Method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method
Through the instant expansion method of high-temperature molten salt intercalation, low-defect graphene powder is prepared by negative pressure high-power microwave or normal pressure high-temperature quenching and peeling method, which solves the problems of high cost, low efficiency and environmental protection in the existing technology, and realizes the problem of high graphene preparation cost, low efficiency and environmental protection. High-quality and low-cost graphene preparation.
Patent Information
- Application Number
- CN202411346120.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-26
AI Technical Summary
The existing graphene preparation methods have high cost, low production efficiency, safety and environmental protection problems, and have a large number of graphene layers prepared and poor conductivity.
Using the instant expansion method of high-temperature molten salt intercalation, low-defect graphene powder is prepared by the preparation, intercalation and instantaneous peeling steps of graphite/molten salt composite electrode, and the low-defective graphene powder is prepared by negative pressure high-power microwave or normal pressure high-temperature quenching peeling method to control graphite The number of olefins is 3-5 layers, and the scale size is 25-300μm.
It realizes the preparation of low-defect graphene powders at low cost, low pollution and efficiently, avoids defects in the redox process, improves product quality and production efficiency, and ensures environmental protection and safe production.
Smart Images

Figure CN118929644A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of graphene preparation, and in particular relates to a method for preparing low-defect graphene powder by a high-temperature molten salt intercalation instantaneous expansion method. Background Art
[0002] Since its advent in 2004, graphene has shown wide application potential in many fields due to its extremely excellent physical properties. For example, due to its thermal conductivity of up to 5300W / mK, it is used in the heat dissipation of electronic products chips, especially portable electronic products; due to its extremely high conductivity and the flexibility of its two-dimensional structure, it is used in the field of high-barrier heavy-duty anti-corrosion paint. Undoubtedly, the preparation method and production technology of graphene are important prerequisites for the promotion and development of graphene applications. The quality, physical properties, cost, impurity content and environmental issues involved in the preparation and production of graphene will affect the development of downstream applications and the promotion of products, and ultimately affect the development and diffusion of technology. Therefore, a low-cost and low-pollution method for preparing high-quality graphene powder is very necessary.
[0003] At present, there are three main methods for preparing graphene powder: 1) Mechanical exfoliation method, which is the main method for some domestic manufacturers to produce non-redox graphene. Graphite is exfoliated by equipment such as grinders, ball mills, and high-pressure homogenizers to obtain graphene or graphite nanosheets with a thickness of more than ten layers. The advantage is low cost, but there are disadvantages such as high energy consumption, long processing time, and easy introduction of metal impurities. In addition, the number of graphene layers prepared is large, which affects flexibility and conductivity, and the product performance is limited. 2) Redox method, using oxidants such as sulfuric acid and potassium permanganate to oxidize graphite into graphite oxide, and then treating graphite oxide into graphene oxide and preparing graphene through chemical reduction or thermal reduction. This method is mature in technology and can achieve large-scale production (annual production of hundreds of tons). However, its production process involves hazardous substances such as concentrated sulfuric acid, and there are problems of production safety and environmental pollution. In addition, the prepared graphene contains metal ion impurities, poor conductivity, and it is difficult to achieve an ideal state. 3) The atmospheric deposition method, including the epitaxial growth method and the metal catalytic vapor deposition method, can produce high-quality graphene close to the theoretical state with excellent conductivity. However, this method has expensive equipment, low production efficiency and high cost. Not only is it difficult for businesses to use it, but even research institutions only have research groups with sufficient funds to carry out application development and physical property exploration of such products. For this reason, a method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method is proposed. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method, aiming to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method comprises the following steps:
[0007] Step 1, preparation of graphite / molten salt composite electrode: use a stirring mixer to preliminarily mix the graphite powder and the salt for intercalation, then feed the preliminarily mixed materials into a single-screw mixer, heat the salt to a molten state, and allow the molten salt to fully infiltrate the surface of the graphite powder; introduce the mixture into a mold, place an electrode current collector at the bottom of the mold in advance, and cover the current collector with the mixture; after sealing the mold, place the mold on a flat vulcanizer for heating and molding, and press the mixture and the current collector into an integrated composite graphite electrode;
[0008] Step 2, intercalation: the prepared composite graphite electrode is installed in a container as an anode, the salt for intercalation is filled in the container as an electrolyte, and the bulk graphite electrode is used as a cathode; after placing the anode and cathode and the electrolyte, the container is sealed, heated until the electrolyte is melted, and pressure is applied to the inside of the container from one end of the cathode to keep the pressure of the molten salt liquid in the range of 2-6 atmospheres; then, power is applied under low voltage of 0.5-1.2V and high current of 5-40A to promote the intercalation reaction (low voltage is to control the electrolyte from being oxidized and reduced, and high current is to promote the efficiency of intercalation); after treatment, the composite graphite electrode of the anode will expand and partially fall off and powder, and the expansion and shedding of the composite graphite electrode of the anode are observed until all the intercalated expanded graphite is separated from the current collector;
[0009] Step 3: instantaneous stripping, using negative pressure high-power microwave stripping method or normal pressure high-temperature quenching stripping method;
[0010] The negative pressure high-power microwave exfoliation method is as follows: the intercalated graphite powder is placed in a closed device that can simultaneously achieve vacuuming and microwave heating, and the graphite powder is instantly heated with a microwave power of 10-15KW, so that the intercalated material is instantly gasified (decomposed into gas), the graphite powder instantly expands and explodes, and the graphite is exfoliated into thinner graphene;
[0011] The atmospheric pressure high temperature quenching stripping method is specifically as follows: the graphite powder after intercalation treatment is instantly subjected to heating or flame burning above 1000°C, so that the intercalated material is instantly released and the graphite is stripped. Due to the use of molten salt intercalation, compared with the intercalation by concentrated sulfuric acid and potassium permanganate oxidation, more salt will be inserted into the graphite layers. Even small flakes of graphite can be stripped by this method.
[0012] Furthermore, in step 1, the molar ratio of graphite powder to the salt used for intercalation is (3-6):1; the salt used for intercalation is mainly sulfate.
[0013] Furthermore, in step 1, the current collector is a rough mesh frame structure, which facilitates the powder to be firmly combined with the current collector under molding. The current collector can be made of metal materials such as copper and aluminum, or carbon fiber materials.
[0014] Furthermore, in step 1, the composite graphite electrode is cylindrical or rectangular.
[0015] Furthermore, in step 1, during the heating and molding, the pressure and temperature are adjusted according to the mesh size of the graphite flakes used and the type and amount of the salt used. The heating temperature does not exceed the decomposition temperature or gasification temperature of the salt.
[0016] Furthermore, in step 2, the heating temperature is higher than the melting point of the salt and lower than the decomposition temperature or the gasification temperature.
[0017] Furthermore, in step 2, the container is a reactor with a ceramic insulating inner layer, or a reaction container with a polytetrafluoroethylene lining is selected according to the melting temperature of the salt.
[0018] Furthermore, in step 2, the molar ratio of the electrolyte to the graphite powder is (5-6):1.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The present invention has developed a method for preparing low-defect graphene powder by a non-redox method of high-temperature molten salt intercalation instantaneous expansion method. The number of graphene layers prepared can be controlled at 3-5 layers, and the flake size can reach 25-300μm.
[0021] 2. In terms of raw material selection, the present invention uses non-corrosive and environmentally friendly salt as a key material to ensure the safety and environmental protection of the production process. The environmental protection treatment of such salt is simple and convenient, which greatly reduces the potential impact on the environment. At the same time, the melting temperature of the selected salt is below 300-400°C, which effectively reduces the energy consumption in the intercalation process. In addition, as a common chemical raw material, its low price also directly guarantees the cost-effectiveness of graphene production.
[0022] 3. The present invention innovatively adopts molten salt electric assisted intercalation technology to improve the distribution uniformity and quantity of intercalation reagents between graphite layers, thereby preparing graphene with fewer layers and a narrower layer distribution range. Compared with the graphene oxide preparation scheme, the present invention avoids the redox process and reduces the defects on the graphene flakes; compared with the mechanical exfoliation method, the graphite raw material is not ground and crushed, retaining a larger flake size and improving product quality.
[0023] 4. The present invention introduces the instantaneous expansion method, especially the negative pressure microwave technology, which is operated in an environment below the standard atmospheric pressure, so that the expansion force applied to the graphite layers when the intercalated material decomposes and gasifies is significantly enhanced, achieving a better peeling effect and preparing fewer graphene layers. Due to the increase in the number of intercalated materials, the force released during decomposition far exceeds the force in the preparation process of expanded graphite, so there is no need for secondary processing of mechanical peeling, and thin-layer graphene is directly produced, which improves production efficiency and product quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a scanning electron microscope image of graphene prepared by the method in Example 1.
[0025] Figure 2 This is a scanning electron microscope image of graphene prepared by the method in Example 2.
[0026] Figure 3 The scanning electron microscope image and the transmission electron microscope image of the graphene prepared by the method in Example 3 are shown; wherein a is a scanning electron microscope image, and b is a transmission electron microscope image.
[0027] Figure 4 This is a scanning electron microscope image of graphene prepared by the method in Example 4.
[0028] Figure 5 This is the flake size distribution diagram of graphene prepared by the method in Example 3.
[0029] Figure 6 This is a distribution diagram of the number of layers of graphene obtained by the method in Example 3. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0031] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.
[0032] Example 1: A method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method, comprising the following steps:
[0033] 1) Ingredients: ammonium bisulfate and 100-mesh graphite powder are used as raw materials, mixed in a stirring mixer according to a molar ratio of 1:4, and then added into a single screw extruder. The heating temperature is controlled at 160°C, and the ammonium bisulfate is heated to a molten state to allow the molten salt to fully infiltrate the surface of the graphite powder.
[0034] 2) Molding: The uniformly mixed graphite / molten salt powder is introduced into the mold, and the electrode current collector (metallic copper) is placed at the bottom of the mold in advance. The mixture is covered on the current collector and vibrated to make the powder fully filled and tightly fit with the current collector. After the mold is sealed, it is heated and molded on a flat vulcanizer at a heating temperature of 160°C and a pressure of 40Mpa. The mixed powder and the current collector are pressed into an integrated cylindrical composite graphite electrode.
[0035] 3) Intercalation: The prepared composite graphite electrode is installed as the anode in a reaction vessel with a polytetrafluoroethylene lining. In addition, a certain amount of ammonium bisulfate is filled as an electrolyte, and the molar ratio of the amount of electrolyte added to the amount of graphite powder is 6:1. The bulk graphite electrode is used as the cathode. After placing the anode and cathode electrolytes, the container is sealed with silicone rubber or a polytetrafluoroethylene gasket. After heating the inside of the container to 160°C, pressure is applied to the inside of the container from one end of the cathode so that the pressure of the molten salt liquid in the container is within 4 atmospheres. Then, the composite graphite electrode of the anode is intercalated with a voltage of 0.8V and a current of 15A. The heating temperature in this process is kept at around 160°C.
[0036] 4) Use negative pressure high-power microwave stripping method for instantaneous stripping: Put the intercalated graphite powder in a ceramic sagger and place it in a vacuum microwave reactor. After sealing the reactor, evacuate the pressure of the box to below 100Pa. Then start microwave instant heating with a microwave power of 15KW. The graphite will expand and explode in an instant and strip into graphene. The sample in the sagger should not be excessive, and it should be determined according to the volume of the box, the pressure it can withstand, and the depth of microwave heating.
[0037] The scanning electron microscope image of the graphene prepared by the method in Example 1 is as follows Figure 1 shown.
[0038] Example 2: A method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method, comprising the following steps:
[0039] The operations of 1) to 3) are consistent with those of 1) to 3) in Example 1. In step 4), a normal pressure high temperature quenching stripping method is selected for instantaneous stripping: the muffle furnace is heated to 1000°C, the ceramic sagger is placed therein, and it is taken out after preheating to the same temperature, and a certain amount of graphite powder is added. The amount of graphite powder used here is related to the structure and bottom area of the sagger. The graphite powder should cover the bottom of the sagger, and the thickness should not exceed 5mm. Considering the production efficiency and the stripping effect, the thickness is preferably about 3mm. The sagger is placed in the muffle furnace again and heated for 60 seconds. After all the graphite powders are fully expanded and turned red, they are taken out to obtain graphene dry powder.
[0040] The scanning electron microscope image of the graphene prepared by the method in Example 2 is as follows: Figure 2shown.
[0041] Example 3: A method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method, comprising the following steps:
[0042] 1) Ingredients: ammonium sulfate and 100-mesh graphite powder are used as raw materials, mixed in a stirring mixer according to a molar ratio of 1:5, and then added into a single-screw extruder. The heating temperature is controlled at 240°C, and the ammonium sulfate is heated to a molten state to allow the molten salt to fully infiltrate the surface of the graphite powder.
[0043] 2) Molding: The uniformly mixed graphite / molten salt powder is introduced into the mold, and the electrode current collector (metallic copper) is placed at the bottom of the mold in advance. The mixture is covered on the current collector and vibrated to make the powder fully filled and tightly fit with the current collector. After the mold is sealed, it is heated and molded on a flat vulcanizer at a heating temperature of 240°C and a pressure of 40Mpa. The mixed powder and the current collector are pressed into an integrated cylindrical composite graphite electrode.
[0044] 3) Intercalation: The prepared composite graphite electrode is installed as the anode in a reaction vessel with a polytetrafluoroethylene lining. In addition, a certain amount of ammonium bisulfate is filled as an electrolyte, and the molar ratio of the amount of electrolyte added to the amount of graphite powder is 5:1. The bulk graphite electrode is used as the cathode. After placing the anode and cathode electrolytes, the container is sealed with silicone rubber or a polytetrafluoroethylene gasket. After heating the inside of the container to 240°C, pressure is applied to the inside of the container from one end of the cathode so that the pressure of the molten salt liquid in the container is within 4 atmospheres. Then, the composite graphite electrode of the anode is intercalated with a voltage of 0.8V and a current of 15A. The heating temperature of this process is kept at around 240°C.
[0045] 4) Negative pressure stripping: Put the intercalated graphite powder in a ceramic sagger and place it in a vacuum microwave reactor. After sealing the reactor, evacuate the pressure of the box to below 100Pa. Then start microwave instant heating with a microwave power of 15KW. The graphite will expand and explode in an instant and strip into graphene. The sample in the sagger should not be excessive. It should be determined according to the volume of the box, the pressure it can withstand, and the depth of microwave heating.
[0046] The scanning electron microscope image of the graphene prepared by the method in Example 3 is as follows: Figure 3 As shown in a, the transmission electron microscopy image is as follows Figure 3 As shown in b. The distribution diagram of the number of graphene layers and the distribution diagram of the flake size are Figure 6 He Ru Figure 5 As shown, the number of graphene layers is 3-5 and the flake size is 25-300 μm.
[0047] Example 4: A method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method, comprising the following steps:
[0048] The operation process was consistent with that of Example 1, except that the salt used for intercalation was replaced by potassium hydrogen sulfate, and the heating temperature for melting was 220°C.
[0049] The scanning electron microscope image of the graphene prepared by the method in Example 4 is as follows Figure 4 shown.
[0050] Example 5: A method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method, comprising the following steps:
[0051] The operation process was consistent with that of Example 2, except that the salt used for intercalation was replaced by ammonium sulfate and the heating temperature for melting was 240°C.
[0052] In addition, the mesh size of the graphite powder used can be changed (50-300 mesh), which determines the flake size of the produced graphene, or the current size can be changed to improve the intercalation efficiency.
[0053] In general, the greater the amount of gas generated when the intercalation agent (molten salt) used decomposes, the better the stripping effect. The heat treatment method will also affect the stripping effect to a certain extent. The negative pressure high-power microwave stripping method is better than the atmospheric pressure high-temperature quenching stripping method, mainly because the instantaneous heating effect of microwave heating is more significant, while high-temperature quenching requires heat conduction between materials, and this process will allow part of the intercalation agent to slowly overflow. Therefore, the stripping effect of Example 3 is the best, and the number of graphene layers is thinner, specifically 3-5 layers, and the flake size is 25-300μm.
[0054] The above are only preferred embodiments of the present invention. It should be pointed out that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention. These should also be regarded as the protection scope of the present invention. These will not affect the effect of the implementation of the present invention and the practicality of the patent.
Claims
1. A method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method, characterized in that: The following steps are involved: Step 1, preparation of graphite / molten salt composite electrode: use a stirring mixer to preliminarily mix the graphite powder and the salt for intercalation, then feed the preliminarily mixed materials into a single-screw mixer, heat the salt to a molten state, and allow the molten salt to fully infiltrate the surface of the graphite powder; introduce the mixture into a mold, place an electrode current collector at the bottom of the mold in advance, and cover the current collector with the mixture; after sealing the mold, place the mold on a flat vulcanizer for heating and molding, and press the mixture and the current collector into an integrated composite graphite electrode; Step 2, intercalation: the prepared composite graphite electrode is installed as an anode in a container, the salt for intercalation is filled in the container as an electrolyte, and the bulk graphite electrode is used as a cathode; the container is sealed and heated until the electrolyte is melted, and pressure is applied to the inside of the container from one end of the cathode to keep the pressure of the molten salt liquid in the range of 2-6 atmospheres; then, power is applied under low voltage of 0.5-1.2V and high current of 5-40A to promote the intercalation reaction; the expansion and shedding of the composite graphite electrode of the anode are observed until all the intercalated expanded graphite is separated from the current collector; Step 3: instantaneous stripping, using negative pressure high-power microwave stripping method or normal pressure high-temperature quenching stripping method; The negative pressure high-power microwave stripping method is as follows: the graphite powder after intercalation treatment is placed in a closed device that can simultaneously realize vacuuming and microwave heating, and the graphite powder is instantly heated with a microwave power of 10-15KW, so that the intercalated material is instantly gasified, the graphite powder instantly expands and explodes, and the graphite is stripped; The atmospheric pressure high temperature quenching stripping method is specifically as follows: the graphite powder after intercalation treatment is instantly subjected to heating or flame burning above 1000°C, so that the intercalated material is instantly released and the graphite is stripped.
2. The method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method according to claim 1, characterized in that: In the step 1, the molar ratio of graphite powder to the salt used for intercalation is (3-6):1; the salt used for intercalation is sulfate.
3. The method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method according to claim 1, characterized in that: In the step 1, the current collector is a mesh frame structure, and the current collector is made of metal or carbon fiber material.
4. The method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method according to claim 1, characterized in that: In the step 1, the composite graphite electrode is cylindrical or rectangular.
5. The method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method according to claim 1, characterized in that: In the step 1, when heating and molding are performed, the heating temperature does not exceed the decomposition temperature or gasification temperature of the salt.
6. The method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method according to claim 1, characterized in that: In step 2, the heating temperature is higher than the melting temperature of the salt and lower than the decomposition temperature or the gasification temperature.
7. The method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method according to claim 1, characterized in that: In step 2, the container is a reactor with a ceramic insulating inner layer, or a reaction container with a polytetrafluoroethylene lining is selected according to the melting temperature of the salt.
8. The method for preparing low-defect graphene powder by high-temperature molten salt intercalation instantaneous expansion method according to claim 1, characterized in that: In step 2, the molar ratio of electrolyte to graphite powder is (5-6):1.
Citation Information
Patent Citations
Method for preparing graphene by electrochemically expanding intercalated graphite
CN111285360A