Method for recycling waste photovoltaic module
By pressurizing and laying the fiber cotton layer on the cell side of the used photovoltaic module and pyrolyzed, the problem of cell breakage risk in the prior art is solved, and efficient glass and crystalline silicon cell recycling is achieved, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202410967345.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-18
AI Technical Summary
The existing recycling process is difficult to effectively recover complete silicon-based battery cells, and high-temperature heat treatment increases the risk of battery fracture and shatter, resulting in low recycling efficiency.
By pressurizing the fiber cotton layer on the cell side of the used photovoltaic module and pyrolysis is performed within a specific temperature range, uniform gas release is promoted, and the cell fragments are avoided, and efficient recycling of glass and crystalline silicon cells is achieved.
It achieves extremely high recovery rate, avoids cell breakage, is suitable for industrial applications, and simplifies the process flow.
Abstract
Description
Technical Field
[0001] The present application relates to the field of new energy, and in particular, to a method for recycling waste photovoltaic modules. Background Art
[0002] Nowadays, energy demand is increasing day by day. In order to alleviate the problem of global energy shortage, countries around the world are vigorously developing the photovoltaic industry. According to statistics, China's photovoltaic installed capacity has steadily increased from 12.9GW in 2013 to 52.3GW in 2017, accounting for more than 50% of the global installed capacity. China has become the largest photovoltaic application market. The life of photovoltaic panels is 25-30 years. Due to the long service life, the recycling of waste photovoltaic panels has been ignored.
[0003] However, according to relevant reports, photovoltaic panels have been installed since the 1980s and 1990s, and some have reached the end of their lifespan in recent years. In addition, due to the replacement of photovoltaic technology, the reduction of photoelectric conversion efficiency, damage to photovoltaic equipment, aging of photovoltaic components and other reasons, the growth of waste photovoltaic panels has been further accelerated, and has attracted widespread attention. The amount of photovoltaic waste will increase significantly after 2016. According to statistics, the global photovoltaic waste reached 43,500-250,000 tons in 2016. It is expected that the global photovoltaic waste will reach 1.7-8 million tons in 2030, and the global photovoltaic waste will reach 60-78 million tons in 2050. Among them, there are about 500 tons of waste photovoltaic panels in China in 2020. It is expected that China will reach 20 million tons in 2050, which is equivalent to 2,000 times the weight of the Eiffel Tower. Therefore, it can be foreseen that there will be a large number of waste photovoltaic panels that need to be processed in the world in the future.
[0004] At present, the existing research methods for the recycling and treatment of waste silicon-based photovoltaic panels at home and abroad mainly include: physical treatment method, chemical treatment method, physical treatment and chemical treatment combined method and external field enhancement method. Different solutions are proposed mainly based on the different characteristics of the components in photovoltaic panels, and the recycling of photovoltaic panels is achieved to a certain extent. However, from the perspectives of environment, economy, industrial application, etc., the existing recycling process still has some problems.
[0005] High-temperature heat treatment increases the risk of silicon-based cells breaking and shattering. As the average thickness of multicrystalline silicon wafers decreases from 550μm to 170μm, the risk of silicon wafers breaking and shattering during processing will increase further due to the reduction in thickness. Currently, it is difficult to recycle complete silicon-based cells and use them to directly re-manufacture photovoltaic panels. Summary of the invention
[0006] The purpose of the present disclosure is to provide a method for recycling waste photovoltaic modules, which has an extremely high recovery rate for glass and crystalline silicon cells in waste photovoltaic modules.
[0007] In order to achieve the above object, the present disclosure provides a method for recycling waste photovoltaic modules, the method comprising:
[0008] S1. Removing the back sheet material of frameless waste photovoltaic modules;
[0009] S2, applying pressure to the cell side of the frameless waste photovoltaic module from which the backboard material has been removed, and laying a fiber cotton layer to obtain a pretreated waste photovoltaic module;
[0010] S3, subjecting the pretreated waste photovoltaic modules to pyrolysis.
[0011] Optionally, in step S2, the thickness of the fiber cotton layer is 3-8 mm, preferably 4-6 mm.
[0012] Optionally, the material of the fiber wool layer is selected from one or more of aluminum silicate fiber wool, asbestos and glass fiber wool.
[0013] Optionally, in step S3, the pyrolysis conditions include: an initial temperature of 20-35°C, an end temperature of 430-480°C, a heating rate of 3-8°C / min, and a time of 1-4 hours.
[0014] Optionally, in step S3, the pyrolysis conditions include: an initial temperature of 25-30°C, an end temperature of 450-460°C, a heating rate of 5-6°C / min, and a time of 3-4 hours.
[0015] Optionally, the removing of the backboard material of the frameless waste photovoltaic modules comprises: cleaning the waste photovoltaic modules and mechanically removing the frames of the waste photovoltaic modules, and then removing the backboard material of the frameless waste photovoltaic modules at 120-140°C.
[0016] Optionally, the method further comprises step S4: cooling after the pyrolysis is completed, and the cooling conditions include: a cooling rate of 3-8°C / min and an end point temperature of 20-35°C.
[0017] Optionally, in step S2, a fiber cotton layer is applied by pressure to the cell side of the frameless waste photovoltaic module from which the back sheet material has been removed in a pressure-applying device;
[0018] Preferably, the frameless waste photovoltaic module with the backboard material removed is horizontally placed between two opposite pressure application surfaces of the pressure device along the length direction, and a fiber cotton layer is laid on the battery cell side; the orthographic projection area of the frameless waste photovoltaic module with the backboard material removed on the pressure application surface is smaller than the area of the pressure application surface.
[0019] Optionally, in step S2, the pressurizing pressure on both sides of the frameless waste photovoltaic assembly from which the backboard material is removed is the same, and the pressurizing pressure on one side is 5-10Pa, preferably 7-8Pa.
[0020] Optionally, in step S3, the pyrolysis is carried out in a tunnel kiln.
[0021] Through the above technical scheme, the present invention adopts the laminated pyrolysis method to recycle waste photovoltaic modules, and cleverly promotes the uniform release of pyrolysis gas through the fiber cotton layer, which can achieve the recycling of glass and crystalline silicon cells in waste photovoltaic modules with an extremely high recovery rate.
[0022] Other features and advantages of the present disclosure will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0023] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0024] The present disclosure provides a method for recycling waste photovoltaic modules, which comprises: S1, removing the backboard material of the frameless waste photovoltaic modules; S2, applying pressure to the cell side of the frameless waste photovoltaic modules from which the backboard material has been removed and laying a fiber cotton layer to obtain pretreated waste photovoltaic modules; S3, subjecting the pretreated waste photovoltaic modules to pyrolysis.
[0025] In the prior art, high-temperature heat treatment of waste photovoltaic modules will increase the risk of silicon-based cells breaking and shattering. The inventors of the present disclosure unexpectedly discovered that by adding a fiber cotton layer on the cell side of the waste photovoltaic modules, the position of the crystalline silicon cell can be strengthened and fixed, while the gas generated by pyrolysis can be released at a uniform rate to avoid the crystalline silicon cell from being broken due to the large amount of carbon dioxide gas generated by pyrolysis being released too quickly. As a result, the glass and crystalline silicon cells in the waste photovoltaic modules can be recycled at an extremely high recovery rate. The method is simple and easy, does not require consumables, and is suitable for industrial applications.
[0026] According to the present disclosure, the thickness of the fiber cotton layer can vary within a large range. In one embodiment of the present disclosure, in step S2, the thickness of the fiber cotton layer is 3-8 mm, preferably 4-6 mm. In the present disclosure, the thickness of the fiber cotton layer refers to the thickness before the fiber cotton is pressurized. If the thickness of the fiber cotton layer is too thin, it may result in uneven pressure applied to the photovoltaic module, and fail to effectively promote uniform gas release; if the thickness of the fiber cotton layer is too thick, the pressure transmitted to the photovoltaic module when pressure is applied is too dispersed, and fail to effectively promote uniform gas release. Within the above range, the thickness of the fiber cotton layer is appropriate, which is more conducive to the uniform release of gas, thereby further improving the recovery rate of glass and crystalline silicon cells.
[0027] According to the present disclosure, the material of the fiber cotton layer can be high temperature resistant fiber cotton well known to technicians in the field, for example, it can withstand high temperatures of 1000-1500°C. In a specific embodiment of the present disclosure, the material of the fiber cotton layer is selected from one or more of aluminum silicate fiber cotton, asbestos and glass fiber cotton.
[0028] In a specific embodiment of the present disclosure, in step S3, the pyrolysis conditions include: an initial temperature of 20-35°C, an end temperature of 430-480°C, a heating rate of 3-8°C / min, and a time of 1-4 hours; preferably, an initial temperature of 25-30°C, an end temperature of 450-460°C, a heating rate of 5-6°C / min, and a time of 3-4 hours. By accurately controlling the pyrolysis conditions as described above, it is possible to avoid the inappropriate gas release rate caused by too fast or too slow heating rates, and further improve the recovery rate of glass and crystalline silicon cells.
[0029] In a specific embodiment of the present disclosure, the removal of the backboard material of the frameless waste photovoltaic modules includes: cleaning the waste photovoltaic modules and mechanically removing the frames of the waste photovoltaic modules, and then removing the backboard material of the frameless waste photovoltaic modules at 120-140°C.
[0030] According to the present disclosure, the dust, oil, etc. on the surface of the waste photovoltaic modules can be cleaned by methods well known to those skilled in the art, such as ultrasonic cleaning, high-pressure water gun washing and roller brush cleaning. The specific operation methods are well known to those skilled in the art and will not be repeated here. According to the present disclosure, the frame can be mechanically removed by methods well known to those skilled in the art, such as a frame disassembly machine.
[0031] In a specific embodiment of the present disclosure, the method also includes step S4: cooling after the pyrolysis is completed, and the cooling conditions include: a cooling rate of 3-8°C / min, an end temperature of 20-35°C, and separating the glass and crystalline silicon cell pieces after cooling to the end temperature. Under the above conditions, the recovery rate of the glass and crystalline silicon cell pieces can be further improved.
[0032] In a specific embodiment of the present disclosure, in step S2, a fiber cotton layer is laid on the cell side of the frameless waste photovoltaic module with the backboard material removed in a pressure-applying device by applying pressure. The pressure-applying device may be, for example, a hydraulic impact device or a hydraulic stretching device. Preferably, the frameless waste photovoltaic module with the backboard material removed is horizontally placed between two opposite pressure-applying surfaces of the pressure-applying device along the length direction, and a fiber cotton layer is laid on the cell side, and more preferably, a fiber cotton layer is laid on the uniform side of the cell; the orthographic projection area of the frameless waste photovoltaic module with the backboard material removed on the pressure-applying surface is smaller than the area of the pressure-applying surface. In this embodiment, the fiber cotton layer fits more closely to the crystalline silicon cell, and has a better fixing effect on the crystalline silicon cell, which is beneficial to further promote the uniform diffusion of gas during the pyrolysis process.
[0033] In a specific embodiment of the present disclosure, in step S2, the pressurized pressure on both sides of the frameless waste photovoltaic assembly from which the backboard material has been removed is the same, and the pressurized pressure on one side is 5-10 Pa, preferably 7-8 Pa. In this embodiment, the pressurized pressure is appropriate, the fiber cotton layer fits more closely to the crystalline silicon cell, and has a better fixing effect on the crystalline silicon cell, which is conducive to further promoting the uniform diffusion of gas during the pyrolysis process.
[0034] According to the present disclosure, pyrolysis can be performed in an apparatus well known to those skilled in the art. In a specific embodiment of the present disclosure, in step S3, the pyrolysis is performed in a tunnel kiln.
[0035] The present disclosure is further illustrated below by way of examples, but the present disclosure is not limited thereby.
[0036] In the following embodiments and comparative examples, the waste photovoltaic modules processed are from retired photovoltaic modules of the State Energy Group.
[0037] Example 1
[0038] S1. Use an ultrasonic cleaning device to clean and remove dust from the waste photovoltaic modules, then use mechanical separation to remove the aluminum frame, and heat the waste photovoltaic modules again on a platform to evenly heat them to 120° C. to remove the backplane material;
[0039] S2. Place the frameless waste photovoltaic module with the backboard material removed horizontally along the length direction between two opposite pressure application surfaces of the planar uniform pressure device, evenly lay aluminum silicate fiber cotton with a thickness of 5 mm on one side of the solar cell and apply a pressure of 8 Pa, and the contact surface of the pressure application surfaces on both sides is larger than the size of the frameless waste photovoltaic module with the backboard material removed;
[0040] S3, set the tunnel kiln to program heating, the pyrolysis heating rate is 5℃ / min, the initial temperature is 25℃, the end temperature is 450℃, and the pyrolysis time is 3 hours. After the heating is completed, set the stable program to cool down, and set the cooling rate to 5℃ / min. After the temperature drops to room temperature, remove the glass plate and the crystalline silicon cell. At this time, the glass plate and the crystalline silicon cell are completely separated.
[0041] The experiment was repeated for 10 groups, and in each group of experiments, the crystalline silicon cell and the glass were completely separated without any breakage of the crystalline silicon cell.
[0042] Example 2
[0043] The same method as in Example 1 is used to recycle waste photovoltaic modules, except that in step S2, aluminum silicate fiber wool with a thickness of 3 mm is evenly applied to one side of the battery cell.
[0044] The experiment was repeated for 10 groups. In 8 groups of experiments, the crystalline silicon cell and the glass were completely separated without any breakage of the crystalline silicon cell. In 2 groups of experiments, the crystalline silicon cell was broken.
[0045] Example 3
[0046] The same method as in Example 1 is used to recycle waste photovoltaic modules, except that in step S2, aluminum silicate fiber wool with a thickness of 8 mm is evenly applied to one side of the solar cell.
[0047] The experiment was repeated for 10 groups. In 7 groups of experiments, the crystalline silicon cell and the glass were completely separated without any breakage of the crystalline silicon cell. In 3 groups of experiments, the crystalline silicon cell was broken.
[0048] Example 4
[0049] The same method as in Example 1 is used to recycle waste photovoltaic modules, except that in step S3, the tunnel kiln is set to program heating, the pyrolysis heating rate is 8°C / min, the initial temperature is 25°C, the terminal temperature is 480°C, and the pyrolysis time is 3 hours. After the heating is completed, a stable program is set to cool down, and the cooling rate is also set to 8°C / min. After the temperature drops to room temperature, the glass plate and the crystalline silicon cell are removed, and the glass plate and the crystalline silicon cell are completely separated.
[0050] The experiment was repeated for 10 groups. In 7 groups of experiments, the crystalline silicon cell and the glass were completely separated without any breakage of the crystalline silicon cell. In 3 groups of experiments, the crystalline silicon cell was broken.
[0051] Example 5
[0052] The same method as in Example 1 is used to recycle waste photovoltaic modules, except that in step S3, the tunnel kiln is set to program heating, the pyrolysis heating rate is 8°C / min, the initial temperature is 25°C, the terminal temperature is 430°C, and the pyrolysis time is 3 hours. After the heating is completed, a stable program is set to cool down, and the cooling rate is also set to 8°C / min. After the temperature drops to room temperature, the glass plate and the crystalline silicon cell are removed, and the glass plate and the crystalline silicon cell are completely separated.
[0053] The experiment was repeated for 10 groups. In 6 groups of experiments, the crystalline silicon cell and the glass were completely separated without any breakage of the crystalline silicon cell. In 4 groups of experiments, the crystalline silicon cell was broken.
[0054] Comparative Example 1
[0055] The same method as in Example 1 was used to recycle waste photovoltaic modules, except that step S2 was omitted. The experiment was repeated for 10 groups, and all the crystalline silicon cells were broken in the 10 groups of experiments.
[0056] It can be seen from the above that the method disclosed in the present invention is simple and easy to implement, and can achieve the recycling of glass and crystalline silicon cells in waste photovoltaic modules at a high recovery rate.
[0057] The preferred embodiments of the present disclosure are described in detail above; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0058] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0059] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A method for recycling waste photovoltaic modules, the method comprising: S1. Removing the back sheet material of frameless waste photovoltaic modules; S2, applying pressure to the cell side of the frameless waste photovoltaic module from which the backboard material has been removed, and laying a fiber cotton layer to obtain a pretreated waste photovoltaic module; S3, subjecting the pretreated waste photovoltaic modules to pyrolysis.
2. The method according to claim 1, wherein: In step S2, the thickness of the fiber cotton layer is 3-8 mm, preferably 4-6 mm.
3. The method according to claim 1, wherein: The material of the fiber wool layer is selected from one or more of aluminum silicate fiber wool, asbestos and glass fiber wool.
4. The method according to claim 1, wherein: In step S3, the pyrolysis conditions include: initial temperature of 20-35°C, end temperature of 430-480°C, heating rate of 3-8°C / min, and time of 1-4 hours.
5. The method according to claim 1, wherein: In step S3, the pyrolysis conditions include: initial temperature of 25-30°C, end temperature of 450-460°C, heating rate of 5-6°C / min, and time of 3-4 hours.
6. The method according to claim 1, wherein: The method of removing the backboard material of the frameless waste photovoltaic modules comprises: cleaning the waste photovoltaic modules and mechanically removing the frames of the waste photovoltaic modules, and then removing the backboard material of the frameless waste photovoltaic modules at 120-140°C.
7. The method according to claim 1, wherein: The method further comprises step S4: cooling down after the pyrolysis is completed, wherein the cooling down conditions include: a cooling rate of 3-8°C / min and an end point temperature of 20-35°C.
8. The method according to claim 1, wherein: In step S2, a fiber cotton layer is applied to the cell side of the frameless waste photovoltaic module from which the back plate material has been removed by a pressure device; Preferably, the frameless waste photovoltaic module with the backboard material removed is horizontally placed between two opposite pressure application surfaces of the pressure application device along the length direction, and a fiber cotton layer is laid on the battery sheet side; The orthographic projection area of the frameless waste photovoltaic assembly with the backboard material removed on the pressure application surface is smaller than the area of the pressure application surface.
9. The method according to claim 8, wherein: In step S2, the pressurizing pressure on both sides of the frameless waste photovoltaic assembly from which the backboard material is removed is the same, and the pressurizing pressure on one side is 5-10Pa, preferably 7-8Pa.
10. The method according to claim 1, wherein: In step S3, the pyrolysis is carried out in a tunnel kiln.
Citation Information
Patent Citations
Method of pyrolysis in process of recovering and treating waste lithium batteries
CN109719117A
Photovoltaic module recovery method
CN110328216A
Heat dissipation and fireproof composite material battery box and preparation method thereof
CN115189083A
Method for efficiently recycling waste photovoltaic module
CN116329256A
Method for recycling waste photovoltaic module
CN116651888A