Preparation method and application of fly ash-based aerogel phase change material

By activating fly ash and modifying nanovermiculite, high-strength and high-quality fly ash-based aerogel was prepared, which solved the problems of harsh high-temperature calcination conditions and low impurity removal efficiency in the existing technology, and achieved It has the high performance and antibacterial properties of aerogels, and is suitable for insulation materials.

CN118925608APending Publication Date: 2024-11-12HENAN XIAN NEW BUILDING MATERIALS
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410991562.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the high-temperature calcination conditions are harsh in the process of preparing silica aerogels by fly ash, and the impurity removal efficiency is not high, and it is difficult to meet the needs of high-strength and high-quality aerogels.

Method used

Activation by reacting fly ash with sodium n-hexadecyl sulfate solution, followed by calcination and treatment in acid and alkali medium, forming a water glass solution, and adding modified nanovermiculite, and finally drying under specific conditions to prepare the powder Fly ash-based aerogel.

Benefits of technology

It improves the porosity and impurity removal efficiency of fly ash surface, enhances the spatial network structure strength and thermal insulation ability of aerogels, and the introduction of nanovermiculite provides antibacterial properties and is suitable for high-performance insulation materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925608A_ABST
    Figure CN118925608A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of fly ash-based aerogel preparation, in particular to a preparation method and application of a fly ash-based aerogel phase change material, the preparation method comprises the following steps: S1, preparing activated fly ash; s2, carrying out acid leaching on the activated fly ash prepared in the step S1, and then carrying out suction filtration; s3, the filter residues prepared in the step S2 are subjected to alkaline leaching, and water glass is obtained; s4, adjusting the pH value of the water glass prepared in the step S3 to obtain hydrogel, and adsorbing the modified nano vermiculite; and S5, immersing the composite wet gel in the step S4 in a mixed solution of normal hexane, trimethylchlorosilane and ethanol for 12 hours to obtain the fly ash-based aerogel phase change material. According to the method, the silicon dioxide aerogel can be rapidly prepared from the fly ash, meanwhile, the strength of the aerogel is high enough, and effective utilization of solid waste is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fly ash-based aerogel preparation, and in particular to a preparation method and application of a fly ash-based aerogel phase change material. Background Art

[0002] Aerogel is a form of solid matter, the lowest density solid in the world. Aerogel has a continuous network structure, microscopically has nanoscale uniformity, high porosity, large specific surface area, and its mechanical, acoustic, optical, thermal and other properties are significantly different from the corresponding macroscopic glassy materials. The particularity of aerogel properties leads to its broad application prospects. Silica aerogel is one of the common aerogels. Silica aerogel generally uses methyl silicate or ethyl orthosilicate as a precursor to prepare silica aerogel. This preparation method has the disadvantage of expensive raw materials.

[0003] Therefore, many people have turned their attention to fly ash. As a common industrial solid waste, fly ash contains a large amount of silicon source. If fly ash can be effectively utilized, it will not only reduce the harm of fly ash to the environment, but also save resources. In order to prepare silica aerogel from fly ash, it is necessary to acid-leach the fly ash to remove metal oxide impurities such as aluminum. Before acid leaching, the fly ash needs to be activated. Generally, high-temperature calcination treatment is adopted. The calcination temperature is above 600-800°C. The reaction conditions are relatively harsh, and the removal efficiency of impurities is not high. Moreover, with the increasing demand for high-strength and high-quality aerogels, it is necessary to develop a high-strength and high-quality aerogel phase change material based on fly ash as the basic material. To this end, in view of the problems raised in the above background technology, technicians in this field propose a method for preparing fly ash-based aerogel phase change material. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a fly ash-based aerogel phase change material and its application, so as to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for preparing a fly ash-based aerogel phase change material, which is prepared by the following method:

[0007] S1. Preparation of activated fly ash

[0008] S101, dispersing fly ash into a sodium hexadecyl sulfate solution with a concentration of 0.2-0.4 mol / L, stirring and heating to react for 0.5-2 h, introducing carbon dioxide gas into the solution during the reaction, the heating temperature is 60-75° C., and then filtering to obtain a crude product;

[0009] S102, washing the crude product obtained in step S101 with deionized water, and then placing it in a muffle furnace into which nitrogen and fluorine gases are introduced, and calcining it at 200-300° C. for 2-3 hours to obtain activated fly ash;

[0010] S2, placing the activated fly ash prepared in step S1 into hydrochloric acid at a temperature of 60-95° C. and a concentration of 3-5 mol / L, stirring for 1-3 h, vacuum filtering and washing with deionized water until the pH value is 7, to obtain a filter residue;

[0011] S3, placing the filter residue prepared in step S2 into a sodium hydroxide solution with a temperature of 60-95° C. and a concentration of 6-8 mol / L, stirring and reacting for 2-4 hours, and vacuum filtering to obtain a water glass solution;

[0012] S4, adding 1 mol / L hydrochloric acid solution to the water glass solution prepared in step S3, adjusting the pH to 9-10, sealing and standing for 48 hours to generate a wet gel and soaking it in deionized water, then placing the wet gel in a 20-50%wt ethanol aqueous solution dispersed with modified nano vermiculite in a closed environment at 110-150° C. for 6-8 hours, and then continuing to react at 60-70° C. for 20-28 hours to obtain a composite wet gel;

[0013] S5. Immerse the wet gel in step S4 in a mixed solution of n-hexane, trimethylchlorosilane and ethanol for 12-16 hours to obtain a modified composite wet gel. After the modified composite wet gel is washed with n-hexane, it is placed at 60-150° C. under normal pressure and dried for 2-4 hours. After naturally cooling to room temperature, a fly ash-based aerogel phase change material is obtained.

[0014] Furthermore, in the step S101, the mass ratio of fly ash to sodium hexadecyl sulfate solution is 1:(20-30), and the volume ratio of nitrogen to fluorine gas in the step S102 is 9:1.

[0015] Furthermore, in step S2, the mass ratio between activated fly ash and hydrochloric acid is 1:(8-10).

[0016] Furthermore, in step S3, the mass ratio of the filter residue to the sodium hydroxide solution is 1:(2.5-5).

[0017] Furthermore, in step S4, the time for soaking the wet gel with deionized water is 24-72 hours, and the deionized water is replaced every 24 hours. The mass ratio of the deionized water for soaking the wet gel to the filter residue used in step S3 is (25-50):1, and the mass ratio of the modified nano-vermiculite and the ethanol aqueous solution to the filter residue used in step S3 is 1:(120-180):(12-16).

[0018] Furthermore, the modified nano vermiculite in step S4 is prepared by the following method:

[0019] S201, dispersing nano vermiculite in a mixed solution of sodium hydroxide and hydrogen peroxide and soaking for 4-6 hours, wherein the molar concentration of sodium hydroxide is 1 mol / L, and the mass fraction of hydrogen peroxide is 30%wt, and after immersion, the nano vermiculite is filtered and placed in a muffle furnace filled with nitrogen and calcined at 350-400°C for 2-3 hours;

[0020] S202, dispersing the expanded vermiculite calcined in step S201 into a 1 mol / L silver nitrate solution, soaking for 2-3 hours and filtering, placing the filtered product into a muffle furnace into which air is passed, and continuing to calcine at 300-450° C. for 1-2 hours to obtain modified nano vermiculite.

[0021] Furthermore, the mass ratio of the nano-vermiculite to the mixed solution of sodium hydroxide and hydrogen peroxide in step S201 is 1:20, and the mass ratio of the nano-vermiculite to the silver nitrate solution in step S202 is 1:30.

[0022] Furthermore, the mass ratio of n-hexane, trimethylchlorosilane and ethanol in step S5 is 10:1:30, and the mass ratio of the mixed solution of n-hexane, trimethylchlorosilane and ethanol to the filter residue used in step S3 is 20:1.

[0023] A method for preparing a fly ash-based aerogel phase change material and application of the prepared fly ash-based aerogel phase change material in thermal insulation materials.

[0024] The thermal insulation material may be thermal insulation felt, thermal insulation board, thermal insulation wall, etc. The fly ash-based aerogel phase change material in the present invention may be used as a material for preparing thermal insulation felt, thermal insulation board, thermal insulation wall, etc.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. Before preparing the aerogel phase change material from fly ash, the present invention first activates the fly ash. During the activation process, the pores on the surface of the fly ash can be effectively increased, which is convenient for the subsequent treatment of the fly ash with fluorine gas and improves the activation efficiency. In the subsequent acid leaching treatment, other impurities in the fly ash except silicon dioxide can be removed to the maximum extent, thereby improving the quality of the prepared aerogel;

[0027] 2. After the wet gel is prepared, the invention uses the adsorption performance of the wet gel itself to add modified nano vermiculite thereto. The modified nano vermiculite effectively improves the strength of the spatial network structure of the formed aerogel. When the solvent evaporates during the preparation of the aerogel, the aerogel is not easy to collapse, and its thermal insulation capacity and porosity are enhanced. At the same time, by using the characteristics of the nano vermiculite itself, silver is conveniently introduced into the aerogel, so that the aerogel has a good antibacterial effect when used as a thermal insulation material. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a process flow chart of the present invention;

[0029] Figure 2 The process flow chart of preparing activated fly ash in the present invention;

[0030] Figure 3 The process flow chart of preparing modified nano vermiculite in the present invention is as follows;

[0031] Figure 4 This is a SEM image of the fly ash-based aerogel phase change material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] See also Figure 1-4 , the present invention provides a technical solution:

[0034] Example 1

[0035] A method for preparing a fly ash-based aerogel phase change material, which is prepared by the following method:

[0036] S1. Preparation of activated fly ash

[0037] S101, dispersing 26.5 g of fly ash into 660 g of 0.3 mol / L sodium hexadecyl sulfate solution, stirring and heating to react for 1.2 h, introducing carbon dioxide gas into the solution during the reaction, heating the solution to 65° C., and then filtering to obtain a crude product;

[0038] S102, washing the crude product obtained in step S101 with deionized water, and then calcining it in a muffle furnace into which nitrogen and fluorine gases are introduced at 260° C. for 2.4 hours, wherein the volume ratio of nitrogen to fluorine is 9:1, to obtain activated fly ash;

[0039] S2, putting 20.6 g of activated fly ash prepared in step S1 into 190 g of hydrochloric acid at a temperature of 70° C. and a concentration of 4 mol / L, stirring for 2 h, vacuum filtering and washing with deionized water until the pH value is 7, to obtain a filter residue;

[0040] S3, putting 13.4 g of the filter residue prepared in step S2 into 54 g of a sodium hydroxide solution at a temperature of 85° C. and a concentration of 6 mol / L, stirring and reacting for 3 h, and vacuum filtering to obtain a water glass solution;

[0041] S4, add 1mol / L hydrochloric acid solution to the water glass solution prepared in step S3, adjust the pH to 10, seal and stand for 48h to generate wet gel and soak it with 530g deionized water for 48h, replace the deionized water every 24h during the soaking process, then place the wet gel in a 40%wt ethanol aqueous solution dispersed with 1.1g modified nano vermiculite and react for 7.2h in a closed environment at 120°C, the ethanol aqueous solution is used in an amount of 170g, and then continue to react at 65°C for 24h to obtain a composite wet gel;

[0042] S5. The wet gel in step S4 is immersed in a mixed solution of 65 g n-hexane, 6.5 g trimethylchlorosilane and 196 g ethanol for 15 h to obtain a modified composite wet gel. After the modified composite wet gel is washed with n-hexane, it is placed at 110° C. for 3 h under normal pressure and naturally cooled to room temperature to obtain a fly ash-based aerogel phase change material.

[0043] The modified nano vermiculite in step S4 is prepared by the following method:

[0044] S201, dispersing 2.4 g of nano vermiculite into 48 g of a mixed solution of 1 mol / L sodium hydroxide and 30% wt hydrogen peroxide and soaking for 5 h, filtering the nano vermiculite after soaking, placing it in a muffle furnace filled with nitrogen and calcining it at 380° C. for 2.6 h;

[0045] S202, dispersing the expanded vermiculite calcined in step S201 into 72 g of 1 mol / L silver nitrate solution, soaking for 2.4 hours and filtering, placing the filtered product into a muffle furnace with air flowing in, and continuing to calcine at 350° C. for 1.5 hours to obtain modified nano vermiculite.

[0046] Example 2

[0047] A method for preparing a fly ash-based aerogel phase change material, which is prepared by the following method:

[0048] S1. Preparation of activated fly ash

[0049] S101, dispersing 24.8 g of fly ash into 496 g of 0.2 mol / L sodium hexadecyl sulfate solution, stirring and heating for 0.5 h, introducing carbon dioxide gas into the solution during the reaction, heating the solution to 60° C., and then filtering to obtain a crude product;

[0050] S102, washing the crude product obtained in step S101 with deionized water, and then calcining it in a muffle furnace into which nitrogen and fluorine gases are introduced at 200° C. for 2 hours, wherein the volume ratio of nitrogen to fluorine is 9:1, to obtain activated fly ash;

[0051] S2, putting 18.5g of activated fly ash prepared in step S1 into 148g of hydrochloric acid at a temperature of 60°C and a concentration of 3mol / L, stirring for 1h, vacuum filtering and washing with deionized water until the pH is 7 to obtain a filter residue;

[0052] S3, putting 11.8 g of the filter residue prepared in step S2 into 29.5 g of a sodium hydroxide solution at a temperature of 60° C. and a concentration of 6 mol / L, stirring and reacting for 2 h, and vacuum filtering to obtain a water glass solution;

[0053] S4, adding 1 mol / L hydrochloric acid solution to the water glass solution prepared in step S3, adjusting the pH to 9, sealing and standing for 48 h to generate a wet gel, and then soaking it in 295 g of deionized water for 24 h, then placing the wet gel in a 20% wt ethanol aqueous solution dispersed with 0.73 g of modified nano vermiculite in a closed environment at 110 ° C for 6 h, the mass of the ethanol aqueous solution is 87.6 g, and then continuing to react at 60 ° C for 20 h to obtain a composite wet gel;

[0054] S5. The wet gel in step S4 is immersed in a mixed solution of 57 g n-hexane, 5.7 g trimethylchlorosilane and 172 g ethanol for 12 hours to obtain a modified composite wet gel. After the modified composite wet gel is washed with n-hexane, it is placed at 60° C. under normal pressure and dried for 2 hours. After naturally cooling to room temperature, a fly ash-based aerogel phase change material is obtained.

[0055] The modified nano vermiculite in step S4 is prepared by the following method:

[0056] S201, dispersing 1.8 g of nano vermiculite into 36 g of a mixed solution of 1 mol / L sodium hydroxide and 30% wt hydrogen peroxide and soaking for 4 h, filtering the nano vermiculite after soaking, placing it in a muffle furnace filled with nitrogen and calcining it at 350° C. for 2 h;

[0057] S202, dispersing the expanded vermiculite calcined in step S201 into 54g of 1mol / L silver nitrate solution, soaking for 2h, filtering, placing the filtered product into a muffle furnace with air flowing in, and continuing to calcine at 300°C for 1h to obtain modified nano vermiculite

[0058] Example 3

[0059] A method for preparing a fly ash-based aerogel phase change material, which is prepared by the following method:

[0060] S1. Preparation of activated fly ash

[0061] S101, dispersing 22.4 g of fly ash into 672 g of 0.4 mol / L sodium hexadecyl sulfate solution, stirring and heating for 2 h, introducing carbon dioxide gas into the solution during the reaction, heating at 5° C., and then filtering to obtain a crude product;

[0062] S102, washing the crude product obtained in step S101 with deionized water, and then calcining it in a muffle furnace into which nitrogen and fluorine gases are introduced at 300° C. for 3 hours, wherein the volume ratio of nitrogen to fluorine is 9:1, to obtain activated fly ash;

[0063] S2, putting 18.1 g of activated fly ash prepared in step S1 into 181 g of hydrochloric acid at a temperature of 95° C. and a concentration of 5 mol / L, stirring for 3 h, vacuum filtering and washing with deionized water until the pH value is 7, to obtain a filter residue;

[0064] S3, putting 10.2 g of the filter residue prepared in step S2 into 51 g of a sodium hydroxide solution at a temperature of 95° C. and a concentration of 8 mol / L, stirring and reacting for 4 h, and vacuum filtering to obtain a water glass solution;

[0065] S4, add 1mol / L hydrochloric acid solution to the water glass solution prepared in step S3, adjust the pH to 10, seal and let stand for 48h to generate wet gel and soak it in 510g deionized water for 72h, replace the deionized water every 24h, then place the wet gel in 50%wt ethanol aqueous solution dispersed with 0.85g modified nano vermiculite and react in a closed environment at 150°C for 8h, the mass of the ethanol aqueous solution is 153g, and then continue to react at 70°C for 28h to obtain a composite wet gel;

[0066] S5. The wet gel in step S4 is immersed in a mixed solution of 50 g n-hexane, 5 g trimethylchlorosilane and 150 g ethanol for 16 hours to obtain a modified composite wet gel. After the modified composite wet gel is washed with n-hexane, it is placed at 150° C. for 4 hours under normal pressure and naturally cooled to room temperature to obtain a fly ash-based aerogel phase change material.

[0067] The modified nano vermiculite in step S4 is prepared by the following method:

[0068] S201, dispersing 2.6 g of nano vermiculite into 52 g of a mixed solution of 1 mol / L sodium hydroxide and 30% wt hydrogen peroxide and soaking for 6 h, filtering the nano vermiculite after soaking, placing it in a muffle furnace filled with nitrogen and calcining it at 400° C. for 3 h;

[0069] S202, dispersing the expanded vermiculite calcined in step S201 into 78 g of 1 mol / L silver nitrate solution, soaking for 3 hours and filtering, placing the filtered product into a muffle furnace with air flowing in and continuing to calcine at 450° C. for 2 hours to obtain modified nano vermiculite.

[0070] Example 4

[0071] A method for preparing a fly ash-based aerogel phase change material, which is prepared by the following method:

[0072] S1. Preparation of activated fly ash

[0073] S101, dispersing 21.6 g of fly ash into 540 g of 0.3 mol / L sodium hexadecyl sulfate solution, stirring and heating for 1.5 h, introducing carbon dioxide gas into the solution during the reaction, heating the solution to 70° C., and then filtering to obtain a crude product;

[0074] S102, washing the crude product obtained in step S101 with deionized water, and then placing it in a muffle furnace into which nitrogen and fluorine gases are introduced, and calcining it at 260° C. for 2.6 hours, wherein the volume ratio of nitrogen to fluorine is 9:1, to obtain activated fly ash;

[0075] S2, putting 16.7 g of activated fly ash prepared in step S1 into 170 g of 5 mol / L hydrochloric acid at a temperature of 80° C. and stirring for 2 h, vacuum filtering and washing with deionized water until the pH value is 7 to obtain a filter residue;

[0076] S3, putting 9.8 g of the filter residue prepared in step S2 into 45 g of a sodium hydroxide solution at a temperature of 85° C. and a concentration of 7 mol / L, stirring for 3 h, and vacuum filtering to obtain a water glass solution;

[0077] S4, adding 1 mol / L hydrochloric acid solution to the water glass solution prepared in step S3, adjusting the pH to 10, sealing and standing for 48 hours to generate a wet gel, and soaking it in 360g deionized water for 48 hours, wherein the deionized water is replaced every 24 hours, and then the wet gel is placed in a 40% ethanol aqueous solution dispersed with 0.8g modified nano vermiculite and reacted in a closed environment at 130°C for 8 hours, the mass of the ethanol aqueous solution is 120g, and then the reaction is continued at 70°C for 26 hours to obtain a composite wet gel;

[0078] S5. The wet gel in step S4 is immersed in a mixed solution of 48 g n-hexane, 4.8 g trimethylchlorosilane and 143 g ethanol for 15 hours to obtain a modified composite wet gel. After the modified composite wet gel is washed with n-hexane, it is placed at 80° C. under normal pressure and dried for 4 hours. After naturally cooling to room temperature, a fly ash-based aerogel phase change material is obtained.

[0079] The modified nano vermiculite in step S4 is prepared by the following method:

[0080] S201, dispersing 1.4 g of nano-vermiculite into a mixed solution of 28 g of 1 mol / L sodium hydroxide and 30% wt hydrogen peroxide and soaking for 4-6 h, filtering the nano-vermiculite after soaking, placing it in a muffle furnace filled with nitrogen and calcining it at 400° C. for 3 h;

[0081] S202, dispersing the expanded vermiculite calcined in step S201 into 42 g of 1 mol / L silver nitrate solution, soaking for 2 hours and filtering, placing the filtered product into a muffle furnace with air flowing in and continuing to calcine at 400° C. for 2 hours to obtain modified nano vermiculite.

[0082] Comparative Example 1

[0083] The difference between Comparative Example 1 and Example 1 is that step S201 is completely omitted, so that nano vermiculite is directly added in step S201, and the remaining steps are exactly the same as those in Example 1.

[0084] Comparative Example 2

[0085] The difference between Comparative Example 2 and Example 1 is that both step S201 and step S202 are omitted, so that nano-vermiculite is directly added in step S4, and the remaining steps are exactly the same as those in Example 1.

[0086] Comparative Example 3

[0087] The difference between Comparative Example 3 and Example 1 is that no nano vermiculite is added in step S4, and the remaining steps are exactly the same as those in Example 1.

[0088] Comparative Example 4

[0089] The difference between Comparative Example 4 and Example 1 is that the preparation of activated fly ash is changed, and the fly ash is calcined at a high temperature of 600-800°C to complete the activation of the fly ash. The remaining steps are exactly the same as in Example 1.

[0090] The fly ash-based aerogel phase change materials prepared in the above Examples 1-4 and Comparative Examples 1-4 were subjected to performance tests, and the test results are shown in Table 1 below:

[0091] Table 1: Performance test table of fly ash-based aerogel phase change materials prepared in Examples 1-4 and Comparative Examples 1-4

[0092] Maximum compressive stress (kPa) Thermal conductivity (W / m·k) Example 1 7.6 0.025 Example 2 6.9 0.034 Example 3 8.1 0.023 Example 1 7.4 0.032 Comparative Example 1 6.4 0.041 Comparative Example 2 6.1 0.049 Comparative Example 3 5.9 0.068 Comparative Example 4 6.9 0.038

[0093] It can be seen from the data of Example 1 and Comparative Examples 1-3 in Table 1 that after adding modified nano vermiculite, the thermal conductivity of the aerogel in the present invention has been significantly reduced, and the thermal insulation performance has been effectively improved, which proves that the thermal insulation performance has been improved. At the same time, the maximum compressive stress has been improved, which proves that the strength of the prepared aerogel material has been improved. In addition, the comparison between Example 1 and Comparative Example 4 shows that the activation method of fly ash in the present invention is relative to the traditional method of high-temperature calcination activation of fly ash. The basic performance of the aerogel has also been improved;

[0094] The above examples 1-4 and comparative examples 1-4 were subjected to antibacterial tests. Escherichia coli was selected as the experimental bacteria. The samples were inoculated in the culture medium, and the bacteria were counted at 0h and 24h, respectively, to obtain the data in the following Table 2:

[0095] Table 2: Antibacterial performance test table of fly ash-based aerogel phase change materials prepared in Examples 1-4 and Comparative Examples 1-4

[0096]

[0097]

[0098] It can be seen from the data of Example 1 and Comparative Example 1 in Table 2 that the antibacterial property of aerogel can be improved by pre-treating nano vermiculite in the present invention, and the combination of nano vermiculite and silver ions can improve the antibacterial property of aerogel materials as a whole. It can also be seen from the data of Example 1 and Comparative Example 4 that the effect of antibacterial material silver when applied in aerogel is also enhanced by pre-treating fly ash in the present invention.

[0099] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a fly ash-based aerogel phase change material, characterized in that: The preparation was carried out by the following method: S1. Preparation of activated fly ash S101, dispersing fly ash into a sodium hexadecyl sulfate solution with a concentration of 0.2-0.4 mol / L, stirring and heating to react for 0.5-2 h, introducing carbon dioxide gas into the solution during the reaction, the heating temperature is 60-75° C., and then filtering to obtain a crude product; S102, washing the crude product obtained in step S101 with deionized water, and then placing it in a muffle furnace into which nitrogen and fluorine gases are introduced, and calcining it at 200-300° C. for 2-3 hours to obtain activated fly ash; S2, placing the activated fly ash prepared in step S1 into hydrochloric acid at a temperature of 60-95° C. and a concentration of 3-5 mol / L, stirring for 1-3 h, vacuum filtering and washing with deionized water until the pH value is 7, to obtain a filter residue; S3, placing the filter residue prepared in step S2 into a sodium hydroxide solution with a temperature of 60-95° C. and a concentration of 6-8 mol / L, stirring and reacting for 2-4 hours, and vacuum filtering to obtain a water glass solution; S4, adding 1 mol / L hydrochloric acid solution to the water glass solution prepared in step S3, adjusting the pH to 9-10, sealing and standing for 48 hours to generate a wet gel and soaking it with deionized water, then placing the wet gel in a 20-50%wt ethanol aqueous solution dispersed with modified nano vermiculite in a closed environment at 110-150° C. for 6-8 hours, and then continuing to react at 60-70° C. for 20-28 hours to obtain a composite wet gel; S5. Immerse the wet gel in step S4 in a mixed solution of n-hexane, trimethylchlorosilane and ethanol for 12-16 hours to obtain a modified composite wet gel. After the modified composite wet gel is washed with n-hexane, it is placed at 60-150° C. under normal pressure and dried for 2-4 hours. After naturally cooling to room temperature, a fly ash-based aerogel phase change material is obtained.

2. The method for preparing a fly ash-based aerogel phase change material according to claim 1, characterized in that: The mass ratio of fly ash to sodium hexadecyl sulfate solution in step S101 is 1:(20-30), and the volume ratio of nitrogen to fluorine gas in step S102 is 9:

1.

3. The method for preparing a fly ash-based aerogel phase change material according to claim 1, characterized in that: The mass ratio of activated fly ash to hydrochloric acid in step S2 is 1:(8-10).

4. The method for preparing a fly ash-based aerogel phase change material according to claim 1, characterized in that: The mass ratio of the filter residue in step S3 to the mass ratio of the sodium hydroxide solution is 1:(2.5-5).

5. The method for preparing a fly ash-based aerogel phase change material according to claim 1, characterized in that: In step S4, the time for soaking the wet gel in deionized water is 24-72 hours, and the deionized water is replaced every 24 hours. The mass ratio of the deionized water soaking the wet gel to the filter residue used in step S3 is (25-50):1, and the mass ratio of the modified nano vermiculite and the ethanol aqueous solution to the filter residue used in step S3 is 1:(120-180):(12-16).

6. The method for preparing a fly ash-based aerogel phase change material according to claim 1, characterized in that: The modified nano vermiculite in step S4 is prepared by the following method: S201, dispersing nano vermiculite in a mixed solution of sodium hydroxide and hydrogen peroxide and soaking for 4-6 hours, wherein the molar concentration of sodium hydroxide is 1 mol / L, and the mass fraction of hydrogen peroxide is 30%wt, and after immersion, the nano vermiculite is filtered and placed in a muffle furnace filled with nitrogen and calcined at 350-400°C for 2-3 hours; S202, dispersing the expanded vermiculite calcined in step S201 into a 1 mol / L silver nitrate solution, soaking for 2-3 hours and filtering, placing the filtered product into a muffle furnace into which air is passed, and continuing to calcine at 300-450° C. for 1-2 hours to obtain modified nano vermiculite.

7. The method for preparing a fly ash-based aerogel phase change material according to claim 6, characterized in that: The mass ratio of the nano-vermiculite to the mixed solution of sodium hydroxide and hydrogen peroxide in step S201 is 1:20, and the mass ratio of the nano-vermiculite to the silver nitrate solution in step S202 is 1:

30.

8. The method for preparing a fly ash-based aerogel phase change material according to claim 1, characterized in that: The mass ratio of n-hexane, trimethylchlorosilane and ethanol in step S5 is 10:1:30, and the mass ratio of the mixed solution of n-hexane, trimethylchlorosilane and ethanol to the filter residue used in step S3 is 20:

1.

9. Application of the fly ash-based aerogel phase change material prepared by the method for preparing a fly ash-based aerogel phase change material according to any one of claims 1 to 8 in thermal insulation materials.

Citation Information

Cited By

  • Composite phase change material with three-layer core-shell structure and preparation method of composite phase change material

    CN119505826A

  • Composite phase change material with three-layer core-shell structure and preparation method thereof

    CN119505826B

  • White carbon black extraction process

    CN120736533A

  • Fly ash low-temperature phase change microbead, preparation method and application thereof

    CN122625125A