Container and method for producing a container

By adopting die-casting liquid forging composite process and multi-layer structural design in the cooking vessel, the problem of insufficient thermal conductivity and thermal storage performance of traditional cooking vessels is solved, efficient heat transfer and insulation effects are achieved, and production costs are reduced.

CN118924100APending Publication Date: 2024-11-12FOSHAN SHUNDE MIDEA ELECTRICAL HEATING APPLIANCES MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310518238.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

There are shortcomings in existing cooking utensils in terms of thermal conductivity and heat storage, and traditional production processes are difficult to achieve differentiation of thermal conductivity and heat storage in multiple regions, resulting in low heat transfer efficiency, poor thermal insulation effect, and high cost.

Method used

By adopting die-casting liquid forging composite process, by adding fillers with different thermal conductivity during the forming process of the container matrix, combining die-casting and liquid die-forging processes, the filling speed and local extrusion are dynamically adjusted to form a multi-layer structure to adjust thermal conductivity and heat storage. performance.

Benefits of technology

The optimal coupling effect of the container's thermal conductivity and thermal storage performance in different locations is achieved, the heat transfer efficiency and thermal insulation ability are improved, the cost is reduced, and the product's compactness and user experience are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118924100A_ABST
    Figure CN118924100A_ABST
Patent Text Reader

Abstract

The invention provides a container and a preparation method of the container, and the container comprises a container base body which is a metal piece; the filling piece is located in the wall of the container base body, the filling piece and the container base body are integrally formed, and the heat conductivity coefficient of the filling piece is different from that of the container base body; the heat conduction coefficient and the heat transfer speed of each position of a cooking utensil and other containers can be dynamically adjusted in a mode of combining two materials with different heat conduction coefficients, and the optimal heat conduction and heat storage coupling effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of container preparation, in particular to a container and a method for preparing the container. Background Art

[0002] Cooking utensils need to have good thermal performance, and the thermal conductivity and heat storage capacity of the material will directly affect the cooking effect of the ingredients. Materials with fast thermal conductivity can achieve faster heat transfer, reduce heat loss, and improve heat transfer efficiency. However, high thermal conductivity can easily cause the local temperature at the bottom of the vessel to rise too quickly, exceeding the set temperature, and there is a risk of burning the ingredients, which in turn affects the user experience. In addition, fast heat transfer of materials is not conducive to heat preservation. Therefore, cooking utensils also need to have good heat storage and heat storage capabilities.

[0003] However, the vessels produced by traditional sheet metal stamping methods have uniform wall thickness due to process limitations, and it is impossible to achieve differentiated heat conduction and heat storage in different areas by changing the thickness. The vessels produced by the die-casting process can be designed and the thickness of local areas can be changed, but the die-casting process cannot produce thick-walled parts, and the ability to adjust the heat storage effect is limited. Moreover, the thermal conductivity of the material is a physical property of the material itself, and it cannot be changed. Therefore, there is not much room for operation to adjust heat conduction and heat storage only by changing the thickness, and in order to pursue the heat storage effect, the wall thickness will be increased, which will also push up the material cost.

[0004] Therefore, how to design a cooking vessel and a cooking method that can enable multiple parts to have different heat transfer speeds and achieve the best heat conduction and heat storage effects has become a problem that needs to be solved urgently. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art or related art.

[0006] To this end, a first object of the present invention is to provide a container.

[0007] The second object of the present invention is to provide a method for preparing a container.

[0008] The technical solution of the first aspect of the present invention provides a container, comprising: a container base, the container base is a metal part; a filler, located in the wall of the container base, and the filler and the container base are integrally formed, and the thermal conductivity of the filler is different from the thermal conductivity of the container base. Further, the strength of the filler is greater than the strength of the container base.

[0009] The container provided by the technical solution of the present invention includes a container base and a filler, and the two parts are integrally formed. For example, when the container base is formed, a filler can be added to the mold, so that the filler and the container base can be integrally formed. And this kind of container includes not only the container base but also the filler, so that the molded container includes a two-layer structure, a filling layer formed by the filler, and a casting layer as the container base. Since the container base and the filler are different parts and their thermal conductivities are different, the container has at least two parts with different thermal conductivities. At the same time, in the actual process, the thickness of the filler at different positions can be reasonably set according to the needs of each position of the container, so as to dynamically adjust the thickness of the container base at different positions, so that the thermal conductivity and heat transfer rate of each position of the container such as the cooking vessel can be dynamically adjusted by combining two materials with different thermal conductivities, so as to achieve the best thermal conduction and heat storage coupling effect.

[0010] In addition, the container in the above technical solution provided by the present invention may also have the following additional technical features:

[0011] Furthermore, the filling piece and the container base are integrally formed by a die-casting and liquid forging composite process.

[0012] In this technical solution, in the process of preparing the container base, the first half of the step adopts the die casting process, and the latter is combined with the liquid die forging process (specifically, the local extrusion of the semi-solid part), thereby combining the two processes of die casting and liquid die forging together, that is, providing a new process, namely, the die casting and liquid forging composite process. This process, through targeted transformation of the die casting technology, injects the function of liquid die forging, and reduces air entrainment by dynamically adjusting the filling speed (filling time) during the die casting process, and uses the extrusion rod in the mold to locally extrude and compensate for the shrinkage of the semi-solid casting when the metal solidifies and shrinks, thereby greatly reducing the holes in the product, and after the container base is subsequently provided with a non-stick coating, the risk of bubbling or local shedding of the coating is significantly reduced, thereby not only improving the product qualification rate, but also enhancing the user experience. In this method, after the molten metal solidifies into a semi-solid part, the semi-solid part is locally extruded until the end. This method is similar to the liquid die forging process, which greatly solves the problems of many pores, non-density and high scrap rate of parts formed by the die-casting process. In this way, the advantages of low die-casting cost and high casting quality of liquid die forging are utilized, and the die-casting-liquid die forging composite process is creatively used to manufacture cooking containers, thereby improving the yield rate of the original die-casting aluminum alloy and improving the cost performance, thereby ensuring the yield rate and quality of the prepared container matrix and reducing its preparation cost.

[0013] Among them, the so-called die casting process is a metal casting process, which is a casting method that uses high pressure to force the molten metal into a complex-shaped metal mold. It has the characteristics of high-speed filling and rapid cooling, but it has many pores, is not dense, and has a high scrap rate.

[0014] The so-called liquid die forging is a metal forming process that has both casting characteristics and is similar to die forging. It is to pour a certain amount of molten metal directly into the mold cavity and solidify it under continuous mechanical static pressure. This process uses the easy flow of metal casting and forging technology during solidification to cause plastic deformation of the solidified hard shell, so that the metal crystallizes and solidifies under pressure and forcibly eliminates shrinkage holes formed by solidification shrinkage, so as to obtain liquid die forging parts without casting defects. Liquid die forging technology can eliminate shrinkage holes formed by solidification shrinkage and obtain high-strength parts with fine and uniform grains and dense structure, but the cost is relatively high.

[0015] Of course, in other technical solutions, the container base and the filling piece may also be integrally manufactured by other processes, for example, by separate liquid forging processes.

[0016] In the above technical solution, the container matrix includes multiple thicknesses, and the thickness of the container matrix at multiple positions meets the preset thickness requirements. Specifically, the container matrix is ​​wrapped outside the filling piece, and the bottom thickness of the container matrix is ​​less than the side wall thickness of the container matrix. This makes the bottom of the container matrix relatively thin, so the thermal conductivity effect is better. The thick side wall can achieve better thermal insulation and heat storage effects. Specifically, when preparing the container, the thickness of the container matrix at various positions can be reasonably controlled by controlling the length of the filling piece and the height of the protrusion at the bottom thereof, so that its thickness meets the requirements of thermal conductivity and heat storage.

[0017] Furthermore, the thermal conductivity of the filler is greater than that of the container base. Because the container base is generally made of aluminum-silicon alloy or aluminum-copper alloy, its high fluidity prevents its thermal conductivity from being too high. Therefore, the filler can be designed as a part with a higher thermal conductivity to ensure the fluidity of the melt used to prepare the container base.

[0018] Furthermore, the thermal conductivity of the container base is greater than or equal to 90 W / m·k and less than or equal to 110 W / m·k. The thermal conductivity of the filler is greater than or equal to 200 W / m·k and less than or equal to 235 W / m·k. By reasonably setting the thermal conductivity of the two, the cooperation of the two parts can ensure both the heat conduction capacity and the heat storage capacity.

[0019] Specifically, the filler is high thermal conductivity aluminum with a thermal conductivity coefficient higher than 200 W / m·k, and the container base is low thermal conductivity aluminum silicon alloy with a thermal conductivity coefficient lower than 110 W / m·k.

[0020] Furthermore, there is no rigid requirement for the strength of the filling piece and the strength of the container base. The strengths of the two may be equal or unequal. Generally, the strength of the filling piece is greater than the strength of the container base.

[0021] In the above technical solution, a first concave-convex structure is arranged on one side of the filling piece close to the bottom of the container base, a second concave-convex structure matching the first concave-convex structure is arranged on the container base, and the convex portion of the first concave-convex structure is flush with the bottom wall surface of the container base.

[0022] In this technical solution, the bottom of the filler and the contact part of the container base are matched by a concave-convex structure. Specifically, a plurality of spaced abutting parts can be provided on the side of the filler close to the bottom of the cavity, and the plurality of abutting parts abut against the bottom of the cavity, so that a gap is provided between the non-abutting part of the filler and the bottom of the cavity, so that after the filler and the container base are integrally formed, the bottom of the filler and the contact part of the container base can form a concave-convex structure. The first concave-convex structure is provided to form a gap between the filler and the bottom of the cavity, so that the thickness of the bottom of the container base can be controlled by the size of the gap, that is, the thickness of the convex part of the second concave-convex structure of the container base can be controlled.

[0023] Furthermore, the length of the filling piece can be reasonably set to control the gap between the filling piece and the side wall of the cavity, thereby controlling the thickness of the side of the container base.

[0024] In the above technical solution, the diameter of the hole in the container matrix is ​​less than or equal to 1.5 mm, and the porosity of the preset hole in the container matrix is ​​greater than 0 and less than or equal to 0.5%. This porosity makes the structure inside the container matrix denser and meets relevant requirements, thus ensuring the performance of the container matrix.

[0025] Specifically, when calculating holes, holes with a diameter less than 0.25mm are not counted. After the container matrix is ​​formed, the number of holes in the unit area of ​​10cm×10cm is no more than 4, and the distance between two holes is not less than 5cm. The diameter of the preset hole is greater than 0.25mm and less than or equal to 1.5mm, and the distance between each preset hole and the outer surface of the container matrix is ​​greater than or equal to 2 times the diameter of each preset hole. This kind of container matrix makes the bubbles less and the interior of the part is denser, ensuring the qualified rate of the product.

[0026] In the above technical solution, the cross-sectional thickness of the filling member, that is, the thickness excluding the convex portion in the first concavo-convex structure, that is, the thickness of the main body of the filling member away from the bottom of the cavity is greater than or equal to 1.5 mm and less than or equal to 5 mm. This dimension should not be too small, otherwise the thermal conductivity of the container cannot be well adjusted.

[0027] In the above technical solution, the thickness of the container base is greater than or equal to 1 mm and less than or equal to 5 mm. The thickness of the container base should not be too large, otherwise it will be difficult to process and will lead to worse thermal conductivity. At the same time, the thickness should not be too thin, otherwise it will lead to serious lack of heat storage capacity. Setting the thickness at 1mm-5mm can make it moderate, so as to take into account the convenience of processing and monitor the heat storage capacity and thermal conductivity.

[0028] In the above technical solution, the container substrate includes an aluminum-silicon alloy substrate and / or an aluminum-copper alloy substrate.

[0029] Furthermore, the container further includes: a non-stick coating, which is located on the inner wall of the container base. The non-stick property of the container is ensured by providing the non-stick coating. Specifically, the non-stick coating can be any one of PTFE (Polytetrafluoroethylene, Teflon) coating, PFA (Polyfluoroalkoxy, soluble polytetrafluoroethylene) coating, PEEK (Polyetheretherketone, polyetheretherketone) coating, and ceramic coating.

[0030] Furthermore, the filler includes a metal filler, because the metal filler has a better thermal conductivity, thereby ensuring the thermal conductivity of the product. The metal filler has a higher strength and is not easily damaged. Of course, the filler can also be made of other materials that can meet the strength and thermal conductivity, such as alloy parts.

[0031] The technical solution of the second aspect of the present invention provides a method for preparing a container, which is used to prepare the container provided by any technical solution of the first aspect. The preparation method comprises: placing a filler in the mold cavity of the mold, the thermal conductivity of the filler is different from the thermal conductivity of the container matrix; filling the molten metal into the mold cavity at a preset filling speed; when the molten metal in the mold cavity is formed into a semi-solid part (i.e., a part in a preset state), a preset part of the semi-solid part is extruded until the molten metal in the cavity is formed into the container matrix. The preset state can be reasonably set according to the actual situation, generally a semi-solid part.

[0032] The preparation method of the container provided by the present invention is specifically used to prepare containers, especially cooking containers. Specifically, the container includes a container base, and the container base has a cavity for accommodating articles, which constitutes the main structure of the container and can meet the basic needs of holding articles. Of course, in addition to the container base, the container can also include a coating arranged on the inner and outer surfaces of the container base, such as a non-stick coating arranged in the container base, or a protective coating arranged outside the container base. When the container base is formed, the container base is integrally prepared by a die-casting liquid forging composite process. Specifically, the preparation steps are: first, the molten metal is filled into the mold cavity of the mold. In this step, the filling speed needs to be fully controlled to ensure that the molten metal can be filled into the mold cavity by high pressure. Specifically, the molten metal is filled into the mold cavity of the mold in the way that the molten metal in the die-casting process is filled into the mold cavity, so that the molten metal can be quickly filled into the mold cavity, and the molten metal can be quickly solidified in the mold cavity. After the molten metal is filled, the molten metal will gradually solidify in the mold cavity. When the molten metal solidifies into a semi-solid part (for example, after the filling is completed for a preset time), the preset part of the semi-solid part is squeezed until the semi-solid part is formed into a container matrix. In this way, after the molten metal solidifies into a semi-solid part, the semi-solid part is locally squeezed until the end, and this method is similar to the liquid die forging process, which greatly solves the problem that the parts formed by the die casting process have many pores, are not dense, and have a high scrap rate. That is, in the process of preparing the container matrix, the first half of the step of this application adopts the die casting process, and the liquid die forging process is combined in the latter step (specifically reflected in the local extrusion of the semi-solid part), thereby combining the two processes of die casting and liquid die forging together, that is, providing a new process, that is, the die casting and liquid forging composite process. This process, through targeted transformation of die casting technology, injects the function of liquid die forging, reduces air entrainment by dynamically adjusting the filling speed (filling time) during the die casting process, and uses the extrusion rod in the die to locally extrude and compensate for the shrinkage of the semi-solid casting when the metal solidifies and shrinks, thereby greatly reducing product holes and significantly reducing the risk of blistering or local shedding of the coating, which not only improves the product qualification rate, but also enhances the user experience. In this way, the respective advantages of low die casting cost and high liquid die forging casting quality are utilized, and the die casting-liquid die forging composite process is creatively used to manufacture cooking containers, thereby improving the yield rate of the original die casting aluminum alloy and improving the cost performance, thereby ensuring the yield rate and quality of the prepared container matrix and reducing its preparation cost.

[0033] When the preset part of the semi-solid part is extruded, the semi-solid part is generally extruded on the side close to the cavity, that is, local extrusion is performed from the bottom of the container base. Specifically, the semi-solid state is a semi-molten state, and the semi-molten state is the state of the material when the temperature is between the solidus and liquidus of the material.

[0034] In the above technical solution, before the step of filling the molten metal into the mold cavity at a preset filling speed, a filler is placed in the mold cavity, and the thermal conductivity of the filler is different from that of the container base.

[0035] At the same time, in this preparation method, when the container base is formed, a filler is added to the mold, so that the filler and the container base can be formed in one piece. The container formed in this way includes not only the container base but also the filler, so that the formed container includes a two-layer structure, a filling layer formed by the filler, and a liquid forging layer as the container base. Since the liquid forging layer and the filling layer are different parts, their thermal conductivity and strength are different, so that the container has at least two positions with different thermal conductivity. In the actual process, the thickness of the filler at different positions can be reasonably set according to the needs of each position of the container, so as to dynamically adjust the thickness of the container base at different positions, so that the thermal conductivity and heat transfer rate of each position of the cooking vessel and other containers are dynamically adjusted by combining two materials with different thermal conductivities, so as to achieve the best thermal conduction and heat storage coupling effect.

[0036] In addition, the method for preparing the container in the above technical solution provided by the present invention may also have the following additional technical features:

[0037] In the step of filling the molten metal into the mold cavity at a preset filling speed, the filling speed of the molten metal is greater than 0 and less than or equal to 0.8 m / s. By controlling the filling speed, the filling time can be controlled to be greater than or equal to 0.02 s and less than or equal to 0.05 s. Avoid the molten metal being filled too quickly, resulting in the part being formed too quickly and causing a large number of bubbles to be unable to be discharged in time.

[0038] When the molten metal is filled into the mold cavity, it is necessary to dynamically adjust the filling speed according to the actual situation to control the filling time, so as to fully control the filling process of the molten metal and avoid the filling speed being too fast or too slow, which may cause the parts to fail to solidify as required. In this way, the quality of the parts after molding can be ensured, and the bubbles in the parts can be reduced, making the inside of the parts denser.

[0039] Furthermore, the thermal conductivity of the filler is greater than that of the container base. Because the container base is generally made of aluminum silicon alloy or aluminum copper alloy, its high fluidity makes its thermal conductivity not too high, so the filler can be designed as a part with higher thermal conductivity to ensure the fluidity of the melt for preparing the container base.

[0040] Furthermore, there is no rigid requirement for the strength of the filling piece and the strength of the container base. The strengths of the two may be equal or unequal. Generally, the strength of the filling piece is greater than the strength of the container base.

[0041] In the above technical solution, a plurality of spaced abutting portions are provided on one side of the filler close to the bottom of the cavity, the plurality of abutting portions abut against the bottom of the cavity, and a gap is provided between the non-abutting portion of the filler and the bottom of the cavity. The abutting portions are provided to form a gap between the filler and the bottom of the cavity, so that the thickness of the bottom of the container base can be controlled by the size of the gap. At the same time, the length of the filler can be reasonably set to control the gap between the filler and the side wall of the cavity, thereby controlling the thickness of the side of the container base.

[0042] In the above technical solution, the thermal conductivity of the container base is greater than or equal to 90W / m·k and less than or equal to 110W / m·k, and the thermal conductivity of the filler is greater than or equal to 200W / m·k and less than or equal to 235W / m·k. By reasonably setting the thermal conductivity of the two, the cooperation of the two parts can ensure both the heat conduction capacity and the heat storage capacity.

[0043] In the above technical solution, the cross-sectional thickness of the filling piece, that is, the thickness excluding the abutting portion, that is, the thickness of the filling piece away from the bottom of the cavity is greater than or equal to 1.5 mm and less than or equal to 5 mm. This size should not be too small, otherwise the thermal conductivity of the container cannot be well adjusted.

[0044] In the above technical solution, the molten metal includes an aluminum-silicon alloy melt and / or an aluminum-copper alloy melt.

[0045] In the above technical solution, the thickness of the container base is greater than or equal to 1 mm and less than or equal to 5 mm. The thickness of the container base should not be too large, otherwise it will be difficult to process and will lead to worse thermal conductivity. At the same time, the thickness should not be too thin, otherwise it will lead to serious lack of heat storage capacity. Setting the thickness at 1mm-5mm can make it moderate, so as to take into account the convenience of processing and monitor the heat storage capacity and thermal conductivity.

[0046] In the above technical solution, the container base includes multiple thicknesses, and the thickness of the container base at multiple locations meets the preset thickness requirements. Specifically, the container base is wrapped outside the filling member, and the bottom thickness of the container base is less than the side wall thickness of the container base. In this way, the bottom of the container base is relatively thin, so the heat conduction effect is better. The thick side wall can achieve better heat preservation and heat storage effects.

[0047] In the above technical solution, the diameter of the holes in the container matrix is ​​less than or equal to 1.5 mm, and the porosity of the preset holes in the container matrix is ​​greater than 0 and less than or equal to 0.5. Specifically, when calculating the holes, holes with a diameter less than 0.25 mm are not counted. After the container matrix is ​​formed, the number of holes in the unit area of ​​10 cm × 10 cm is no more than 4, and the distance between two holes is not less than 5 cm. The diameter of the preset holes is greater than 0.25 mm and less than or equal to 1.5 mm, and the distance between each preset hole and the outer surface of the container matrix is ​​greater than or equal to twice the diameter of each preset hole itself. This type of container matrix makes the bubbles relatively small, the interior of the parts is denser, and ensures the qualified rate of the product.

[0048] In the above technical solution, the preparation method of the container also includes demolding pretreatment. The demolding pretreatment specifically includes opening the mold, taking out the container matrix and cooling it after the molten metal in the cavity is formed into the container matrix, and processing the cooled container matrix to a preset size and / or preset accuracy. When the container matrix is ​​processed by the die-casting liquid forging composite process, some processing allowances are generally reserved for the container matrix. Therefore, after the container matrix is ​​prepared and formed, the container matrix can be processed into the size and accuracy (such as roughness, flatness and coaxiality, etc.) required by the drawing by machining or other methods.

[0049] Furthermore, the preparation method of the container also includes roughness treatment. The roughness treatment specifically includes: roughening the inner and outer surfaces of the container substrate until the roughness Ra of the inner and outer surfaces of the container substrate is greater than or equal to 2μm and less than or equal to 5μm. Furthermore, the roughness treatment includes sandblasting and / or grinding. Furthermore, this step is generally performed after the demolding pretreatment. If there is no demolding pretreatment step, the roughness treatment can be performed directly after the part is demolded. By performing roughness treatment on the container substrate, the surface quality of the container substrate can be guaranteed, and preparations can be made for subsequent coating spraying on the container substrate.

[0050] Furthermore, the preparation method of the container further comprises forming a non-stick coating. The step of forming the non-stick coating specifically comprises: forming a non-stick coating on the inner wall surface of the container substrate. The non-stick property of the inner wall surface of the container can be improved by providing the non-stick coating. The non-stick coating specifically comprises one or more of a PTFE coating, a PFA coating, a PEEK coating, and a ceramic coating.

[0051] Furthermore, the preparation method of the container also includes: before the step of forming the non-stick coating, the container substrate is degreased. Among them, after the prepared container substrate is processed by machining and the like, there will be some grease on the surface, so before forming the non-stick coating, it needs to be degreased. The degreasing method can be high-temperature heating. At this time, the container can be heated. The specific heating temperature can be 350°C-420°C, and the heating duration can be 8min-15min. Of course, the degreasing treatment can also be carried out by other methods such as chemical degreasing.

[0052] Furthermore, the filler includes a metal filler, because the metal filler has a better thermal conductivity, thereby ensuring the thermal conductivity of the product. The metal filler has a higher strength and is not easily damaged. Of course, the filler can also be made of other materials that can meet the strength and thermal conductivity, such as alloy parts.

[0053] Additional aspects and advantages of the present invention will become apparent from the following description or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0055] Figure 1 A schematic structural diagram of a container according to an embodiment of the present invention is shown;

[0056] Figure 2 A schematic structural diagram of a container according to another embodiment of the present invention is shown;

[0057] Figure 3 A schematic flow chart of a method for preparing a container according to an embodiment of the present invention is shown;

[0058] Figure 4 A schematic flow chart of a method for preparing a container according to another embodiment of the present invention is shown;

[0059] Figure 5 The microscopic morphology at the interface between the liquid forging layer and the filling layer is shown.

[0060] in, Figure 1 , Figure 2 and Figure 5 The corresponding relationship between the reference numerals and the component names is as follows:

[0061] 1 container, 12 container base, 120 liquid forging layer, 122 second protrusion, 124 second groove, 14 filling piece, 140 filling layer, 142 first protrusion, 144 first groove, 16 non-stick coating, 18 anti-rust layer. DETAILED DESCRIPTION

[0062] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0063] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.

[0064] Refer to the following Figures 1 to 5 The present invention provides a container 1 and a method for preparing the container.

[0065] like Figure 1 and Figure 2 As shown, an embodiment of the first aspect of the present invention provides a container 1, comprising a container base 12 and a filler 14. The container base 12 is a metal part. The filler 14 is located in the wall of the container base 12, and the filler 14 and the container base 12 are integrally formed, and the thermal conductivity of the filler 14 is different from the thermal conductivity of the container base 12. Further, the strength of the filler 14 is greater than the strength of the container base 12.

[0066] The container 1 provided according to the embodiment of the present invention includes a container base 12 and a filler 14, and the two parts are integrally formed. For example, when the container base 12 is formed, the filler 14 can be added to the mold, so that the filler 14 and the container base 12 can be integrally formed. And this kind of container 1 not only includes the container base 12 but also includes the filler 14, so that the formed container 1 includes a two-layer structure, a filling layer 140 formed by the filler 14, and a liquid forging layer 120 as the container base 12. Since the container base 12 and the filler 14 are different parts and their thermal conductivities are different, the container 1 has at least two parts with different thermal conductivities. At the same time, in the actual process, the thickness of the filler 14 at different positions can be reasonably set according to the needs of each position of the container 1, so as to dynamically adjust the thickness of the container base 12 at different positions, so that the thermal conductivity and heat transfer rate of each position of the container 1 such as the cooking vessel can be dynamically adjusted by combining two materials with different thermal conductivities, so as to achieve the best heat conduction and heat storage coupling effect.

[0067] Furthermore, the filling member 14 and the container base 12 are integrally formed by a die-casting and liquid forging composite process.

[0068] In this embodiment, in the process of preparing the container base 12, the first half of the step adopts the die casting process, and the latter is combined with the liquid die forging process (specifically, the local extrusion of the semi-solid part), thereby combining the two processes of die casting and liquid die forging together, that is, providing a new process, that is, the die casting and liquid forging composite process. This process, by targeted transformation of the die casting technology, injects the function of liquid die forging, and reduces the air entrainment by dynamically adjusting the filling speed (filling time) during the die casting process, and uses the extrusion rod in the mold to locally extrude and compensate the shrinkage of the semi-solid casting when the metal solidifies and shrinks, thereby greatly reducing the holes in the product, and after the container base 12 is subsequently provided with a non-stick coating 16, the risk of bubbling or local shedding of the coating is significantly reduced, thereby not only improving the product qualification rate, but also enhancing the user experience. In this method, after the molten metal solidifies into a semi-solid part, the semi-solid part is locally extruded until the end. This method is similar to the liquid die forging process, which greatly solves the problems of many pores, non-density and high scrap rate of parts formed by the die-casting process. In this way, the advantages of low die-casting cost and high liquid die forging casting quality are utilized, and the cooking container 1 is manufactured by creatively utilizing the die-casting-liquid die forging composite process, thereby improving the yield rate of the original die-casting aluminum alloy and improving the cost performance, thereby ensuring the yield rate and quality of the prepared container base 12 and reducing its preparation cost.

[0069] Among them, the so-called die casting process is a metal casting process, which is a casting method that uses high pressure to force the molten metal into a complex-shaped metal mold. It has the characteristics of high-speed filling and rapid cooling, but it has many pores, is not dense, and has a high scrap rate.

[0070] The so-called liquid die forging is a metal forming process that has both casting characteristics and is similar to die forging. It is to pour a certain amount of molten metal directly into the mold cavity and solidify it under continuous mechanical static pressure. This process uses the easy flow of metal casting and forging technology during solidification to cause plastic deformation of the solidified hard shell, so that the metal crystallizes and solidifies under pressure and forcibly eliminates shrinkage holes formed by solidification shrinkage, so as to obtain liquid die forging parts without casting defects. Liquid die forging technology can eliminate shrinkage holes formed by solidification shrinkage and obtain high-strength parts with fine and uniform grains and dense structure, but the cost is relatively high.

[0071] Furthermore, the filler 14 includes a metal filler, because the metal filler has a better thermal conductivity, which can ensure the thermal conductivity of the product. The metal filler 14 is stronger and not easily damaged. Of course, the filler 14 can also be made of other materials that can meet the strength and thermal conductivity, such as alloys.

[0072] In the above embodiment, if Figure 1As shown, the container base 12 includes multiple thicknesses, and the thickness of the container base 12 at multiple positions meets the preset thickness requirements. Specifically, the container base 12 is wrapped outside the filler 14, and the bottom thickness H1 of the container base 12 is less than the side wall thickness H2 of the container base 12. In this way, the bottom of the container 1 is relatively thin, so the thermal conductivity is better. The thick side wall can achieve better thermal insulation and heat storage effects. Specifically, when preparing the container 1, the thickness of the container base 12 at various positions can be reasonably controlled by controlling the length of the filler 14 and the height of the bottom protrusion thereof, so that its thickness meets the required thermal conductivity and heat storage requirements.

[0073] Furthermore, the thermal conductivity of the filler 14 is greater than the thermal conductivity of the container base 12. Because the container base 12 is generally made of aluminum silicon alloy or aluminum copper alloy, its high fluidity makes its thermal conductivity not too high, so the filler 14 can be designed as a part with higher thermal conductivity to ensure the fluidity of the molten liquid for preparing the container base 12.

[0074] Furthermore, the thermal conductivity of the container base 12 is greater than or equal to 90 W / m·k and less than or equal to 110 W / m·k. The thermal conductivity of the filler 14 is greater than or equal to 200 W / m·k and less than or equal to 235 W / m·k. By reasonably setting the thermal conductivity of the two, the cooperation of the two parts can ensure both the heat conduction capacity and the heat storage capacity.

[0075] Furthermore, there is no rigid requirement for the strength of the filling member 14 and the strength of the container base 12 . The strengths of the two may be equal or unequal. Generally, the strength of the filling member 14 is greater than the strength of the container base 12 .

[0076] In the above embodiment, a first concave-convex structure is provided on one side of the filling member 14 close to the bottom of the container base 12, which specifically includes a first protrusion 142 and a first groove 144. A second concave-convex structure adapted to the first concave-convex structure is provided on the container base 12. The second concave-convex structure specifically includes a second protrusion 122 and a second groove 124. And the first protrusion 142 of the first concave-convex structure is flush with the bottom wall surface of the container base 12.

[0077] In this embodiment, the bottom of the filler 14 and the contact part of the container base 12 are matched by a concave-convex structure. Specifically, a plurality of spaced abutting parts can be provided on the side of the filler 14 close to the bottom of the cavity, and the plurality of abutting parts abut against the bottom of the cavity, so that a gap is provided between the non-abutting part of the filler 14 and the bottom of the cavity, so that after the filler 14 and the container base 12 are integrally formed, the bottom of the filler 14 and the contact part of the container base 12 can form a concave-convex structure. The first concave-convex structure is provided to form a gap between the filler 14 and the bottom of the cavity, so that the thickness of the bottom of the container base 12 can be controlled by the size of the gap, that is, the thickness of the convex part of the second concave-convex structure of the container base 12 can be controlled.

[0078] Furthermore, the length of the filling piece 14 can be reasonably set to control the gap between the filling piece 14 and the side wall of the cavity, thereby controlling the thickness of the basic side of the container 1.

[0079] In the above embodiment, the diameter of the hole in the container base 12 is less than or equal to 1.5 mm, and the porosity of the preset hole in the container base 12 is greater than 0 and less than or equal to 0.5%. Such porosity makes the structure inside the container base 12 more compact and meets relevant requirements, thus ensuring the performance of the container base 12.

[0080] Specifically, when calculating the holes, holes with a diameter less than 0.25 mm are not counted. After the container base 12 is formed, the number of holes in the unit area of ​​10 cm × 10 cm is no more than 4, and the distance between two holes is not less than 5 cm. The diameter of the preset holes is greater than 0.25 mm and less than or equal to 1.5 mm, and the distance between each preset hole and the outer surface of the container base 12 is greater than or equal to 2 times the diameter of each preset hole itself. This type of container base 12 makes the bubbles less, the interior of the part is denser, and ensures the qualified rate of the product.

[0081] In the above embodiment, the cross-sectional thickness H3 of the filling member 14, that is, the thickness excluding the convex portion in the first concavo-convex structure, that is, the thickness of the body of the filling member 14 away from the bottom of the cavity is greater than or equal to 1.5 mm and less than or equal to 5 mm. This dimension should not be too small, otherwise the thermal conductivity of the container 1 cannot be well adjusted.

[0082] In the above embodiment, the thickness of the container base 12 is greater than or equal to 1 mm and less than or equal to 5 mm. The thickness of the container base 12 should not be too large, otherwise it will be difficult to process and will result in a worse thermal conductivity. At the same time, the thickness should not be too thin, otherwise it will result in a serious lack of heat storage capacity. Setting the thickness at 1 mm-5 mm can make it moderate, thereby taking into account the convenience of processing and being able to monitor the heat storage capacity and thermal conductivity.

[0083] In the above-mentioned embodiments, the container substrate 12 includes an aluminum-silicon alloy substrate or an aluminum-copper alloy substrate.

[0084] Furthermore, if Figure 1 As shown, the container 1 further includes a non-stick coating 16. The non-stick coating 16 is located on the inner wall of the container substrate 12. The non-stick property of the container 1 is ensured by providing the non-stick coating 16. Specifically, the non-stick coating 16 can be any one of a PTFE coating, a PFA coating, a PEEK coating, and a ceramic coating.

[0085] Furthermore, if Figure 2 As shown, the container 1 further includes: a protective layer, which is arranged on the outer wall surface of the container base 12, such as an anti-rust layer 18, so as to protect the outer surface of the container base 12 and prevent the container base 12 from being corroded.

[0086] The embodiment of the second aspect of the present invention provides a method for preparing a container, which is used to prepare the container provided by any embodiment of the first aspect. Figure 3 As shown, the preparation method comprises:

[0087] S302, placing a filling piece in the mold cavity, wherein the thermal conductivity of the filling piece is different from the thermal conductivity of the container base.

[0088] S304, filling the molten metal into the mold cavity at a preset filling speed.

[0089] S306, when the molten metal in the mold cavity is formed into a semi-solid part, a preset portion of the semi-solid part is extruded until the molten metal in the mold cavity is formed into a container matrix.

[0090] Among them, the so-called semi-solid part is a state in which the temperature is controlled between the liquid phase line and the solid phase line.

[0091] The preparation method of the container provided by the present invention is specifically used to prepare containers, especially cooking containers. Specifically, the container includes a container base, and the container base has a cavity for accommodating articles, which constitutes the main structure of the container and can meet the basic needs of holding articles. Of course, in addition to the container base, the container can also include a coating arranged on the inner and outer surfaces of the container base, such as a non-stick coating arranged in the container base, or a protective coating arranged outside the container base. When the container base is formed, the container base is integrally prepared by a die-casting liquid forging composite process. Specifically, the preparation steps are: first, the molten metal is filled into the mold cavity of the mold. In this step, the filling speed needs to be fully controlled to ensure that the molten metal can be filled into the mold cavity by high pressure. Specifically, the molten metal is filled into the mold cavity of the mold in the way that the molten metal in the die-casting process is filled into the mold cavity, so that the molten metal can be quickly filled into the mold cavity, and the molten metal can be quickly solidified in the mold cavity. After the molten metal is filled, the molten metal will gradually solidify in the mold cavity. When the molten metal solidifies into a semi-solid part (for example, after the filling is completed for a preset time), the preset part of the semi-solid part is squeezed until the semi-solid part is formed into a container matrix. In this way, after the molten metal solidifies into a semi-solid part, the semi-solid part is locally squeezed until the end, and this method is similar to the liquid die forging process, which greatly solves the problem that the parts formed by the die casting process have many pores, are not dense, and have a high scrap rate. That is, in the process of preparing the container matrix, the first half of the step of this application adopts the die casting process, and the liquid die forging process is combined in the latter step (specifically reflected in the local extrusion of the semi-solid part), thereby combining the two processes of die casting and liquid die forging together, that is, providing a new process, that is, the die casting and liquid forging composite process. This process, through targeted transformation of die casting technology, injects the function of liquid die forging, reduces air entrainment by dynamically adjusting the filling speed (filling time) during the die casting process, and uses the extrusion rod in the die to locally extrude and compensate for the shrinkage of the semi-solid casting when the metal solidifies and shrinks, thereby greatly reducing product holes and significantly reducing the risk of blistering or local shedding of the coating, which not only improves the product qualification rate, but also enhances the user experience. In this way, the respective advantages of low die casting cost and high liquid die forging casting quality are utilized, and the die casting-liquid die forging composite process is creatively used to manufacture cooking containers, thereby improving the yield rate of the original die casting aluminum alloy and improving the cost performance, thereby ensuring the yield rate and quality of the prepared container matrix and reducing its preparation cost.

[0092] In the above embodiment, before the step of filling the molten metal into the mold cavity at a preset filling speed, a filling piece is placed in the mold cavity, and the thermal conductivity of the filling piece is different from the thermal conductivity of the container base.

[0093] At the same time, in this preparation method, when the container base is formed, a filler is added to the mold, so that the filler and the container base can be formed in one piece. The container formed in this way includes not only the container base but also the filler, so that the formed container includes a two-layer structure, a filling layer 140 formed by the filler, and a liquid forging layer 120 as the container base. Since the liquid forging layer 120 and the filling layer 140 are different parts, their thermal conductivity and strength are different, so that the container has at least two positions with different thermal conductivity. In the actual process, the thickness of the filler at different positions can be reasonably set according to the needs of each position of the container, so as to dynamically adjust the thickness of the container base at different positions, so as to dynamically adjust the thermal conductivity and heat transfer rate of each position of the container such as the cooking vessel by combining two materials with different thermal conductivities, and achieve the best thermal conduction and heat storage coupling effect.

[0094] In the step of filling the molten metal into the mold cavity at a preset filling speed, the filling speed of the molten metal is greater than 0 and less than or equal to 0.8%. By controlling the filling speed, the filling time can be controlled to be greater than or equal to 0.02s and less than or equal to 0.05s. Avoiding the molten metal from being filled too quickly and causing the parts to be formed too quickly, resulting in a large number of bubbles that cannot be discharged in time.

[0095] When the molten metal is filled into the mold cavity, it is necessary to dynamically adjust the filling speed according to the actual situation to control the filling time, so as to fully control the filling process of the molten metal and avoid the filling speed being too fast or too slow, which may cause the parts to fail to solidify as required. In this way, the quality of the parts after molding can be ensured, and the bubbles in the parts can be reduced, making the inside of the parts denser.

[0096] Furthermore, the filler includes a metal filler, because the metal filler has a better thermal conductivity, thereby ensuring the thermal conductivity of the product. The metal filler has a higher strength and is not easily damaged. Of course, the filler can also be made of other materials that can meet the strength and thermal conductivity, such as alloy parts.

[0097] Furthermore, the thermal conductivity of the filler is greater than that of the container base. Because the container base is generally made of aluminum silicon alloy or aluminum copper alloy, its high fluidity makes its thermal conductivity not too high, so the filler can be designed as a part with higher thermal conductivity to ensure the fluidity of the melt for preparing the container base.

[0098] Furthermore, there is no rigid requirement for the strength of the filling piece and the strength of the container base. The strengths of the two may be equal or unequal. Generally, the strength of the filling piece is greater than the strength of the container base.

[0099] In the above embodiment, a plurality of abutting portions arranged at intervals are provided on one side of the filling member close to the bottom of the cavity, the plurality of abutting portions abut against the bottom of the cavity, and a gap is provided between the non-abutting portion of the filling member and the bottom of the cavity. The abutting portions are provided to form a gap between the filling member and the bottom of the cavity, so that the thickness of the bottom of the container base can be controlled by the size of the gap. At the same time, the length of the filling member can be reasonably set to control the gap between the filling member and the side wall of the cavity, thereby controlling the thickness of the side of the container base.

[0100] In the above embodiment, the thermal conductivity of the container base is greater than or equal to 90 W / m·k and less than or equal to 110 W / m·k, and the thermal conductivity of the filler is greater than or equal to 200 W / m·k and less than or equal to 235 W / m·k. By reasonably setting the thermal conductivity of the two, the cooperation of the two parts can ensure both the heat conduction capacity and the heat storage capacity.

[0101] In the above embodiment, the cross-sectional thickness of the filling member, that is, the thickness excluding the abutting portion, that is, the thickness of the body of the filling member away from the bottom of the cavity is greater than or equal to 1.5 mm and less than or equal to 5 mm. This dimension should not be too small, otherwise the thermal conductivity of the container cannot be well adjusted.

[0102] In the above embodiments, the molten metal includes an aluminum-silicon alloy melt or an aluminum-barrel alloy melt.

[0103] In the above embodiment, the thickness of the container base is greater than or equal to 1 mm and less than or equal to 5 mm. The thickness of the container base should not be too large, otherwise it will be difficult to process and will result in a worse thermal conductivity. At the same time, the thickness should not be too thin, otherwise it will result in a serious lack of heat storage capacity. Setting the thickness to 1 mm-5 mm can make it moderate, thereby taking into account the convenience of processing and being able to monitor the heat storage capacity and thermal conductivity.

[0104] In the above embodiment, the container base includes multiple thicknesses, and the thickness of the container base at multiple locations meets the preset thickness requirements. Specifically, the container base is wrapped outside the filling member, and the bottom thickness of the container base is less than the side wall thickness of the container base. In this way, the bottom of the container base is relatively thin, so the heat conduction effect is better. The thick side wall can achieve better heat preservation and heat storage effects.

[0105] In the above embodiment, the diameter of the hole in the container matrix is ​​less than or equal to 1.5 mm, and the porosity of the preset holes in the container matrix is ​​greater than 0 and less than or equal to 0.5%. Specifically, when calculating the holes, holes with a diameter less than 0.25 mm are not counted. After the container matrix is ​​formed, the number of holes in the unit area of ​​10 cm × 10 cm is no more than 4, and the distance between two holes is not less than 5 cm. The diameter of the preset holes is greater than 0.25 mm and less than or equal to 1.5 mm, and the distance between each preset hole and the outer surface of the container matrix is ​​greater than or equal to twice the diameter of each preset hole itself. This kind of container matrix makes the bubbles less, the interior of the parts is denser, and ensures the qualified rate of the product.

[0106] In the above embodiment, the preparation method of the container also includes demolding pretreatment. The demolding pretreatment specifically includes opening the mold, taking out the container matrix and cooling it after the molten metal in the cavity is formed into the container matrix, and processing the cooled container matrix to a preset size and / or a preset accuracy. When the container matrix is ​​processed by the die-casting liquid forging composite process, some processing allowances are generally reserved for the container matrix. Therefore, after the container matrix is ​​prepared and formed, the container matrix can be processed into the size and accuracy (such as roughness, flatness and coaxiality, etc.) required by the drawing by machining or other methods.

[0107] Furthermore, the preparation method of the container also includes roughness treatment. The roughness treatment specifically includes: roughening the inner and outer surfaces of the container substrate until the roughness Ra of the inner and outer surfaces of the container substrate is greater than or equal to 2μm and less than or equal to 5μm. Furthermore, the roughness treatment includes sandblasting and / or grinding. Furthermore, this step is generally performed after the demolding pretreatment. If there is no demolding pretreatment step, the roughness treatment can be performed directly after the part is demolded. By performing roughness treatment on the container substrate, the surface quality of the container substrate can be guaranteed, and preparations can be made for subsequent coating spraying on the container substrate.

[0108] Furthermore, the preparation method of the container further comprises forming a non-stick coating. The step of forming the non-stick coating specifically comprises: forming a non-stick coating on the inner wall surface of the container substrate. The non-stick property of the inner wall surface of the container can be improved by providing the non-stick coating. The non-stick coating specifically comprises one or more of a PTFE coating, a PFA coating, a PEEK coating, and a ceramic coating.

[0109] Furthermore, the preparation method of the container also includes: before the step of forming the non-stick coating, the container substrate is degreased. Among them, after the prepared container substrate is processed by machining and the like, there will be some grease on the surface, so before forming the non-stick coating, it needs to be degreased. The degreasing method can be high-temperature heating. At this time, the container can be heated. The specific heating temperature can be 350°C-420°C, and the heating duration can be 8min-15min. Of course, the degreasing treatment can also be carried out by other methods such as chemical degreasing.

[0110] Furthermore, the method for preparing the container also includes: forming a protective layer, such as an anti-rust layer, on the outer wall surface of the container base, so as to protect the outer surface of the container base and prevent the container base from being corroded.

[0111] The following uses a cooking vessel as an example to further introduce the method for preparing a container provided by the present application and the container prepared by the method. Specifically:

[0112] The present invention belongs to the technical field of kitchen utensil production and manufacturing, and specifically relates to a method for preparing a composite multi-layer cooking utensil that increases the bonding effect of an internal coating, reduces a product defect rate, and utilizes the difference between the material of an outer filling layer 140 and the material of a liquid forging layer 120 to improve the thermal conductivity or heat preservation properties of a multi-layer pot body.

[0113] The vessel is produced by a combination of filling and liquid forging, and specifically comprises a filling layer 140 and a liquid forging layer 120 as a container base, a non-stick coating disposed inside the liquid forging layer 120 , and an anti-rust layer located on the outer surface of the liquid forging layer 120 .

[0114] The filling layer 140 is formed by filling a metal core with high thermal conductivity and high structural strength in the liquid forging die according to the design requirements of the thermal conductivity and structural strength of the cooking vessel.

[0115] Specifically, the first protrusion of the metal core abuts against the mold portion (eg Figure 1 As shown in the figure, after the liquid metal (such as liquid aluminum) is injected into the mold cavity, the liquid metal can fill to the bottom of the metal material core during the liquid forging process.

[0116] Specifically, the cross-sectional thickness of the high thermal conductivity metal core filling layer 140 is not less than 1.5 mm. If it is too thin, the high thermal conductivity advantage cannot be effectively exerted.

[0117] The liquid forging layer 120 is made of aluminum-silicon alloy with low thermal conductivity and high fluidity, and is formed by a die-casting-liquid forging composite process.

[0118] Specifically, the liquid forging layer 120 has a thickness of 1 mm to 5 mm, and utilizes its low thermal conductivity to achieve heat storage capacity. The actual thickness value at each position is determined based on heat storage requirements.

[0119] Specifically, the filling layer 140 is high thermal conductivity aluminum with a thermal conductivity higher than 200 W / m·k, and the liquid forging layer 120 is low thermal conductivity aluminum-silicon alloy with a thermal conductivity lower than 110 W / m·k.

[0120] When the low thermal conductivity liquid forging layer 120 is filled and solidified in the mold, due to the release of a large amount of heat, the elements will diffuse with the preset filling layer 140 and form a metallurgical bonding interface (such as Figure 5 As shown in Table 1, a diffusion transition layer is formed at the interface between the high thermal conductivity filling layer 140 and the low thermal conductivity liquid forging layer 120 due to element diffusion. Microstructure observation and element analysis show that the thickness of the transition layer is less than 5um, and the element distribution at the interface is between the filling layer 140 and the liquid forging layer 120 (as shown in Table 1).

[0121] Table 1. Typical element distribution of filling layer, liquid forging layer and transition layer

[0122] Location Si Cu Fe Zn Al Filling layer 1 0.2 \ 0.28 \ margin Filling layer 2 0.17 \ 0.23 \ margin Liquid forging layer 1 10.5 2.4 1.1 0.9 margin Liquid forging layer 2 10.8 2.2 0.8 1.3 margin Transition layer 1 2.6 0.4 0.35 0.2 margin Transition layer 2 4.5 0.9 0.6 0.7 margin

[0123] Specifically, the maximum diameter of a single hole inside a cooking pot produced by the die-casting-liquid forging composite process shall not exceed 1.5mm, and holes with a diameter less than 0.25mm shall not be counted. Within a unit area of ​​10cm×10cm, the number of holes shall not exceed 4, and the distance between two holes shall not be less than 5cm, and the distance between the center point of the hole and the surface of the casting shall not be less than 2 times the diameter of the hole itself.

[0124] The cooking vessel is prepared by a die-casting-liquid forging composite process, and the preparation method specifically includes the following steps:

[0125] S402, after the molten aluminum is hydraulically injected into the mold cavity, the filling speed is dynamically adjusted to reduce air entrainment, and then the extrusion rod in the mold is used to locally extrude and compensate for the shrinkage of the semi-solid casting formed in the cavity to increase the density.

[0126] S404: After the cooking utensils are removed from the mold and cooled, they are processed to the specified size and accuracy according to the drawing requirements.

[0127] S406, sandblasting the inside and outside of the cooking vessel, and the outer surface roughness Ra after sandblasting is 2μm-5μm.

[0128] S408, high temperature degreasing is performed, the degreasing temperature is 350°C-420°C, and the degreasing time is 8min-15min.

[0129] S410, spraying a non-stick coating on the inside of the cooking vessel, including but not limited to a coating that can achieve non-stick properties, such as PTFE, PFA, PEEK, ceramics, etc.

[0130] This solution combines the two processes of die casting and liquid die forging, taking advantage of the respective advantages of low die casting cost and high liquid die forging casting quality, and creatively uses the die casting-liquid die forging composite process to manufacture cooking utensils, thereby improving the yield of the original die-casting aluminum alloy and enhancing the cost-effectiveness.

[0131] Die casting is a metal casting process that uses high pressure to force molten metal into a complex metal mold. It has the characteristics of high-speed filling and rapid cooling, but it has many pores, is not dense, and has a high scrap rate. The typical process parameters of cooking utensils using traditional die casting are as follows: specific pressure: above 65MPa; injection speed: 5m / s-8m / s; aluminum liquid filling time: 0.02m / s-0.05s.

[0132] Liquid die forging is a metal forming process that has both casting characteristics and is similar to die forging. It is a process in which a certain amount of molten metal is directly poured into the mold cavity and solidified under continuous mechanical static pressure. Liquid die forging technology can eliminate shrinkage cavities formed by solidification shrinkage and obtain high-strength parts with fine and uniform grains and dense structure, but the cost is relatively high. The punch extrusion pressure of liquid die forging is generally selected to be above 60MPa, the filling speed of the molten metal is controlled below 0.8m / s, the punch pressurization speed is 0.1m / s-0.4m / s, and the holding time is 10s-30s.

[0133] The die-casting-liquid forging composite process injects the function of liquid die forging by making targeted modifications to the die-casting technology. It reduces air entrapment by dynamically adjusting the filling speed during the die-casting process, and uses the extrusion rod in the mold to locally extrude and compensate for the shrinkage of the semi-solid casting when the metal solidifies and shrinks. This greatly reduces product holes, and the risk of blistering or local shedding of the coating is significantly reduced, which not only improves the product qualification rate, but also enhances the user experience. Specific implementation method:

[0135] Test method: Use a 3L rice cooker pot, add 600g of raw rice, and then fill in 20℃ pure water to the standard water level, and perform a quick cooking test on a 1000W heating platform, an ambient temperature of 23℃, a humidity of 45%, and an atmospheric pressure of 101kPa. After the test system jumps to the insulation mode, take out the inner pot immediately and leave it in the above environment to cool naturally, measure the power consumption during the heating process, the cooling rate of the rice inside the pot, and the degree of browning of the rice at the bottom of the pot.

[0136] Example:

[0137] The inner pot is produced by a layered liquid forging composite process of high thermal conductivity filling layer 140 + low thermal conductivity liquid forging layer 120. The bottom of the pot is designed to be a 3mm thick filling layer 140 + a 2mm liquid forging layer 120, and the pot wall is designed to be a 2mm filling layer 140 + a 5mm liquid forging layer 120, with a uniform transition between the bottom and the wall.

[0138] Comparative Example 1:

[0139] The inner pot is made of high thermal conductivity aluminum in one step, with a bottom thickness of 5mm and a wall thickness of 7mm, and a uniform transition between the bottom and the wall.

[0140] Comparative Example 2:

[0141] The inner pot is formed in one step using low thermal conductivity aluminum silicon alloy, the bottom thickness is 5mm, the wall thickness is 7mm, and the transition between the bottom and the wall is uniform.

[0142] After the rice cooking test, the power consumption, the cooling speed of the rice inside the pot, and the degree of browning of the rice at the bottom of the pot of the embodiment and the comparative example are shown in Table 2:

[0143] Table 2 Test results of embodiments and comparative examples

[0144]

[0145] The test results in the table show that the layered liquid forging composite process has the best comprehensive effect in terms of power consumption, rice heat preservation performance, and bottom overheating degree. The power consumption of this process is almost the same as that of the high thermal conductivity aluminum inner pot. This is because the bottom of the embodiment not only has enough filling layers to ensure heat transfer, but also the low thermal conductivity layer of 5mm on the surrounding walls can play a good heat preservation and heat storage effect, thereby reducing heat outflow and improving the effective use of heat. The heat preservation effect and the degree of bottom browning during cooling of the embodiment are basically at the same level as the inner pot (Comparative Example 2) made entirely of low thermal conductivity materials due to the presence of the heat storage layer. On the other hand, Comparative Example 1 is made of high thermal conductivity materials. Due to the high thermal conductivity coefficient of the bottom of the pot, the local temperature rise is too fast, so that it exceeds the set value, so that the rice at the bottom of the pot is browned. If a thinner bottom is used, this phenomenon will be more obvious, and there is even a potential risk of the bottom being burnt. Since Comparative Example 2 is made entirely of low thermal conductivity materials, the heat transfer speed is slow and the heat utilization rate is low. The result is that the power consumption is significantly higher than that of the embodiment and Comparative Example 1.

[0146] In the description of this specification, the terms "connection", "installation", "fixation" and the like should be understood in a broad sense. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0147] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0148] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A container, characterized in that: include: A container base, wherein the container base is a metal part; A filler is located in the wall of the container base, and the filler and the container base are integrally formed, and the thermal conductivity of the filler is different from the thermal conductivity of the container base.

2. The container according to claim 1, characterized in that The filling piece and the container base are integrally formed by a die-casting and liquid-forging composite process.

3. The container according to claim 1, characterized in that The container base is wrapped outside the filling piece, and the bottom thickness of the container base is smaller than the side wall thickness of the container base.

4. The container according to claim 1, characterized in that The thermal conductivity of the filler is greater than the thermal conductivity of the container base; or The thermal conductivity of the container base is greater than or equal to 90 W / m·k and less than or equal to 110 W / m·k, and the thermal conductivity of the filler is greater than or equal to 200 W / m·k and less than or equal to 235 W / m·k.

5. The container according to claim 1, characterized in that A first concave-convex structure is arranged on one side of the filling piece close to the bottom of the container base, a second concave-convex structure matching the first concave-convex structure is arranged on the container base, and a convex portion of the first concave-convex structure is flush with the bottom wall of the container base.

6. The container according to any one of claims 1 to 5, characterized in that The diameter of the holes in the container matrix is ​​less than or equal to 1.5 mm, the porosity of the preset holes in the container matrix is ​​greater than 0 and less than or equal to 0.5%, the diameter of the preset holes is greater than 0.25 mm and less than or equal to 1.5 mm, and / or the distance between each of the preset holes and the outer surface of the container matrix is ​​greater than or equal to twice the diameter of each of the preset holes.

7. The container according to any one of claims 1 to 5, characterized in that The cross-sectional thickness of the filler is greater than or equal to 1.5 mm and less than or equal to 5 mm; and / or The thickness of the container base is greater than or equal to 1 mm and less than or equal to 5 mm.

8. The container according to any one of claims 1 to 5, characterized in that The filler comprises a metal filler; and / or The container substrate comprises an aluminum-silicon alloy substrate and / or an aluminum-copper alloy substrate; and / or The container further comprises a non-stick coating located on the inner wall of the container base.

9. A method for preparing a container, characterized in that: Used to prepare a container according to any one of claims 1 to 8, the preparation method comprising: A filler is placed in the mold cavity of the mold, wherein the thermal conductivity of the filler is different from the thermal conductivity of the container base; Filling the molten metal into the cavity of the mold at a preset filling speed; When the molten metal in the mold cavity is formed into a semi-solid part, a preset portion of the semi-solid part is extruded until the molten metal in the mold cavity is formed into a container matrix.

10. The method for preparing a container according to claim 9, characterized in that: In the step of filling the molten metal into the mold cavity at a preset filling speed, the filling speed of the molten metal is greater than 0 and less than or equal to 0.8 m / s.

11. The method for preparing a container according to claim 9 or 10, characterized in that: The molten metal includes an aluminum-silicon alloy melt and / or an aluminum-copper alloy melt.

12. The method for preparing a container according to claim 9 or 10, characterized in that: Also includes: Demolding pretreatment: after the molten metal in the cavity is formed into the container matrix, the mold is opened, the container matrix is ​​taken out and cooled, and the cooled container matrix is ​​processed to a preset size and / or preset accuracy; Roughness treatment: roughening the inner and outer surfaces of the container substrate until the roughness Ra of the inner and outer surfaces of the container substrate is greater than or equal to 2 μm and less than or equal to 5 μm; Formed non-stick coating: a non-stick coating is formed on the inner wall surface of the container substrate, and the non-stick coating includes at least one of PTFE coating, PFA coating, PEEK coating and ceramic coating.