Preparation method of floatable net-shaped water treatment material
By coating the silicon oxide film and cerium titanate film on the glass pipe network and modifying tin oxide, a mesh water treatment material with photocatalytic activity was prepared, which solved the problem that the material cannot be regenerated after adsorption and saturation in the prior art. It achieves continuous purification effect under light and is suitable for large-scale wastewater treatment.
Patent Information
- Application Number
- CN202411089772.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
AI Technical Summary
The existing mesh materials cannot continue to play a purification role after being saturated with adsorbed organic pollutants, and the regeneration process is complicated and is not suitable for large-scale continuous treatment of wastewater.
The glass tube network is coated with silicon oxide film and cerium titanate film and modified with tin oxide, and floating mesh water treatment material with a photocatalytic active layer is prepared. The material can degrade organic pollutants under light and avoid washing Remove treatment.
It realizes that the material continuously purifies organic pollutants in the water under light, is suitable for continuous treatment of large-scale wastewater, and has good structural stability and mechanical strength.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of environmental pollution purification materials, and in particular relates to a method for preparing a floating net-shaped water treatment material. Background Art
[0002] Organic pollutants in water mainly come from industrial and civil sewage. Toxic and harmful organic pollutants pose a huge threat to human health. Effective measures must be taken to purify them before they are discharged into environmental water bodies. Mesh materials play an important role in water pollution control. This material can be fixed in a water treatment device, and organic pollutants in the water can be removed when water flows through it. Mesh materials mainly remove organic pollutants in water by adsorption, and the strength of the adsorption capacity depends on the composition and structure of the mesh material. The main problem with the adsorption purification method is that the mesh material can no longer continue to play a purification role after it is saturated with organic matter. The commonly used method is to regenerate the mesh material, such as heating or using solvent elution. However, both of these regeneration methods require the mesh material to be removed from the wastewater, which increases the complexity of the operation and is not suitable for large-scale continuous wastewater treatment. Summary of the invention
[0003] In view of the problems existing in the prior art, the present invention aims to provide a method for preparing a floating mesh water treatment material, which can be used for purifying and treating organic pollutants in water.
[0004] The method for preparing the floating net-shaped water treatment material of the present invention comprises the following process steps:
[0005] Step 1: Silicon oxide membrane coated glass tube network
[0006] (1) Add 0.3-0.5 mL of concentrated hydrochloric acid to 20-22 mL of pure water and stir to form solution A;
[0007] (2) Add 130-165 mL of ethanol, 9.5-10.2 mL of tetraethyl silicate, and 3.1-3.3 mL of emulsifier OP-10 into a container and stir to form solution B;
[0008] (3) Solution A and solution B were mixed and stirred in a constant temperature water bath at 55° C. for 30 min to obtain silica sol;
[0009] (4) The glass tube network was immersed in silica sol for 5 minutes, taken out and allowed to stand for 15 minutes, dried at 80°C for 2 hours, and then calcined at 630-640°C for 2 hours to obtain a silicon oxide film-coated glass tube network.
[0010] Step 2: Prepare cerium titanate precursor
[0011] (1) Add 85-100 mL of ethanol, 3.5-3.8 mL of n-butyl titanate, and 5.2-5.5 mL of propylene glycol to a container in sequence and stir to form a solution C;
[0012] (2) Add 35-39 mL of pure water, 4.3-4.6 g of cerium nitrate hexahydrate, and 1.2-1.5 mL of concentrated hydrochloric acid into a container and stir to form a solution D;
[0013] (3) Solution D and solution C were mixed, placed in a constant temperature water bath at 55° C. and stirred for 30 min to obtain a cerium titanate precursor.
[0014] Step 3: Cerium titanate film coated glass tube network
[0015] (1) immersing the silicon oxide film-coated glass tube obtained in step 1 into a cerium titanate precursor, keeping it in a constant temperature water bath at 55° C. for 10 min, taking it out and letting it stand for 15 min;
[0016] (2) Dry the glass tube net treated in step 3 (1) at 85° C. for 2 h, and then calcine at 620-630° C. for 2 h to obtain a cerium titanate film-coated glass tube net.
[0017] Step 4: Tin Oxide Modification
[0018] (1) Add 56-65 mL of pure water, 3.8-4.5 g of stannous chloride, and 0.8-1.1 mL of concentrated hydrochloric acid into a container, stir to form a solution E, and keep it warm in a constant temperature water bath at 50°C;
[0019] (2) immersing the cerium titanate film-coated glass tube network prepared in step 3 into solution E for 10 min, taking it out and letting it stand for 15 min, and drying it at 115° C. for 1 h;
[0020] (3) Repeat step 4 (2) twice, and then calcine at 550-580° C. for 2 h to obtain a tin oxide-modified glass tube network, that is, a floating mesh water treatment material.
[0021] The glass tube network is a grid-shaped network formed by connecting closed glass tubes with a diameter of 7 mm, with a spacing of 5 mm between the glass tubes and a density of 0.6 g / cm 3 , the withstand temperature is not less than 660℃.
[0022] The various chemical raw materials are all pure materials.
[0023] The glass tube net is first coated with a silicon oxide film as a base film, and then a cerium titanate film is coated on the base film, and then the cerium titanate film is modified with tin oxide; the density of the prepared floating mesh water treatment material is 0.73-0.76 g / cm 3 .
[0024] The floatable mesh water treatment material prepared by the above method is composed of a glass tube network, a base film, and a photocatalytic active layer; the base film is a silicon oxide film coated on the glass tube network, and the photocatalytic active layer is coated on the base film; the photocatalytic active layer is composed of a cerium titanate film and tin oxide particles, wherein the cerium titanate film accounts for 3.5% to 3.8% of the mass percentage of the water treatment material, and the tin oxide particles account for 2.6% to 2.9% of the mass percentage of the water treatment material; the water treatment material maintains stable structure and performance when the temperature does not exceed 530°C.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] By optimizing the raw materials and preparation process, a coating with photocatalytic purification activity is prepared on the glass tube network. The composition ratio of the cerium titanate film and the tin oxide particles in the coating has been scientifically designed and optimized, and the unique preparation process is also a key factor in ensuring the stability of the material. The photocatalytic active coating has a strong bonding force with the glass tube network, good compatibility, and ideal mechanical strength. The floating mesh water treatment material has a low density, floats on the water surface during use, can fully receive light, and has a high photocatalytic purification activity. The material not only has a strong ability to adsorb organic pollutants in water, but also has the activity of degrading organic pollutants under light, and can be widely used in the purification of various organic pollutants in water. The organic pollutants adsorbed on the material can be decomposed in time under light, thereby releasing the material surface to continuously purify the organic pollutants in the water. There is no need to perform additional elution treatment on the material, which is suitable for large-scale continuous wastewater treatment. DETAILED DESCRIPTION
[0027] Example 1
[0028] Step 1: Silicon oxide membrane coated glass tube network
[0029] (1) Add 0.3 mL of concentrated hydrochloric acid to 20 mL of pure water and stir to form solution A;
[0030] (2) Add 130 mL of ethanol, 9.5 mL of tetraethyl silicate, and 3.1 mL of emulsifier OP-10 into a beaker and stir to form solution B;
[0031] (3) adding solution A to solution B and stirring in a constant temperature water bath at 55°C for 30 min to obtain silica sol;
[0032] (4) The glass tube network was immersed in silica sol for 5 minutes, taken out and allowed to stand for 15 minutes, dried at 80°C for 2 hours, and then calcined at 630°C for 2 hours to obtain a silicon oxide film-coated glass tube network.
[0033] Step 2: Prepare cerium titanate precursor
[0034] (1) Add 85 mL of ethanol, 3.5 mL of n-butyl titanate, and 5.2 mL of propylene glycol to a beaker and stir to form solution C;
[0035] (2) Add 35 mL of pure water, 4.3 g of cerium nitrate hexahydrate, and 1.2 mL of concentrated hydrochloric acid into a beaker and stir to form a solution D;
[0036] (3) Solution D was added to solution C, and the mixture was placed in a constant temperature water bath at 55° C. and stirred for 30 min to obtain a cerium titanate precursor.
[0037] Step 3: Cerium titanate film coated glass tube network
[0038] (1) immersing the silicon oxide film-coated glass tube obtained in step 1 into a cerium titanate precursor, keeping it in a constant temperature water bath at 55° C. for 10 min, taking it out and letting it stand for 15 min;
[0039] (2) The glass tube net treated in step 3 (1) was dried at 85° C. for 2 h, and then calcined at 620° C. for 2 h to obtain a cerium titanate film-coated glass tube net.
[0040] Step 4: Tin Oxide Modification
[0041] (1) Add 56 mL of pure water, 3.8 g of stannous chloride, and 0.8 mL of concentrated hydrochloric acid into a beaker, stir to form solution E, and keep warm in a constant temperature water bath at 50°C;
[0042] (2) immersing the cerium titanate film-coated glass tube network prepared in step 3 into solution E for 10 min, taking it out and letting it stand for 15 min, and drying it at 115° C. for 1 h;
[0043] (3) Repeat step 4 (2) twice, and then calcine at 550° C. for 2 h to obtain a tin oxide-modified glass tube network, which is a floating mesh water treatment material.
[0044] Example 2
[0045] Step 1: Silicon oxide membrane coated glass tube network
[0046] (1) Add 0.35 mL of concentrated hydrochloric acid to 20.5 mL of pure water and stir to form solution A;
[0047] (2) Add 135 mL of ethanol, 9.6 mL of tetraethyl silicate, and 3.1 mL of emulsifier OP-10 into a beaker and stir to form solution B;
[0048] (3) adding solution A to solution B and stirring in a constant temperature water bath at 55°C for 30 min to obtain silica sol;
[0049] (4) The glass tube network was immersed in silica sol for 5 minutes, taken out and allowed to stand for 15 minutes, dried at 80°C for 2 hours, and then calcined at 630°C for 2 hours to obtain a silicon oxide film-coated glass tube network.
[0050] Step 2: Prepare cerium titanate precursor
[0051] (1) Add 88 mL of ethanol, 3.6 mL of n-butyl titanate, and 5.2 mL of propylene glycol to a beaker in sequence and stir to form a solution C;
[0052] (2) Add 36 mL of pure water, 4.3 g of cerium nitrate hexahydrate, and 1.2 mL of concentrated hydrochloric acid into a beaker and stir to form a solution D;
[0053] (3) Solution D was added to solution C, and the mixture was placed in a constant temperature water bath at 55° C. and stirred for 30 min to obtain a cerium titanate precursor.
[0054] Step 3: Cerium titanate film coated glass tube network
[0055] (1) immersing the silicon oxide film-coated glass tube obtained in step 1 into a cerium titanate precursor, keeping it in a constant temperature water bath at 55° C. for 10 min, taking it out and letting it stand for 15 min;
[0056] (2) The glass tube net treated in step 3 (1) was dried at 85° C. for 2 h, and then calcined at 620° C. for 2 h to obtain a cerium titanate film-coated glass tube net.
[0057] Step 4: Tin Oxide Modification
[0058] (1) Add 58 mL of pure water, 3.9 g of stannous chloride, and 0.8 mL of concentrated hydrochloric acid into a beaker, stir to form solution E, and keep warm in a constant temperature water bath at 50°C;
[0059] (2) immersing the cerium titanate film-coated glass tube network prepared in step 3 into solution E for 10 min, taking it out and letting it stand for 15 min, and drying it at 115° C. for 1 h;
[0060] (3) Repeat step 4 (2) twice, and then calcine at 555° C. for 2 h to obtain a tin oxide-modified glass tube network, which is a floating mesh water treatment material.
[0061] Example 3
[0062] Step 1: Silicon oxide membrane coated glass tube network
[0063] (1) Add 0.4 mL of concentrated hydrochloric acid to 21 mL of pure water and stir to form solution A;
[0064] (2) Add 145 mL of ethanol, 9.8 mL of tetraethyl silicate, and 3.2 mL of emulsifier OP-10 into a beaker and stir to form solution B;
[0065] (3) adding solution A to solution B and stirring in a constant temperature water bath at 55°C for 30 min to obtain silica sol;
[0066] (4) The glass tube network was immersed in silica sol for 5 minutes, taken out and allowed to stand for 15 minutes, dried at 80°C for 2 hours, and then calcined at 635°C for 2 hours to obtain a silicon oxide film-coated glass tube network.
[0067] Step 2: Prepare cerium titanate precursor
[0068] (1) Add 92 mL of ethanol, 3.6 mL of n-butyl titanate, and 5.3 mL of propylene glycol to a beaker and stir to form a solution C;
[0069] (2) Add 37 mL of pure water, 4.4 g of cerium nitrate hexahydrate, and 1.3 mL of concentrated hydrochloric acid into a beaker and stir to form a solution D;
[0070] (3) Solution D was added to solution C, and the mixture was placed in a constant temperature water bath at 55° C. and stirred for 30 min to obtain a cerium titanate precursor.
[0071] Step 3: Cerium titanate film coated glass tube network
[0072] (1) immersing the silicon oxide film-coated glass tube obtained in step 1 into a cerium titanate precursor, keeping it in a constant temperature water bath at 55° C. for 10 min, taking it out and letting it stand for 15 min;
[0073] (2) The glass tube net treated in step 3 (1) was dried at 85° C. for 2 h, and then calcined at 625° C. for 2 h to obtain a cerium titanate film-coated glass tube net.
[0074] Step 4: Tin Oxide Modification
[0075] (1) Add 60 mL of pure water, 4.1 g of stannous chloride, and 0.9 mL of concentrated hydrochloric acid into a beaker, stir to form solution E, and keep warm in a constant temperature water bath at 50°C;
[0076] (2) immersing the cerium titanate film-coated glass tube network prepared in step 3 into solution E for 10 min, taking it out and letting it stand for 15 min, and drying it at 115° C. for 1 h;
[0077] (3) Repeat step 4 (2) twice, and then calcine at 565° C. for 2 h to obtain a tin oxide-modified glass tube network, which is a floating mesh water treatment material.
[0078] Example 4
[0079] Step 1: Silicon oxide membrane coated glass tube network
[0080] (1) Add 0.4 mL of concentrated hydrochloric acid to 21 mL of pure water and stir to form solution A;
[0081] (2) Add 160 mL of ethanol, 10 mL of tetraethyl silicate, and 3.2 mL of emulsifier OP-10 into a beaker and stir to form solution B;
[0082] (3) adding solution A to solution B and stirring in a constant temperature water bath at 55°C for 30 min to obtain silica sol;
[0083] (4) The glass tube network was immersed in silica sol for 5 minutes, taken out and allowed to stand for 15 minutes, dried at 80°C for 2 hours, and then calcined at 637°C for 2 hours to obtain a silicon oxide film-coated glass tube network.
[0084] Step 2: Prepare cerium titanate precursor
[0085] (1) Add 95 mL of ethanol, 3.7 mL of n-butyl titanate, and 5.4 mL of propylene glycol to a beaker and stir to form a solution C;
[0086] (2) Add 38 mL of pure water, 4.5 g of cerium nitrate hexahydrate, and 1.4 mL of concentrated hydrochloric acid into a beaker and stir to form a solution D;
[0087] (3) Solution D was added to solution C, and the mixture was placed in a constant temperature water bath at 55° C. and stirred for 30 min to obtain a cerium titanate precursor.
[0088] Step 3: Cerium titanate film coated glass tube network
[0089] (1) immersing the silicon oxide film-coated glass tube obtained in step 1 into a cerium titanate precursor, keeping it in a constant temperature water bath at 55° C. for 10 min, taking it out and letting it stand for 15 min;
[0090] (2) The glass tube net treated in step 3 (1) was dried at 85° C. for 2 h, and then calcined at 627° C. for 2 h to obtain a cerium titanate film-coated glass tube net.
[0091] Step 4: Tin Oxide Modification
[0092] (1) Add 62 mL of pure water, 4.2 g of stannous chloride, and 1.0 mL of concentrated hydrochloric acid into a beaker, stir to form solution E, and keep warm in a constant temperature water bath at 50°C;
[0093] (2) immersing the cerium titanate film-coated glass tube network prepared in step 3 into solution E for 10 min, taking it out and letting it stand for 15 min, and drying it at 115° C. for 1 h;
[0094] (3) Repeat step 4 (2) twice, and then calcine at 570° C. for 2 h to obtain a tin oxide-modified glass tube network, which is a floating mesh water treatment material.
[0095] Example 5
[0096] Step 1: Silicon oxide membrane coated glass tube network
[0097] (1) Add 0.5 mL of concentrated hydrochloric acid to 22 mL of pure water and stir to form solution A;
[0098] (2) Add 165 mL of ethanol, 10.2 mL of tetraethyl silicate, and 3.3 mL of emulsifier OP-10 into a beaker and stir to form solution B;
[0099] (3) adding solution A to solution B and stirring in a constant temperature water bath at 55°C for 30 min to obtain silica sol;
[0100] (4) The glass tube network was immersed in silica sol for 5 minutes, taken out and allowed to stand for 15 minutes, dried at 80°C for 2 hours, and then calcined at 640°C for 2 hours to obtain a silicon oxide film-coated glass tube network.
[0101] Step 2: Prepare cerium titanate precursor
[0102] (1) Add 100 mL of ethanol, 3.8 mL of n-butyl titanate, and 5.5 mL of propylene glycol to a beaker in sequence and stir to form solution C;
[0103] (2) Add 39 mL of pure water, 4.6 g of cerium nitrate hexahydrate, and 1.5 mL of concentrated hydrochloric acid into a beaker and stir to form a solution D;
[0104] (3) Solution D was added to solution C, and the mixture was placed in a constant temperature water bath at 55° C. and stirred for 30 min to obtain a cerium titanate precursor.
[0105] Step 3: Cerium titanate film coated glass tube network
[0106] (1) immersing the silicon oxide film-coated glass tube obtained in step 1 into a cerium titanate precursor, keeping it in a constant temperature water bath at 55° C. for 10 min, taking it out and letting it stand for 15 min;
[0107] (2) The glass tube net treated in step 3 (1) was dried at 85° C. for 2 h, and then calcined at 630° C. for 2 h to obtain a cerium titanate film-coated glass tube net.
[0108] Step 4: Tin Oxide Modification
[0109] (1) Add 65 mL of pure water, 4.5 g of stannous chloride, and 1.1 mL of concentrated hydrochloric acid into a beaker, stir to form solution E, and keep warm in a constant temperature water bath at 50°C;
[0110] (2) immersing the cerium titanate film-coated glass tube network prepared in step 3 into solution E for 10 min, taking it out and letting it stand for 15 min, and drying it at 115° C. for 1 h;
[0111] (3) Repeat step 4 (2) twice, and then calcine at 580° C. for 2 h to obtain a tin oxide-modified glass tube network, which is a floating mesh water treatment material.
[0112] The above descriptions are merely embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any equivalent transformations made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the protection scope of the present invention.
Claims
1. A method for preparing a floating net-shaped water treatment material, It is characterized in that The process includes the following steps: Step 1: Silicon oxide membrane coated glass tube network (1) Add 0.3-0.5 mL of concentrated hydrochloric acid to 20-22 mL of pure water and stir to form solution A; (2) Add 130-165 mL of ethanol, 9.5-10.2 mL of tetraethyl silicate, and 3.1-3.3 mL of emulsifier OP-10 into a container and stir to form solution B; (3) Solution A and solution B were mixed and stirred in a constant temperature water bath at 55° C. for 30 min to obtain silica sol; (4) immersing the glass tube network in silica sol for 5 minutes, taking it out and letting it stand for 15 minutes, drying it at 80° C. for 2 hours, and then calcining it at 630-640° C. for 2 hours to obtain a silicon oxide film-coated glass tube network; Step 2: Prepare cerium titanate precursor (1) Add 85-100 mL of ethanol, 3.5-3.8 mL of n-butyl titanate, and 5.2-5.5 mL of propylene glycol to a container in sequence and stir to form a solution C; (2) Add 35-39 mL of pure water, 4.3-4.6 g of cerium nitrate hexahydrate, and 1.2-1.5 mL of concentrated hydrochloric acid into a container and stir to form a solution D; (3) Solution D and Solution C were mixed, placed in a constant temperature water bath at 55° C. and stirred for 30 min to obtain a cerium titanate precursor; Step 3: Cerium titanate film coated glass tube network (1) immersing the silicon oxide film-coated glass tube obtained in step 1 into a cerium titanate precursor, keeping it in a constant temperature water bath at 55° C. for 10 min, taking it out and letting it stand for 15 min; (2) drying the glass tube net treated in step 3 (1) at 85° C. for 2 h, and then calcining at 620-630° C. for 2 h to obtain a cerium titanate film-coated glass tube net; Step 4: Tin Oxide Modification (1) Add 56-65 mL of pure water, 3.8-4.5 g of stannous chloride, and 0.8-1.1 mL of concentrated hydrochloric acid into a container, stir to form a solution E, and keep it warm in a constant temperature water bath at 50°C; (2) immersing the cerium titanate film-coated glass tube network prepared in step 3 into solution E for 10 min, taking it out and letting it stand for 15 min, and drying it at 115° C. for 1 h; (3) Repeat step 4 (2) twice, and then calcine at 550-580° C. for 2 h to obtain a tin oxide-modified glass tube network, that is, a floating mesh water treatment material.
2. A method for preparing a floating net-shaped water treatment material according to claim 1, It is characterized in that The glass tube network used for immersion in silica sol in step 1 is a grid-shaped network formed by connecting closed glass tubes with a diameter of 7 mm, with a spacing of 5 mm between the glass tubes and a density of 0.6 g / cm 3 , the withstand temperature is not less than 660℃.
3. A method for preparing a floating net-shaped water treatment material according to claim 1, It is characterized in that The glass tube net is first coated with a silicon oxide film as a base film, and then coated with a cerium titanate film on the base film, and then the cerium titanate film is modified with tin oxide.
4. The method for preparing a floating net-shaped water treatment material according to claim 1, It is characterized in that The density of the floating net-shaped water treatment material is 0.73-0.76 g / cm 3 .
5. A floating mesh water treatment material, It is characterized in that The floating mesh water treatment material is prepared by the method described in any one of claims 1 to 4, and is composed of a glass tube network, a base membrane, and a photocatalytic active layer; the base membrane is a silicon oxide film coated on the glass tube network, and the photocatalytic active layer is coated on the base membrane; the photocatalytic active layer is composed of a cerium titanate film and tin oxide particles.
6. A floating net-like water treatment material according to claim 5, It is characterized in that The mass percentage of the cerium titanate film in the water treatment material is 3.5% to 3.8%, and the mass percentage of the tin oxide particles in the water treatment material is 2.6% to 2.9%.
7. A floating net-like water treatment material according to claim 5, It is characterized in that The floatable net-like water treatment material maintains stable structure and performance at a temperature not exceeding 530°C.
Citation Information
Patent Citations
Photocatalysis oxidation treated high concentration organic trade waste
CN101219371A
Monoclinic CeTi2O6 thin film and sol-gel process for the preparation thereof
CN101400822A
Complex multi-functional indoor air pollution control unit
CN104422019A
Photocatalytic net for purifying water and preparation and application of photocatalytic net
CN109603794A
Photocatalytic filter screen, air purifier and preparation method of photocatalytic filter screen
CN113617347A