Composite film

By using copper foil with a large surface roughness and an optimized design of the conductive layer, the connection resistance of the composite film is reduced, and the shielding and electromagnetic interference suppression capabilities of the EMI countermeasure film are improved, making it suitable for electronic devices such as smartphones.

CN118923221APending Publication Date: 2024-11-08FURUKAWA ELECTRIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032573.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-20
Filing Date
2023-04-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing composite films have high connection resistance, making it difficult to meet the requirements of electronic devices for low electromagnetic interference.

Method used

A conductive layer structure with copper foil having a relatively large surface roughness and conductive filler having a number-average particle size, unfolded area ratio, and skewness within a specified range is used to ensure full contact between the conductive filler and the copper foil surface, thereby reducing connection resistance.

Benefits of technology

The composite film achieves low connection resistance, improves electromagnetic wave shielding and electromagnetic interference suppression performance, and is suitable for electronic devices such as smartphones and medical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118923221A_ABST
    Figure CN118923221A_ABST
Patent Text Reader

Abstract

Provided is a composite film having low connection resistance. A composite film (1) is provided with: a copper foil (10); and a conductive layer (20) comprising a conductive adhesive containing a conductive filler or a conductive adhesive containing a conductive filler, the conductive layer (20) being laminated on at least one surface (10a) of the two surfaces of the copper foil (10). The conductive filler has a number average particle diameter of 0.12 [mu] m or more and 7 [mu] m or less. The surface (10a) of the copper foil (10) on which the conductive layer (20) is laminated has a spread area ratio (Sdr) of 0.01% to 40%, a skewness (Ssk) of-1.0 to 1.0, and a contact resistance of 2 to 30 m [Omega], among the two surfaces of the copper foil (10), the spread area ratio (Sdr) being 0.01% to 40%, the skewness (Ssk) being-1.0 to 1.0, and the contact resistance being 2 to 30 m [Omega].
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite film. Background Art

[0002] In recent years, electronic devices such as smartphones, medical equipment, and automobiles have been increasingly integrated and high-performance, and at the same time, the importance of EMI countermeasures to suppress electromagnetic interference (EMI) in electronic devices has increased. Therefore, in order to prevent malfunctions of electronic devices and degradation of communication data quality caused by electromagnetic waves from inside and outside the housing of electronic devices, noise filters, electromagnetic wave absorbing sheets, and other components are used in electronic devices.

[0003] Among such components, composite films called EMI countermeasure films are used in many electronic devices. EMI countermeasure films are composite films having a structure in which an electromagnetic wave shielding layer composed of a metal or the like and a conductive layer composed of a conductive adhesive or a conductive bonding agent are laminated. From the viewpoint of high conductivity, shielding properties, and industrial productivity, copper foil is sometimes used as the electromagnetic wave shielding layer.

[0004] In addition, EMI countermeasure films are widely used as shielding films in flexible substrates (FPC: Flexible printed circuits), chip on film (COF: Chip on Film), or conductive tapes for grounding reinforcement in the casing of electronic equipment.

[0005] When an EMI countermeasure film is installed in an electronic device, usually, the electromagnetic wave shielding layer is attached to the metal part in the electronic device through the conductive layer. In addition, when the electromagnetic wave shielding layer of the EMI countermeasure film is attached to the metal part in the electronic device, the lower the connection resistance from the electromagnetic wave shielding layer to the metal part in the electronic device, the better the performance of suppressing electromagnetic interference (hereinafter, the performance of suppressing electromagnetic interference of the EMI countermeasure film is sometimes also recorded as "EMI resistance"). This EMI resistance can be evaluated by the above-mentioned connection resistance, but sometimes it can also be simulated by wiring resistance.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Publication No. 6872449 Summary of the invention

[0009] Technical problem to be solved by the invention

[0010] As described above, in recent years, as the importance of EMI countermeasures has increased, a composite film having lower connection resistance has been required.

[0011] The technical problem of the present invention is to provide a composite film with low connection resistance.

[0012] Technical solutions for solving technical problems

[0013] In order to solve the above technical problems, the inventors believe that it is effective to use copper foil with low contact resistance as the electromagnetic wave shielding layer, i.e., copper foil, in order to reduce the connection resistance (wiring resistance) of the composite film, and pay attention to the surface shape of the copper foil. However, it is known that even if a copper foil with a clean and smooth surface (small surface roughness) with the lowest contact resistance in principle is used to make an EMI countermeasure film, the wiring resistance of the EMI countermeasure film will not be reduced to the predicted level. On the other hand, compared with a smooth copper foil with a small surface roughness, the use of a copper foil with a relatively large surface roughness can sometimes obtain experimental results that the wiring resistance of the EMI countermeasure film is low, and the inventors have paid attention to this.

[0014] The "Measurement Method of Surface Contact Resistance of Japan Copper and Copper Alloy Association Technical Standard JCBA T323:2011" stipulates the measurement of the contact resistance between the object to be measured and the gold (Au) probe. When measuring the contact resistance of copper foil, since it is the contact resistance between metal rigid bodies, gaps corresponding to the surface shapes of each other are naturally generated at the contact interface, and the actual contact area at the microscopic level becomes smaller accordingly. Therefore, it can be understood that there is a tendency that if the surface roughness of the copper foil is large and the actual contact area with the Au probe is small, the measured value of the contact resistance becomes large, and if the surface roughness of the copper foil is small and the actual contact area with the Au probe is large, the measured value of the contact resistance is low.

[0015] On the other hand, in the case of a composite film used for EMI countermeasure film purposes, what is in contact with the copper foil is a conductive adhesive or a conductive adhesive. When bonded to the copper foil, the conductive adhesive or the conductive adhesive follows the surface shape of the copper foil, so it is basically difficult to generate gaps at the contact interface between the copper foil and the conductive adhesive or the conductive adhesive.

[0016] Therefore, it can be considered that when a composite film is used as an EMI countermeasure film, the contact resistance of the copper foil becomes smaller when a copper foil with a relatively large surface roughness is used compared to a copper foil with the smallest surface roughness, that is, compared to a copper foil with a completely smooth surface. In other words, it can be considered that even if the surface roughness of the copper foil becomes larger, since the conductive layer follows its shape, it is not easy to generate gaps at the contact interface between the copper foil and the conductive layer, and the actual contact area becomes larger according to the amount of the surface roughness of the copper foil, and the contact resistance of the copper foil becomes smaller.

[0017] The present inventors have verified the above viewpoints and found that the wiring resistance of an EMI countermeasure film using a copper foil having a relatively large surface roughness is lower than that of an EMI countermeasure film using a copper foil having a completely smooth surface.

[0018] Furthermore, based on these findings, the inventors conducted in-depth studies and found that the relationship between the number average particle size of the conductive filler contained in the conductive layer and the surface roughness of the copper foil is important in order to obtain an EMI countermeasure film with lower wiring resistance. That is, the inventors found that not only the conductive layer corresponds to and follows the surface shape of the copper foil, but also the distribution of the conductive filler follows the surface shape of the copper foil, and thus it is necessary to increase the contact points between the conductive filler and the surface of the copper foil, and therefore the relationship between the number average particle size of the conductive filler and the surface roughness of the copper foil is important.

[0019] Specifically, it was found that if the number average particle size of the conductive filler, the surface development area ratio Sdr of the copper foil, the surface skewness Ssk of the copper foil, and the contact resistance of the copper foil are controlled within the specified range, the wiring resistance of the EMI countermeasure film can be greatly reduced compared to using only a smooth copper foil with low contact resistance.

[0020] That is, a composite film according to one embodiment of the present invention comprises: a copper foil; and a conductive layer, which is composed of a conductive adhesive containing a conductive filler or a conductive adhesive containing a conductive filler and is laminated on at least one of the two surfaces of the copper foil. Furthermore, the gist of the composite film according to one embodiment of the present invention is that the number average particle size of the conductive filler is 0.12 μm or more and 7 μm or less, the developed area ratio Sdr of the surface on which the conductive layer is laminated among the two surfaces of the copper foil is 0.01% or more and 40% or less, the skewness Ssk is -1.0 or more and 1.0 or less, and the contact resistance is 2 mΩ or more and 30 mΩ or less.

[0021] Effects of the Invention

[0022] The composite film according to the present invention has low connection resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a cross-sectional view illustrating a composite film according to one embodiment of the present invention.

[0024] Figure 2 Yes Description Figure 1 A cross-sectional view of a modified example of the composite membrane. DETAILED DESCRIPTION

[0025] One embodiment of the present invention will be described. In addition, the embodiment described below is an example of the present invention. In addition, various changes or improvements can be added to this embodiment, and the form to which such changes or improvements are added can also be included in the present invention.

[0026] like Figure 1 As shown, the composite film 1 involved in this embodiment comprises: a copper foil 10, forming an electromagnetic wave shielding layer; a conductive layer 20, which is composed of a conductive adhesive containing a conductive filler or a conductive adhesive containing a conductive filler, and is stacked on at least one surface 10a of the two surfaces of the copper foil 10. Figure 1 The composite film 1 is an example in which the conductive layer 20 is laminated only on one surface 10 a of the two surfaces of the copper foil 10 .

[0027] The number average particle size of the conductive filler contained in the conductive layer 20 is 0.12 μm or more and 7 μm or less. In addition, the developed area ratio Sdr of the surface 10a on which the conductive layer 20 is stacked among the two surfaces of the copper foil 10 is 0.01% or more and 40% or less, and similarly, the skewness Ssk of the surface 10a is -1.0 or more and 1.0 or less. Furthermore, the contact resistance of the surface 10a on which the conductive layer 20 is stacked among the two surfaces of the copper foil 10 is 2 mΩ or more and 30 mΩ or less.

[0028] With such a structure, the composite film 1 according to the present embodiment has low connection resistance (wiring resistance). Therefore, the composite film 1 according to the present embodiment has high shielding properties and excellent electromagnetic interference suppression performance (EMI resistance), and can be suitably used as an EMI countermeasure film.

[0029] Therefore, the composite film 1 of this embodiment can be used as an EMI countermeasure film for various electronic devices and exhibits excellent EMI resistance. The composite film 1 of this embodiment can be suitably used in electronic devices such as smartphones, medical devices, and automobiles, and can be suitably used in mobile electronic devices such as smartphones.

[0030] In addition, the composite film 1 according to the present embodiment may further include at least one of a release film 30, an insulating layer 40, and a carrier film 50. Figure 2 As shown in FIG. 1 , a modified example of the composite film 1 according to the present embodiment may have a structure in which a release film 30 is further laminated on the conductive layer 20. Figure 2 As shown, a modified example of the composite film 1 according to the present embodiment may also have a structure in which an insulating layer 40 for electrically protecting the copper foil 10 is further laminated on the surface 10b opposite to the surface 10a on which the conductive layer 20 is laminated, of the two surfaces of the copper foil 10. Figure 2As shown, a modified example of the composite film 1 according to the present embodiment may have a structure in which a carrier film 50 as a support is further laminated on the insulating layer 40 .

[0031] exist Figure 2 , an example of a composite film 1 including a release film 30, an insulating layer 40, and a carrier film 50 is shown, but the modified example of the composite film 1 involved in this embodiment is not limited to this. However, when the conductive layer 20 is laminated on both surfaces 10a and 10b of the copper foil 10, the composite film 1 does not include the insulating layer 40 and the carrier film 50.

[0032] Hereinafter, the composite film 1 according to the present embodiment will be described in further detail.

[0033] (1) About copper foil

[0034] As the copper foil 10 of the composite film 1 involved in this embodiment, any of electrolytic copper foil and rolled copper foil can be used, and copper foil formed by known methods such as evaporation and sputtering can also be used. In addition, copper foil whose surface shape and thickness are adjusted by known methods such as etching and electrolytic polishing can also be used as the copper foil 10 of the composite film 1 involved in this embodiment.

[0035] Examples of the etching solution used for etching include CZ-8100 and CB-5602AY manufactured by MEC Corporation. Etching conditions such as the temperature of the etching solution, etching time, and stirring conditions of the etching solution can be adjusted as appropriate.

[0036] Copper foil subjected to roughening plating can also be used, but since the surface development area ratio Sdr tends to become too large, it is preferred to reduce the current density and electrolysis time during roughening plating. When plating is used, plating based on copper (Cu) is preferred from the viewpoint of conductivity and contact resistance.

[0037] The thickness of the copper foil 10 of the composite film 1 according to the present embodiment is preferably 2 μm or more and 40 μm or less.

[0038] In addition, for the purpose of preventing discoloration during storage and preventing discoloration during the manufacture and use of the composite film in the thermal history, a copper foil subjected to rust-proof treatment after adjusting the surface shape and thickness may be used as the copper foil 10 of the composite film 1 involved in the present embodiment. Examples of rust-proof treatment include plating treatment containing at least one metal selected from nickel (Ni), zinc (Zn), chromium (Cr), molybdenum (Mo), cobalt (Co), silicon (Si), and tungsten (W), and organic treatment using an organic compound such as benzotriazole.

[0039] The developed area ratio Sdr of the surface 10a on which the conductive layer 20 is stacked, of the two surfaces 10a and 10b of the copper foil 10 of the composite film 1 according to the present embodiment, needs to be 0.01% to 40%, but in order to further reduce the connection resistance of the composite film 1, it is preferably 0.01% to 10%, and more preferably 0.05% to 10%.

[0040] The skewness Ssk of the surface 10a on which the conductive layer 20 is stacked, of the two surfaces 10a and 10b of the copper foil 10, needs to be -1.0 to 1.0, but is preferably -0.7 to 1.0, more preferably -0.5 to 0.8, in order to further reduce the connection resistance of the composite film 1.

[0041] Furthermore, the contact resistance of the surface 10a on which the conductive layer 20 is stacked, of the two surfaces 10a and 10b of the copper foil 10, needs to be 2 mΩ to 30 mΩ, but in order to further reduce the connection resistance of the composite film 1, it is preferably 2 mΩ to 25 mΩ, and more preferably 2 mΩ to 20 mΩ.

[0042] Furthermore, in order to further reduce the connection resistance of the composite film 1 , the kurtosis Sku of the surface 10 a on which the conductive layer 20 is laminated, of the two surfaces 10 a and 10 b of the copper foil 10 , is preferably 3.0 or more and 3.6 or less.

[0043] (2) About the conductive layer

[0044] The conductive layer 20 of the composite film 1 according to the present embodiment is composed of a conductive binder containing a conductive filler or a conductive adhesive containing a conductive filler. The conductive binder and the conductive adhesive contain a conductive filler and a resin that impart conductivity to the conductive layer 20.

[0045] The conductive adhesive may also have adhesiveness at room temperature. The resin contained in the conductive adhesive may be a thermosetting resin or a thermoplastic resin. The conductive adhesive containing a thermosetting resin may be in any state of uncured, B stage, or cured in the composite film 1.

[0046] Examples of the resins contained in the conductive adhesive and the conductive bonding agent include epoxy, phenol, amino, alkyd, polyurethane, synthetic rubber, acrylate, acrylic, silicone, imide, isocyanate, vinyl chloride, vinyl acetate, styrene, hydrocarbon resins and adhesives. Among these resins, epoxy resins are preferred because of their excellent heat resistance.

[0047] Examples of conductive fillers include metal particles and carbon particles. Examples of metal types include silver (Ag), platinum (Pt), gold, copper, nickel, palladium (Pd), aluminum (Al), solder, or alloys thereof. Examples of carbon particles include graphite particles, calcined carbon particles, and plated calcined carbon particles. Among these particles, copper particles and graphite particles are preferred from the perspective of formability and industrial productivity when making the conductive layer 20.

[0048] The number average particle size of the conductive filler needs to be 0.12 μm or more and 7 μm or less. If the number average particle size of the conductive filler is 0.12 μm or more, the number of contact points between the conductive filler and the copper foil 10 and the surface area of ​​the conductive filler can be increased, so the conductivity of the conductive layer 20 is excellent. On the other hand, if the number average particle size of the conductive filler is 7 μm or less, the conductive adhesive and the conductive adhesive flow, and the conductive layer 20 becomes easy to follow the shape and height difference of the ground (GND) opening of the printed wiring board and the metal shell, so the conductive layer 20 can be fully filled in the target part.

[0049] Furthermore, in the cross-section of the conductive layer 20 that appears when the conductive layer 20 is cut along a plane perpendicular to the surface of the copper foil 10, the ratio of the cross-sectional area of ​​the conductive filler to the cross-sectional area of ​​the conductive layer 20 (hereinafter sometimes also referred to as "cross-sectional area ratio of the conductive filler") is preferably 30% or more and 85% or less, and more preferably 45% or more and 80% or less.

[0050] When the cross-sectional area ratio of the conductive filler is 30% or more, the number of contact points between the conductive filler and the copper foil 10 and the surface area of ​​the conductive filler can be increased, so that the conductivity of the conductive layer 20 is excellent. On the other hand, when the cross-sectional area ratio of the conductive filler is 85% or less, the flexibility of the composite film 1 is excellent.

[0051] The thickness of the conductive layer 20 is preferably 5 μm or more and 50 μm or less. If the thickness of the conductive layer 20 is 5 μm or more, the conductive layer 20 becomes easy to follow the shape and height difference of the ground (GND) opening of the metal case of the printed wiring board or electronic device, and the target part can be fully filled with the conductive layer 20. On the other hand, if the thickness of the conductive layer 20 is 50 μm or less, the composite film 1 has excellent flexibility, so the composite film 1 can be installed in a thinner space.

[0052] Furthermore, the conductive layer 20 may have isotropic conductivity or anisotropic conductivity.

[0053] Furthermore, the conductive filler may be in the form of particles, needles or fibers. When the conductive filler is in the form of needles or fibers, the number average particle size of the conductive filler is a number average diameter calculated based on the diameter of the needle-shaped or fiber-shaped conductive filler.

[0054] Furthermore, in order to impart flexibility to the conductive layer 20, additives such as rubber components (carboxyl-modified nitrile rubber, acrylic rubber, etc.), tackifiers, and curing agents (isocyanate compounds, etc.) may be added to the conductive adhesive or conductive bonding agent. In addition, in order to improve the flame retardancy, moldability, and mechanical properties of the conductive layer 20, additives that improve these properties may be added to the conductive adhesive or conductive bonding agent.

[0055] (3) About release film

[0056] The release film 30 is a film obtained by treating the surface of the substrate with a release agent, and is used to protect the conductive layer 20. That is, by covering the surface of the conductive layer 20 opposite to the surface facing the copper foil 10, the adhesiveness and adhesion of the conductive layer 20 are prevented from being reduced. In addition, the release film 30 is laminated on the conductive layer 20 in such a manner that the surface of the release film 30 treated with the release agent faces the conductive layer 20.

[0057] Examples of the material of the base material of the release film 30 include resin and paper. Examples of the type of resin include polyethylene isophthalate, polybutylene terephthalate, polyethylene naphthalate, polyolefin, polyacetate, polycarbonate, polyphenylene sulfide, polyamide, ethylene-vinyl acetate copolymer, polyvinyl chloride, polystyrene, polyvinylidene chloride, synthetic rubber, and liquid crystal polymer. In addition, examples of the release film 30 using paper as the base material include release paper.

[0058] (4) About the insulation layer

[0059] The insulating layer 40 is a layer for protecting the copper foil 10 when the composite film 1 is mounted on an electronic device, etc. That is, by covering the copper foil 10 with the insulating layer 40 , electrical contact with the copper foil 10 is prevented.

[0060] The insulating layer 40 can be formed, for example, by applying a coating containing a thermosetting resin and a curing agent to the surface 10b on the opposite side of the surface 10a on which the conductive layer 20 is laminated, and semi-curing or curing the coating. In addition, the insulating layer 40 can also be formed, for example, by applying a coating containing a thermoplastic resin to the surface 10b on the opposite side of the surface 10a on which the conductive layer 20 is laminated, of the two surfaces of the copper foil 10. Furthermore, the insulating layer 40 can also be formed, for example, by melt-molding a resin composition containing a thermoplastic resin into a film on the surface 10b on the opposite side of the surface 10a on which the conductive layer 20 is laminated, of the two surfaces of the copper foil 10.

[0061] Since the composite film 1 is sometimes mounted on electronic devices or the like by welding or the like, the insulating layer 40 preferably has heat resistance. From this point of view, the insulating layer 40 is preferably formed using a coating material containing a thermosetting resin and a curing agent.

[0062] Examples of thermosetting resins used in forming the insulating layer 40 include amide resins, epoxy resins, phenolic resins, amino resins, alkyd resins, polyurethane resins, synthetic rubbers, and ultraviolet curing acrylate resins. Among these thermosetting resins, amide resins and epoxy resins are preferred from the viewpoint of excellent heat resistance.

[0063] Examples of the thermoplastic resin used for forming the insulating layer 40 include aromatic polyether ketone, polyimide, polyamide-imide, polyamide, polysulfone, polyether sulfone, polyphenylene sulfone, polyphenylene sulfide, polyphenylene sulfide sulfone, and polyphenylene sulfide ketone.

[0064] A known filler may be blended in the insulating layer 40 for the purpose of imparting weather resistance, concealing property, flame retardancy, design properties, or coloring.

[0065] (5) About carrier film

[0066] The carrier film 50 is a support body that strengthens and protects the composite film 1. In addition, the carrier film 50 is laminated on the surface opposite to the surface facing the copper foil 10 of the two surfaces of the insulating layer 40. As an example of the structure of the carrier film 50, a laminated structure of a base material and an adhesive layer can be cited. As the base material of the carrier film 50, the same base material as the base material exemplified as the base material of the release film 30 can be used. As the material forming the adhesive layer, acrylic adhesives, polyurethane adhesives, rubber adhesives, etc. can be cited.

[0067] [Example]

[0068] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples.

[0069] (A) Copper foil

[0070] As the raw material copper foil for manufacturing the composite films of Examples 1 to 16 and Comparative Examples 1 to 5, a copper foil with a thickness of 6 μm having the surface roughness (surface development area ratio Sdr, skewness Ssk, and kurtosis Sku) shown in Table 1 was prepared. These copper foils were commercially available electrolytic copper foils or copper foils whose surface roughness was adjusted by etching the commercially available electrolytic copper foils. The etching solution used for the etching treatment was CB-5601AY manufactured by MEC Co., Ltd., and the surface roughness was adjusted by adjusting the temperature of the etching solution, the etching time, the stirring conditions of the etching solution, and the like.

[0071] The surface roughness of the copper foil was measured using confocal laser microscopes VK-X1050 and VK-X1000 manufactured by KEYENCE Co., Ltd. The numerical values ​​shown in Table 1 for any of the surface development area ratio Sdr, skewness Ssk, and kurtosis Sku are the average values ​​of the measured values ​​at any three points.

[0072] The objective lens magnification of the confocal laser microscope was 100 times, the scanning mode was laser confocal, the measurement size was 2048×1536, the measurement quality was High Precision, and the pitch was 0.08 μm.

[0073] The surface development area ratio Sdr, skewness Ssk, and kurtosis Sku are calculated by performing calculations in an arbitrary field of view of 100 μm×100 μm using the attached analysis software after performing reference plane correction, smoothing image processing, and filtering processing on the measurement data as shown below.

[0074] Reference surface correction: entire surface

[0075] Smoothing: 3×3, Gaussian

[0076] Filtering: L filter 0.025mm

[0077] Furthermore, for the surface of the laminated conductive layer of the two surfaces of these copper foils, before laminating the conductive layer, the contact resistance is measured by the method specified in the "Measurement method of surface contact resistance of the technical standard JCBA T323:2011 of the Japan Copper Association". In the measurement of the contact resistance, an electric contact simulator CRS-113-AU manufactured by Yamazaki Seiki Research Institute Co., Ltd. is used, and an Au probe with a diameter of 1 mm is used as a probe. The measurement conditions are a contact load of 0.1N, an AC frequency of 287Hz, and a measurement current of 1mA. The results are shown in Table 1. In addition, the numerical values ​​shown in Table 1 are the average values ​​of the measured values ​​at any 10 points.

[0078]

Table 1

[0079]

[0080] (B) Conductive layer

[0081] A conductive layer was laminated on one of the two surfaces of the copper foil to produce composite films of Examples 1 to 16 and Comparative Examples 1 to 5. The conductive layer was formed by applying a conductive adhesive containing an acrylic resin and a conductive filler on the copper foil in a film form and then heating at 80° C. for 3 minutes to volatilize the solvent.

[0082] The acrylic resin was an acrylic adhesive FINETAC CT-5030 manufactured by DIC Corporation, and the conductive filler was copper powder. The number average particle size of the copper powder is shown in Table 1.

[0083] The content of the conductive filler in the conductive adhesive was adjusted so that the cross-sectional area ratio of the conductive filler in the conductive layer was the value described in Table 1. The thickness of the film-like conductive adhesive applied on the copper foil was adjusted so that the thickness of the conductive layer of the composite film was 30 μm.

[0084] (C) Composite membrane

[0085] The number average particle size and cross-sectional area ratio of the conductive filler were calculated for the composite films of Examples 1 to 16 and Comparative Examples 1 to 5. The results are shown in Table 1.

[0086] The following is a method for calculating the cross-sectional area ratio of the conductive filler. First, an arbitrary square region in the cross section of the conductive layer is observed using a scanning electron microscope to obtain image data of the square region. The cross section of the conductive layer is a cross section of the conductive layer that appears when the conductive layer is cut with a plane orthogonal to the surface of the copper foil (i.e., a plane parallel to the thickness direction of the conductive layer). In addition, one side of the observed square region is 25 μm.

[0087] Next, the image data is processed by image editing software to produce a binary image of the portion of the conductive filler particles and the portion other than the conductive filler particles. Then, based on the obtained binary image, the cross-sectional area of ​​the conductive layer (i.e., the area of ​​the square region) and the cross-sectional area of ​​the conductive filler are obtained, and the cross-sectional area ratio of the conductive filler is calculated by dividing the cross-sectional area of ​​the conductive filler by the area of ​​the square region. The above steps are performed for any three locations, and the average value of their cross-sectional area ratios is calculated. The results are shown in Table 1.

[0088] The following describes the calculation method of the number average particle size of the conductive filler. The minimum diameter and the maximum diameter of the conductive filler particles present in the above-mentioned square region are measured, and the average value of the minimum diameter and the maximum diameter is taken as the particle size of the particle. Then, the particle size of all the conductive filler particles present in the above-mentioned square region is measured, and the arithmetic average value is taken as the number average particle size of the conductive filler. The results are shown in Table 1.

[0089] The wiring resistance of the composite films of Examples 1 to 16 and Comparative Examples 1 to 5 was measured. The wiring resistance measurement method is described below. A printed wiring board with two copper sample pasting electrodes exposed side by side was prepared. These sample pasting electrodes were square with a side of 4 mm, and the center distance between the two sample pasting electrodes was 12 mm.

[0090] The resistance measuring electrode is exposed near each of the two sample pasting electrodes. Specifically, the resistance measuring electrode is formed on a side different from the side with the adjacent sample pasting electrode in the vicinity of the sample pasting electrode. The sample pasting electrode and the resistance measuring electrode formed near it are electrically connected to form a pair through the inner layer circuit of the printed wiring board, but the two sample pasting electrodes are not electrically connected to each other. In addition, the two sample pasting electrodes and the two resistance measuring electrodes are subjected to electroless nickel plating and gold plating generally used in printed wiring board applications to minimize the effects of oxidation on the electrode surface.

[0091] First, for two pairs of electrodes for sample attachment and electrodes for resistance measurement, the resistance between the electrodes for sample attachment and the electrodes for resistance measurement is measured by a four-terminal method without the composite film attached to the electrodes for sample attachment. Then, the sum of the two resistances obtained is recorded as the measured substrate resistance.

[0092] Next, the composite film of the embodiment or comparative example is attached in a manner spanning between two sample pasting electrodes, and after being pressed using the peeling test pressing roller APR-97 manufactured by IMADA Co., Ltd., it is left to stand for 30 minutes. Then, the resistance between the two resistance measuring electrodes is measured by the four-terminal method, and the value after subtracting the measured substrate resistance from the measured value is used as the wiring resistance of the composite film. The wiring resistance is measured five times, and the average value is used as the wiring resistance of each composite film of Examples 1 to 16 and Comparative Examples 1 to 5. The above resistance measurements were all carried out in an environment of temperature 25°C and humidity 40~50%RH.

[0093] The measurement results of the wiring resistance are shown in Table 1. The measurement results of the wiring resistance shown in Table 1 show the results evaluated based on the following evaluation criteria.

[0094] AA (qualified): wiring resistance is less than 10mΩ

[0095] A (pass): Wiring resistance is 10 mΩ or more and less than 30 mΩ

[0096] B (pass): Wiring resistance is 30mΩ or more and less than 100mΩ

[0097] C (Unqualified): Wiring resistance is 100mΩ or more and less than 500mΩ

[0098] D (Unqualified): Wiring resistance is 500mΩ or more

[0099] As can be seen from Table 1, the composite films of Examples 1 to 16 have lower wiring resistance than the composite films of Comparative Examples 1 to 5. Therefore, it can be considered that the composite films of Examples 1 to 16 have better electromagnetic interference suppression performance (EMI resistance) than the composite films of Comparative Examples 1 to 5. Therefore, the composite films of Examples 1 to 16 can be suitably used as EMI countermeasure films.

[0100] Description of Reference Numerals

[0101] 1: composite film; 10: copper foil; 10a: surface on which the conductive layer is laminated; 10b: surface opposite to the surface on which the conductive layer is laminated; 20: conductive layer; 30: release film; 40: insulating layer; 50: carrier film.

Claims

1. A composite film comprising: a copper foil; and a conductive layer, which is composed of a conductive adhesive containing a conductive filler or a conductive adhesive containing a conductive filler and is laminated on at least one of the two surfaces of the copper foil, The number average particle size of the conductive filler is 0.12 μm or more and 7 μm or less, The copper foil has a surface on which the conductive layer is laminated, of both surfaces, with a developed area ratio Sdr of 0.01% to 40%, a skewness Ssk of -1.0 to 1.0, and a contact resistance of 2 mΩ to 30 mΩ.

2. The composite film according to claim 1, wherein In a cross section of the conductive layer shown when the conductive layer is cut along a plane perpendicular to the surface of the copper foil, a ratio of a cross-sectional area of ​​the conductive filler to a cross-sectional area of ​​the conductive layer is 30% to 85%.

3. The composite film according to claim 1 or 2, wherein The kurtosis Sku of the surface on which the conductive layer is stacked, of the two surfaces of the copper foil, is 3.0 or more and 3.6 or less.

4. The composite film according to claim 1 or 2, wherein A release film is further laminated on the conductive layer.

5. The composite film according to claim 3, wherein A release film is further laminated on the conductive layer.

6. The composite film according to claim 1 or 2, wherein An insulating layer for electrically protecting the copper foil is further laminated on the surface opposite to the surface on which the conductive layer is laminated, of the two surfaces of the copper foil.

7. The composite film according to claim 3, wherein An insulating layer for electrically protecting the copper foil is further laminated on the surface opposite to the surface on which the conductive layer is laminated, of the two surfaces of the copper foil.

8. The composite film according to claim 6, wherein A carrier film as a support is further laminated on the insulating layer.

9. The composite film according to claim 7, wherein A carrier film as a support is further laminated on the insulating layer.

10. The composite film according to claim 1 or 2, wherein The composite film is used as an EMI countermeasure film.