Method for preparing Si-doped magnetostrictive Fe-Ga alloy through laser powder bed melting

By increasing the resistivity and magnetostrictive strain of Fe-Ga alloy under low doping amount by laser powder bed melting process, the problem of insufficient magnetostrictive strain at high doping level is solved, and the problem of existing Fe-Ga alloys is realized The integrated manufacturing of performance and structure has expanded the application range of alloys.

CN118926548APending Publication Date: 2024-11-12CENT SOUTH UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411018661.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

Smart Images

  • Figure CN118926548A_ABST
    Figure CN118926548A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing Si-doped magnetostrictive Fe-Ga alloy through laser powder bed melting, and belongs to the field of additive manufacturing. According to the method, the laser powder bed melting technology is proposed for the first time to prepare the polycrystalline Fe-Ga-Si alloy with the optimal combination of the resistivity and the magnetostrictive strain, and the prepared alloy shows the enhanced electron scattering effect and the reduced number of conducted electrons as well as lt; 001gt, 001gt; columnar crystal grains are preferentially oriented, and the optimal combination of the resistivity (104.5 + / -4.1 mu omega.cm) and the magnetostrictive strain (73ppm) is obtained. According to the method, the alloy is endowed with enhanced resistivity and magnetostrictive strain, personalized customization of the appearance and the structure can be realized, and a new insight is provided for integrated manufacturing of the magnetostrictive alloy with excellent comprehensive performance and a personalized structure. Meanwhile, the composition is simple, the process is controllable, and large-scale industrial application is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of additive manufacturing, and in particular relates to a method for preparing Si-doped magnetostrictive Fe-Ga alloy by laser powder bed melting. Background Art

[0002] In 1842, British scientist Joule discovered the magnetostrictive effect of ferromagnetic materials (ferrous) and also known as the Joule effect, which is the phenomenon that the length and volume of ferromagnetic materials or ferrimagnetic materials change due to the change of magnetization state. Among them, the change in length is called linear magnetostriction, and the change in volume is called volume magnetostriction. Magnetostrictive materials. Magnetostrictive materials have high mechanical energy-electric energy conversion efficiency, high energy density, high response speed, good reliability, and simple driving mode. Therefore, they have important applications in national defense science and technology, electronics industry, machinery industry, ultrasonic technology and other fields. At present, the main magnetostrictive materials are traditional magnetostrictive materials (Ni, Ni-Co, Fe-Al, Co ferrite, etc.), rare earth giant magnetostrictive materials (Tb-Dy-Fe) and new Fe-Ga alloy magnetostrictive materials. Among them, the new Fe-Ga alloy is a new type of magnetostrictive material after the traditional magnetostrictive material and rare earth giant magnetostrictive material, which has the advantages of low saturation magnetic field, high magnetic permeability, high strength, and good temperature characteristics. Among them, although single crystal alloys usually exhibit large magnetostrictive strain, due to the limitations of strict production conditions, single crystals can often only obtain limited structures such as rods and films. In contrast, polycrystalline Fe-Ga alloys have attracted widespread attention from many scholars due to their good mechanical properties and low production costs, and have broad application potential in energy conversion fields such as transducers, energy harvesters and sensing materials. However, the large eddy current losses caused by low resistivity and the insufficient magnetostrictive strain caused by random grain structure have become the main limitations of their widespread application. It is well known that the resistance in solid conductors is closely related to the periodic destruction of the lattice structure, which is usually caused by defects in the lattice structure (grain boundaries, dislocations and vacancies) or doping elements (impurities) occupying the lattice space. Previously, people used three-element doping to increase the resistivity of magnetic materials. For example, Jen et al. prepared Co-doped Fe-Ga films and found that when the Co doping content was as high as 7 at.%, the resistivity increased to 191 μΩ·cm, but the magnetostrictive strain significantly deteriorated to 30 ppm (Jen SU, Tsai TL, Kuo PC, et al. Magnetostrictive and structural properties of FeCoGa films [J]. Journal of Applied Physics, 2010, 107 (1)). It can be seen that the alloy prepared by the method has a certain increase in resistivity at a high doping level, but a high doping level is often required and is accompanied by a significant deterioration in magnetostrictive strain. In addition, traditional processes such as traditional smelting, directional solidification and forging can only produce structures with limited sizes and shapes such as rods, plates, and films, which greatly limits the application range of the alloy.

[0003] Therefore, if a new preparation technology can be developed to obtain the optimal combination of resistivity and magnetostrictive strain at low doping content and at the same time give Fe-Ga alloys personalized structural shapes, it will have great engineering significance. Summary of the invention

[0004] In order to overcome the above problems, the present invention proposes a method for preparing Si-doped magnetostrictive Fe-Ga alloy by laser powder bed melting. Specifically, the first object of the present invention is to develop a Fe-Ga-Si alloy with an optimal combination of resistivity and magnetostriction. The resistivity of the Fe-Ga alloy can be increased at a lower doping amount. The Fe-Ga-Si alloy has <001> Preferentially oriented columnar grains, more electron scattering sites and fewer conduction electrons, the Fe-Ga-Si alloy finally obtains the best combination of resistivity (104.5±4.1μΩ·cm) and magnetostrictive strain (73ppm).

[0005] The second purpose of the present invention is to develop a method for preparing Fe-Ga-Si alloy by laser powder bed melting. The present invention proposes for the first time to use laser powder bed melting process to prepare Fe-Ga-Si alloy with the best combination of resistivity and magnetostriction: on the one hand, the rapid solidification characteristics of laser powder bed melting are used to further expand the solid solubility of Si in the Fe-Ga matrix, thereby enhancing the lattice distortion and dislocation density. At the same time, the high temperature gradient characteristics of laser powder bed melting are used to promote <001> The formation of preferentially oriented columnar grains is achieved, thereby obtaining enhanced resistivity and magnetostrictive strain. In addition, based on the layer-by-layer stacking manufacturing characteristics of laser powder bed melting, the process can also give the Fe-Ga alloy a personalized structural shape, realizing integrated manufacturing of performance and structure. The present invention provides a Fe-Ga-Si alloy with an optimal combination of resistivity and magnetostriction, in which the atomic ratio of Fe to Ga is 70 to 90:30 to 10, preferably 81:19; in addition, the Si content is 0.05 to 3 at.%, preferably 0.08 to 0.5 at.%, and further preferably 0.18 to 0.22 at.%. In the Fe-Ga-Si alloy designed by the present invention, all Si is solid dissolved in the alloy.

[0006] The present invention provides a method for preparing a Fe-Ga-Si alloy having an optimal combination of resistivity and magnetostriction, comprising the following steps:

[0007] (1) The Fe-Ga pre-alloyed powder is prepared by a powder making process, and the particle size of the pre-alloyed powder is preferably 10-90 μm, preferably 20-60 μm, and more preferably 20-40 μm, so as to meet the process requirements of laser powder bed melting. In addition, the powder making process includes gas atomization powder making, which helps to ensure that the split body has good sphericity, smooth surface, uniform composition and high purity.

[0008] (2) Si powder is added to the Fe-Ga pre-alloyed powder according to the set composition, and mixed using a ball mill to obtain a uniformly mixed Fe-Ga-Si powder.

[0009] (3) Using the above Fe-Ga-Si powder as raw material, Fe-Ga-Si alloy was prepared by laser powder bed melting under a protective atmosphere. During the preparation process, the laser power was controlled to be 80-155 W, the scanning speed was 30-200 mm / s, the scanning spacing was 20-90 μm, the laser spot diameter was 50-100 μm, and the layer thickness was 50-150 μm.

[0010] Preferably, the content of Si in the Fe-Ga-Si mixed powder in step (2) is 0.05 to 3 at.%, preferably 0.08 to 0.5 at.%, and more preferably 0.18 to 0.22 at.%.

[0011] Preferably, the laser process parameters in step (3) are: laser power of 110-135 W, scanning speed of 80-120 mm / s, scanning spacing of 40-60 μm, laser spot diameter of 50-60 μm, and layer thickness of 80-120 μm.

[0012] Further preferably, the laser process parameters are: laser power of 125 W, scanning speed of 100 mm / s, scanning spacing of 50 μm, laser spot diameter of 50 μm, and layer thickness of 100 μm.

[0013] In the present invention, when the molar ratio of Fe to Ga is 81:19 and the Si doping content is 0.1 at.%, the Fe-Ga-Si alloy prepared by laser powder bed melting has an A2 phase structure and a lattice constant of The average orientation difference of the core of the dislocation density is 0.52°, and the grain structure of the alloy is <001> The final alloy has a resistivity of 94.1±4.7μΩ·cm and a magnetostrictive strain of 78ppm.

[0014] In the present invention, when the molar ratio of Fe to Ga is 81:19 and the Si doping content is 0.2 at.%, the Fe-Ga-Si alloy prepared by laser powder bed melting has an A2 phase structure, but the lattice constant is The core average orientation difference of the alloy's dislocation density is 0.55°, the resistivity of the final alloy is 104.5±4.1μΩ·cm, and the magnetostrictive strain is 73ppm.

[0015] In the present invention, when the molar ratio of Fe to Ga is 81:19 and the Si doping content is 0.3 at.%, the Fe-Ga-Si alloy prepared by laser powder bed melting has an A2 phase structure, but the lattice constant is The core average orientation difference of the alloy's dislocation density is 0.56°, the resistivity of the final alloy is 122.7±5.5μΩ·cm, and the magnetostrictive strain is 56ppm.

[0016] After optimization, the Fe-Ga-Si alloy finally obtained by the present invention obtains the best combination of resistivity (104.5±4.1μΩ·cm) and magnetostrictive strain (73ppm).

[0017] Principles and advantages

[0018] This invention is the first to attempt to use the laser powder bed melting process to prepare Fe-Ga-Si alloys with the best combination of resistivity and magnetostriction. On the one hand, the rapid solidification characteristics of laser powder bed melting are used to further expand the solid solubility of Si in the Fe-Ga matrix, thereby enhancing the lattice distortion and dislocation density. At the same time, the high temperature gradient characteristics of laser powder bed melting are used to promote <001> The formation of preferentially oriented columnar grains can obtain enhanced resistivity and magnetostrictive strain. In addition, based on the characteristics of layer-by-layer stacking manufacturing, laser powder bed melting can also give Fe-Ga alloys a personalized structural shape, realizing integrated manufacturing of performance and structure. Moreover, the present invention does not require remelting, and the resulting product has excellent performance, achieving for the first time that both resistivity and magnetostrictive strain are at a relatively high value.

[0019] The doping amount of Si element in the present invention affects the resistivity and grain structure of the alloy, and the amount of Si must be controlled and a suitable doping amount must be selected. When the Si doping amount is too high, it is easy to agglomerate or even precipitate in the matrix, thereby reducing the forming performance of the alloy, and also hindering the grain growth during the forming process, destroying the trend of epitaxial growth of the grains along the construction direction. If the Si doping amount is too low, the lattice distortion caused by doping is limited, and the role of Si as a dopant cannot be fully utilized, and the role of the rapid solidification characteristics in the laser powder bed melting process to improve the solid solubility cannot be fully utilized, and the final resistivity improvement effect is limited.

[0020] The laser powder bed melting process parameters of the present invention, such as laser power and scanning speed, directly determine the forming quality of the Fe-Ga alloy. When the laser power is too low or the scanning speed is too high, due to insufficient energy input during the laser powder bed melting process, unmelted powder appears on the surface of the alloy, resulting in reduced alloy density or even failure to form. On the contrary, when the laser power is high or the scanning speed is low, a large amount of metal vapor is generated during the forming process, which leads to internal pore defects. At the same time, excessive energy input will also lead to excessive thermal stress, causing thermal cracks on the surface of the alloy, ultimately resulting in poor forming quality. Therefore, the laser process parameters within the scope of the present invention should be selected to obtain Fe-Ga-Si alloys with good forming quality.

[0021] The Fe-Ga-Si alloy prepared by the present invention has enhanced resistivity and magnetostrictive strain. Due to rapid solidification during laser powder bed melting, the solid solubility of Si in the Fe-Ga matrix is ​​further expanded, and the randomly distributed Si atoms in the unit cell act as scattering centers to cause strong scattering of electrons to weaken the carrier mobility. At the same time, the solid-dissolved Si atoms tend to form covalent bonds with adjacent atoms, resulting in a decrease in the number of conductive electrons, that is, a decrease in carrier concentration. The increase in Si solid solubility also indirectly leads to an increase in dislocation density, which helps to enhance the resistivity caused by dislocation scattering. In addition, the grain boundary, where the atomic arrangement is different from that inside the grain, is usually the natural reflection center of the electron. The decrease in texture strength caused by the increase in Si doping will also lead to an increase in grain boundary scattering sites, thereby increasing the interface scattering resistivity. In summary, the enhancement of impurity scattering, dislocation scattering and interface scattering effects induced by laser powder bed melting and Si doping and the change in electronic structure promote the enhancement of the alloy resistivity. At the same time, due to the high temperature gradient during laser powder bed melting, the columnar grains in the prepared Fe-Ga alloy preferentially grow along the construction direction. Finally, the optimal combination of resistivity and magnetostrictive strain was obtained simultaneously by laser powder bed melting and Si doping.

[0022] The main advantages of the present invention are:

[0023] (1) The present invention utilizes the characteristics of semiconductor Si element, which has a small atomic radius and high resistivity, to improve the resistivity of Fe-Ga alloy under low doping conditions.

[0024] (2) The present invention utilizes the rapid solidification and high temperature gradient characteristics of laser powder bed melting to expand the solid solubility of Si in the Fe-Ga matrix to enhance lattice distortion and dislocation density, while promoting <001> The growth of columnar grains is preferentially oriented, thus obtaining the best combination of resistivity and magnetostrictive strain of the alloy.

[0025] (3) The present invention proposes for the first time the use of laser powder bed melting technology to prepare Si-doped Fe-Ga alloys. By controlling the Si doping amount and laser process parameters, not only can the alloy be given enhanced resistivity and magnetostrictive strain, but also personalized customization of shape and structure can be achieved, providing new insights into the integrated manufacturing of high-performance and personalized magnetostrictive alloys, thereby realizing a wider range of potential applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Attached Figure 1 is the X-ray diffraction pattern of Fe-Ga alloy at different Si doping contents in Examples 1-3;

[0027] Attached Figure 2 is the dislocation distribution diagram of Fe-Ga alloy at different Si doping contents in Examples 1-3;

[0028] Attached Figure 3 The grain morphology of the Fe-Ga alloy at different Si doping contents in Examples 1-3;

[0029] Attached Figure 4 is the resistivity of the Fe-Ga alloy at different Si doping contents in Examples 1-3;

[0030] Attached Figure 5 : The magnetostrictive strain of the Fe-Ga alloy at different Si doping contents in Examples 1-3. DETAILED DESCRIPTION

[0031] The specific implementation mode of the present invention is described below by way of examples:

[0032] The test conditions of the magnetostrictive strain of the present invention are as follows: the resistivity and magnetostrictive strain are tested respectively using a four-probe tester and a resistance strain gauge. The resistivity test is carried out at room temperature, and three random positions are selected for measurement. The magnetostrictive test is also carried out at room temperature, and the test is repeated three times. The magnetostrictive strain parallel and perpendicular to the construction direction of the laser powder bed melting are measured using a resistance strain gauge. The final magnetostrictive strain result is expressed as the difference between the strains in the parallel and perpendicular directions. It should be pointed out that in order to obtain the true magnetostrictive strain size of the alloy in a free state, no prestress loading is performed during the magnetostrictive strain test of the present invention.

[0033] Example 1

[0034] High-purity (99.99%) spherical Fe powder and Ga metal were used as raw materials, and the ingredients were prepared according to the atomic fraction of 81:19. The Fe particles with a particle size distribution of 20 to 40 μm were prepared by gas atomization method. 81 Ga 19 Pre-alloyed powder. The atomized Fe81 Ga 19 After pre-alloying the powder, 0.1at.% Si powder is added and mixed by a ball mill to obtain a uniformly mixed Fe-Ga-Si powder. The uniformly mixed Fe-Ga-Si powder is used as a raw material, and a Fe-Ga-Si alloy is prepared by laser powder bed melting under an argon protective atmosphere. During the preparation process, the laser process parameters are controlled as follows: laser power is 125W, scanning speed is 100mm / s, scanning spacing is 50μm, laser spot diameter is 50μm, and layer thickness is 100μm.

[0035] The test found that when the Si doping content is 0.1at.%, the Fe-Ga-Si alloy prepared by laser powder bed melting has an A2 phase structure with a lattice constant of (Attached Figure 1 ), the average orientation difference of the core representing the dislocation density is 0.52° (Appendix Figure 2 ), and the grain structure of the alloy is <001> Columnar grains (with Figure 3 The final resistivity of the alloy was 94.1±4.7μΩ·cm (attached Figure 4 ), magnetostrictive strain is 78ppm (attached Figure 5 ).

[0036] Example 2

[0037] High-purity (99.99%) spherical Fe powder and Ga metal were used as raw materials, and the ingredients were prepared according to the atomic fraction of 81:19. The Fe particles with a particle size distribution of 20 to 40 μm were prepared by gas atomization method. 81 Ga 19 Pre-alloyed powder. The atomized Fe 81 Ga 19 After pre-alloying the powder, 0.2at.% Si powder was added and mixed by a ball mill to obtain a uniformly mixed Fe-Ga-Si powder. The uniformly mixed Fe-Ga-Si powder was used as a raw material, and Fe-Ga-Si alloy was prepared by laser powder bed melting under an argon protective atmosphere. During the preparation process, the laser process parameters were controlled as follows: laser power of 125W, scanning speed of 100mm / s, scanning spacing of 50μm, laser spot diameter of 50μm, and layer thickness of 100μm.

[0038] The test found that when the Si doping content was 0.2 at.%, the Fe-Ga-Si alloy prepared by laser powder bed melting still showed an A2 phase structure, but the lattice constant Compared with Example 1, it is reduced (see Figure 1 ), indicating that the lattice distortion increases. The average orientation difference of the core of the alloy dislocation density is 0.55° (Appendix Figure 2), the dislocation density is further improved compared with Example 1, and the grain size of the alloy is <001> The preferential orientation has slightly weakened (see Appendix Figure 3 ), the resistivity of the final alloy is 104.5±4.1μΩ·cm (Appendix Figure 4 ), magnetostrictive strain is 73ppm (attached Figure 5 ).

[0039] Example 3

[0040] High-purity (99.99%) spherical Fe powder and Ga metal were used as raw materials, and the ingredients were prepared according to the atomic fraction of 81:19. The Fe particles with a particle size distribution of 20 to 40 μm were prepared by gas atomization method. 81 Ga 19 Pre-alloyed powder. The atomized Fe 81 Ga 19 After pre-alloying the powder, 0.3at.% Si powder was added and mixed by a ball mill to obtain a uniformly mixed Fe-Ga-Si powder. The uniformly mixed Fe-Ga-Si powder was used as a raw material, and Fe-Ga-Si alloy was prepared by laser powder bed melting under an argon protective atmosphere. During the preparation process, the laser process parameters were controlled as follows: laser power of 125W, scanning speed of 100mm / s, scanning spacing of 50μm, laser spot diameter of 50μm, and layer thickness of 100μm.

[0041] The test found that when the Si doping content was 0.3 at.%, the Fe-Ga-Si alloy prepared by laser powder bed melting still showed an A2 phase structure, but the lattice constant Compared with Example 2, it is further reduced (attached Figure 1 ), that is, the lattice distortion increases further. The dislocation density of the alloy (attached Figure 2 ) is further improved compared with Example 2 (the average orientation difference of the core is 0.56°), and the grain size of the alloy is <001> The preferential orientation is further weakened (see Appendix Figure 3 ), the resistivity of the final alloy is 122.7±5.5μΩ·cm (Appendix Figure 4 ), magnetostrictive strain is 56ppm (attached Figure 5 ).

[0042] Example 4

[0043] Other conditions were consistent with those in Example 2, except that the laser power was 140 W and the scanning speed was 80 mm / s; the resistivity of the final alloy was 108±6.1 μΩ·cm, and the magnetostrictive strain was 57 ppm.

[0044] Example 5

[0045] Other conditions were consistent with those in Example 2, except that the laser power was 105 W and the scanning speed was 120 mm / s; the resistivity of the final alloy was 118±5.6 μΩ·cm, and the magnetostrictive strain was 44 ppm.

[0046] Comparative Example 1

[0047] The other parameters are consistent with those in Example 2, except that the Si doping content is 0 at.%, that is, no Si powder is doped.

[0048] The test found that the Fe-Ga alloy prepared by laser powder bed melting still has an A2 phase structure, but the lattice constant is (Attached Figure 1 ), and its lattice distortion is almost nonexistent. The average orientation difference of the core, which characterizes the dislocation density, is 0.47° (see Appendix Figure 2 ), indicating a lower dislocation density. The grain structure of the alloy still presents <001> Columnar grains (with Figure 3 ), the resistivity of the final alloy is 75.9±3.9μΩ·cm, and the magnetostrictive strain is 83ppm.

[0049] Comparative Example 2

[0050] The other parameters are the same as those in Example 2, except that the laser power is controlled to be 160 W and the scanning speed is 60 mm / s.

[0051] Tests found that the Fe-Ga-Si alloy prepared by laser powder bed melting still exhibits an A2 phase structure and has similar dislocation density and lattice distortion. However, due to the high energy input, a large amount of metal vapor is generated during the forming process, which in turn leads to internal porosity defects. At the same time, excessive energy input will also lead to excessive thermal stress, causing thermal cracks on the alloy surface, ultimately resulting in poor forming quality.

[0052] Comparative Example 3

[0053] The other parameters are the same as those in Example 2, except that the laser power is controlled to be 75 W and the scanning speed is 150 mm / s.

[0054] Tests have found that due to insufficient energy input during the laser powder bed melting process, unmelted powder appears on the surface of the Fe-Ga-Si alloy prepared by laser powder bed melting, which reduces the density of the alloy and makes it difficult to form, significantly deteriorating the magnetostrictive properties of the alloy.

[0055] Comparative Example 4

[0056] The other parameters were the same as those in Example 2, except that the laser power was controlled to be 125 W and the scanning speed was 250 mm / s. The resistivity of the final alloy was 144±7.5 μΩ·cm and the magnetostrictive strain was 34 ppm.

[0057] Comparative Example 5

[0058] The other parameters were the same as those in Example 2, except that the laser power was controlled to be 125 W and the scanning speed was 25 mm / s. The resistivity of the final alloy was 112±4.8 μΩ·cm and the magnetostrictive strain was 41 ppm.

Claims

1. A method for preparing Si-doped magnetostrictive Fe-Ga alloy by laser powder bed melting, characterized in that: In the Fe-Ga-Si alloy, the atomic ratio of Fe to Ga is 70-90:30-10, and the Si content is 0.05-3 at.% In the Fe-Ga-Si alloy, all Si is solid-dissolved in the alloy; The Fe-Ga-Si alloy is prepared by the following steps: (1) preparing Fe-Ga pre-alloyed powder by a powder making process, wherein the pre-alloyed powder has a particle size of 10 to 90 μm; (2) adding Si powder to Fe-Ga pre-alloyed powder according to the set composition, and mixing them using a ball mill to obtain a uniformly mixed Fe-Ga-Si powder. (3) Using the above Fe-Ga-Si powder as raw material, Fe-Ga-Si alloy was prepared by laser powder bed melting under a protective atmosphere. During the preparation process, the laser power was controlled to be 80-155 W, the scanning speed was 30-200 mm / s, the scanning spacing was 20-90 μm, the laser spot diameter was 50-100 μm, and the layer thickness was 50-150 μm.

2. The method for preparing Si-doped magnetostrictive Fe-Ga alloy by laser powder bed melting according to claim 1, characterized in that: In the Fe-Ga-Si alloy, the atomic ratio of Fe to Ga is 81:19; and the Si content is 0.08-0.5 at.%.

3. The method for preparing Si-doped magnetostrictive Fe-Ga alloy by laser powder bed melting according to claim 1, characterized in that: In the Fe-Ga-Si alloy, the Si content is 0.18-0.22 at.%.

4. The method for preparing Si-doped magnetostrictive Fe-Ga alloy by laser powder bed melting according to claim 1, characterized in that: The laser process parameters in step (3) are: laser power of 110-135 W, scanning speed of 80-120 mm / s, scanning spacing of 40-60 μm, laser spot diameter of 50-60 μm, and layer thickness of 80-120 μm.

5. The method for preparing Si-doped magnetostrictive Fe-Ga alloy by laser powder bed melting according to claim 4, characterized in that: The laser process parameters are: laser power is 125 W, scanning speed is 100 mm / s, scanning spacing is 50 μm, laser spot diameter is 50 μm, and layer thickness is 100 μm.

6. The method for preparing Si-doped magnetostrictive Fe-Ga alloy by laser powder bed melting according to claim 1, characterized in that: When the Fe:Ga molar ratio is 81:19 and the Si doping content is 0.1at.%, the Fe-Ga-Si alloy prepared by laser powder bed melting has an A2 phase structure with a lattice constant of The average orientation difference of the core of the dislocation density is 0.52°, and the grain structure of the alloy is <001> The final alloy has a resistivity of 94.1±4.7μΩ·cm and a magnetostrictive strain of 78ppm.

7. The method for preparing Si-doped magnetostrictive Fe-Ga alloy by laser powder bed melting according to claim 1, characterized in that: When the Fe:Ga molar ratio is 81:19 and the Si doping content is 0.2 at.%, the Fe-Ga-Si alloy prepared by laser powder bed melting has an A2 phase structure, but the lattice constant is The core average orientation difference of the alloy's dislocation density is 0.55°, the resistivity of the final alloy is 104.5±4.1μΩ·cm, and the magnetostrictive strain is 73ppm.

8. The method for preparing Si-doped magnetostrictive Fe-Ga alloy by laser powder bed melting according to claim 1, characterized in that: When the Fe:Ga molar ratio is 81:19 and the Si doping content is 0.3at.%, the Fe-Ga-Si alloy prepared by laser powder bed melting has an A2 phase structure, but the lattice constant is The core average orientation difference of the alloy's dislocation density is 0.56°, the resistivity of the final alloy is 122.7±5.5μΩ·cm, and the magnetostrictive strain is 56ppm.

Citation Information

Cited By

  • A method for manufacturing terbium-dysprosium-iron supermagnetic alloy based on stereolithography

    CN120572732B