Amorphous carbon material as well as preparation method and application thereof

By designing semiconductor catalyst materials at the edge position and a catalyst with strong electron separation capability, the problems of high energy consumption and carbon emissions in the CO2 cycloaddition reaction are solved, and the effect of efficient synthesis of styrene carbonate at room temperature is achieved.

CN118925706APending Publication Date: 2024-11-12UNIV OF SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410976949.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art requires high temperature and high air pressure in CO2 cycloaddition reaction, resulting in high energy consumption and increased carbon emissions, and traditional catalyst designs are difficult to effectively promote the reaction speed-determination process.

Method used

Design a semiconductor catalyst material with suitable band edge positions, generate electrons through photoexcitation to transform CO2 into anionic radical, and use a catalyst with strong electron separation ability to accelerate the breaking of the C-O bond under light conditions to reduce the reaction activation energy.

Benefits of technology

The efficient synthesis of styrene carbonate at room temperature and pressure is achieved, the product yield is improved, and the reaction is promoted through the high specific surface area and charge conduction ability of the amorphous carbon material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925706A_ABST
    Figure CN118925706A_ABST
Patent Text Reader

Abstract

The invention is suitable for the technical field of chemistry, and provides a preparation method of an amorphous carbon material, which comprises the following steps: adding a metal salt into an alcohol solvent, and fully stirring to completely dissolve the metal salt; adding the chelating ligand into an alcohol solvent, and fully stirring to completely dissolve the chelating ligand; fully grinding the polymerization carrier to enable the texture to be fine and uniform; adding the solution into a polymerization carrier, and grinding to obtain a raw material precursor; transferring the raw material precursor into a ceramic boat, then putting the ceramic boat into a closed tubular furnace, firstly introducing a carrier gas shielding gas, and then heating and calcining to obtain a primary material; and washing and drying the primary material to obtain the amorphous carbon material. The invention also provides an amorphous carbon material. The invention also provides an application of the amorphous carbon material as a catalyst in direct synthesis of styrene carbonate by photocatalytic oxidation of styrene and carbon dioxide. The carbon-based bio-enzyme-like metal monatomic material is effectively prepared in a mode of high-temperature thermal polymerization of the metal salt and the chelating ligand, and the carbon-based bio-enzyme-like metal monatomic material is prepared by constructing a precisely coordinated bio-enzyme-like metal monatomic active center and utilizing the strong light-generated electron separation capacity of the monatomic center. According to the present invention, the adsorption and the activation of carbon dioxide and styrene oxide molecules are promoted, the activation energy barrier of the reaction is reduced, the high specific surface area and the charge conduction capability of the amorphous carbon substrate are adopted to achieve the photocatalytic efficient synthesis of styrene carbonate at the normal temperature and the normal pressure, and the yield of the product styrene carbonate is substantially improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical technology, and in particular relates to an amorphous carbon material and a preparation method and application thereof. Background Art

[0002] Excessive CO2 emissions have led to global warming, melting of polar glaciers, ocean acidification and many other problems. Converting CO2 into high value-added chemicals and achieving rapid decarbonization in industrial processes can reduce the concentration of CO2 in the atmosphere and achieve carbon cycle. CO2 reduction reaction (CRR) and non-oxidative CO2 chemical fixation are two main pathways. In addition, CO2 is reduced to C l Compared with chemicals (such as methanol, methane or formate), non-redox CO2 chemical fixation provides a potential path for high value-added multi-carbon products. In the non-redox strategy, cyclic carbonate compounds have high product value and many application pathways in the industrial field, including being widely used as aprotic polar solvents, electrolytes in lithium-ion batteries, and raw materials for the synthesis of polycarbonate. At present, CO2 cycloaddition reactions in industry are mainly achieved by thermal catalysis, which often requires relatively harsh reaction conditions (high reaction temperature and high gas pressure). Such reaction processes also face problems such as high energy consumption and increased carbon emissions. Based on this, it is of great significance to develop and explore the use of clean energy and realize the synthesis of cyclic carbonates under mild conditions.

[0003] Among many cyclic carbonates, styrene carbonate is one of the most important chemicals with the greatest industrial application value. The market value of styrene carbonate prepared by the reaction of CO2 and styrene oxide is dozens of times higher than that of the raw material styrene oxide. As an important raw material in the field of energy and chemical industry, styrene carbonate needs to maintain high temperature during the ester exchange reaction process of the traditional industrial synthesis route, and dimethyl carbonate, which is the raw material for ester exchange, is also expensive. Therefore, using the inexhaustible energy of sunlight to directly synthesize styrene carbonate from styrene oxide and carbon dioxide through a more mild and environmentally friendly photocatalytic method has great application prospects, and this field has become a key research direction in recent years.

[0004] Photocatalytic technology can convert renewable solar energy into chemical energy, providing a very promising way for the utilization of CO2. So far, the feasibility of photocatalytic CO2 reduction to prepare other carbon-containing organic matter has been widely demonstrated, while there are few reports on the chemical fixation of CO2 by non-redox methods. For example, the design of efficient catalysts and mechanism research for the synthesis of styrene carbonate by photocatalytic CO2 cycloaddition have yet to be developed. In fact, the energy consumption source and rate-determining step of the CO2 cycloaddition reaction mainly come from the two elementary reaction steps of the epoxide itself being attacked by the halogen anion in the nucleophile and the CO2 attacking and inserting into the ring-opened epoxide. If the rate-determining step in these two steps can be promoted by photocatalysis, the entire reaction can be effectively promoted. Therefore, by designing semiconductor catalyst materials with suitable band edge positions, the electrons generated under suitable photoexcitation conditions can realize the conversion of CO2 to ·CO2 - The transformation of anionic radicals, and such highly active radical ions have the hope of overcoming the high energy barrier in the CO2 attack process; or designing a catalyst with strong electron separation ability under light conditions, so that under light excitation conditions, it can directly inject photogenerated electrons into the epoxide molecules adsorbed on the active sites, thereby weakening the CO bond and accelerating its bond breaking and ring opening process. Therefore, how to design and develop catalysts with high potential for photocatalytic CO2 cycloaddition is very critical. Summary of the invention

[0005] The purpose of the embodiments of the present invention is to provide a method for preparing an amorphous carbon material, aiming to solve the problems existing in the above-mentioned background technology.

[0006] The embodiment of the present invention is implemented as follows: a method for preparing an amorphous carbon material comprises the following steps: S1. Add the metal salt into the alcohol solvent and stir thoroughly to make it completely dissolved; S2, adding the chelating ligand into the alcohol solvent and stirring it thoroughly to make it completely dissolved; S3, grinding the polymer carrier fully to make it fine and uniform in texture; S4, adding the solutions in steps S1 and S2 to the polymer carrier in step S3, grinding to fully disperse them in the polymer carrier, and obtaining a raw material precursor; S5, transferring the raw material precursor in step S4 into a ceramic boat, then placing the ceramic boat in a closed tube furnace, first continuously introducing a carrier gas and protective gas to replace the internal air, then heating and calcining it to coordinate and crack it to obtain an amorphous carbon preliminary material with a biological enzyme-like metal single atom active center; S6. Wash the preliminary amorphous carbon material obtained in step S5 with ethanol and deionized water for multiple times, respectively, and dry to obtain an amorphous carbon material with a biological enzyme-like metal single atom active center.

[0007] Preferably, in S1, the metal salt is one or more of nitrate, chloride, carbonate, acetate, sulfate, and acetylacetonate; and the alcohol solvent is one or more of ethanol, methanol, and n-propanol.

[0008] Preferably, in S2, the chelating ligand is one or more of 1,10-phenanthroline, 2,2'-bipyridine, and 4,4'-bipyridine; the alcohol solvent is one or more of ethanol, methanol, and n-propanol; and the molar ratio of the chelating ligand to the metal salt is 4-1:1.

[0009] Preferably, in S3, the polymer carrier is one or more of melamine, urea, and dicyandiamide; and the molar ratio of the polymer carrier to the metal salt is 20-5:1.

[0010] Preferably, in S4, the grinding is performed by ball milling, the ball milling speed is 40-80 r / min, and the ball milling time is 1-3 h.

[0011] Preferably, in S5, the carrier gas shielding gas is one or a combination of nitrogen, argon, and helium, and the replacement time is 0.5-2h; the temperature rising process is a linear program temperature rising until the reaction temperature is reached, the reaction temperature is 700-900°C, the heating rate is 2-5°C / min, and the reaction time is 4-6h.

[0012] Preferably, in S6, the drying temperature is 55-85°C, and the drying time is 12-24h; the coordination structure of the metal center of the amorphous carbon material catalyst with the bio-enzyme-like metal single-atom active center is a tetracoordinate structure of any combination of nitrogen or carbon.

[0013] Another object of an embodiment of the present invention is to provide an amorphous carbon material, which is prepared by the above preparation method.

[0014] Another object of the embodiment of the present invention is to provide an application of the above-mentioned amorphous carbon material as a catalyst in the direct synthesis of styrene carbonate by photocatalytic oxidation of styrene and carbon dioxide, comprising the following steps: S1. Adding an amorphous carbon material as a catalyst into a transparent reaction bottle containing styrene oxide, and obtaining a uniformly dispersed mixed solution through ultrasonic treatment; S2, adding a nucleophile to the mixed solution in S1 and dissolving it completely by ultrasound; S3, continuously introducing an inert gas into the mixed solution in S2 to remove the air dissolved in the reaction flask and the mixed solution to obtain a mixed solution to be reacted; S4, placing a magnetic stirrer in the reaction bottle containing the reaction mixture in S3, sealing the bottle mouth, and introducing high-purity carbon dioxide gas to replace the inert gas therein, and then connecting a retractable container filled with carbon dioxide to the sealed bottle mouth; S5. Set the speed of the magnetic stirrer, turn on the xenon lamp light source, adjust the light power density and illumination time, and let the light shine perpendicularly to the wall of the transparent reaction bottle to start the catalytic reaction; S6. The mixed solution after the reaction in S5 is separated by high-speed centrifugation to obtain a supernatant, i.e., a product solution.

[0015] Preferably, in S1 and S2, the frequency of the ultrasound is 60-120 kHz, and the duration of the ultrasound is 10-30 min; In S2, the nucleophilic reagent is one of tetra-n-butylammonium bromide and tetra-n-butylammonium chloride, or a mixture of the two; In S3, the inert gas is one or more of argon, helium, and nitrogen, the ventilation rate is 5-50 mL / min, and the ventilation time is 10-30 min; In S4, the time for introducing high-purity carbon dioxide gas is 5-10 minutes, and the pressure is 0.1-0.5 MPa; In S5, the speed of the magnetic stirrer is 500-1200 r / min, and the optical power density is 1-5 W / cm 2 , the photoperiod is 6-24 h; In S6, the centrifugation time is 5-10 min, and the rotation speed is 12000-16000 r / min.

[0016] A method for preparing an amorphous carbon material provided in an embodiment of the present invention realizes the effective preparation of a carbon-based bio-enzyme-like metal single-atom material by high-temperature thermal polymerization of a metal salt and a chelating ligand. The single-atom site can be various transition metal elements and different coordination structures. By constructing a precisely coordinated bio-enzyme-like metal single-atom active center and utilizing the strong photogenerated electron separation ability of the single-atom center, the adsorption and activation of carbon dioxide and styrene oxide molecules are promoted, the activation energy barrier of the reaction is reduced, and the high specific surface area and charge conduction ability of the amorphous carbon substrate are used to realize the photocatalytic efficient synthesis of styrene carbonate at room temperature and pressure, ultimately achieving a significant increase in the yield of the product styrene carbonate. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 A scanning electron microscope analysis diagram of an amorphous carbon material provided in Example 1 of the present invention; Figure 2 A spherical aberration-corrected transmission electron microscope analysis diagram of an amorphous carbon material provided in Example 1 of the present invention; Figure 3 This is a hydrogen nuclear magnetic resonance spectrum analysis diagram of the product provided in Example 2 of the present invention; Figure 4 This is a hydrogen nuclear magnetic resonance spectrum analysis diagram of the product provided in Example 3 of the present invention. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0019] An amorphous carbon material, the preparation method of which comprises the following steps: S1. Add a metal salt to an alcohol solvent and stir to completely dissolve it, wherein the metal salt is one or more of nitrate, chloride, carbonate, acetate, sulfate, and acetylacetonate, and the alcohol solvent is one or more of ethanol, methanol, and n-propanol, and the concentration of the metal salt in the alcohol solvent is 0.01-1 mol / L, and the volume of the solvent is 0.1-100 L; S2, adding a chelating ligand to an alcohol solvent and stirring to completely dissolve it, wherein the chelating ligand is one or more of 1,10-phenanthroline, 2,2'-bipyridine, and 4,4'-bipyridine, and the alcohol solvent is one or more of ethanol, methanol, and n-propanol, and the concentration of the chelating ligand in the alcohol solvent is 0.01-4 mol / L, the volume of the solvent is 0.1-100 L, and the molar ratio of the chelating ligand to the metal salt is 4-1:1; S3, putting the polymer carrier into a ball mill, grinding it vigorously to make it fine and uniform, the polymer carrier is one or more of melamine, urea, dicyandiamide, the amount of the polymer carrier added is 10-500 g, and the molar ratio of the polymer carrier to the metal salt is 20-5:1; S4, adding the solution in step S1 and S2 to the ball mill in step S3, grinding and dispersing vigorously to obtain a raw material precursor, the ball mill material can be agate, stainless steel, metal alloy, the ball mill speed is 40-80 r / min, and the ball milling time is 1-3h; S5. Transfer the raw material precursor in step S4 to a ceramic boat and then place the ceramic boat in a closed tubular furnace, first continuously introduce a carrier gas protective gas to replace the internal air, then increase the temperature and calcine it to coordinate and decompose it to obtain an amorphous carbon preliminary material with a biological enzyme-like metal single atom active center, wherein the carrier gas protective gas is one or a combination of nitrogen, argon, and helium, the nitrogen replacement time is 0.5-2 h, the calcination temperature is 700-900 ° C, the calcination time is 4-6 h, the heating method is programmed heating, and the heating rate is 2-5 ° C / min.

[0020] S6. Wash the product obtained in step S5 with ethanol and deionized water for three times respectively, and obtain an amorphous carbon material containing enzyme-like metal single atoms after drying. The drying temperature is 55-85°C, and the drying time is 12-24h. The mass of the obtained amorphous carbon material containing enzyme-like metal single atom active centers is 0.1-1000 g, and the coordination structure of the metal center is a tetracoordinate structure of any combination of nitrogen or carbon.

[0021] The method for synthesizing styrene carbonate by photocatalytically oxidizing styrene and carbon dioxide using an amorphous carbon material containing a biological enzyme-like metal single atom as a catalyst comprises the following steps: S1. Adding an amorphous carbon material containing a biological enzyme-like metal single atom active center as a catalyst into a transparent reaction bottle containing styrene oxide, and obtaining a uniformly dispersed mixed solution through ultrasound, wherein the mass of the amorphous carbon material containing a biological enzyme-like metal single atom active center is 10-1000 mg, the volume of the styrene oxide is 1-20 mL, the frequency of ultrasound is 60-120 kHz, the duration of ultrasound is 10-30 min, and the transparent reaction bottle can be made of a highly light-transmitting material such as quartz, crystal, or glass; S2, adding a nucleophilic reagent to the mixed solution in S1, and dissolving it completely by ultrasound, wherein the nucleophilic reagent is one or a mixture of tetra-n-butylammonium bromide and tetra-n-butylammonium chloride, the amount of the nucleophilic reagent added is 10-100 mg, the frequency of ultrasound is 60-120 kHz, and the duration of ultrasound is 10-30 min; S3, continuously introducing an inert gas into the mixed solution in S2 to remove the air dissolved in the reaction flask and the mixed solution to obtain a mixed solution to be reacted, wherein the inert gas is one or more of argon, helium, and nitrogen, the ventilation rate is 5-50 mL / min, and the ventilation time is 10-30 min; S4, placing a magnetic stirrer in the reaction bottle containing the liquid to be reacted in S3 and sealing the bottle mouth, and passing high-purity carbon dioxide gas into the bottle for a certain period of time to replace the inert gas therein, and then connecting a retractable container filled with carbon dioxide to the sealed bottle mouth, wherein the ventilation time is 5-10 minutes, the pressure of the carbon dioxide gas is 0.1-0.5 MPa, the retractable container can be an air bag, a balloon, a syringe, etc., and the sealing method can be plastic, rubber, sealing film, etc.; S5. Set the speed of the magnetic stirrer, turn on the xenon lamp light source, adjust the light power density and illumination time, and let the light shine perpendicularly to the wall of the transparent reaction bottle to start the catalytic reaction. The speed is 500-1200 r / min, the light source is a full-spectrum xenon lamp light source close to the solar spectrum, and the light power density is 1-5 W / cm 2 , the photoperiod is 6-24h; S6. After the reaction in S5 is completed, the mixed solution is subjected to high-speed centrifugation for a certain period of time to obtain a supernatant, i.e., a product solution, wherein the centrifugation time is 5-10 min and the rotation speed is 12000-16000 r / min.

[0022] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0023] An amorphous carbon material having a bio-enzyme-like zinc single-atom active center, wherein the preparation method thereof comprises the following steps: S1. Add 1 mmol of zinc nitrate into 6 mL of ethanol and completely dissolve it by magnetic stirring for 10 min at a stirring rate of 800 r / min. S2, add 2.5 mmol of 1,10-phenanthroline to 6 mL of ethanol and completely dissolve it by magnetic stirring for 10 min at a stirring rate of 800 r / min; S3, add 20 mmol of melamine into the ball mill and grind it thoroughly to make it fine and uniform. The ball milling speed is 60 r / min and the ball milling time is 1 h. S4, adding the solution obtained in step S1 and step S2 into the ball milling tank of step S3, and continuing to grind until the ethanol evaporates naturally, so that the zinc nitrate and 1,10-phenanthroline are fully dispersed, the ball milling speed is 60 r / min, and the ball milling time is 6 hours, to obtain a raw material precursor; S5, transferring the raw material precursor obtained in step S4 into a ceramic boat, then placing it in a closed tube furnace, continuously introducing nitrogen protective gas at 10 mL / min for 1 h to replace the internal air, then heating to 800 °C at a heating rate of 5 °C / min, and continuously calcining for 4 h to obtain a preliminary product of an amorphous carbon material with a single-atom active center of bio-enzyme-like zinc; S6. The preliminary product obtained in step S5 was washed three times with ethanol and deionized water respectively, and dried at 80° C. for 24 h to obtain 0.4 g of amorphous carbon material with a single-atom active center of zinc similar to that of biological enzymes.

[0024] The morphology and single-atom characteristics of the amorphous carbon material prepared in Example 1 were analyzed, and the analysis diagrams were obtained as follows: Figure 1 and Figure 2 As shown, according to Figure 1 It can be seen that the obtained amorphous carbon material containing the enzyme-like zinc single-atom active center has only one morphology, which is an amorphous wrinkled shape; Figure 2 It can be seen that the corresponding zinc single atom dispersion structure is composed of independent bright spots in the spherical aberration corrected transmission electron microscopy analysis image. Example 2

[0025] A method for directly synthesizing styrene carbonate by photocatalytically oxidizing styrene and carbon dioxide using the amorphous carbon material containing a bio-enzyme-like zinc single-atom active center prepared in Example 1 as a catalyst comprises the following steps: S1. Take 0.01 g of the amorphous carbon material containing the bio-enzyme-like zinc single-atom active center prepared in Example 1 and add it to a transparent quartz bottle containing 2 mL of styrene oxide, and ultrasonicate at a frequency of 120 kHz for 20 min to obtain a uniformly dispersed mixed solution; S2, add 0.02 mg of tetra-n-butylammonium bromide to the mixed solution in S1, and sonicate at a frequency of 120 kHz for 10 min to completely dissolve it; S3, passing argon gas at 20 mL / min to remove the air dissolved in styrene oxide to obtain a mixed solution to be reacted; S4, placing a magnetic stirrer in the quartz bottle containing the reaction solution in S3 and sealing the bottle mouth, and passing high-purity carbon dioxide gas into the bottle for 10 minutes to replace the inert gas therein, and then connecting a balloon filled with carbon dioxide to the sealed bottle mouth; S5. Set the speed of the magnetic stirrer to 600 r / min, turn on the xenon lamp light source and adjust the light power density to 1 W / cm 2 , the illumination time was set to 12 h, and the light was irradiated perpendicularly to the wall of the quartz bottle to start the photocatalytic reaction; S6. Centrifuge the reaction solution obtained in S5 at 14000 r / min for 5 min, and take the supernatant to obtain the product styrene carbonate.

[0026] The yield of the product prepared in Example 2 was analyzed by hydrogen nuclear magnetic resonance spectroscopy. Figure 3 As shown, according to Figure 3 It can be seen that the selectivity of the amorphous carbon material containing a bio-enzyme-like zinc single-atom active center as a catalyst for the photocatalytic oxidation of styrene and carbon dioxide to synthesize styrene carbonate is 100%, no signal peaks of other by-products are detected, and the mass conversion rate of styrene carbonate relative to styrene oxide is 10.1%. Example 3

[0027] A method for directly synthesizing styrene carbonate by photocatalytically oxidizing styrene and carbon dioxide using the amorphous carbon material containing a bio-enzyme-like zinc single-atom active center prepared in Example 1 as a catalyst comprises the following steps: S1. Take 0.02 g of the amorphous carbon material containing the bio-enzyme-like zinc single-atom active center prepared in Example 1 and add it to a transparent quartz bottle containing 3 mL of styrene oxide, and ultrasonicate at a frequency of 100 kHz for 15 min to obtain a uniformly dispersed mixed solution; S2, add 0.05 mg of tetra-n-butylammonium bromide to the mixture in S1, and sonicate at a frequency of 110 kHz for 8 min to completely dissolve it; S3, passing argon gas at 15 mL / min to remove the air dissolved in styrene oxide to obtain a mixed solution to be reacted; S4, placing a magnetic stirrer in the quartz bottle containing the reaction solution in S3 and sealing the bottle mouth, and passing high-purity carbon dioxide gas into the bottle for 15 minutes to replace the inert gas therein, and then connecting a balloon filled with carbon dioxide to the sealed bottle mouth; S5. Set the speed of the magnetic stirrer to 800 r / min, turn on the xenon lamp light source and adjust the light power density to 2 W / cm 2 , the illumination time was set to 24 h, and the light was irradiated perpendicularly to the wall of the quartz bottle to start the photocatalytic reaction; S6. Centrifuge the reaction solution obtained in S5 at 16000 r / min for 10 min, and take the supernatant to obtain the product styrene carbonate.

[0028] The yield of the product prepared in Example 3 was analyzed by hydrogen nuclear magnetic resonance spectroscopy. Figure 4 As shown, according to Figure 4It can be seen that the selectivity of the amorphous carbon material containing a bio-enzyme-like zinc single-atom active center as a catalyst for the photocatalytic oxidation of styrene and carbon dioxide to synthesize styrene carbonate is 100%, no signal peaks of other by-products are detected, and the mass conversion rate of styrene carbonate relative to styrene oxide is 41.9%.

[0029] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an amorphous carbon material, characterized in that: The following steps are involved: S1. Add the metal salt into the alcohol solvent and stir thoroughly to make it completely dissolved; S2, adding the chelating ligand into the alcohol solvent and stirring it thoroughly to make it completely dissolved; S3, grinding the polymer carrier fully to make it fine and uniform in texture; S4, adding the solutions in steps S1 and S2 to the polymer carrier in step S3, grinding to fully disperse them in the polymer carrier, and obtaining a raw material precursor; S5, transferring the raw material precursor in step S4 into a ceramic boat, then placing the ceramic boat in a closed tube furnace, first continuously introducing a carrier gas and protective gas to replace the internal air, then heating and calcining it to coordinate and crack it to obtain an amorphous carbon preliminary material with a biological enzyme-like metal single atom active center; S6. Wash the preliminary amorphous carbon material obtained in step S5 with ethanol and deionized water for multiple times, respectively, and dry to obtain an amorphous carbon material with a biological enzyme-like metal single atom active center.

2. The method for preparing an amorphous carbon material according to claim 1, characterized in that: In S1, the metal salt is one or more of nitrate, chloride, carbonate, acetate, sulfate, and acetylacetonate; and the alcohol solvent is one or more of ethanol, methanol, and n-propanol.

3. The method for preparing an amorphous carbon material according to claim 1, characterized in that: In S2, the chelating ligand is one or more of 1,10-phenanthroline, 2,2'-bipyridine, and 4,4'-bipyridine; the alcohol solvent is one or more of ethanol, methanol, and n-propanol; and the molar ratio of the chelating ligand to the metal salt is 4-1:

1.

4. The method for preparing an amorphous carbon material according to claim 1, characterized in that: In S3, the polymer carrier is one or more of melamine, urea, and dicyandiamide; and the molar ratio of the polymer carrier to the metal salt is 20-5:

1.

5. The method for preparing an amorphous carbon material according to claim 1, characterized in that: In S4, the grinding is performed by ball milling, the ball milling speed is 40-80 r / min, and the ball milling time is 1-3 h.

6. The method for preparing an amorphous carbon material according to claim 1, characterized in that: In S5, the carrier gas protection gas is one or a combination of nitrogen, argon, and helium, and the replacement time is 0.5-2h; the temperature rising process is a linear program temperature rising until the reaction temperature is reached, the reaction temperature is 700-900°C, the heating rate is 2-5°C / min, and the reaction time is 4-6h.

7. The method for preparing an amorphous carbon material according to claim 1, characterized in that: In S6, the drying temperature is 55-85°C and the drying time is 12-24h; the coordination structure of the metal center of the amorphous carbon material with a biological enzyme-like metal single atom active center is a tetra-coordinate structure of any combination of nitrogen or carbon.

8. An amorphous carbon material, characterized in that The invention is prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the amorphous carbon material as claimed in claim 8 as a catalyst for direct synthesis of styrene carbonate by photocatalytic oxidation of styrene and carbon dioxide, characterized in that: The following steps are involved: S1. Adding an amorphous carbon material as a catalyst into a transparent reaction bottle containing styrene oxide, and obtaining a uniformly dispersed mixed solution through ultrasonic treatment; S2, adding a nucleophile to the mixed solution in S1 and dissolving it completely by ultrasound; S3, continuously introducing an inert gas into the mixed solution in S2 to remove the air dissolved in the reaction flask and the mixed solution to obtain a mixed solution to be reacted; S4, placing a magnetic stirrer in the reaction bottle containing the reaction mixture in S3, sealing the bottle mouth, and introducing high-purity carbon dioxide gas to replace the inert gas therein, and then connecting a retractable container filled with carbon dioxide to the sealed bottle mouth; S5. Set the speed of the magnetic stirrer, turn on the xenon lamp light source, adjust the light power density and illumination time, and let the light shine perpendicularly to the wall of the transparent reaction bottle to start the catalytic reaction; S6. The mixed solution after the reaction in S5 is separated by high-speed centrifugation to obtain a supernatant, i.e., a product solution.

10. The use according to claim 9, characterized in that: In S1 and S2, the ultrasound frequency is 60-120 kHz, and the ultrasound duration is 10-30 min; In S2, the nucleophilic reagent is one of tetra-n-butylammonium bromide and tetra-n-butylammonium chloride, or a mixture of the two; In S3, the inert gas is one or more of argon, helium, and nitrogen, the ventilation rate is 5-50 mL / min, and the ventilation time is 10-30 min; In S4, the time for introducing high-purity carbon dioxide gas is 5-10 minutes, and the pressure is 0.1-0.5 MPa; In S5, the speed of the magnetic stirrer is 500-1200 r / min, and the optical power density is 1-5 W / cm 2 , the photoperiod is 6-24 h; In S6, the centrifugation time is 5-10 min, and the rotation speed is 12000-16000 r / min.