20% K value) of the conductive particles at 20% deformation is a value obtained by measuring using a micro compression tester (Fischerscope H-100, manufactured by Fischer Instruments).

[0081] Examples 1 to 4, Comparative Examples 1 to 3

[0082] (1) Manufacturing of anisotropic conductive films

[0083] An insulating adhesive composition for retaining conductive particles was prepared by mixing as shown in Table 1. The minimum melt viscosity of the composition is 3000-5000 Pa·s (measuring device: rotational rheometer (manufactured by TA Instruments), measuring conditions: measuring pressure 5 g constant, measuring plate diameter 8 mm, temperature range 30-200°C, heating rate 10°C / min, measuring frequency 10 Hz, load variation on measuring plate 5 g). The composition was coated on a PET (polyethylene terephthalate) film with a film thickness of 50 μm using a rod coater, and dried in an oven at 80°C for 5 minutes to form an insulating adhesive layer A with a thickness of 4 μm on the PET (polyethylene terephthalate) film.

[0084] The convex portions corresponding to the concave portions for accommodating the conductive particles having the average particle size and the compression hardness at 20% deformation (20% K value) shown in Table 2 were prepared at a number density of 56,000 / mm. 2 A mold in which the particles are arranged in a hexagonal lattice (the angle between the arrangement axis and the film long side direction is 30°) is formed. Pellets of a known transparent polycarbonate resin are poured into the mold in a molten state, cooled and solidified, thereby forming a transfer mold in which the recesses are arranged in a hexagonal lattice pattern.

[0085] One conductive particle was filled in one concave portion of the transfer mold, and the insulating adhesive layer A was covered thereon, and extrusion was performed at 60°C and 0.5 MPa, thereby bonding and transferring the conductive particles to the insulating adhesive layer A. Then, the insulating adhesive layer A to which the conductive particles were bonded and transferred was peeled off from the PET film, and the conductive particles on the insulating adhesive layer A were pressed into the insulating adhesive layer A (extrusion conditions: 60-70°C, 0.5 MPa), thereby forming a layer containing conductive particles (Examples 1-4, Comparative Examples 1-3).

[0086] The conductive particles (trade name: Micropearl (manufactured by Sekisui Chemical Co., Ltd.)) used in Examples 1 to 4 and Comparative Examples 1 to 3 had 20% K values ​​shown in Table 2.

[0087] [Table 1]

[0088]

[0089] Next, the insulating adhesive composition of Table 1 was applied to the surface of the conductive particle-containing layer on the side where the conductive particles were pressed using a bar coater, and dried in an oven at 80° C. for 5 minutes to form an insulating adhesive layer B with a thickness of 4 μm, thereby producing an anisotropic conductive film. (2) Preparation of connection structure A for initial conduction reliability evaluation

[0090] The anisotropic conductive film prepared in (1) was cut into an area sufficient for connection, and sandwiched between an FPC (flexible printed circuit) for initial conduction resistance evaluation and a glass substrate shown below, and heated and pressed with a hot press head through a 50 μm thick Teflon (registered trademark) sheet cushioning material under the conditions of 170°C, 6 MPa, and 5 seconds to obtain a connection structure A for initial conduction reliability evaluation. At this time, the thrust required by the hot press head was 240N.

[0091] (FPC for initial on-resistance evaluation)

[0092] Sn-plated wiring: L / S=8[μm] / 12[μm].

[0093] (Glass Substrate)

[0094] Glass material: 1737F manufactured by Corning;

[0095] Outer diameter: 30×50mm;

[0096] Thickness: 0.5mm;

[0097] Electrode: AL / Mo / ITO wiring (line width 150μm);

[0098] (Initial conduction reliability evaluation test)

[0099] The initial conduction resistance of the connection structure A was measured by a four-terminal method, and the obtained measurement results are shown in Table 2. When the conduction resistance value was less than 4.0Ω, it was evaluated that the initial conduction reliability was good, and when it was 4.0Ω or more, it was evaluated as poor.

[0100] (3) Production of connection structure B for short circuit occurrence evaluation

[0101] The anisotropic conductive film prepared in (1) was cut to an area sufficient for connection, and sandwiched between the FPC (flexible printed circuit) for short circuit evaluation shown below and the glass substrate, and heated and pressed with a hot press head through a 50 μm thick Teflon (registered trademark) sheet cushioning material under the conditions of 170°C, 6 MPa, and 5 seconds to obtain a connection structure B for short circuit evaluation. At this time, the thrust required by the hot press head was 240N.

[0102] (FPC for short circuit evaluation)

[0103] Sn-plated wiring: bump width is 8μm, bump pitch is 12μm.

[0104] (Glass Substrate)

[0105] Glass material: 1737F manufactured by Corning;

[0106] Electrode: Ti pattern wire TEG; width 0.7mm;

[0107] (10 intervals per channel: a 5-branched comb-shaped electrode and a 6-branched comb-shaped electrode are combined to form a gap of 10 intervals (distance between terminals) in each channel. At this time, the combination is made in such a way that the shortest distance between terminals is 1μm, 2μm, 3μm, 4μm or 5μm).

[0108] (Short circuit occurrence evaluation test)

[0109] A voltage of 30 V was applied between the comb-shaped electrodes of the connection structure B for short circuit evaluation, and the shortest distance between the terminals when conduction was achieved (i.e., when a short circuit occurred) was studied. The results are shown in Table 2. The shorter the shortest distance between the terminals when a short circuit occurs, the less likely it is to short circuit, and it can be evaluated as suitable for high-density mounting. In actual use, it is hoped that the distance is less than 4 μm.

[0110] (4) Evaluation of rebound characteristics

[0111] The electrode portion bonded from the glass substrate side of the connection structure A for initial conduction reliability evaluation was observed under an optical microscope to examine whether there was an indentation caused by the conductive particles. The case where the indentation was clearly observed was evaluated as good rebound characteristics, and the case where the indentation was not clearly observed was evaluated as poor. The results are shown in Table 2.

[0112] [Table 2]

[0113]

[0114] According to Table 2, the average particle size of the conductive particles used is less than 3 μm, and the compression hardness (20% K value) of the conductive particles when deformed by 20% is 1500 N / mm 2 Above and 8000N / mm 2 The connection structures of Examples 1 to 4 below show an initial conduction resistance value of less than 4Ω and good initial conduction characteristics. In addition, the rebound characteristics are also good. In particular, the compression hardness (20% K value) of the conductive particles at 20% deformation is 6300N / mm 2 In the case of the connection structure of Example 3, the initial on-resistance was 2.0Ω, and the initial on-characteristics were better than those of the connection structures of other examples.

[0115] On the other hand, in the case of the connection structure of Comparative Example 1, the connection structure has a strength of 1500 N / mm 2 Above and 8000N / mm 2The K value is within the range of 20% below, but because the conductive particles with an average particle size of more than 3 μm are used, the shortest distance between terminals for short circuit is 5 μm, which is more likely to cause short circuit than the connection structure of the embodiment. In the case of the connection structure of Comparative Example 2, the average particle size is less than 3 μm, but because the conductive particles with an average particle size of more than 8000 N / mm 2 The conductive particles with a 20% K value are used, so the initial conduction resistance is much more than 4Ω, and the initial conduction characteristics are poor. The rebound characteristics are also poor. In the case of the connection structure of Comparative Example 3, the average particle size is less than 3μm, but because a particle size of less than 1500N / mm 2 The conductive particles with a K value of 20% have an initial on-resistance far exceeding 4Ω, and the initial on-characteristics are poor. The rebound characteristics are also poor.

[0116] Industrial Applicability

[0117] The connection structure of the present invention has a structure in which the first electronic component and the second electronic component are connected via conductive particles arranged between the electrodes of the first electronic component and the electrodes of the second electronic component and an insulating adhesive, and is characterized in that: as the conductive particles, very fine conductive particles with an average particle size of less than 3 μm are used. Therefore, the connection structure of the present invention is suitable for high-density mounting. Moreover, as the conductive particles, a compressive hardness of 1500 N / mm when deformed by 20% is used. 2 Above and 8000N / mm 2 Therefore, during the thermal compression bonding, the problem of the conductive particles moving is not likely to occur, which can not only suppress the reduction of the initial conduction reliability, but also suppress the occurrence of short circuits. In addition, the deterioration of the rebound characteristics can also be suppressed.

[0118] Explanation of symbols

[0119] 1, 21: 1st electronic component;

[0120] 1a, 21a: electrodes of the first electronic component;

[0121] 2, 22: second electronic component;

[0122] 2a, 22a: electrodes of the second electronic component;

[0123] 3, 23: conductive particles;

[0124] 4, 24: Insulating adhesive;

[0125] 25: stage;

[0126] 26: hot pressing head;

[0127] 30: conductive particles;

[0128] 31, 32: a pair of electrodes;

[0129] 33: Insulating adhesive;

[0130] 100, 200: connecting structure;

[0131] S: Inter-electrode spacing.

Claims

1. A connection structure in which a first electronic component and a second electronic component are connected via conductive particles and an insulating adhesive disposed between an electrode of the first electronic component and an electrode of the second electronic component, The average particle size of the conductive particles is less than 3 μm. The compression hardness of the conductive particles at 20% deformation (20% K value) is 1500N / mm 2 Above and 8000N / mm 2 the following.

2. The connection structure according to claim 1, wherein: The average particle size of the conductive particles is greater than 1 μm and less than 2.8 μm.

3. The connection structure according to claim 1, wherein: The average particle diameter of the conductive particles is 1.1 μm or more and 2.5 μm or less.

4. The connection structure according to any one of claims 1 to 3, wherein The compression hardness of the conductive particles at 20% deformation (20% K value) is 2000N / mm 2 Above and 7000N / mm 2 the following.

5. The connection structure according to any one of claims 1 to 4, wherein The conductive particles are metal-coated resin particles having a metal layer formed on the surface of a resin core.

6. The connection structure according to claim 5, wherein: An insulating film is further formed on the surface of the metal layer of the metal-coated resin particles.

7. The connection structure according to any one of claims 1 to 6, wherein The conductive particles have protrusions on the surface.

8. The connection structure according to any one of claims 1 to 6, wherein The minimum melt viscosity of the insulating adhesive is 2000 Pa·s or more and 15000 Pa·s or less.

9. A method for manufacturing a connection structure, which is the method for manufacturing a connection structure according to claim 1, wherein: Conductive particles and an insulating adhesive are disposed between electrodes of a first electronic component and a second electronic component, and the conductive particles and the insulating adhesive are heated and pressurized from either the first electronic component or the second electronic component to connect the first electronic component and the second electronic component.

10. The manufacturing method according to claim 9, wherein: An anisotropic conductive film or conductive film in which conductive particles are held in a film-like insulating adhesive is sandwiched between the electrode of the first electronic component and the electrode of the second electronic component, so that the conductive particles and the insulating adhesive are arranged between the electrode of the first electronic component and the electrode of the second electronic component.