Method for forming prepreg in non-autoclave

By using the design of multi-layer film and sealed space in the non-hot press tank prepreg molding, combined with vacuum and pressurization technology, the problems of high porosity and bridge defects of composite materials are solved, and an efficient forming process is achieved and low porosity finished products.

CN118927668APending Publication Date: 2024-11-12LANZHOU UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411265230.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the absence of hot pressing tanks, the porosity of composite parts is difficult to reduce, especially in the double diaphragm molding method, due to the limited vacuum negative pressure, the prepreg cannot fully adhere to the mold's femoral angle, forming a bridge defect. And the gas cannot be completely discharged, resulting in high porosity.

Method used

By adopting a non-hot press tank prepreg molding method, by forming a second sealing space between the upper and lower films, and providing the first and third sealing spaces in the molding device, vacuum and pressurization techniques are ensured. After the gas is discharged, the negative pressure on the third sealing space is increased to pressurize the first sealing space until the prepreg is fully fitted with the mold, and the bridging defects are eliminated.

Benefits of technology

A simple and efficient molding process is realized, ensuring that the prepreg resin fully impregnates the fibers, eliminates pores and bridge defects, and improves the molding quality of the composite material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118927668A_ABST
    Figure CN118927668A_ABST
Patent Text Reader

Abstract

A method for forming non-autoclave prepreg relates to the technical field of prepreg forming and comprises the following steps: S1, laminating non-autoclave prepreg between an upper film and a lower film; s2, placing the upper-layer film and the lower-layer film in a forming device; s3, the forming device is placed in heating equipment; s4, vacuumizing equipment is used for vacuumizing the first sealed space, the second sealed space and the third sealed space at the same time; s5, the first inflation and deflation connector and the third inflation and deflation connector are disconnected from the vacuumizing equipment; s6, negative pressure pumping is conducted on the third sealed space; pressurizing the first sealed space; s7, the temperature of the forming device is increased to the forming temperature of the non-autoclave prepreg lamination layer, and heat preservation is conducted till the non-autoclave prepreg lamination layer is solidified; s8, demolding is conducted; according to the method, the problem that bridging defects easily occur at the internal corner position of the mold in the non-autoclave prepreg lamination is effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of prepreg molding, in particular to a method for non-autoclave prepreg molding. Background Art

[0002] When manufacturing composite parts, the aerospace industry often uses automatic tape laying equipment to lay thermosetting prepreg into laminated flat plates to ensure that the manufactured composite parts have accurate fiber volume ratios and laying angles. Then, the preforms are obtained through a hot diaphragm molding process, and finally the preforms are sent to an autoclave for curing. During curing, the high pressure of 0.3 to 0.8 MPa can cause bubbles such as enclosed air or generated volatiles to rupture, thereby effectively inhibiting the generation of pores. Therefore, the use of an autoclave curing process can ensure that the porosity of the cured parts is extremely low (less than 1%), thereby improving their mechanical properties and reliability.

[0003] Under the demand for low-cost and ultra-large-scale manufacturing of composite parts, the autoclave process with large investment and high energy consumption has become a "bottleneck" that restricts the widespread application of composite materials. Therefore, researchers have explored new technologies that can achieve the manufacturing of low-porosity parts without the use of autoclave curing conditions, collectively referred to as non-autoclave processes. By developing this process, it aims to break through the original technical bottleneck and achieve efficient and energy-saving large-scale production of composite parts.

[0004] In the context of non-autoclave processes that do not have a high-pressure environment, how to effectively reduce the porosity of the parts has become a core challenge that needs to be overcome. Among them, the double vacuum bag molding process is a valuable practical exploration. This process adjusts the pressure difference between the inner and outer vacuum bags to achieve dynamic compaction of the non-autoclave prepreg stack during vacuuming and heating curing, thereby promoting the discharge of interlayer gas and other volatiles.

[0005] In recent years, a new branch of hot diaphragm technology, the double diaphragm molding method, combined with automatic tape laying technology, has the advantages of high stacking efficiency and good quality of molded parts. The autoclave equipment used in this process has significant advantages in achieving low porosity, but it is also accompanied by problems such as high investment costs and excessive energy consumption. If the autoclave is abandoned and the DDF process is directly used to manufacture composite parts, the problem of high porosity is often faced; at the same time, the vacuum negative pressure is limited during vacuuming, resulting in the prepreg being unable to fully fit the mold inner corner, forming a bridging defect.

[0006] A Chinese patent (Announcement No.: CN106142587A) discloses a composite material double-bag hot diaphragm preforming method; the patent first encapsulates the prepreg layer in a double-diaphragm bag composed of an inner diaphragm bag and an outer diaphragm bag, and then installs the double-diaphragm bag containing the prepreg layer on a preforming device to perform double-bag hot diaphragm preforming; after the prepreg is stacked, the prepreg layer is placed on a layer of diaphragm, and breathable felt is evenly placed around the prepreg layer. Then, a layer of diaphragm is used to cover the prepreg layer, and the inner diaphragm bag is encapsulated with sealing putty; the method has cumbersome operating steps and complex processes; in addition, during the operation, it was found that when the outer diaphragm bag was evacuated, the vacuum negative pressure was limited, resulting in the prepreg being unable to fully fit the mold inner corner, resulting in a bridging defect; at the same time, when the prepreg layer of the patent was vented, it was under pressure, resulting in the inability to completely discharge the entrained gas, resulting in a defect of high porosity. Summary of the invention

[0007] In order to overcome the deficiencies in the background technology, the present invention discloses a method for non-autoclave prepreg molding.

[0008] In order to achieve the above-mentioned invention object, the present invention adopts the following technical scheme: A method for non-autoclave prepreg molding, comprising the following steps: S1. Place the non-autoclave prepreg laminate between the upper film and the lower film, seal the upper film and the lower film on all sides to form a second sealed space, and set a second charging and discharging interface corresponding to the second sealed space; S2, placing the upper film and the lower film in a molding device, forming a first sealed space between the upper film and the molding device, and providing a first gas charging and discharging interface corresponding to the first sealed space; forming a third sealed space between the lower film and the molding device, and providing a third gas charging and discharging interface corresponding to the third sealed space, and providing a mold for laminating non-autoclave prepreg in the third sealed space; S3, placing the molding device in a heating device, heating to the preforming temperature of the non-autoclave prepreg stack, the temperature value is 70°C to 90°C; S4, using a vacuuming device to simultaneously vacuum the first sealed space, the second sealed space, and the third sealed space through the first charging and discharging interface, the second charging and discharging interface, and the third charging and discharging interface; and making the vacuum degree of the first sealed space = the vacuum degree of the third sealed space ≥ the vacuum degree of the second sealed space; and maintaining the pressure until the gas in the non-autoclave prepreg laminate is completely discharged; S5. Maintain the negative pressure in the second sealed space, disconnect the first and third charging and discharging interfaces from the vacuum pumping device, and connect them to the atmosphere; S6, keep the second sealed space under negative pressure, connect the third gas charging and discharging interface with the vacuum pumping device, and apply negative pressure to the third sealed space; connect the first gas charging and discharging interface with the gas charging device, and pressurize the first sealed space at a pressure of 0.2-0.5 MPa, until the non-autoclave prepreg laminate is completely fitted with the mold; S7, raising the temperature of the molding device to the molding temperature of the non-autoclave prepreg stack, the temperature value is 110° C. to 140° C., and keeping the temperature until the non-autoclave prepreg stack is cured; S8, cancel the heat preservation, wait for the temperature to cool to the demoulding temperature, turn off the vacuum equipment, and demould.

[0009] Preferably, in step S1, a release layer is provided between the non-autoclave prepreg laminate and the upper film and between the non-autoclave prepreg laminate and the lower film; the release layer is an isolation film or a release agent coated on the surface of the non-autoclave prepreg laminate.

[0010] Preferably, the molding device includes an external fixed frame fixedly connected to a molding box body that cooperates with the lower film to form a third sealed space, and a sealing cover that is detachably connected to the upper side of the external fixed frame corresponding to the molding box body and is used to cooperate with the upper film to form a first sealed space; a pressurizing stud for tightening the sealing cover is provided between the external fixed frame and the sealing cover.

[0011] Preferably, a diaphragm sealing frame is provided between the upper film and the lower film for forming a second sealed space between the upper film and the lower film, and the diaphragm sealing frame is provided with a second gas charging and discharging interface correspondingly connected to the second sealed space.

[0012] Preferably, sealing rings are provided between the sealing cover and the upper film and between the molding box and the lower film.

[0013] Preferably, the third air charging and discharging interface passes through the inner corner of the mold and is correspondingly connected to the third sealed space.

[0014] Preferably, the upper film and the lower film are high molecular polymers.

[0015] Preferably, the high molecular polymer is silicone rubber, high performance polyamide (PA) or polyimide (PI) film.

[0016] Due to the adoption of the above-mentioned technical solution, the present invention has the following beneficial effects: (1) The present invention discloses a method for non-autoclave prepreg molding, which is simple to operate and has high molding efficiency. A vacuum pump is used to make the vacuum degree of the first sealed space = the vacuum degree of the third sealed space ≥ the vacuum degree of the second sealed space. At this time, the second sealed space will not be compressed, and the non-autoclave prepreg stack will not be pressed by the upper film and the lower film. This state is maintained until the gas between the upper film and the lower film is exhausted, so that the resin in the non-autoclave prepreg stack can fully infiltrate the fibers, and at the same time, the gas resistance in the subsequent compaction process and the pores that may be caused by the gas are eliminated. (2) The present invention further connects the third air charging and discharging interface with the vacuum pumping device while maintaining the negative pressure in the second sealed space, thereby applying negative pressure to the third sealed space; then connects the first air charging and discharging interface with the inflation device, thereby pressurizing the first sealed space, until the non-autoclave prepreg laminate is completely fitted to the mold, at which point the bridging defect of the non-autoclave prepreg laminate at the inner corner of the mold disappears. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a structural schematic diagram of the present invention; Figure 2 It is a schematic diagram of the changing state in step S4; Figure 3 It is a schematic diagram of the changing state in step S5; Figure 4 This is a schematic diagram of the changing state when the inflation device is not connected in step S6; Figure 5 This is a schematic diagram of the changing state when the inflation device is connected in step S6.

[0018] In the figure: 1. External fixing frame; 2. Pressurized studs; 3. Sealing cover; 4. Sealing ring; 5. Diaphragm sealing frame; 6. Upper film; 7. Lower film; 8. Mould; 9. Forming box; 10. Non-autoclave prepreg stack. DETAILED DESCRIPTION

[0019] The present invention can be explained in detail through the following embodiments. The purpose of disclosing the present invention is to protect all technical improvements within the scope of the present invention. In the description of the present invention, it should be understood that if there are terms such as "upper", "lower", "front", "back", "left", "right", etc. indicating directions or positional relationships, they only correspond to the drawings of the present application for the convenience of describing the present invention, and do not indicate or imply that the device or element referred to must have a specific direction.

[0020] Combined with Figures 1 to 5 , a method for non-autoclave prepreg molding, comprising the following steps: S1. Place the non-autoclave prepreg laminate 10 between the upper film 6 and the lower film 7. The upper film 6 and the lower film 7 are sealed on all sides to form a second sealed space, and a second gas charging and discharging interface corresponding to the second sealed space is provided; as needed, a release agent can be applied to the upper film 6 and the lower film 7, or an isolation film can be laid between the upper film 6 and the non-autoclave prepreg laminate 10 and between the lower film 7 and the non-autoclave prepreg laminate 10 to facilitate subsequent demoulding operations; The upper film 6 and the lower film 7 are high molecular polymers, such as silicone rubber, high-performance polyamide (PA) or polyimide (PI) films; The non-autoclave prepreg laminate 10 can be a certain company model ACTECH ® 1203 / GW700S / 38 Medium temperature curing epoxy carbon fiber unidirectional tape prepreg.

[0021] S2, placing the upper film 6 and the lower film 7 in a molding device, forming a first sealed space between the upper film 6 and the molding device, and providing a first gas charging and discharging interface corresponding to the first sealed space; forming a third sealed space between the lower film 7 and the molding device, and providing a third gas charging and discharging interface corresponding to the third sealed space, and providing a mold 8 for molding the non-autoclave prepreg laminate 10 in the third sealed space; It should be noted that the third air filling and discharging interface passes through the inner corner of the mold 8 and is connected to the corresponding third sealed space, which can further prevent the non-autoclave prepreg laminate 10 from bridging at the inner corner of the mold 8.

[0022] The molding device comprises an external fixed frame 1 fixedly connected to a molding box 9 which cooperates with a lower film 7 to form a third sealed space, that is, the mold 8 is located in the molding box 9; the external fixed frame 1 is detachably connected to a sealing cover 3 which is used to cooperate with an upper film 6 to form a first sealed space above the molding box 9, that is, after the operation of step S1, the upper film 6 and the lower film 7 can be placed on the top of the molding box 9, and the non-autoclave prepreg laminate 10 is made to correspond to the mold 8, and then the sealing cover 3 is covered on the upper film 6; a pressurizing stud 2 for pressing the sealing cover 3 is provided between the external fixed frame 1 and the sealing cover 3, that is, the pressurizing stud 2 is threadedly connected to the external fixed frame 1, and the pressurizing stud 2 can be screwed to squeeze the sealing cover 3, and the sealing cover 3 presses down the upper film 6 and the lower film 7, so that a first sealed space is formed between the upper film 6 and the sealing cover 3, and a third sealed space is formed between the lower film 7 and the molding box 9; It should be noted that the pressurizing stud 2 is rotatably connected to the top of the sealing cover 3, which makes it easy for the operator to screw the pressurizing stud 2, thereby adjusting the downward pressure of the pressurizing stud 2 on the sealing cover 3; Furthermore, a diaphragm sealing frame 5 is provided between the upper film 6 and the lower film 7 to form a second sealed space between the upper film 6 and the lower film 7, and the diaphragm sealing frame 5 is provided with a second gas charging and discharging interface corresponding to the second sealed space; the diaphragm sealing frame 5 can not only seal the upper film 6 and the lower film 7 on all sides, but also space the upper film 6 and the lower film 7 to form a second sealed space; through the extrusion of the sealing cover 3, the upper film 6 and the lower film 7 are both in close contact with the diaphragm sealing frame 5, thereby achieving the purpose of sealing the second sealed space; Furthermore, sealing rings 4 are provided between the sealing cover 3 and the upper film 6 and between the forming box 9 and the lower film 7 , and the first sealing space and the third sealing space can be quickly formed by squeezing the sealing cover 3 .

[0023] S3, placing the molding device in a heating device, and heating it to the preforming temperature of the non-autoclave prepreg laminate 10, the temperature value being 70°C to 90°C.

[0024] S4, using a vacuuming device to simultaneously vacuum the first sealed space, the second sealed space, and the third sealed space through the first charging and discharging interface, the second charging and discharging interface, and the third charging and discharging interface; and making the vacuum degree of the first sealed space = the vacuum degree of the third sealed space ≥ the vacuum degree of the second sealed space; and maintaining the pressure until the gas in the non-autoclave prepreg laminate 10 is completely discharged; It should be noted that if Figure 2 As shown, at this time, the second sealed space will not be compressed, and the non-autoclave prepreg laminate 10 will not be compressed by the upper film 6 and the lower film 7; this state is maintained until the gas between the upper film 6 and the lower film 7 is discharged, so that the resin in the non-autoclave prepreg laminate 10 can fully infiltrate the fibers, while eliminating the gas resistance of the subsequent compaction process and the pores that may be caused by the gas.

[0025] S5. Maintain the negative pressure in the second sealed space, disconnect the first and third charging and discharging interfaces from the vacuum pumping device, and connect them to the atmosphere; It should be noted that at this time, the upper film 6 and the lower film 7 compact the non-autoclave prepreg laminate 10 under the pressure difference; Figure 3 As shown, the upper film 6 and the lower film 7 impose certain constraints on the non-autoclave prepreg laminate 10, which can ensure the stability of the non-autoclave prepreg laminate 10 in the subsequent mold bonding process and further discharge the included gas.

[0026] S6. Maintain the negative pressure in the second sealed space, connect the third gas filling and discharging interface with the vacuum pumping device, and pump negative pressure into the third sealed space. Figure 4As shown, at this time, the non-autoclave prepreg laminate 10 has a bridging defect at the inner corner of the mold 8; the first inflation and deflation interface is connected to the inflation device, and the first sealed space is pressurized with a pressure value of 0.2-0.5MPa until the non-autoclave prepreg laminate 10 is completely attached to the mold 8. Figure 5 As shown, at this time, the bridging defect of the non-autoclave prepreg laminate 10 at the inner corner of the mold 8 disappears; It should be noted that by inflating and pressurizing the first sealed space with an inflation device, the non-autoclave prepreg laminate 10 can be made to completely fit the mold, thereby suppressing the generation of voids and eliminating bridging phenomena.

[0027] S7, raising the temperature of the molding device to the molding temperature of the non-autoclave prepreg laminate 10, the temperature value is 110°C to 140°C, and maintaining the temperature until the non-autoclave prepreg laminate 10 is cured.

[0028] S8, cancel the heat preservation, wait until the temperature is cooled to the demoulding temperature, turn off the vacuum equipment, and connect the first charging and discharging interface, the second charging and discharging interface and the third charging and discharging interface to the atmosphere, and then demould.

[0029] The parts of the present invention that are not described in detail are prior art. It is obvious to those skilled in the art that the present invention is not limited to the details of the above-mentioned exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic characteristics of the present invention; therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive, and it is intended that all changes that fall within the meaning and scope of equivalent elements are included in the present invention.

Claims

1. A method for non-autoclave prepreg molding, characterized in that: The following steps are involved: S1, placing the non-autoclave prepreg laminate (10) between the upper film (6) and the lower film (7), sealing the upper film (6) and the lower film (7) on all sides to form a second sealed space, and providing a second gas charging and discharging interface connected to the second sealed space; S2, placing the upper film (6) and the lower film (7) in a molding device, forming a first sealed space between the upper film (6) and the molding device, and providing a first gas charging and discharging interface corresponding to the first sealed space; forming a third sealed space between the lower film (7) and the molding device, and providing a third gas charging and discharging interface corresponding to the third sealed space, and providing a mold (8) in the third sealed space for molding the non-autoclave prepreg laminate (10); S3, placing the molding device in a heating device, and heating it to the preforming temperature of the non-autoclave prepreg stack (10), the temperature being 70°C to 90°C; S4, using a vacuuming device to simultaneously vacuum the first sealed space, the second sealed space, and the third sealed space through the first charging and discharging interface, the second charging and discharging interface, and the third charging and discharging interface; and making the vacuum degree of the first sealed space = the vacuum degree of the third sealed space ≥ the vacuum degree of the second sealed space; and maintaining the pressure until the gas in the non-autoclave prepreg stack (10) is completely discharged; S5. Maintain the negative pressure of the second sealed space, and adjust the negative pressure to 0.02-0.04 MPa, so that the first and third charging and discharging interfaces are disconnected from the vacuum equipment and connected to the atmospheric environment; S6, maintaining negative pressure in the second sealed space, connecting the third air charging and discharging interface to the vacuum pumping device, and discharging negative pressure in the third sealed space; connecting the first air charging and discharging interface to the inflation device, and pressurizing the first sealed space, with a pressure value of 0.2 to 0.5 MPa, until the non-autoclave prepreg stack (10) is completely fitted to the mold (8); S7, raising the temperature of the molding device to a molding temperature of the non-autoclave prepreg stack (10), the temperature being 110° C. to 140° C., and maintaining the temperature until the non-autoclave prepreg stack (10) is cured; S8, cancel the heat preservation, wait for the temperature to cool to the demoulding temperature, turn off the vacuum equipment, and demould.

2. The method for non-autoclave prepreg molding according to claim 1, characterized in that: In S1, a release layer is provided between the non-autoclave prepreg laminate (10) and the upper film (6) and between the non-autoclave prepreg laminate (10) and the lower film (7); the release layer is an isolation film or a release agent coated on the surface of the non-autoclave prepreg laminate (10).

3. The method for non-autoclave prepreg molding according to claim 1, characterized in that: The molding device comprises an external fixed frame (1) fixedly connected to a molding box (9) for cooperating with a lower film (7) to form a third sealed space; a sealing cover (3) for cooperating with an upper film (6) to form a first sealed space is detachably connected to the upper portion of the external fixed frame (1) corresponding to the molding box (9); and a pressurizing stud (2) for pressing the sealing cover (3) is provided between the external fixed frame (1) and the sealing cover (3).

4. The method for non-autoclave prepreg molding according to claim 1 or 3, characterized in that: A diaphragm sealing frame (5) is provided between the upper film (6) and the lower film (7) for forming a second sealed space between the upper film (6) and the lower film (7), and the diaphragm sealing frame (5) is provided with a second gas charging and discharging interface corresponding to the second sealed space.

5. The method for non-autoclave prepreg molding according to claim 3, characterized in that: A sealing ring (4) is provided between the sealing cover (3) and the upper film (6), and between the molding box (9) and the lower film (7).

6. The method for non-autoclave prepreg molding according to claim 1, characterized in that: The third gas charging and discharging interface passes through the inner corner of the mold (8) and is correspondingly connected to the third sealed space.

7. The method for non-autoclave prepreg molding according to claim 1, characterized in that: The upper film (6) and the lower film (7) are high molecular polymers.

8. The method for non-autoclave prepreg molding according to claim 7, characterized in that: The high molecular polymer is silicone rubber, high performance polyamide (PA) or polyimide (PI) film.