By using the ratio of natural rubber, calcium powder, cooking oil and sleep aid agent in pet toys, the problem that existing pet toys cannot promote deep sleep in pets is solved, and the soothing effect of pet toys when biting or licking is achieved is achieved. , improves the quality of sleep and physical and mental health of pets.
Patent Information
- Application Number
- CN202410983467.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
Existing pet toys often fail to create an environment that helps relax and quiet when the pet falls asleep, making it difficult for pets to enter deep sleep, ignoring the importance of pet sleep quality to physical and mental health.
Use natural rubber, calcium powder, cooking oil, zinc oxide and sleep aid mixture (chamomile, valerian root, lavender, melatonin) to be proportioned in a certain proportion, and after refining, compacting, spinning and injection molding, it is helpful to form A sleep function pet toy helps pets soothe their emotions while chewing or licking, and promotes deep sleep.
Through the use of this pet toy, pets can enter deep sleep faster, reduce night agitation and restlessness, improve sleep quality, meet pets' sleep needs, and enhance immunity and emotional state.
Abstract
Description
Technical Field
[0001] The invention relates to a pet toy, in particular to a pet toy with a sleep-aiding function and a preparation method thereof. Background Art
[0002] Pet toys are toys for pets to play with, which are different from traditional toys. Traditional toys are toys for children or girls and boys to eliminate boredom or to kill time. Pet toys are a type of parent-child toy that was born based on pets as human partnerships. The purpose of this toy is to allow humans to truly interact with their babies and get greater emotional communication and interaction.
[0003] Existing pet toys usually focus on providing entertainment value, such as letting pets chase, chew, and play to consume their energy. However, these toys often fail to create a relaxing and quiet environment when pets are ready to fall asleep. For example, toys that make loud noises or have strong colors and stimulating shapes may become a distraction when pets are sleeping, making it difficult for pets to enter a deep sleep state, and the quality of sleep for pets is crucial to their physical and mental health. Just as humans need sufficient and good sleep to maintain physical functions and mental health, pets also need a stable sleep to stay energetic, enhance immunity, and maintain a good emotional state. However, the design focus of most pet toys on the market is often on entertainment and interaction, ignoring the key need of sleep assistance. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a pet toy with a sleep-aiding function. The raw material components are composed of: 62-66 parts of natural rubber, 16-20 parts of calcium powder, 2-6 parts of edible oil, 3-7 parts of auxiliary agents and 4-6 parts of sleep-aiding mixtures.
[0005] Furthermore, the auxiliary agent is zinc oxide.
[0006] Furthermore, the sleep-aiding mixture consists of chamomile, valerian root, lavender and melatonin.
[0007] Furthermore, the raw material components are composed of 0.5-1.5 parts of chamomile, valerian root, lavender and melatonin.
[0008] Furthermore, the raw material components also include mint, and the component composition is: 4-6 parts of mint.
[0009] The present application also provides a method for preparing a pet toy with a sleep-aiding function, comprising the following steps:
[0010] S1: accurately weigh and mix the selected raw materials in a certain proportion;
[0011] S2: Put the prepared raw materials into the internal mixer. The rotor of the internal mixer rotates at a high speed, which produces shear, extrusion and friction on the raw materials, so that the raw materials are evenly mixed and stirred together, and gradually form a rubber compound with a certain plasticity;
[0012] S3: placing the rubber material into a double-roller press for repeated compaction and drying, and after the rubber material is cooled, cutting it into sheets;
[0013] S4: The sheet rubber is placed in a granulator to form granules, and then the granular rubber is placed in a stirring air dryer, and is blown dry with warm air at 50 degrees while being continuously stirred;
[0014] S5: Put the above granular rubber material into an injection molding machine for injection molding and vulcanization molding.
[0015] The present application also provides a second method for preparing a pet toy with a sleep-aiding function, comprising the following steps:
[0016] S1: accurately weigh and mix the selected raw materials in a certain proportion;
[0017] S2: Put the prepared raw materials into the internal mixer. The rotor of the internal mixer rotates at a high speed, which produces shear, extrusion and friction on the raw materials, so that the raw materials are evenly mixed and stirred together, and gradually form a rubber compound with a certain plasticity;
[0018] S3: putting the rubber material into a double-roller press for repeated compaction and drying, cooling it rapidly in a water tank, and then cutting it into sheets or strips of corresponding sizes;
[0019] S4: Put the sheet or strip rubber material into a corresponding mold, and then use a hot press to stamp it.
[0020] Furthermore, the mixing time of the internal mixer is 25-35 minutes, and in the first 10 minutes of mixing, the operating temperature of the internal mixer is between 120-180 degrees, between the 10th minute and the 20th minute of mixing, the operating temperature of the internal mixer is 80-110 degrees, and after the 20th minute of mixing, the operating temperature of the internal mixer is 60 degrees.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention utilizes natural rubber, calcium powder, edible oil, auxiliary agents and sleep-aiding mixtures which are mixed in a certain weight ratio, and then subjected to heating, stirring, pressing, drying, shaping and injection molding. In addition to ensuring that the pets can eat, digest and absorb the food, the food can help the pets soothe and relax when the pets chew or lick the food, thereby helping the pets to enter deep sleep faster and reduce restlessness and anxiety at night.
[0023] Additional aspects and advantages of the present invention will be given in part in the description which follows, and in part will be obvious from the description which follows, or may be learned through practice of the present invention. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The present application provides a pet toy with a sleep-aiding function, wherein the raw material components are composed of natural rubber, calcium powder, edible oil, auxiliary agent and sleep-aiding mixture, wherein the natural rubber has good elasticity and flexibility, so that the toy can withstand the biting, pulling and throwing of the pet, and is not easy to be damaged. For example, a frisbee toy made of rubber can keep its shape unchanged and continue to be used even if it is thrown to the ground by the pet. The durability of rubber makes it an ideal choice for making pet chewing toys. When pets chew rubber toys, they can help them clean their teeth and relieve gum discomfort. Chewing toys in the shape of bones made of rubber can satisfy the nature of pets to chew. And calcium powder allows pets to ingest a small amount of calcium powder when playing and chewing toys, thereby supplementing a certain amount of calcium. This is an additional supplement for pets who may not have enough calcium in their diet. For example, some pets may lack calcium due to an unbalanced diet or specific health problems, and toys containing calcium powder can play a certain supplementary role. At the same time, the combination of calcium powder and natural rubber can increase the hardness of the toy, making it more suitable for pets to grind their teeth. In the process of grinding teeth, it can also help to remove dirt and food residues on teeth, play a certain tooth cleaning effect, and prevent oral diseases. Edible oil can make the material of making toys (such as the natural rubber material used in this application) softer and more flexible, so that pets feel more comfortable when playing, and can also increase the durability of toys, reducing the rupture or damage caused by too hard materials. At the same time, in the production process, it helps to separate the mold from the product, making production smoother and improving production efficiency. The auxiliary agent is specifically used to improve the strength, wear resistance and tear resistance of rubber. This makes pet toys more durable and can withstand the behaviors of biting, scratching and pulling of pets. At the same time, in the natural rubber processing process, it helps the vulcanization reaction to make natural rubber reach the required performance and hardness faster. This helps to improve production efficiency and ensure the stable quality of toys. Preferably, in this application, the auxiliary agent is zinc oxide, and the role of the sleep-aiding mixture is that when the pet bites or licks, it can help the pet soothe and relax the mood, thereby helping the pet to enter deep sleep faster and reduce restlessness and anxiety at night.
[0026] In some embodiments, the sleep-aiding mixture is composed of chamomile, valerian root, lavender and melatonin, wherein chamomile has a certain sedative and soothing effect, which can help pets relax during play and reduce anxiety and tension. In particular, for pets that are easily disturbed or stressed, such as pets in the adaptation period in a new environment, it may bring emotional comfort. At the same time, the smell of chamomile may help pets to enter a quiet and relaxed state more easily, which has a certain potential help in improving the sleep quality of pets; the role of valerian root is that first, the smell of valerian root has a unique attraction, which may prompt pets to pay more attention to and contact toys, and secondly, valerian root also has a certain sedative and soothing effect, which may help reduce the anxiety of pets and make them more relaxed during play. The aroma of lavender has a certain sedative and soothing effect. For some pets that are prone to tension, anxiety or excitement, such as cats and dogs, contact with toys with lavender scent may help them relax and reduce restless emotions. At the same time, the scent of lavender can create a peaceful atmosphere, which may help pets to fall asleep more easily during rest time and improve sleep quality. For example, when some pet dogs have trouble falling asleep at night, they may fall asleep more easily by holding toys with lavender. Melatonin helps adjust the sleep rhythm of pets. For pets with sleep problems, such as insomnia and irregular sleep, contact with toys containing melatonin may help them fall asleep more easily and improve the depth and quality of sleep.
[0027] Further on the basis of the above embodiments, the present application provides a method for preparing a pet toy with a sleep-aiding function:
[0028] Embodiment 1:
[0029] S1: Prepare the following raw materials, which are 66 parts by weight of natural rubber, 16 parts of calcium powder, 2 parts of edible oil, 7 parts of zinc oxide, and 0.5 parts each of chamomile, valerian root, lavender and melatonin.
[0030] S2: Put the prepared raw materials into the internal mixer and stir for 35 minutes. The internal mixer is a closed and powerful stirring device that can fully mix and plasticize the materials under high temperature and high pressure. During the internal mixing process, the rotor of the internal mixer rotates at a high speed, which produces strong shearing, extrusion and friction effects on the materials, so that the materials are evenly mixed together and gradually form a rubber compound with a certain plasticity. In some embodiments, during the first 10 minutes of stirring, the operating temperature of the internal mixer is between 120-180 degrees, which can ensure that the prepared raw materials are melted to form a gel. Since long-term stirring under high temperature may weaken or even lose the effects of chamomile, valerian root and lavender, the operating temperature of the internal mixer is reduced to 80-110 degrees between the 10th and 20th minutes of stirring. This can keep the raw materials in a gel state and reduce the loss of the effects of chamomile, valerian root and lavender. Finally, when the entire stirring process has been going on for more than 20 minutes, the operating temperature of the internal mixer is maintained at 60 degrees. This can keep the raw materials in a gel state while maintaining the effects of chamomile, valerian root and lavender unchanged.
[0031] S3: putting the above-mentioned colloid material into a double-roller press for repeated compacting and drying, so that the natural rubber, calcium powder, edible oil, auxiliary agent and sleep-aiding mixture in the colloid material are compacted and compacted more densely, and during the compacting process, the colloid material is allowed to cool naturally. After 25 minutes, the transitional material is cooled and hardened, and then cut into sheets;
[0032] S4: The sheet-like rubber material is placed in a granulator and formed into granules. Since water vapor will penetrate into the transitional material during the granulation process, the granular rubber material is placed in a stirring air dryer after granulation is completed. It is blown dry with warm air at 50 degrees while being continuously stirred. 50 degrees can effectively maintain the solid stability of the transitional material and perform secondary drying on the rubber material to remove moisture from its interior.
[0033] S5: Put the above granular rubber material into an injection molding machine for injection molding and vulcanization molding.
[0034] Embodiment 2:
[0035] S1: Prepare the following raw materials, which are 62 parts by weight of natural rubber, 20 parts by weight of calcium powder, 6 parts by weight of edible oil, 3 parts by weight of zinc oxide, and 1.5 parts by weight of chamomile, valerian root, lavender, and melatonin.
[0036] S2: Put the prepared raw materials into the internal mixer and stir for 25 minutes. The internal mixer is a closed and powerful stirring device that can fully mix and plasticize the materials under high temperature and high pressure. During the internal mixing process, the rotor of the internal mixer rotates at high speed, which produces strong shearing, extrusion and friction effects on the materials, so that the materials are evenly mixed together and gradually form a rubber compound with a certain plasticity. In some embodiments, during the first 10 minutes of stirring, the operating temperature of the internal mixer is between 120-180 degrees, which can ensure that the prepared raw materials are melted to form a gel. Since long-term stirring under high temperature may weaken or even lose the effects of chamomile, valerian root and lavender, the operating temperature of the internal mixer is reduced to 80-110 degrees between the 10th and 20th minutes of stirring. This can keep the raw materials in a gel state and reduce the loss of the effects of chamomile, valerian root and lavender. Finally, when the entire stirring process has been going on for more than 20 minutes, the operating temperature of the internal mixer is maintained at 60 degrees. This can keep the raw materials in a gel state while maintaining the effects of chamomile, valerian root and lavender unchanged.
[0037] S3: putting the above-mentioned colloid material into a double-roller press for repeated compacting and drying, so that the natural rubber, calcium powder, edible oil, auxiliary agent and sleep-aiding mixture in the colloid material are compacted and compacted more densely, and during the compacting process, the colloid material is allowed to cool naturally. After 25 minutes, the transitional material is cooled and hardened, and then cut into sheets;
[0038] S4: The sheet-like rubber material is placed in a granulator and formed into granules. Since water vapor will penetrate into the transitional material during the granulation process, the granular rubber material is placed in a stirring air dryer after granulation is completed. It is blown dry with warm air at 50 degrees while being continuously stirred. 50 degrees can effectively maintain the solid stability of the transitional material and perform secondary drying on the rubber material to remove moisture from its interior.
[0039] S5: Put the above granular rubber material into an injection molding machine for injection molding and vulcanization molding.
[0040] In addition, in some embodiments, the present application provides a second method for preparing a pet toy with a sleep-aiding function:
[0041] Embodiment 3:
[0042] S1: Prepare the following raw materials, which are 66 parts by weight of natural rubber, 16 parts of calcium powder, 2 parts of edible oil, 7 parts of zinc oxide, and 0.5 parts each of chamomile, valerian root, lavender and melatonin.
[0043] S2: Put the prepared raw materials into the internal mixer and stir for 35 minutes. The internal mixer is a closed and powerful stirring device that can fully mix and plasticize the materials under high temperature and high pressure. During the internal mixing process, the rotor of the internal mixer rotates at a high speed, which produces strong shearing, extrusion and friction effects on the materials, so that the materials are evenly mixed together and gradually form a rubber compound with a certain plasticity. In some embodiments, during the first 10 minutes of stirring, the operating temperature of the internal mixer is between 120-180 degrees, which can ensure that the prepared raw materials are melted to form a gel. Since long-term stirring under high temperature may weaken or even lose the effects of chamomile, valerian root and lavender, the operating temperature of the internal mixer is reduced to 80-110 degrees between the 10th and 20th minutes of stirring. This can keep the raw materials in a gel state and reduce the loss of the effects of chamomile, valerian root and lavender. Finally, when the entire stirring process has been going on for more than 20 minutes, the operating temperature of the internal mixer is maintained at 60 degrees. This can keep the raw materials in a gel state while maintaining the effects of chamomile, valerian root and lavender unchanged.
[0044] S3: putting the rubber material into a double-roller press for repeated compacting and drying, so that the natural rubber, calcium powder, edible oil, auxiliary agent and sleep-aiding mixture of the rubber material are compacted more densely, and during the compacting process, the rubber material is allowed to cool naturally. After 10-20 minutes, the transitional material cools and hardens;
[0045] S4: Place the sheet or strip rubber material into the corresponding mold, and then use a hot press to stamp it into shape.
[0046] Embodiment 4:
[0047] S1: Prepare the following raw materials, which are 62 parts by weight of natural rubber, 20 parts by weight of calcium powder, 6 parts by weight of edible oil, 3 parts by weight of zinc oxide, and 1.5 parts by weight of chamomile, valerian root, lavender, and melatonin.
[0048] S2: Put the prepared raw materials into the internal mixer and stir for 25 minutes. The internal mixer is a closed and powerful stirring device that can fully mix and plasticize the materials under high temperature and high pressure. During the internal mixing process, the rotor of the internal mixer rotates at high speed, which produces strong shearing, extrusion and friction effects on the materials, so that the materials are evenly mixed together and gradually form a rubber compound with a certain plasticity. In some embodiments, during the first 10 minutes of stirring, the operating temperature of the internal mixer is between 120-180 degrees, which can ensure that the prepared raw materials are melted to form a gel. Since long-term stirring under high temperature may weaken or even lose the effects of chamomile, valerian root and lavender, the operating temperature of the internal mixer is reduced to 80-110 degrees between the 10th and 20th minutes of stirring. This can keep the raw materials in a gel state and reduce the loss of the effects of chamomile, valerian root and lavender. Finally, when the entire stirring process has been going on for more than 20 minutes, the operating temperature of the internal mixer is maintained at 60 degrees. This can keep the raw materials in a gel state while maintaining the effects of chamomile, valerian root and lavender unchanged.
[0049] S3: putting the rubber material into a double-roller press for repeated compacting and drying, so that the natural rubber, calcium powder, edible oil, auxiliary agent and sleep-aiding mixture of the rubber material are compacted more densely, and during the compacting process, the rubber material is allowed to cool naturally. After 10-20 minutes, the transitional material cools and hardens;
[0050] S4: Place the sheet or strip rubber material into the corresponding mold, and then use a hot press to stamp it into shape.
[0051] The present application utilizes natural rubber, calcium powder, edible oil, auxiliary agents and sleep-aiding mixtures which are mixed in a certain weight ratio, and then subjected to heating, stirring, pressing, drying, shaping and injection molding. In addition to ensuring that the pets can eat and digest the rubber, the pets can be soothed and relaxed when they chew or lick the rubber, thereby helping the pets to enter a deep sleep faster and reduce restlessness and anxiety at night.
[0052] The details of the exemplary embodiments described above are not limited to the embodiments described above, and the invention may be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be regarded as exemplary and non-restrictive in all respects, and the scope of the invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the invention.
Claims
1. A pet toy with a sleep-aiding function, characterized in that: Calculated by weight, the raw material components are composed of: 62-66 parts of natural rubber, 16-20 parts of calcium powder, 2-6 parts of edible oil, 3-7 parts of auxiliary agents and 4-6 parts of sleep-aiding mixture.
2. The pet toy with sleep-aiding function according to claim 1, characterized in that: The auxiliary agent is zinc oxide.
3. The pet toy with sleep-aiding function according to claim 1, characterized in that: The sleep-aiding mixture consists of chamomile, valerian root, lavender and melatonin.
4. The pet toy with sleep-aiding function according to claim 3, characterized in that: The raw material components are composed of 0.5-1.5 parts of chamomile, valerian root, lavender and melatonin.
5. The pet toy with sleep-aiding function according to claim 1, characterized in that: The raw material components also include mint, and the components are composed of 4-6 parts of mint.
6. The method for preparing a pet toy with a sleep-aiding function according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1: accurately weigh and mix the selected raw materials in a certain proportion; S2: Put the prepared raw materials into the internal mixer. The rotor of the internal mixer rotates at a high speed, which produces shear, extrusion and friction on the raw materials, so that the raw materials are evenly mixed and stirred together, and gradually form a rubber compound with a certain plasticity; S3: placing the rubber material into a double-roller press for repeated compaction and drying, and after the rubber material is cooled, cutting it into sheets; S4: The sheet rubber is placed in a granulator to form granules, and then the granular rubber is placed in a stirring air dryer, and is blown dry with warm air at 50 degrees while being continuously stirred; S5: Put the above granular rubber material into an injection molding machine for injection molding and vulcanization molding.
7. The method for preparing a pet toy with a sleep-aiding function according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1: accurately weigh and mix the selected raw materials in a certain proportion; S2: Put the prepared raw materials into the internal mixer. The rotor of the internal mixer rotates at a high speed, which produces shear, extrusion and friction on the raw materials, so that the raw materials are evenly mixed and stirred together, and gradually form a rubber compound with a certain plasticity; S3: putting the rubber material into a double-roller press for repeated compaction and drying, cooling it rapidly in a water tank, and then cutting it into sheets or strips of corresponding sizes; S4: Put the sheet or strip rubber material into a corresponding mold, and then use a hot press to stamp it.
8. The method for preparing a pet toy with a sleep-aiding function according to claim 6, characterized in that: The mixing time of the internal mixer is 25-35 minutes, and in the first 10 minutes of mixing, the working temperature of the internal mixer is between 120-180 degrees, between the 10th minute and the 20th minute of mixing, the working temperature of the internal mixer is 80-110 degrees, and after the 20th minute of mixing, the working temperature of the internal mixer is 60 degrees.
9. The method for preparing a pet toy with a sleep-aiding function according to claim 7, characterized in that: The mixing time of the internal mixer is 25-35 minutes, and in the first 10 minutes of mixing, the working temperature of the internal mixer is between 120-180 degrees, between the 10th minute and the 20th minute of mixing, the working temperature of the internal mixer is 80-110 degrees, and after the 20th minute of mixing, the working temperature of the internal mixer is 60 degrees.