Method for preparing matrix backing material from activated carbon decolorized by monopotassium phosphate
By steam activation and binder treatment of activated carbon after decolorization of potassium dihydrogen phosphate, matrix activated carbon was prepared, which solved the problems of matrix pollution and solid waste treatment in facility agriculture, achieved adsorption of hazardous substances and improved matrix, and improved plant growth and Economic benefits of the enterprise.
Patent Information
- Application Number
- CN202411003930.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
In modern facility agriculture, the use of pesticides and fertilizers leads to an increase in residues in the cultivation matrix, affecting crop growth, and the used activated carbon is treated as solid waste, increasing enterprise costs and possibly causing environmental pollution.
The activated carbon after decolorization of potassium dihydrogen phosphate is steam-activated, and is granulated and dried with binders (such as potassium humate and carboxymethyl cellulose) to prepare the finished product of matrix activated carbon to improve the physical properties of the matrix and promote plant growth. .
Effectively adsorb harmful substances, reduce harm to plants, avoid solid waste generation, increase corporate economic benefits, improve the aeration and water utilization efficiency of the substrate, and prolong the durability and stability of soilless cultivation substrates.
Smart Images

Figure BDA0004962442200000051 
Figure BDA0004962442200000061 
Figure BDA0004962442200000062
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of activated carbon recovery and treatment, and in particular to a method for preparing a matrix base material by utilizing activated carbon decolorized by potassium dihydrogen phosphate. Background Art
[0002] In the process of modern facility agriculture production, the extensive use of pesticides and fertilizers has led to more and more pesticide and fertilizer residues in the cultivation medium, causing the medium to become compacted and acidified, and the physical and chemical properties and structure of the medium to become increasingly poor, affecting the growth of crops.
[0003] Adding a certain proportion of activated carbon to the matrix can improve the physical properties of the matrix. The high porosity and high specific surface area of biochar can increase the aeration and water use efficiency of the matrix, improve the bulk density and water retention, and also reduce the loss of salt and nitrogen in the matrix, increase the durability and stability of the soilless cultivation matrix; it can also absorb harmful substances such as heavy metal ions, organic pollutants and pesticide residues, and reduce the harm of pesticide residues and pollutants to crops. At the same time, activated carbon can also increase the number and types of microorganisms in the matrix, promote matrix respiration and organic matter decomposition, improve matrix fertility and increase crop yields.
[0004] In the process of producing inositol and potassium dihydrogen phosphate using potassium phytate as raw material, activated carbon is needed for decolorization. At present, used activated carbon is mostly treated as solid waste, which not only increases the processing cost of the enterprise, but also easily causes secondary pollution. In addition, used activated carbon contains a certain amount of potassium dihydrogen phosphate, protein hydrolyzate, pigment and other ingredients, which are not only harmless to crops, but also can be used as nutrients to promote plant growth. Therefore, in view of the above problems, it is necessary to develop a method for preparing a matrix base material using activated carbon decolorized by potassium dihydrogen phosphate. Summary of the invention
[0005] The technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, a method for preparing a matrix base material by using activated carbon decolorized by potassium dihydrogen phosphate is provided. The method can avoid environmental pollution, turn waste into treasure, and increase the economic benefits of the enterprise.
[0006] In order to solve the above technical problems, the technical solution of the present invention is:
[0007] A method for preparing a matrix base material using activated carbon decolorized by potassium dihydrogen phosphate, the method comprising the following steps:
[0008] (1) taking the activated carbon decolorized by potassium dihydrogen phosphate and activating it to obtain an activated carbon material for later use;
[0009] (2) taking the activated carbon material after the activation treatment in step (1), adding a binder, mixing and granulating, and obtaining wet granules for use;
[0010] (3) taking the wet particles described in step (2) and drying them to obtain a finished matrix activated carbon product.
[0011] As an improved technical solution, during the activation treatment in step (1), the activated carbon is spread out in layers and then activated with steam at 60-80° C., and the activation time is controlled to be 1-3 hours.
[0012] As an improved technical solution, the adhesive in step (2) includes potassium humate and carboxymethyl cellulose, and the potassium humate and carboxymethyl cellulose are mixed in a mass ratio of 10:1-5.
[0013] As an improved technical solution, the amount of the binder added in step (2) is 0.5-1‰ of the weight of the activated carbon material after activation treatment.
[0014] As an improved technical solution, the particle size of the wet granules in step (2) is 20-40 mesh.
[0015] As an improved technical solution, air flow drying is adopted in step (3), and the air inlet temperature is controlled at 120-150°C and the air outlet temperature is controlled at 60-80°C.
[0016] After adopting the above technical solution, the beneficial effects of the present invention are:
[0017] The present invention uses activated carbon decolorized by potassium dihydrogen phosphate as raw material. The activated carbon after steam activation can adsorb harmful substances in the matrix, such as heavy metals, pesticides, etc., reduce their damage to plants, and effectively promote plant growth and development; then the activated carbon after activation treatment is mixed with a binder, granulated, and dried to obtain a matrix activated carbon product. The above method can effectively treat the decolorized solid waste activated carbon, avoid the generation of solid waste, and reduce environmental pressure; make full use of the residual value of the waste activated carbon and increase corporate profits. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0019] Example 1
[0020] A method for preparing a matrix base material using activated carbon decolorized by potassium dihydrogen phosphate, comprising the following steps:
[0021] (1) 500 kg of activated carbon (water content 50%, iodine value 200) decolorized with potassium dihydrogen phosphate was taken, layered and flattened, and activated with 60° C. steam. After activation treatment for 1 hour, 490 kg of activated carbon material (water content 49%) was obtained for standby use;
[0022] (2) taking 490 kg of the activated carbon material after the activation treatment in step (1), adding 0.5‰ of a binder (potassium humate and carboxymethyl cellulose mixed in a mass ratio of 10:5, and then adding 10 kg of the steam condensate obtained in step (1), heating and dissolving), mixing and granulating to obtain wet granules with a particle size of 20-40 mesh for later use;
[0023] (3) The wet particles in step (2) are dried by air flow (the air inlet temperature is controlled at 120° C. and the air outlet temperature is controlled at 60° C.) to obtain a finished matrix activated carbon product.
[0024] Example 2
[0025] A method for preparing a matrix base material using activated carbon decolorized by potassium dihydrogen phosphate, comprising the following steps:
[0026] (1) 500 kg of activated carbon (water content 50%, iodine value 200) decolorized with potassium dihydrogen phosphate was taken, layered and then activated with 65° C. steam. After activation for 1.5 h, 485 kg of activated carbon material (water content 48.5%) was obtained for later use;
[0027] (2) taking 485 kg of the activated carbon material after the activation treatment in step (1), adding 0.65‰ of a binder (potassium humate and carboxymethyl cellulose mixed in a mass ratio of 10:4, and then adding 10 kg of the steam condensate obtained in step (1), heating and dissolving), mixing and granulating to obtain wet granules with a particle size of 20-40 mesh for later use;
[0028] (3) The wet particles in step (2) are dried by air flow (the air inlet temperature is controlled at 128° C. and the air outlet temperature is controlled at 65° C.) to obtain a finished matrix activated carbon product.
[0029] Example 3
[0030] A method for preparing a matrix base material using activated carbon decolorized by potassium dihydrogen phosphate, comprising the following steps:
[0031] (1) 500 kg of activated carbon (water content 50%, iodine value 200) decolorized with potassium dihydrogen phosphate was taken, layered and then activated with 70° C. steam. After activation for 2 hours, 470 kg of activated carbon material (water content 46.5%) was obtained for later use;
[0032] (2) taking 470 kg of the activated carbon material after the activation treatment in step (1), adding 0.75‰ of the weight of the activated carbon material as a binder (potassium humate and carboxymethyl cellulose are mixed in a mass ratio of 10:3, and then adding 10 kg of the steam condensate obtained in step (1), heating and dissolving), mixing and granulating to obtain wet granules with a particle size of 20-40 mesh for later use;
[0033] (3) The wet particles in step (2) are dried by air flow (the air inlet temperature is controlled at 135° C. and the air outlet temperature is controlled at 70° C.) to obtain a matrix activated carbon product.
[0034] Example 4
[0035] A method for preparing a matrix base material using activated carbon decolorized by potassium dihydrogen phosphate, comprising the following steps:
[0036] (1) 500 kg of activated carbon (water content 50%, iodine value 200) decolorized with potassium dihydrogen phosphate was taken, layered and then activated with 75° C. steam. After activation for 2.5 h, 460 kg of activated carbon material (water content 45.7%) was obtained for later use;
[0037] (2) taking 460 kg of the activated carbon material after the activation treatment in step (1), adding 0.85‰ of the weight of the activated carbon material as a binder (potassium humate and carboxymethyl cellulose are mixed in a mass ratio of 10:2, and then adding 10 kg of the steam condensate obtained in step (1), heating and dissolving), mixing and granulating to obtain wet granules with a particle size of 20-40 mesh for later use;
[0038] (3) The wet particles in step (2) are dried by air flow (the air inlet temperature is controlled at 142° C. and the air outlet temperature is controlled at 75° C.) to obtain a finished matrix activated carbon product.
[0039] Example 5
[0040] A method for preparing a matrix base material using activated carbon decolorized by potassium dihydrogen phosphate, comprising the following steps:
[0041] (1) 500 kg of activated carbon (water content 50%, iodine value 200) decolorized with potassium dihydrogen phosphate was taken, layered and then activated with 80° C. steam. After activation for 3 hours, 450 kg of activated carbon material (water content 44.4%) was obtained for standby use;
[0042] (2) taking 450 kg of the activated carbon material after the activation treatment in step (1), adding 1‰ of the weight of the activated carbon material to a binder (potassium humate and carboxymethyl cellulose are mixed in a mass ratio of 10:1, adding 10 kg of the steam condensate obtained in step (1), heating and dissolving), mixing and granulating to obtain wet granules with a particle size of 20-40 mesh for later use;
[0043] (3) The wet particles in step (2) are dried by air flow (the air inlet temperature is controlled at 150° C. and the air outlet temperature is controlled at 80° C.) to obtain a finished matrix activated carbon product.
[0044] In order to better prove that the method of the present invention can obtain a matrix activated carbon product with better indicators, 11 comparative examples are given with reference to Example 3, as shown in the following content; the iodine value is tested in accordance with GB / T12496.7-1990 "Test Method for Wood Activated Carbon".
[0045] Comparative Example 1
[0046] The difference from Example 3 is that the temperature of the steam in step (1) is 55° C., and the remaining operations are the same.
[0047] Comparative Example 2
[0048] The difference from Example 3 is that the activation treatment time in step (1) is 0.5 h, and the other operations are the same.
[0049] Comparative Example 3
[0050] The difference from Example 3 is that the activation treatment time in step (1) is 3.5 h, and the other operations are the same.
[0051] Comparative Example 4
[0052] The difference from Example 3 is that the adhesive in step (2) does not contain potassium humate, and the remaining operations are the same.
[0053] Comparative Example 5
[0054] The difference from Example 3 is that the adhesive in step (2) does not contain carboxymethyl cellulose, and the remaining operations are the same.
[0055] Comparative Example 6
[0056] The difference from Example 3 is that the amount of binder used in step (2) is 0.3‰ of the weight of the activated carbon material, and the rest of the operations are the same.
[0057] Comparative Example 7
[0058] The difference from Example 3 is that the amount of binder used in step (2) is 1.5‰ of the weight of the activated carbon material, and the rest of the operations are the same.
[0059] Comparative Example 8
[0060] The difference from Example 3 is that the air inlet temperature of the air flow drying in step (3) is 115° C., and the rest of the operations are the same.
[0061] Comparative Example 9
[0062] The difference from Example 3 is that the air inlet temperature of the air flow drying in step (3) is 155° C., and the rest of the operations are the same.
[0063] Comparative Example 10
[0064] The difference from Example 3 is that the outlet temperature of the air flow drying in step (3) is 55° C., and the rest of the operations are the same.
[0065] Comparative Example 11
[0066] The difference from Example 3 is that the outlet temperature of the air flow drying in step (3) is 85° C., and the rest of the operations are the same.
[0067] Table 1 (Is the smaller the ash content, the better? Is the smaller the apparent density, the better? Is the larger the iodine value, the better? Is the smaller the uniformity coefficient, the better?)
[0068]
[0069]
[0070] It can be found from the data in Table 1 that, by adopting the method of the present invention, the comprehensive indexes of the matrix activated carbon product obtained in Example 3 are higher than those in other embodiments and Comparative Examples 1-11.
[0071] In order to better prove that adding the activated carbon recovered by the present invention to the matrix can improve the physical properties of the matrix and promote plant growth and development, the activated carbon matrix prepared in Implementation 3 is mixed with field soil at a ratio of 20%, 40% and 50% (corresponding to test group 1, test group 2 and test group 3, respectively), and an equal amount of organic fertilizer is added and mixed evenly, and a strawberry seedling planting test is carried out. The control group 1 is not added with the matrix activated carbon in Example 3 of the present invention, the control group 2 is added with the matrix activated carbon in Comparative Example 1, the control group 3 is added with the matrix activated carbon in Comparative Example 2, and the control group 4 is added with the matrix activated carbon in Comparative Example 3. The specific test results are as follows.
[0072] Table 2
[0073]
[0074]
[0075] The test results in Table 2 show that adding activated carbon matrix can significantly improve the growth of strawberry seedlings. The test group is significantly better than the control group in terms of plant height, rhizome diameter, root number and plant fresh weight.
[0076] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a matrix base material using activated carbon decolorized by potassium dihydrogen phosphate, characterized in that: The method comprises the following steps: (1) taking the activated carbon decolorized by potassium dihydrogen phosphate and activating it to obtain an activated carbon material for later use; (2) taking the activated carbon material after the activation treatment in step (1), adding a binder, mixing and granulating, and obtaining wet granules for use; (3) taking the wet particles described in step (2) and drying them to obtain a finished matrix activated carbon product.
2. The method for preparing a matrix base material by using activated carbon decolorized by potassium dihydrogen phosphate according to claim 1, characterized in that: During the activation treatment in step (1), the activated carbon is spread out in layers and then activated with steam at 60-80° C. The activation time is controlled to be 1-3 hours.
3. The method for preparing a matrix base material by using activated carbon decolorized by potassium dihydrogen phosphate according to claim 1, characterized in that: The adhesive in step (2) includes potassium humate and carboxymethyl cellulose, and the potassium humate and carboxymethyl cellulose are mixed in a mass ratio of 10:1-5.
4. The method for preparing a matrix base material by using activated carbon decolorized by potassium dihydrogen phosphate according to claim 1, characterized in that: The amount of the binder added in step (2) is 0.5-1‰ of the weight of the activated carbon material after activation treatment.
5. The method for preparing a matrix base material by using activated carbon decolorized by potassium dihydrogen phosphate according to claim 1, characterized in that: The particle size of the wet granules in step (2) is 20-40 mesh.
6. The method for preparing a matrix base material by using activated carbon decolorized by potassium dihydrogen phosphate according to claim 1, characterized in that: In step (3), air flow drying is adopted, and the air inlet temperature is controlled at 120-150°C and the air outlet temperature is controlled at 60-80°C.
Citation Information
Patent Citations
A method for preparing potassium dihydrogen phosphate
CN102285649A
Columnar activated carbon based on coal pitch binders and preparation method of columnar activated carbon
CN102674341A
Wooden activated carbon for vehicle carbon tank and preparation technology
CN113753891A
Base fertilizer auxiliary agent prepared after active carbon decoloration and enzymolysis of peptide, and preparation method and application of base fertilizer auxiliary agent
CN114853544A
Decoloration waste powdered activated carbon forming and regenerating product and preparation thereof