Method for preparing graphene double-layer heterogeneous wave-absorbing structure based on fused deposition 3D printing
The Hummers method oxidizes graphene with active oxygen-containing functional groups and combines with melt deposition 3D printing technology to prepare a double-layer heterostructure, which solves the problem of insufficient performance of the existing graphene absorbing structure and achieves low graphene load The wideband and efficient electromagnetic wave absorption and mechanical performance are improved.
Patent Information
- Application Number
- CN202410971025.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The existing graphene absorbing structure has limited performance in electromagnetic wave absorption, and improvement methods usually require high graphene addition, resulting in poor mechanical properties and difficult to achieve high-efficiency absorption in wide frequency.
The Hummers method is used to oxidize and reactive oxygen-containing functional groups to derivatize modified graphene, and prepare a double-layer heterostructure, including a wave-transmitting layer and an absorbing layer, using the excellent mechanical properties and orientation of the modified graphene to achieve electromagnetic waves. The wideband efficient absorption.
With low graphene load, the wide frequency and efficient absorption of electromagnetic waves is achieved, and good mechanical properties are maintained, the process flow is simplified, the production cost is reduced, and it is suitable for the customization of complex structures.
Smart Images

Figure CN118927606A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of absorbing materials, and in particular to a method for preparing a graphene double-layer heterogeneous absorbing structure based on fused deposition 3D printing. Background Art
[0002] Graphene is considered to be an efficient microwave absorber due to its high electrical conductivity, high specific surface area, high thermal conductivity and low density. However, the electromagnetic incompatibility characteristics of the single component and structure of the original graphene make its impedance performance poor, and the electromagnetic waves are almost reflected rather than dissipated, resulting in extremely limited absorption performance. A common improvement method is to modify the graphene surface, such as loading magnetic particles and surface oxidation; or to construct a special microstructure, such as a porous structure and a honeycomb structure, to improve the interface performance and introduce multiple reflections, thereby improving the absorption performance of the overall structure. However, the above improvement methods all rely on complex preparation processes and a high amount of graphene added, resulting in poor mechanical properties of the prepared absorbing components, making it difficult to achieve broadband and efficient absorption of electromagnetic waves, and unable to meet actual application requirements. Based on this, the present application proposes a method for preparing a graphene double-layer heterogeneous absorbing structure based on fused deposition 3D printing to achieve broadband and efficient absorption of electromagnetic waves at a low graphene loading and maintain good mechanical properties. Summary of the invention
[0003] The main purpose of this application is to provide a method for preparing a graphene double-layer heterogeneous absorbing structure based on fused deposition 3D printing, aiming to solve the technical problems that the existing absorbing structures are difficult to achieve broadband and efficient absorption of electromagnetic waves and have poor mechanical properties.
[0004] To achieve the above objectives, the present application proposes a method for preparing a graphene double-layer heterogeneous absorbing structure based on fused deposition 3D printing, comprising the following steps:
[0005] The original graphene is oxidized by the Hummers method to obtain graphene oxide; the graphene oxide is then derivatized and modified by active oxygen-containing functional groups to graft macromolecular chains onto the surface of the graphene oxide to obtain modified graphene;
[0006] The modified graphene, the thermoplastic matrix and the plasticizer are mixed, dried and screw extruded to obtain a wave-transmitting layer printing filament; and the original graphene and the modified graphene are used to prepare a wave-absorbing layer printing filament;
[0007] By melt deposition 3D printing, a wave-transmitting layer cube is prepared with the wave-transmitting layer printing filament, so that the modified graphene in the wave-transmitting layer cube is oriented along the X-0° direction, and then the wave-transmitting layer cube is cut perpendicular to the X direction to obtain a flat plate with the modified graphene oriented along the Z-0° direction, which is the upper wave-transmitting structure;
[0008] The upper wave-transmitting structure is used as a substrate, and melt deposition 3D printing is adopted to prepare a wave-absorbing layer cube on the substrate through the wave-absorbing layer printing filament, so that the original graphene and the modified graphene in the wave-absorbing layer cube are oriented along the XY direction, that is, a double-layer heterogeneous wave-absorbing structure is obtained.
[0009] Optionally, the step of oxidizing the original graphene by the Hummers method to obtain graphene oxide comprises:
[0010] The original graphene, concentrated sulfuric acid, potassium persulfate and phosphorus pentoxide were stirred and mixed, and then heated to 75°C-85°C in an oil bath and kept warm for 4.5h-5.5h, and then naturally cooled to room temperature, and ice water was added for dilution, and then filtered and washed to a pH of 6.8-7.2, and dried at room temperature for 45h-50h to obtain pre-oxidized graphene;
[0011] The pre-oxidized graphene is added to concentrated sulfuric acid, and then potassium permanganate is added, and the mixture is stirred in an ice bath for 0.8h-1.2h, and reacted at 45°C-55°C for 8h-72h, and then placed in ice water, and hydrogen peroxide is added for continuous stirring. When a bright yellow color appears, the mixture is allowed to stand for 45h-50h, and the supernatant is discarded to obtain a lower precipitate. The lower precipitate is washed with deionized water and hydrochloric acid respectively until the pH value is 6.8-7.2, and dried at room temperature for 45h-50h to obtain graphene oxide.
[0012] Optionally, the step of derivatizing and modifying the graphene oxide by active oxygen-containing functional groups to graft macromolecular chains onto the surface of the graphene oxide to obtain modified graphene comprises:
[0013] The graphene oxide is added to anhydrous ethanol, ultrasonically dispersed for 25 minutes to 35 minutes, and then a silane coupling agent containing a macromolecular chain is added and magnetically stirred. The graphene oxide is naturally cooled to room temperature after being heated to 65° C. to 75° C. in a water bath and kept warm for 8 hours to 12 hours. The graphene oxide is then filtered and washed to remove the ungrafted silane coupling agent, and dried at room temperature for 45 hours to 50 hours to obtain modified graphene.
[0014] Optionally, the macromolecular chain includes one of an alkane chain, a siloxane molecular chain and a fluorine-containing molecular chain.
[0015] Optionally, the step of blending the modified graphene, the thermoplastic matrix and the plasticizer, drying and screw extruding to obtain the wave-transmitting layer printing filament comprises:
[0016] The modified graphene, thermoplastic matrix and plasticizer are added into a mixer, and grinding balls of different diameters are added, and the speed is set to 45 r / min. -1 -55r·min -1 , the mixing time is 6h-10h to obtain a mixture;
[0017] The mixed material is dried at 110° C. to 130° C. for 11 h to 13 h, added into a screw machine and extruded into filaments through different heating zones, and after cooling, is wound through a traction wheel to obtain a wave-transmitting layer printing filament;
[0018] The temperatures of different heating zones are set to 327°C, 339°C, 343°C, 346°C, 345°C, 343°C and 341°C respectively; the screw speed of the screw machine is 30 r·min -1 -40r·min -1 , winding speed is 9mm·s -1 -13mm·s -1 .
[0019] Optionally, in the step of blending the modified graphene, the thermoplastic matrix and the plasticizer, drying and screw extruding to obtain the wave-transmitting layer printing filament, the thermoplastic matrix includes one of polylactic acid, ABS, nylon, polycarbonate, polyphenylene sulfide, polyetherimide, polyetheretherketone and polyetherketoneketone.
[0020] Optionally, in the step of blending the modified graphene, the thermoplastic matrix and the plasticizer, drying and screw extruding to obtain the wave-transmitting layer printing filament, the content of the modified graphene in the wave-transmitting layer printing filament is 1wt%-20wt%.
[0021] Optionally, in the step of preparing the absorbing layer printing filament with the original graphene and the modified graphene, the mass ratio of the original graphene to the modified graphene is (1-5):(6-9); and the total content of the original graphene and the modified graphene in the absorbing layer printing filament is 1wt%-10wt%.
[0022] Optionally, the step of preparing a wave-transmitting layer cube using the wave-transmitting layer printing filament by melt deposition 3D printing, and orienting the modified graphene in the wave-transmitting layer cube along the X-0° direction, comprises:
[0023] Drawing the model to be printed and slicing it, determining the printing rate and the slice thickness, placing the wave-transmitting layer printing filament in the FDM device, selecting the printing needle, and starting printing along the X-0° direction according to the digital model to prepare a wave-transmitting layer cube, wherein the modified graphene in the wave-transmitting layer cube is oriented along the X-0° direction;
[0024] Wherein, the diameter of the printing needle is set to 0.25mm-0.8mm.
[0025] Optionally, in the step of cutting the wave-transmitting layer cube perpendicularly to the X direction to obtain a flat plate with the modified graphene oriented along the Z-0° direction, the thickness of the flat plate is 0.5 mm-4 mm.
[0026] Optionally, the step of using the upper wave-transparent structure as a substrate, adopting fused deposition 3D printing, preparing a wave-absorbing layer cube on the substrate by printing the wave-absorbing layer filament, and aligning the original graphene and the modified graphene in the wave-absorbing layer cube along the XY direction, that is, obtaining a double-layer heterogeneous wave-absorbing structure, comprises:
[0027] The wave absorbing layer printing filament is placed in an FDM device, the upper wave-transmitting structure is used as a substrate, a printing needle is selected, and printing is started along the direction of 0°+90° or 45° according to the digital model, and a wave absorbing layer cube is prepared on the substrate, so that the original graphene and the modified graphene in the wave absorbing layer cube are both oriented along the XY direction. After printing is completed, the substrate is placed upward, so as to obtain a double-layer heterogeneous wave absorbing structure in which the upper modified graphene is oriented along the Z-0° direction and the lower original graphene and the modified graphene are both oriented along the XY direction;
[0028] Wherein, the diameter of the printing needle is set to 0.25mm-0.8mm, and the thickness of the absorbing layer cube is 0.5mm-4mm.
[0029] The beneficial effects of this application include:
[0030] The present application can not only break the large conjugated structure of the original graphene, regulate the conductivity of the original graphene, and introduce dipole polarization, but also introduce reaction sites to graft macromolecular chains, thereby improving the problem of easy agglomeration between the original graphene, thereby improving the orientation degree of the original graphene along the printing direction, and improving the impedance matching of the original graphene, thereby improving the wave absorption performance of the overall structure;
[0031] The present application constructs a honeycomb-like "wave-transmitting" structure with graphene vertically oriented in the upper layer, which has excellent impedance and is conducive to the incidence of electromagnetic waves, and a "wave-absorbing" structure with graphene vertically and horizontally oriented in the lower layer, which has excellent wave-absorbing performance. The double-layer heterogeneous wave-absorbing structure composed of the two exhibits excellent broadband wave-absorbing ability at low graphene content and low thickness.
[0032] This application arranges the modified graphene in a vertical plane as a "wave-transmitting" channel, and thanks to the excellent mechanical properties and dense composite structure of the modified graphene, compared with the traditional method of introducing gaps or cavities, the overall structure can have excellent mechanical properties and can meet the use requirements of most scenarios;
[0033] This application prepares a double-layer heterogeneous absorbing structure based on the principle of fused deposition 3D printing. The structural design of "wave-transmitting" and "wave-absorbing" is easy to optimize and flexible. It not only has high material utilization and less post-processing processes, but also can shorten the design and manufacturing cycle and reduce production costs. At the same time, various complex structures can be designed according to service requirements, thereby realizing flexible and efficient customization of target components, providing a rapid way for the development and flexible mass production of absorbing components. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.
[0035] Figure 1 A schematic diagram of the modification process of the modified graphene described in the embodiment of the present application;
[0036] Figure 2 Schematic diagram of preparing a double-layer heterogeneous absorbing structure by fused deposition 3D printing as described in an embodiment of the present application, wherein (a) is a schematic diagram of the lower layer of original graphene and modified graphene being oriented along the XY direction; (b) is a schematic diagram of the upper layer of modified graphene being oriented along the Z-0° direction; (c) is a schematic diagram of the orientation of original graphene and modified graphene in the printed filament of the absorbing layer;
[0037] Figure 3 This is a schematic diagram of adding a roller pressing device to the FDM device according to an embodiment of the present application;
[0038] Figure 4 This is a schematic diagram of the effect of the double-layer heterogeneous absorbing structure described in an embodiment of the present application on electromagnetic waves.
[0039] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0040] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0041] At present, the common method to improve graphene absorbing structures is to modify the graphene surface, such as loading magnetic particles and surface oxidation; or to construct special microstructures, such as porous structures and honeycomb structures, to improve interface performance and introduce multiple reflections, thereby improving the absorbing performance of the overall structure. However, the above improvement methods all rely on complex preparation processes and high amounts of graphene addition, resulting in poor mechanical properties of the prepared absorbing components, making it difficult to achieve broadband and efficient absorption of electromagnetic waves, and unable to meet actual application needs. The emerging additive manufacturing (3D printing) technology is based on the principle of discrete stacking, and uses automatic control to stack materials layer by layer to achieve rapid manufacturing of complex parts. It has the advantages of flexible structural design, integrated processing and molding, high preparation accuracy, and short preparation cycle, providing a new way to prepare absorbing parts with complex structures. Among them, fused deposition 3D printing technology (FDM) is a method of melting various fusible filaments or granules by heating, solidifying them layer by layer on the printing table of the machine to finally obtain a three-dimensional component. During the material melting and deposition process, the internal filler will be oriented along the path direction to form a special anisotropic configuration, providing a new path for the design and preparation of new absorbing components.
[0042] In view of the technical problems existing in the prior art, an embodiment of the present application provides a method for preparing a graphene double-layer heterogeneous absorbing structure based on fused deposition 3D printing, comprising the following steps:
[0043] S1. The original graphene is oxidized by the Hummers method to obtain graphene oxide; and the graphene oxide is derivatized and modified by active oxygen-containing functional groups to graft macromolecular chains on the surface of the graphene oxide to obtain modified graphene.
[0044] The present application adopts the Hummers method to oxidize the original graphene, thereby obtaining graphene oxide with a locally destroyed conjugated structure and a large number of oxygen-containing functional groups on the surface, and then the graphene oxide is derivatized and modified to introduce reaction sites on the surface of the graphene oxide to graft macromolecular chains, thereby regulating the conductivity of the original graphene, introducing dipole polarization, improving the problem of easy agglomeration between the original graphene, and then improving the orientation degree of the original graphene along the printing direction, and improving the impedance matching of the original graphene, thereby improving the wave absorption performance of the overall structure.
[0045] Specifically, the Hummers method refers to a method of treating pristine graphene with an inorganic strong proton acid to allow small molecules of strong acid to enter the graphite interlayers, followed by oxidation with a strong oxidant. The graphite oxide obtained by the Hummers method has a wrinkled sheet structure and contains abundant oxygen-containing functional groups, and has good dispersibility in aqueous solution. Pristine graphene is the first untreated two-dimensional material composed of layers of carbon atoms.
[0046] The step of oxidizing the original graphene by the Hummers method to obtain graphene oxide comprises:
[0047] The original graphene, concentrated sulfuric acid, potassium persulfate and phosphorus pentoxide were stirred and mixed, and then heated to 75°C-85°C in an oil bath and kept warm for 4.5h-5.5h, and then naturally cooled to room temperature, and ice water was added for dilution, and then filtered and washed to a pH of 6.8-7.2, and dried at room temperature for 45h-50h to obtain pre-oxidized graphene;
[0048] The pre-oxidized graphene is added to concentrated sulfuric acid, and then potassium permanganate is added, and the mixture is stirred in an ice bath for 0.8h-1.2h, and reacted at 45°C-55°C for 8h-72h, and then placed in ice water, and hydrogen peroxide is added for continuous stirring. When a bright yellow color appears, the mixture is allowed to stand for 45h-50h, and the supernatant is discarded to obtain a lower precipitate. The lower precipitate is washed with deionized water and hydrochloric acid respectively until the pH value is 6.8-7.2, and dried at room temperature for 45h-50h to obtain graphene oxide.
[0049] Furthermore, the step of derivatizing and modifying the graphene oxide by active oxygen-containing functional groups so as to graft macromolecular chains onto the surface of the graphene oxide to obtain modified graphene comprises:
[0050] The graphene oxide is added to anhydrous ethanol, ultrasonically dispersed for 25 minutes to 35 minutes, and then a silane coupling agent containing a macromolecular chain is added and magnetically stirred. The graphene oxide is naturally cooled to room temperature after being heated to 65° C. to 75° C. in a water bath and kept warm for 8 hours to 12 hours. The graphene oxide is then filtered and washed to remove the ungrafted silane coupling agent, and dried at room temperature for 45 hours to 50 hours to obtain modified graphene.
[0051] The grafted macromolecular chain includes one of an alkane chain, a siloxane molecular chain and a fluorine-containing molecular chain, preferably a fluorine-containing molecular chain.
[0052] S2. After blending the modified graphene, the thermoplastic matrix and the plasticizer, drying and screw extrusion are performed to obtain a wave-transmitting layer printing filament; and then the original graphene and the modified graphene are used to prepare a wave-absorbing layer printing filament.
[0053] In a specific implementation process, the modified graphene, the thermoplastic matrix and the plasticizer are blended, and then dried and screw extruded to obtain the wave-transmitting layer printing filament, comprising:
[0054] The modified graphene, thermoplastic matrix and plasticizer are added into a mixer, and grinding balls of different diameters are added, and the speed is set to 45 r / min. -1 -55r·min -1 , the mixing time is 6h-10h to obtain a mixture;
[0055] The mixed material is dried at 110° C. to 130° C. for 11 h to 13 h, added into a screw machine and extruded into filaments through different heating zones, and after cooling, is wound through a traction wheel to obtain a wave-transmitting layer printing filament;
[0056] The temperatures of different heating zones are set to 327°C, 339°C, 343°C, 346°C, 345°C, 343°C and 341°C respectively; the screw speed of the screw machine is 30 r·min -1 -40r·min -1 , winding speed is 9mm·s -1 -13mm·s -1 .
[0057] Specifically, the thermoplastic matrix includes one of polylactic acid, ABS, nylon, polycarbonate, polyphenylene sulfide, polyetherimide, polyetheretherketone and polyetherketoneketone, which can be selected according to the temperature and environmental requirements. The plasticizer can be selected from N-butylbenzenesulfonamide and phthalate.
[0058] Wherein, the content of the modified graphene in the wave-transmitting layer printing filament is 1wt%-20wt%, preferably 2.4wt%.
[0059] In a specific implementation process, the step of preparing the wave absorbing layer printing filament with the original graphene and the modified graphene includes:
[0060] The original graphene, modified graphene, thermoplastic matrix and plasticizer are blended and then dried and screw extruded, wherein the steps of blending, drying and screw extrusion are the same as the steps of preparing the wave-transmitting layer printing filament.
[0061] The mass ratio of the original graphene to the modified graphene is (1-5): (6-9), preferably 1:9; the total content of the original graphene and the modified graphene in the absorbing layer printing filament is 1wt%-10wt%, preferably 1.5wt%.
[0062] S3. Prepare a wave-transmitting layer cube using the wave-transmitting layer printing filament by melt deposition 3D printing, so that the modified graphene in the wave-transmitting layer cube is oriented along the X-0° direction, and then cut the wave-transmitting layer cube perpendicular to the X direction to obtain a flat plate with the modified graphene oriented along the Z-0° direction, which is the upper wave-transmitting structure.
[0063] In a specific implementation process, the step of preparing a wave-transmitting layer cube by using the wave-transmitting layer printing filament through fused deposition 3D printing, and orienting the modified graphene in the wave-transmitting layer cube along the X-0° direction includes:
[0064] The model to be printed is obtained by drawing with Materialise Magics software, and then sliced with Cura software to determine the printing rate and slice thickness, the wave-transmitting layer printing filament is placed in the FDM device, the printing needle is selected, and printing is started along the X-0° direction according to the digital model to prepare a wave-transmitting layer cube, wherein the modified graphene in the wave-transmitting layer cube is oriented along the X-0° direction;
[0065] The diameter of the printing needle is set to 0.25 mm-0.8 mm, preferably 0.6 mm; the thickness of the flat plate is 0.5 mm-4 mm, preferably 1.2 mm.
[0066] The present application arranges the modified graphene in a vertical plane as a "wave-transmitting" channel, thereby obtaining a "honeycomb wave-transmitting" structure with excellent upper impedance and conducive to the incidence of electromagnetic waves. Thanks to the excellent mechanical properties and dense composite structure of the modified graphene, the overall structure has excellent mechanical properties compared to the traditional method of introducing gaps or cavities.
[0067] In the specific implementation process, a roller pressing device can be added to the FDM device, such as Figure 3 As shown, by rolling the wave-transmitting layer printing filament, the orientation degree of the modified graphene in the wave-transmitting layer printing filament along the plane can be improved, and the interlayer bonding force can be improved, thereby increasing the excellent mechanical properties and density of the upper wave-transmitting structure.
[0068] S4. Using the upper wave-transmitting structure as a substrate, using fused deposition 3D printing, preparing a wave-absorbing layer cube on the substrate through the wave-absorbing layer printing filament, so that the original graphene and the modified graphene in the wave-absorbing layer cube are oriented along the XY direction, that is, a double-layer heterogeneous wave-absorbing structure is obtained.
[0069] In a specific implementation process, the wave absorbing layer printing filament is placed in an FDM device, the upper wave-transmitting structure is used as a substrate, a printing needle is selected, and printing is started along the 0°+90° or 45° direction according to the digital model, and a wave absorbing layer cube is prepared on the substrate, so that the original graphene and the modified graphene in the wave absorbing layer cube are oriented along the XY direction. After printing is completed, the substrate is placed upward, so as to obtain a double-layer heterogeneous wave absorbing structure in which the upper modified graphene is oriented along the Z-0° direction and the lower original graphene and the modified graphene are oriented along the XY direction;
[0070] The diameter of the printing needle is set to 0.25 mm-0.8 mm, preferably 0.8 mm, and the thickness of the absorbing layer cube is 0.5 mm-4 mm, preferably 1.6 mm.
[0071] The present application utilizes the characteristics of FDM, firstly prepares a cube with a certain thickness in which modified graphene is oriented along the X-0° direction, and then obtains a flat plate with a certain thickness by cutting perpendicular to the X direction, in which the modified graphene in the flat plate is oriented along the Z-0° direction, forming a wave-transmitting structure similar to a "honeycomb", and then continues to print a wave-absorbing structure containing original graphene and modified graphene of a certain thickness using the flat plate as a substrate, with a path of 0°+90° or 45°. After printing, the product is taken out and the substrate is placed upward to obtain a "wave-transmitting-wave-absorbing" double-layer heterostructure in which the upper graphene is oriented along the Z-0° direction and the lower graphene is oriented along the XY direction. The upper graphene of the double-layer heterostructure is vertically oriented, which is conducive to the incidence of electromagnetic waves and has excellent impedance. The lower graphene is oriented vertically and horizontally in the plane and has excellent wave-absorbing performance, thereby achieving broadband and efficient absorption of electromagnetic waves at a low graphene loading and maintaining good mechanical properties of the structure. In addition, the double-layer heterogeneous structure is prepared by utilizing the principle of additive manufacturing, which not only has high material utilization and fewer post-processing processes, but can also shorten the design and manufacturing cycle and reduce production costs. At the same time, various complex structures can be designed according to service requirements, thereby achieving flexible and efficient customization of target components.
[0072] It should be noted that, in addition to being applicable to a variety of low-dielectric thermoplastic substrates, this method is also applicable to low-dielectric ceramic-based composite materials formed by precursor transformation, such as absorbing silicon oxide, silicon nitride and aluminum oxide.
[0073] In addition, this application is not only applicable to fused deposition 3D printing, but also to a variety of additive manufacturing processes, such as ink direct writing of absorbent polyvinyl alcohol. At the same time, in addition to using filaments as printing materials, it can also be formed by granular fused deposition.
[0074] The above technical solution of the present application is described in detail below in conjunction with specific embodiments.
[0075] Example 1
[0076] A method for preparing a graphene double-layer heterogeneous wave absorbing structure based on fused deposition 3D printing comprises the following steps:
[0077] S1. Modification of pristine graphene.
[0078] like Figure 1 As shown, the original graphene is oxidized according to the improved Hummers method. The oxidation process mainly has two stages:
[0079] Pre-oxidation stage: add original graphene, concentrated sulfuric acid, potassium persulfate and phosphorus pentoxide into a beaker and stir, heat to 80°C in an oil bath and keep for 5 hours, cool naturally to room temperature, slowly add 500 mL of ice water to dilute, finally filter and wash to pH 7, dry at room temperature for 48 hours to obtain pre-oxidized graphene.
[0080] Oxidation stage: Add the above pre-oxidized graphene to 120mL concentrated sulfuric acid, slowly add 9g potassium permanganate, stir in an ice bath for 1h, adjust the temperature to 50℃ and react for 12h. Put the product obtained so far into ice water, add appropriate amount of hydrogen peroxide and stir continuously. When the solution color begins to show bright yellow, it can be left to stand for 48h and the supernatant can be poured out. The lower precipitate is washed with deionized water and hydrochloric acid respectively to make the pH of the product about 7, and dried at room temperature for 48h to obtain the desired graphene oxide.
[0081] The graphene oxide was then derivatized and modified by active oxygen-containing functional groups. 3 g of graphene oxide was added to 500 mL of anhydrous ethanol and dispersed by ultrasound for 30 minutes. Subsequently, 500 mg of fluorinated silane coupling agent was added and magnetically stirred. The mixture was heated to 70°C in a water bath and maintained for 10 hours. The mixture was naturally cooled to room temperature and finally filtered and washed to remove the ungrafted coupling agent. The mixture was dried at room temperature for 48 hours to obtain modified graphene.
[0082] S2. Preparation of printing filament.
[0083] Preparation of wave-transmitting layer printing filament:
[0084] Add modified graphene, polyetheretherketone and plasticizer into the mixing barrel of the V-type mixer, add grinding balls of different diameters, start the drive motor, and set the parameters: the speed is 50r·min -1 , the mixing time is 8h, and the mixture is taken out from the discharge port after the mixing is completed; since the mixing time is as long as 8h, in order to ensure the quality of extrusion, the mixture needs to be dried, and the drying temperature is set to 120℃ and the drying time is 12h; then the blended, dispersed and dried mixture is added to the feeding port of the screw machine, and it undergoes a transformation from solid to glassy state and then to viscous flow state through different heating zones, and finally the desired composite material filament is extruded from the die, and after being cooled by air in the air cooling tank, it is wound by the traction wheel to obtain the wave-transmitting layer printing filament;
[0085] The temperatures of different heating zones were set to 327°C, 339°C, 343°C, 346°C, 345°C, 343°C and 341°C respectively; the screw speed was 35 r·min -1 , winding speed is 11mm·s -1 ; The content of modified graphene in the wave-transmitting layer printing filament is 2.4wt%.
[0086] Preparation of filament for printing the absorbing layer:
[0087] Add the original graphene, modified graphene, polyetheretherketone and plasticizer into the mixing barrel of the V-type mixer, and the remaining steps are the same as the steps for preparing the wave-transmitting layer printing filament;
[0088] The mass ratio of the original graphene to the modified graphene is 1:9; the total content of the original graphene and the modified graphene in the absorbing layer printing filament is 1.5wt%.
[0089] S3, fused deposition 3D printing of the upper wave-transmitting structure.
[0090] The model to be printed is obtained by drawing with Materialise Magics software, and then sliced with Cura software; before printing, the printability of the wave-transmitting layer printing filament needs to be tested to determine the appropriate printing rate and slice thickness; the wave-transmitting layer printing filament is placed in the FDM device, the nozzle diameter is selected to be 0.6mm, and printing is started along the X-0° direction according to the digital model to prepare a cube with a certain thickness of modified graphene oriented along the X-0° direction, and then a flat plate with a thickness of 1.2mm is obtained by cutting the printed cube perpendicular to the X direction, and the modified graphene in the flat plate is oriented along the Z-0° direction.
[0091] S4, fused deposition 3D printing of the lower absorbing structure.
[0092] like Figure 2 As shown, the wave-absorbing layer printing filament is placed in the FDM device, the upper wave-transmitting structure is used as the substrate, the nozzle diameter is selected to be 0.8 mm, and printing is started along the 45° direction according to the digital model to prepare a cube with a thickness of 1.6 mm, in which both the original graphene and the modified graphene are oriented along the XY direction, which is the lower wave-absorbing structure; after printing, the product is taken out and the substrate is placed upward to obtain a "wave-transmitting-wave-absorbing" heterostructure in which the upper modified graphene is oriented along the Z-0° direction and the lower original graphene and the modified graphene are oriented along the XY direction. The action process of the heterostructure on electromagnetic waves is shown in the following figure. Figure 4 shown.
[0093] After testing, the double-layer heterogeneous absorbing structure has a tensile strength of 104MPa and a bending strength of 134MPa. It has excellent mechanical properties and is far superior to conventional porous structures.
[0094] Test example
[0095] The wave absorbing capabilities of the upper wave-transmitting structure, the lower wave-absorbing structure, and the double-layer heterogeneous wave-absorbing structure prepared according to the method described in Example 1 and the graphene wave-absorbing structure prepared by the traditional method were tested respectively. The test results are shown in Table 1 below.
[0096] Table 1
[0097]
[0098] Note: The smaller the reflection loss (RL), the stronger the ability of the absorbing material to absorb electromagnetic waves, that is, the higher the degree to which the interference of electromagnetic waves is reduced.
[0099] As can be seen from Table 1, the double-layer heterogeneous absorbing structure of the present application exhibits excellent broadband absorbing capability at low graphene content (upper layer 2.4wt% + lower layer 1.5wt%) and low thickness (upper layer 1.2mm + lower layer 1.6mm), and the reflection loss in the 8GHz-18GHz band is less than -10dB, achieving full absorption in this band, and its effective absorption (RL<-10dB) bandwidth can reach 8.2GHz. Compared with traditional absorbing structures, the broadband absorbing capability of the double-layer heterogeneous absorbing structure is significantly improved.
[0100] The above description is only an optional embodiment of the present application, and does not limit the patent scope of the present application. All equivalent structural transformations made by using the contents of the present application specification and drawings under the inventive concept of the present application, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present application.
Claims
1. A method for preparing a graphene double-layer heterogeneous absorbing structure based on fused deposition 3D printing, characterized in that: The following steps are involved: The original graphene is oxidized by the Hummers method to obtain graphene oxide; the graphene oxide is then derivatized and modified by active oxygen-containing functional groups to graft macromolecular chains onto the surface of the graphene oxide to obtain modified graphene; The modified graphene, the thermoplastic matrix and the plasticizer are mixed, dried and screw extruded to obtain a wave-transmitting layer printing filament; and the original graphene and the modified graphene are used to prepare a wave-absorbing layer printing filament; By melt deposition 3D printing, a wave-transmitting layer cube is prepared with the wave-transmitting layer printing filament, so that the modified graphene in the wave-transmitting layer cube is oriented along the X-0° direction, and then the wave-transmitting layer cube is cut perpendicular to the X direction to obtain a flat plate with the modified graphene oriented along the Z-0° direction, which is the upper wave-transmitting structure; The upper wave-transmitting structure is used as a substrate, and melt deposition 3D printing is adopted to prepare a wave-absorbing layer cube on the substrate through the wave-absorbing layer printing filament, so that the original graphene and the modified graphene in the wave-absorbing layer cube are oriented along the XY direction, that is, a double-layer heterogeneous wave-absorbing structure is obtained.
2. The method for preparing a graphene double-layer heterogeneous wave absorbing structure based on fused deposition 3D printing according to claim 1, characterized in that: The step of oxidizing the original graphene by the Hummers method to obtain graphene oxide comprises: The original graphene, concentrated sulfuric acid, potassium persulfate and phosphorus pentoxide were stirred and mixed, and then heated to 75°C-85°C in an oil bath and kept warm for 4.5h-5.5h, and then naturally cooled to room temperature, and ice water was added for dilution, and then filtered and washed to a pH of 6.8-7.2, and dried at room temperature for 45h-50h to obtain pre-oxidized graphene; The pre-oxidized graphene is added to concentrated sulfuric acid, and then potassium permanganate is added, and the mixture is stirred in an ice bath for 0.8h-1.2h, and reacted at 45°C-55°C for 8h-72h, and then placed in ice water, and hydrogen peroxide is added for continuous stirring. When a bright yellow color appears, the mixture is allowed to stand for 45h-50h, and the supernatant is discarded to obtain a lower precipitate. The lower precipitate is washed with deionized water and hydrochloric acid respectively until the pH value is 6.8-7.2, and dried at room temperature for 45h-50h to obtain graphene oxide.
3. The method for preparing a graphene double-layer heterogeneous absorbing structure based on fused deposition 3D printing according to claim 1, characterized in that: The step of derivatizing and modifying the graphene oxide by active oxygen-containing functional groups to graft macromolecular chains onto the surface of the graphene oxide to obtain modified graphene comprises: The graphene oxide is added to anhydrous ethanol, ultrasonically dispersed for 25 minutes to 35 minutes, and then a silane coupling agent containing a macromolecular chain is added and magnetically stirred. The graphene oxide is naturally cooled to room temperature after being heated to 65° C. to 75° C. in a water bath and kept warm for 8 hours to 12 hours. The graphene oxide is then filtered and washed to remove the ungrafted silane coupling agent, and dried at room temperature for 45 hours to 50 hours to obtain modified graphene.
4. The method for preparing a graphene double-layer heterogeneous wave absorbing structure based on fused deposition 3D printing according to claim 1 or 3, characterized in that: The macromolecular chain includes one of an alkane chain, a siloxane molecular chain and a fluorine-containing molecular chain.
5. The method for preparing a graphene double-layer heterogeneous wave absorbing structure based on fused deposition 3D printing according to claim 1, characterized in that: The step of blending the modified graphene, the thermoplastic matrix and the plasticizer, drying and screw extruding to obtain the wave-transmitting layer printing filament comprises: The modified graphene, thermoplastic matrix and plasticizer are added into a mixer, and grinding balls of different diameters are added, and the speed is set to 45 r / min. -1 -55r·min -1 , the mixing time is 6h-10h to obtain a mixture; The mixed material is dried at 110° C. to 130° C. for 11 h to 13 h, added into a screw machine and extruded into filaments through different heating zones, and after cooling, is wound through a traction wheel to obtain a wave-transmitting layer printing filament; The temperatures of different heating zones are set to 327°C, 339°C, 343°C, 346°C, 345°C, 343°C and 341°C respectively; the screw speed of the screw machine is 30 r·min -1 -40r·min -1 , winding speed is 9mm·s -1 -13mm·s -1 .
6. The method for preparing a graphene double-layer heterogeneous wave absorbing structure based on fused deposition 3D printing according to claim 1 or 5, characterized in that: In the step of blending the modified graphene, the thermoplastic matrix and the plasticizer, drying and screw extruding to obtain the wave-transmitting layer printing filament, the thermoplastic matrix includes one of polylactic acid, ABS, nylon, polycarbonate, polyphenylene sulfide, polyetherimide, polyetheretherketone and polyetherketoneketone.
7. The method for preparing a graphene double-layer heterogeneous wave absorbing structure based on fused deposition 3D printing according to claim 1 or 5, characterized in that: In the step of blending the modified graphene, the thermoplastic matrix and the plasticizer, drying and screw extruding to obtain the wave-transmitting layer printing filament, the content of the modified graphene in the wave-transmitting layer printing filament is 1wt%-20wt%.
8. The method for preparing a graphene double-layer heterogeneous wave absorbing structure based on fused deposition 3D printing according to claim 1, characterized in that: In the step of preparing the wave absorbing layer printing filament with the original graphene and the modified graphene, the mass ratio of the original graphene to the modified graphene is (1-5):(6-9); the total content of the original graphene and the modified graphene in the wave absorbing layer printing filament is 1wt%-10wt%.
9. The method for preparing a graphene double-layer heterogeneous wave absorbing structure based on fused deposition 3D printing according to claim 1, characterized in that: The step of preparing a wave-transmitting layer cube by using the wave-transmitting layer printing filament through melt deposition 3D printing, and orienting the modified graphene in the wave-transmitting layer cube along the X-0° direction, comprises: Drawing the model to be printed and slicing it, determining the printing rate and the slice thickness, placing the wave-transmitting layer printing filament in the FDM device, selecting the printing needle, and starting printing along the X-0° direction according to the digital model to prepare a wave-transmitting layer cube, wherein the modified graphene in the wave-transmitting layer cube is oriented along the X-0° direction; Wherein, the diameter of the printing needle is set to 0.25mm-0.8mm.
10. The method for preparing a graphene double-layer heterogeneous wave absorbing structure based on fused deposition 3D printing according to claim 1, characterized in that: In the step of cutting the wave-transmitting layer cube perpendicularly to the X direction to obtain a flat plate with the modified graphene oriented along the Z-0° direction, the thickness of the flat plate is 0.5 mm-4 mm.
11. The method for preparing a graphene double-layer heterogeneous wave absorbing structure based on fused deposition 3D printing according to claim 1, characterized in that: The step of using the upper wave-transmitting structure as a substrate, adopting fused deposition 3D printing, preparing a wave-absorbing layer cube on the substrate by using the wave-absorbing layer printing filament, and making the original graphene and the modified graphene in the wave-absorbing layer cube oriented along the XY direction, that is, obtaining a double-layer heterogeneous wave-absorbing structure, comprises: The wave absorbing layer printing filament is placed in an FDM device, the upper wave-transmitting structure is used as a substrate, a printing needle is selected, and printing is started along the direction of 0°+90° or 45° according to the digital model, and a wave absorbing layer cube is prepared on the substrate, so that the original graphene and the modified graphene in the wave absorbing layer cube are both oriented along the XY direction. After printing is completed, the substrate is placed upward, so as to obtain a double-layer heterogeneous wave absorbing structure in which the upper modified graphene is oriented along the Z-0° direction and the lower original graphene and the modified graphene are both oriented along the XY direction; Wherein, the diameter of the printing needle is set to 0.25mm-0.8mm, and the thickness of the absorbing layer cube is 0.5mm-4mm.
Citation Information
Patent Citations
Flexible circuit conductive composition and 3D (three dimensional) printing based flexible circuit construction method
CN105623215A
Graphene / polyimide composite foam wave-absorbing material with oriented pore structure and preparation method of graphene / polyimide composite foam wave-absorbing material
CN113321844A
3D printing reduced graphene oxide / polylactic acid composite wave-absorbing wire and preparation method thereof
CN116575140A
Shape memory polymer inks and methods of printing the same
US10906238B1
3D print bed having permanent coating
WO2015149054A1