Silicon-carbon composite material with silicon-carbon alternate multi-level structure and preparation method and application thereof

By growing carbon nanotubes in situ inside and on the surface of porous carbon, a three-dimensional conductive network structure of silicon-carbon alternating multi-level composite material is formed, which solves the problem of poor stability of porous carbon matrix and improves the cycle performance and specific capacity of lithium-ion battery.

CN118929633APending Publication Date: 2024-11-12YINSI (NINGBO) TECH CO LTD

Patent Information

Application Number
CN202411192592.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing porous carbon matrix has poor pore structure stability, and the material's crystal structure collapses severely during repeated lithium-ion insertion and extraction, resulting in poor cycle performance of lithium-ion batteries.

Method used

Carbon nanotubes were grown in situ inside and on the surface of porous carbon using chemical vapor deposition to form a three-dimensional conductive network structure. A silicon-carbon composite material with alternating silicon-carbon multilevel structure was prepared by silane deposition and carbon coating.

Benefits of technology

It improves the structural stability and conductivity of the material, alleviates the volume expansion of silicon-based anodes, and enhances the specific capacity and cycle performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929633A_ABST
    Figure CN118929633A_ABST
Patent Text Reader

Abstract

The invention provides a silicon-carbon composite material with a silicon-carbon alternate multi-level structure as well as a preparation method and application thereof, and belongs to the technical field of lithium ion batteries. According to the preparation method disclosed by the invention, the carbon nanotubes are firstly grown on the porous carbon skeleton in situ, then silane deposition and carbon coating are carried out, and in the prepared silicon-carbon composite material, the carbon nanotubes are embedded into the porous carbon structure and uniformly grow in and on the surface of the porous carbon structure to form a three-dimensional conductive network structure, so that the structural stability of the silicon-carbon negative electrode material is improved; and the in-situ growth of the carbon nanotube network can improve the conductivity of the material, alleviate the volume expansion of the silicon-based negative electrode, and improve the specific capacity and cycle performance of the silicon-based negative electrode material. Meanwhile, a silicon / carbon multi-level alternate structure is formed by adopting silicon / carbon alternate multi-level deposition, so that the structural stability of the material can be improved, structural collapse can be avoided, and the specific capacity and the cycle performance of the silicon-carbon negative electrode material can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a silicon-carbon composite material with a silicon-carbon alternating multi-layer structure, and a preparation method and application thereof. Background Art

[0002] In recent years, the rapid development of portable electronic devices, electric vehicles, aerospace, etc. has brought opportunities for the rapid development of lithium-ion batteries. However, as a commercial negative electrode material for lithium-ion batteries, graphite has a low theoretical specific capacity and can no longer meet market demand. Si has a high theoretical specific capacity (4200mAh / g) and a relatively low discharge voltage (~0.4V), but its lithiation process is accompanied by a huge volume change (>300%) and a low conductivity (6.7×10 - 4 S / cm) also limits the transport of ions / electrons, resulting in unsatisfactory cycle performance, and limiting market promotion and application. The current main solution strategy is to nano-scale or composite it. However, nano-sized silicon particles are easy to agglomerate, resulting in battery capacity decay, and the cost is high and the process is complicated, which poses difficulties in practical applications. Composite silicon with other materials (such as graphene, carbon nanotubes, etc.) can improve its conductivity, thereby improving the specific capacity and cycle performance of silicon-based negative electrodes. Surface carbon coating can inhibit silicon surface oxidation, and the addition of porous structure conductive materials is beneficial to improving lithium ion transmission capacity and the release of volume expansion stress, thereby obtaining a high-stability negative electrode. For example, patent CN114695865A synthesizes Si@Si / C@C with a multi-layer core-shell structure similar to watermelon pulp, which is used to improve the cycle performance of silicon particles. However, it still faces the problem of gas production caused by silicon particle expansion during the cycle, and there is still room for improvement in the cycle performance; patent CN114976026A obtains silicon-carbon negative electrode material by depositing nano-silicon inside porous carbon and then coating the porous carbon with gas-phase carbon. However, its porous structure is unstable and the structure easily collapses during lithium ion insertion and extraction, resulting in poor rate performance and reduced cycle stability. Summary of the invention

[0003] The purpose of the present invention is to provide a silicon-carbon composite material with a silicon-carbon alternating multi-level structure and a preparation method and application thereof, so as to solve the problem of poor pore structure stability of the existing porous carbon matrix and the problem of serious collapse of the material lattice structure caused by repeated insertion and extraction of lithium ions.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing a silicon-carbon composite material with a silicon-carbon alternating multi-level structure, comprising the following steps:

[0006] carbonizing the first carbon source to obtain a carbon precursor;

[0007] The carbon precursor is mixed with an activator and subjected to a first sintering to obtain a porous carbon skeleton;

[0008] Compounding the porous carbon skeleton with a metal catalyst to obtain a porous carbon-catalyst precursor;

[0009] The porous carbon-catalyst precursor is mixed with a second carbon source, and a second sintering is performed, and the obtained porous carbon-carbon nanotube precursor is acid-washed to obtain porous carbon-carbon nanotubes;

[0010] Using a pulse deposition method, under a protective gas condition, the porous carbon-carbon nanotube is deposited under a silane gas condition to obtain a silane-deposited porous carbon-carbon nanotube precursor;

[0011] A carbon source gas is introduced to carbon-coat the silane-deposited porous carbon-carbon nanotube precursor, and the deposition and carbon coating are repeated alternately to obtain a silicon-carbon composite material with a silicon-carbon alternating multi-level structure.

[0012] Preferably, the first carbon source includes one or more of rice, wheat flour, soybean meal, rapeseed, fish scales, green leaves, fungus, bark, sugarcane, rice husks, epoxy resin, phenolic resin, asphalt and chitosan; the carbonization temperature is 300-800°C, and the time is 1-3h; the heating rate to the carbonization temperature is 1-20°C / min.

[0013] Preferably, the activator includes one or more of calcium carbonate, magnesium oxide, iron oxide, potassium hydroxide, sodium hydroxide, sodium chloride and zinc chloride; the mass ratio of the carbon precursor to the activator is 1:2-10; the temperature of the first sintering is 500-900°C, and the time is 2-6h; the heating rate to the first sintering temperature is 1-20°C / min.

[0014] Preferably, the metal catalyst includes one or more of cobalt chloride, cobalt nitrate, cobalt sulfate, nickel chloride, nickel nitrate, nickel sulfate, cupric chloride, cupric nitrate, cupric sulfate and ferrocene; the mass ratio of the metal catalyst to the porous carbon skeleton is (1-25):1; the composite method is immersion or spraying; and the composite time is 2-12 hours.

[0015] Preferably, the second carbon source includes one or more of methane, ethane, propane, acetylene and propyne; and the flow rate of the second carbon source is 0.5 to 5 L / min.

[0016] Preferably, the temperature of the second sintering is 300-900° C., and the time is 5-30 min; the acid used for the pickling includes one or more of hydrochloric acid, nitric acid, sulfuric acid and phosphoric acid.

[0017] Preferably, the silane gas includes one or more of silane, disilane, tetrafluorosilane, hexamethyldisilane, dichlorodimethylsilane and trimethylsilane; the protective gas includes one or more of nitrogen, argon and helium, and the deposition conditions include: the deposition temperature is 500-600°C, the deposition time is 100-200s, the silane gas flow rate is 1-8L / min, and the flow ratio of silane gas to protective gas is 1:1-15.

[0018] Preferably, the carbon source gas includes one or more of methane, ethane, propane, acetylene, propyne, acetone and cyclohexane; the carbon coating conditions include: the deposition temperature is 600-900°C, the deposition time is 100-200s, the carbon source gas flow rate is 1-8L / min; the flow ratio of the carbon source gas to the protective gas is 1:1-15.

[0019] The present invention provides a silicon-carbon composite material with a silicon-carbon alternating multi-layer structure prepared by the preparation method described in the above technical solution, wherein the Si content is 10-90wt% and the carbon content is 10-90wt%.

[0020] The present invention provides the application of the silicon-carbon composite material with the silicon-carbon alternating multi-layer structure described in the above technical solution in lithium-ion batteries.

[0021] The present invention provides a method for preparing a silicon-carbon composite material with a silicon-carbon alternating multi-level structure, wherein carbon nanotubes are first grown in situ on a porous carbon skeleton, and then silane deposition and carbon coating are performed. In the prepared silicon-carbon composite material, carbon nanotubes are embedded in the porous carbon structure, and uniformly grow inside and on the surface thereof to form a three-dimensional conductive network structure, thereby improving the structural stability of the silicon-carbon negative electrode material; and the in-situ growth of the carbon nanotube network can improve the conductivity of the material, alleviate the volume expansion of the silicon-based negative electrode, and enhance the specific capacity and cycle performance of the silicon-based negative electrode material. At the same time, the present invention adopts silicon / carbon alternating multi-level deposition to form a silicon / carbon multi-level alternating structure, which can improve the structural stability of the material, avoid structural collapse, improve the specific capacity and cycle performance of the silicon-carbon negative electrode material, and solve the problem of poor stability of the porous matrix pore structure in the existing silicon-carbon material and the problem of serious collapse of the material lattice structure during the repeated insertion and extraction of lithium ions.

[0022] The present invention adopts chemical vapor deposition method to in-situ grow carbon nanotubes inside and on the surface of porous carbon, and embeds them into the porous structure to form a three-dimensional conductive network structure, thereby improving the stability and conductivity of the porous carbon structure. In-situ growth of carbon nanotubes inside and on the surface of porous carbon, and controlling the reaction conditions to better control the content of carbon nanotubes grown on the porous carbon, in-situ growth of carbon nanotubes can not only ensure that the structure of carbon nanotubes is not destroyed, but also the interface between carbon nanotubes and porous carbon is strongly bonded, thereby improving the structural stability.

[0023] The present invention deposits silane gas on the surface of carbon nanotubes, which can improve the conductivity of silicon-carbon negative electrode materials; the presence of carbon nanotubes can significantly reduce electrode polarization impedance, while alleviating the volume expansion of the battery during charging and discharging, reducing particle pulverization, and thus improving the cycle stability of the battery.

[0024] The present invention adopts pulse deposition to realize the silicon / carbon alternating multi-level structure of silicon-carbon negative electrode material, which can effectively buffer the volume expansion of silicon and improve the stability of the structure of silicon-carbon negative electrode material, thereby significantly improving the coulombic efficiency and cycle performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The present invention is a flow chart for preparing the silicon-carbon composite material with a silicon-carbon alternating multi-layer structure. DETAILED DESCRIPTION

[0026] like Figure 1 As shown, the present invention provides a method for preparing a silicon-carbon composite material with a silicon-carbon alternating multi-level structure, comprising the following steps:

[0027] carbonizing the first carbon source to obtain a carbon precursor;

[0028] The carbon precursor is mixed with an activator and subjected to a first sintering to obtain a porous carbon skeleton;

[0029] Compounding the porous carbon skeleton with a metal catalyst to obtain a porous carbon-catalyst precursor;

[0030] The porous carbon-catalyst precursor is mixed with a second carbon source, and a second sintering is performed, and the obtained porous carbon-carbon nanotube precursor is acid-washed to obtain porous carbon-carbon nanotubes;

[0031] Using a pulse deposition method, under a protective gas condition, the porous carbon-carbon nanotube is deposited under a silane gas condition to obtain a silane-deposited porous carbon-carbon nanotube precursor;

[0032] A carbon source gas is introduced to carbon-coat the silane-deposited porous carbon-carbon nanotube precursor, and the deposition and carbon coating are repeated alternately to obtain a silicon-carbon composite material with a silicon-carbon alternating multi-level structure.

[0033] In the present invention, unless otherwise specified, the required raw materials for preparation are all commercially available products well known to those skilled in the art.

[0034] The present invention carbonizes the first carbon source to obtain a carbon precursor.

[0035] In the present invention, the first carbon source is preferably crushed and sieved, then carbonized under a protective atmosphere, cooled to room temperature, washed with water, and dried to obtain a carbon precursor.

[0036] In the present invention, the first carbon source (corresponding to Figure 1 The medium carbon source 1) preferably includes one or more of rice, wheat flour, soybean meal, rapeseed, fish scales, green leaves, fungus, bark, sugarcane, rice husk, epoxy resin, phenolic resin, asphalt and chitosan. When the carbon source is two or more of the above, the present invention has no particular limitation on the ratio of different types of carbon sources, and any ratio is acceptable.

[0037] In the present invention, the pulverization method is preferably mechanical pulverization, grinding or ball milling; the gas used in the protective atmosphere is preferably one or more of argon, helium and hydrogen. When the gas is two or more of the above, the present invention has no special limitation on the ratio of different types of gases, and any ratio is acceptable.

[0038] In the present invention, the carbonization temperature is preferably 300-800°C, more preferably 500-700°C, further preferably 600°C, and the time is preferably 1-3h, more preferably 2-3h; the heating rate to the carbonization temperature is preferably 1-20°C / min, more preferably 5-15°C / min.

[0039] In the present invention, the drying temperature is preferably 20-100°C, more preferably 60-80°C, the drying time is preferably 1-24h, more preferably 10-16h; the drying method is preferably oven drying, spray drying, stirring drying, flash drying or filter press drying.

[0040] The carbon precursor ( Figure 1 After Q1), the present invention mixes the carbon precursor with an activator and performs a first sintering to obtain a porous carbon skeleton.

[0041] In the present invention, the activator preferably includes one or more of calcium carbonate, magnesium oxide, iron oxide, potassium hydroxide, sodium hydroxide, sodium chloride and zinc chloride; when the activator is two or more of the above, the present invention has no special restrictions on the ratio of different types of activators, and any ratio is acceptable. The present invention uses the activator to form pores, and the carbon precursor forms a pore structure after activation.

[0042] In the present invention, the mass ratio of the carbon precursor to the activator is preferably 1:2-10, more preferably 1:5.

[0043] In the present invention, the carbon precursor and the activator are preferably mixed by mechanical stirring, ball milling or grinding; the mixing time is preferably 1 to 12 hours, more preferably 6 hours.

[0044] In the present invention, the temperature of the first sintering is preferably 500-900°C, more preferably 700°C, the time is preferably 2-6h, more preferably 4h; the heating rate to the temperature of the first sintering is preferably 1-20°C / min, more preferably 5°C / min; the atmosphere used for the first sintering is preferably one or more of argon, helium and hydrogen. After the sintering, the present invention preferably cools the obtained product to room temperature, washes it with water until the solution is neutral, and dries it (specifically, dries it at 60°C for 10h) to obtain a porous carbon skeleton (corresponding to Figure 1 (middle Q2).

[0045] After obtaining the porous carbon skeleton, the present invention composites the porous carbon skeleton with a metal catalyst to obtain a porous carbon-catalyst precursor.

[0046] In the present invention, the metal catalyst preferably includes one or more of cobalt chloride, cobalt nitrate, cobalt sulfate, nickel chloride, nickel nitrate, nickel sulfate, cupric chloride, cupric nitrate, cupric sulfate and ferrocene; when the metal catalyst is two or more of the above, the present invention has no special limitation on the ratio of different types of catalysts, and any ratio is acceptable.

[0047] In the present invention, the mass ratio of the metal catalyst to the porous carbon skeleton is preferably (1-25):1, more preferably 10-15:1.

[0048] In the present invention, the compounding method is preferably immersion or spraying; the compounding time is preferably 2 to 12 hours, more preferably 6 hours.

[0049] The present invention preferably immerses the porous carbon skeleton in an aqueous solution of the metal catalyst, or sprays the aqueous solution of the metal catalyst on the porous carbon skeleton, and dries to obtain a porous carbon-catalyst precursor; the present invention has no special limitation on the concentration of the aqueous solution of the metal catalyst, and can be adjusted according to the above-mentioned mass ratio according to actual needs; in an embodiment of the present invention, it is specifically 2 mol / L; the drying temperature is preferably 60-120°C, more preferably 100°C, and the drying time is preferably 2-24h, more preferably 12h.

[0050] Obtain porous carbon-catalyst precursor (corresponding to Figure 1After Q3), the present invention mixes the porous carbon-catalyst precursor with a second carbon source, performs a second sintering, and acid-washes the obtained porous carbon-carbon nanotube precursor to obtain porous carbon-carbon nanotubes.

[0051] In the present invention, the second carbon source (corresponding to Figure 1 The medium carbon source 2) preferably includes one or more of methane, ethane, propane, acetylene and propyne; when the second carbon source is two or more of the above, the present invention has no special limitation on the ratio of different types of second carbon sources, and any ratio is acceptable; the flow rate of the second carbon source is preferably 0.5 to 5 L / min, more preferably 1 to 3 L / min.

[0052] In the present invention, the temperature of the second sintering is preferably 300-900°C, more preferably 400-800°C, further preferably 500-600°C, the time is preferably 5-30 minutes, more preferably 10-20 minutes; the gas used for the second sintering is preferably one or more of argon, nitrogen and helium; the second sintering is carried out in a fluidized bed reactor. During the second sintering, the second carbon source forms carbon nanotubes under the action of a metal catalyst and grows uniformly on the porous carbon.

[0053] In the present invention, after the second sintering, the obtained porous carbon-carbon nanotube precursor (corresponding to Figure 1 Q4) pickling, the acid used for pickling preferably includes one or more of hydrochloric acid, nitric acid, sulfuric acid and phosphoric acid; when the acid is two or more of the above, the present invention has no special restrictions on the ratio of different types of acids, and any ratio is acceptable; the concentration of the acid is preferably 2 mol / L. The present invention has no special restrictions on the amount of the acid, and it is sufficient to ensure that the pickling is complete.

[0054] After the acid washing, the present invention preferably washes the obtained product with water until it is neutral, and then dries it to obtain porous carbon-carbon nanotubes (corresponding to Figure 1 The drying method is preferably drying, freeze drying or spray drying.

[0055] In the porous carbon-carbon nanotubes prepared by the present invention, the carbon nanotubes are multi-walled tubes and single-walled tubes or a combination of the two.

[0056] After obtaining the porous carbon-carbon nanotubes, the present invention adopts a pulse deposition method to deposit the porous carbon-carbon nanotubes under silane gas conditions under protective gas conditions to obtain a silane-deposited porous carbon-carbon nanotube precursor (corresponding to Figure 1 Q6); introducing a carbon source gas, the silane deposited porous carbon - carbon nanotube precursor is carbon coated, and the deposition and carbon coating are repeated alternately to obtain a silicon-carbon composite material with a silicon-carbon alternating multi-level structure.

[0057] In the present invention, the silane gas preferably includes one or more of silane, disilane, tetrafluorosilane, hexamethyldisilane, dichlorodimethylsilane and trimethylsilane; when the silane gas is two or more of the above, the present invention has no special limitation on the ratio of different types of silane gas, and any ratio is acceptable.

[0058] In the present invention, the protective gas preferably includes one or more of nitrogen, argon and helium. When the protective gas is two or more of the above, the present invention has no special limitation on the ratio of different types of protective gases, and any ratio is acceptable.

[0059] In the present invention, the deposition conditions preferably include: a deposition temperature of 500-600°C, more preferably 550°C, a deposition time of 100-200s, a silane gas flow rate of 1-8L / min, more preferably 2-5L / min, and a flow ratio of silane gas to protective gas of 1:1-15, more preferably 1:10.

[0060] After completing the deposition, the present invention preferably uses a protective gas (one or more of argon, nitrogen, and helium) to discharge the silane gas remaining in the deposition equipment after deposition, introduces a carbon source gas, and continues to use a pulse deposition method for carbon coating under protective gas conditions.

[0061] In the present invention, the carbon source gas (corresponding to Figure 1 The medium carbon source 3) preferably includes one or more of methane, ethane, propane, acetylene, propyne, acetone and cyclohexane; when the carbon source gas is two or more of the above, the present invention has no special limitation on the ratio of different types of carbon source gases, and any ratio is acceptable.

[0062] In the present invention, the carbon coating conditions preferably include: a deposition temperature of 600-900°C, more preferably 700°C, a deposition time of 100-200s, more preferably 150s, a carbon source gas flow rate of 1-8L / min, more preferably 2-5L / min; a flow ratio of the carbon source gas to the protective gas of 1:1-15, more preferably 1:10.

[0063] The present invention has no special limitation on the number of times the deposition and carbon coating are repeated alternately, as long as the Si content and carbon content in the silicon-carbon composite material are reached; one repetition is completed by alternating deposition and carbon coating once; in an embodiment of the present invention, the number of repetitions is specifically 8 or 10 times.

[0064] The present invention provides a silicon-carbon composite material with a silicon-carbon alternating multi-layer structure prepared by the preparation method described in the above technical solution (i.e. Figure 1The porous carbon / carbon nanotube silicon-carbon negative electrode material with medium and multi-layer coating has a Si content of 10 to 90 wt%, more preferably 40 to 50 wt%, and further preferably 42 to 48 wt%, and a carbon content of 10 to 90 wt%, more preferably 50 to 60 wt%, and further preferably 52 to 58 wt%.

[0065] The present invention provides the application of the silicon-carbon composite material with the silicon-carbon alternating multilayer structure in lithium-ion batteries. The present invention has no special limitation on the application method, and the silicon-carbon negative electrode material can be applied as a silicon-carbon negative electrode material according to methods well known in the art.

[0066] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0067] Example 1

[0068] S1, grinding and sieving the biomass carbon source (rice), carbonizing it at 600°C for 2h at a heating rate of 5°C / min under an argon atmosphere, cooling it to room temperature, washing it with water, and drying it at 80°C for 10h to obtain a carbon precursor Q1;

[0069] S2, the Q1 carbon precursor obtained in S1 was mixed with potassium hydroxide in a mass ratio of 1:5 by ball milling for 6 hours, and the temperature was raised to 700°C at a heating rate of 5°C / min in an argon atmosphere for the first sintering for 4 hours, and then cooled to room temperature, washed with water until the solution was neutral, and dried at 60°C for 10 hours to obtain a porous carbon skeleton Q2;

[0070] S3, according to the mass ratio of cobalt chloride: precursor Q2 = 10:1, the porous carbon skeleton Q2 obtained in S2 is immersed in a 2 mol / L cobalt chloride aqueous solution for 6 hours, and then dried at 100° C. for 12 hours to obtain a porous carbon-catalyst precursor Q3;

[0071] S4, placing the precursor Q3 obtained in S3 in a fluidized bed reactor, heating it to 500° C. under an argon atmosphere, introducing ethane gas at a flow rate of 1 L / min, performing a second sintering for 10 min under an argon atmosphere, and cooling it to room temperature to obtain a porous carbon-carbon nanotube precursor Q4;

[0072] S5, washing the porous carbon-carbon nanotube precursor Q4 obtained in S4 with hydrochloric acid (concentration of 2 mol / L) for multiple times, washing with water until neutral, and drying to obtain porous carbon-carbon nanotube Q5;

[0073] S6. Under the protection of argon gas, silane gas is deposited on the porous carbon-carbon nanotubes obtained in S5 by pulse deposition. The deposition temperature is 550° C., the deposition time is 100 s, the silane gas flow rate is 5 L / min, and the flow ratio of the protective gas to silane is 1:10, thereby obtaining a silane-deposited porous carbon-carbon nanotube precursor Q6.

[0074] S7. Use argon gas to discharge the gas remaining in the deposition equipment after deposition, introduce ethane gas, and carbon-coat the precursor Q6. The deposition temperature is 700°C, the deposition time is 150s, and the ethane gas flow rate is 5L / min; wherein the flow ratio of protective gas to ethane is 10:1, and a primary coated silicon-carbon negative electrode material is obtained. Repeat steps S6 and S7 10 times to obtain a silicon-carbon alternating multi-layer structure of a silicon-carbon negative electrode material, with a Si content of 48wt% and a carbon content of 52wt%.

[0075] Example 2

[0076] The only difference from Example 1 is that the rice in S1 is replaced with epoxy resin, and the material is carbonized at a heating rate of 5°C / min to 600°C for 2h to prepare a silicon-carbon negative electrode material with a silicon-carbon alternating multilayer structure, with a Si content of 45wt% and a carbon content of 55wt%.

[0077] Example 3

[0078] The only difference from Example 1 is that the number of repeated depositions in S7 is changed to 8 times, and the other conditions remain unchanged, thereby obtaining a silicon-carbon negative electrode material with a silicon-carbon alternating multi-layer structure, with a Si content of 42wt% and a carbon content of 58wt%.

[0079] Example 4

[0080] The only difference from Example 1 is that the rice in S1 is replaced with asphalt;

[0081] In S6, silane gas is deposited on the porous carbon-carbon nanotubes obtained in S5, the deposition temperature is 600°C, the deposition time is 100s, the silane gas flow rate is 2L / min, and the flow ratio of the protective gas to silane is 10:1, to obtain a silane-deposited porous carbon-carbon nanotube precursor Q6;

[0082] In S7, the ethane gas deposition temperature is 700°C, the deposition time is 100s, and the carbon source gas flow rate is 2L / min; the flow rate ratio of the protective gas to ethane is 10:1, and a primary coated silicon-carbon negative electrode material is obtained. Steps S6 and S7 are repeated 10 times in sequence to obtain a silicon-carbon alternating multi-layer structure of a silicon-carbon negative electrode material, with a Si content of 42wt% and a carbon content of 58wt%.

[0083] Comparative Example 1

[0084] The only difference from Example 1 is that the porous carbon skeleton Q2 prepared from rice is not subjected to S3, S4 and S5, but directly subjected to S6 and S7 to deposit silicon / carbon by pulse deposition, the silane deposition temperature is 550°C, the deposition time is 150s, the silane gas flow rate is 5L / min, and the flow ratio of protective gas to silane is 10:1, to obtain a silane-deposited porous carbon-carbon nanotube precursor Q6; the ethane deposition temperature is 700°C, the deposition time is 150s, and the carbon source gas flow rate is 5L / min; wherein the flow ratio of protective gas to ethane is 10:1; S6 and S7 are repeated ten times to obtain a silicon-carbon negative electrode material with a silicon-carbon alternating multi-level structure, with a Si content of 40wt% and a carbon content of 60wt%.

[0085] Characterization and performance testing

[0086] The negative electrode materials obtained in the above embodiments and comparative examples are assembled into lithium ion batteries and the method for testing the charge and discharge performance comprises the following steps:

[0087] Add binder, conductive agent and single-walled carbon nanotube (SWCNT) to the negative electrode material, stir to make slurry, coat on copper foil, dry and roll to obtain negative electrode sheet; the binder used is LA132, the conductive agent is conductive carbon black (SP), and the mass ratio of negative electrode material, SP, SWCNT and LA123 is 94:1:1:4. The electrolyte used is LiPF 6 The electrolyte was 1.2 mol / L, and the solvent was a mixture of EC and DEC in a volume ratio of 1:1; the metal lithium sheet was the counter electrode, and the diaphragm was a polypropylene (PP) film. The button cell was assembled in an argon-filled glove box. The electrochemical performance was tested on a Wuhan Blue Electric CT2001A battery tester. The charge and discharge voltage range was 0.005-1.5 V, the charge and discharge rate was 0.1 C, and its rate performance (0.1-2.0 C) was tested.

[0088] The test results of the negative electrode materials in the above Examples 1 to 4 and Comparative Example 1 are shown in Table 1.

[0089] Table 1 Test results of negative electrode materials in Examples 1 to 4 and Comparative Example 1

[0090] Case First charge specific capacity (mAh / g) First efficiency (%) Capacity retention rate (%) (50 weeks) Example 1 1905 92.7 91.7 Example 2 1802 91.1 91.5 Example 3 1705 90.3 88.9 Example 4 1650 91.2 90.2 Comparative Example 1 1572 88.9 87.3

[0091] It can be seen from Table 1 that the silicon-carbon negative electrode material prepared in the embodiment of the present invention exhibits more excellent electrochemical performance (first charge specific capacity, first efficiency and capacity retention rate) than the comparative example.

[0092] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a silicon-carbon composite material with a silicon-carbon alternating multi-layer structure, characterized in that: The following steps are involved: carbonizing the first carbon source to obtain a carbon precursor; The carbon precursor is mixed with an activator and subjected to a first sintering to obtain a porous carbon skeleton; Compounding the porous carbon skeleton with a metal catalyst to obtain a porous carbon-catalyst precursor; The porous carbon-catalyst precursor is mixed with a second carbon source, and a second sintering is performed, and the obtained porous carbon-carbon nanotube precursor is acid-washed to obtain porous carbon-carbon nanotubes; Using a pulse deposition method, under a protective gas condition, the porous carbon-carbon nanotube is deposited under a silane gas condition to obtain a silane-deposited porous carbon-carbon nanotube precursor; A carbon source gas is introduced to carbon-coat the silane-deposited porous carbon-carbon nanotube precursor, and the deposition and carbon coating are repeated alternately to obtain a silicon-carbon composite material with a silicon-carbon alternating multi-level structure.

2. The preparation method according to claim 1, characterized in that: The first carbon source includes one or more of rice, wheat flour, soybean meal, rapeseed, fish scales, green leaves, fungus, bark, sugarcane, rice husks, epoxy resin, phenolic resin, asphalt and chitosan; the carbonization temperature is 300-800°C, and the time is 1-3h; the heating rate to the carbonization temperature is 1-20°C / min.

3. The preparation method according to claim 1, characterized in that: The activator includes one or more of calcium carbonate, magnesium oxide, iron oxide, potassium hydroxide, sodium hydroxide, sodium chloride and zinc chloride; the mass ratio of the carbon precursor to the activator is 1:2-10; the temperature of the first sintering is 500-900°C, and the time is 2-6h; the heating rate to the first sintering temperature is 1-20°C / min.

4. The preparation method according to claim 1, characterized in that: The metal catalyst includes one or more of cobalt chloride, cobalt nitrate, cobalt sulfate, nickel chloride, nickel nitrate, nickel sulfate, cupric chloride, cupric nitrate, cupric sulfate and ferrocene; the mass ratio of the metal catalyst to the porous carbon skeleton is (1-25):1; the composite method is immersion or spraying; and the composite time is 2-12 hours.

5. The preparation method according to claim 1, characterized in that: The second carbon source includes one or more of methane, ethane, propane, acetylene and propyne; and the flow rate of the second carbon source is 0.5 to 5 L / min.

6. The preparation method according to claim 5, characterized in that: The temperature of the second sintering is 300-900° C., and the time is 5-30 minutes; the acid used for the pickling includes one or more of hydrochloric acid, nitric acid, sulfuric acid and phosphoric acid.

7. The preparation method according to claim 1, characterized in that: The silane gas includes one or more of silane, disilane, tetrafluorosilane, hexamethyldisilane, dichlorodimethylsilane and trimethylsilane; the protective gas includes one or more of nitrogen, argon and helium, and the deposition conditions include: a deposition temperature of 500 to 600°C, a deposition time of 100 to 200s, a silane gas flow rate of 1 to 8L / min, and a flow ratio of silane gas to protective gas of 1:1 to 15.

8. The preparation method according to claim 1, characterized in that: The carbon source gas includes one or more of methane, ethane, propane, acetylene, propyne, acetone and cyclohexane; the carbon coating conditions include: a deposition temperature of 600 to 900°C, a deposition time of 100 to 200s, a carbon source gas flow rate of 1 to 8L / min; and a flow ratio of the carbon source gas to the protective gas of 1:1 to 15.

9. The silicon-carbon composite material having a silicon-carbon alternating multi-layer structure prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The Si content is 10 to 90 wt%, and the carbon content is 10 to 90 wt%.

10. Use of the silicon-carbon composite material with a silicon-carbon alternating multi-layer structure as claimed in claim 9 in lithium-ion batteries.

Citation Information

Patent Citations

  • Negative electrode material and preparation method thereof, negative electrode plate and lithium ion battery

    CN116093287A

  • Silicon-carbon composite material, preparation method and application thereof, and lithium ion secondary battery

    CN116742002A

  • Preparation method of high-strength silicon-carbon negative electrode material

    CN117727913A

  • Porous carbon few-walled carbon nanotube silicon nano composite material and preparation and application methods thereof

    CN118352507A

  • Preparation method of improved silicon-carbon negative electrode material

    CN118458746A

Cited By

  • Preparation method of hydrogen storage material with CNTs (at) C structure

    CN119370832A

  • Activated carbon, silicon-carbon composite material and preparation method and application thereof

    CN119706832A

  • Silicon-carbon composite material, preparation method and application thereof, and lithium ion battery

    CN119797369A

  • Silicon-carbon negative electrode material, preparation method thereof and battery

    CN119943923A

  • Charge-discharge low-expansion spherical silicon-carbon composite negative electrode material and preparation method thereof

    CN121076116A