Dispersion containing graphene carbon nanoparticles and dispersant resin
Through grinding and combining with the polymer dispersant resin, the dispersion and stability of graphene carbon nanoparticles are solved, and its effective use and high loading in a variety of applications are achieved.
Patent Information
- Application Number
- CN202411141340.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-02-20
- Filing Date
- 2020-02-19
- Publication Date
- 2024-11-12
AI Technical Summary
Graphene carbon nanoparticles have poor dispersion and stability in other materials, making it difficult to disperse and use effectively.
Graphene carbon nanoparticles were treated with grinding techniques and combined with an additive dispersant resin containing vinyl heterocyclic amide residues, which were mixed into the solvent to improve dispersion and stability.
The uniform dispersion and long-term stability of graphene carbon nanoparticles have been achieved, the scope of its applications in conductive inks, battery manufacturing, thermal coatings, etc. has been expanded, and the load capacity and the stability of the dispersion have been improved.
Smart Images

Figure CN118929646A_ABST
Abstract
Description
[0001] This application is a divisional application of the Chinese patent application with application number 202080015403.7.
[0002] CROSS-REFERENCE TO RELATED APPLICATIONS
[0003] This application claims priority to U.S. Provisional Patent Application No. 62 / 808,126, filed on February 20, 2019, which is incorporated herein by reference. Technical Field
[0004] The present invention relates to a dispersion containing graphene carbon particles and a dispersant resin, and more particularly to a dispersion of ground graphene carbon particles and a dispersant resin in an aqueous solvent and / or an organic solvent. Background Art
[0005] Graphene nanoparticles have many current and potential uses. However, such nanoparticles can be difficult to disperse in other materials. Summary of the invention
[0006] The present invention provides a dispersion comprising a solvent, graphene carbon nanoparticles having an average aspect ratio greater than 3:1 and a Raman 2D:G peak ratio of at least 1:1, and a polymer dispersant resin comprising an addition polymer comprising a vinyl heterocyclic amide residue.
[0007] The present invention also provides a dispersion comprising an organic solvent, graphene carbon nanoparticles, and a polymer dispersant resin comprising an addition polymer, wherein the addition polymer comprises a homopolymer, a block (co)polymer, a random (co)polymer, an alternating (co)polymer, a graft (co)polymer, a brush (co)polymer, a star (co)polymer, and a telechelic (co)polymer.
[0008] The present invention also provides a method for dispersing graphene carbon nanoparticles in a solvent, the method comprising mixing a dispersant resin into the solvent, wherein the dispersant resin comprises an addition polymer comprising a vinyl heterocyclic amide residue, an addition polymer comprising a homopolymer, a block (co)polymer, a random (co)polymer, an alternating (co)polymer, a graft (co)polymer, a brush (co)polymer, a star (co)polymer, a telechelic (co)polymer or a combination thereof; and mixing the graphene carbon nanoparticles into the solvent and the dispersant resin mixture. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 is a plot of the instability index versus time for oil dispersions containing ground plasma graphene carbon particles and ground exfoliated graphene carbon.
[0010] Figure 2is a plot of the instability index versus time for aqueous dispersions containing milled plasma graphene carbon particles and milled exfoliated graphene carbon particles.
[0011] Figure 3 is a photograph of a dried graphene carbon nanoparticle dispersion showing a more uniform particle dispersion of milled graphene carbon nanoparticles relative to unmilled graphene carbon nanoparticles.
[0012] Figure 4 and Figure 5 are micrographs and corresponding line graphs showing non-uniformly sized aggregated graphene carbon nanoparticles resulting from an unmilled graphene carbon nanoparticle dispersion.
[0013] Figure 6 and Figure 7 are photographs and corresponding line graphs showing uniformly dispersed non-aggregated graphene carbon nanoparticles of uniform size produced from a milled graphene carbon nanoparticle dispersion.
[0014] Figure 8 is a graph of the oxygen content of the graphene carbon nanoparticle samples versus the milling time.
[0015] Fig. 9 is a plot of defect levels of graphene carbon nanoparticle samples versus milling time.
[0016] Fig.10 and Fig.11 TEM images of unground graphene carbon nanoparticles and ground graphene carbon nanoparticles, respectively.
[0017] Figure 12 to Figure 14 are the dynamic frequency sweep results of dispersions of unmilled graphene carbon nanoparticles containing different loading amounts, showing the storage modulus (G'), loss modulus (G") and complex viscosity, respectively.
[0018] Figures 15 to 17 are the dynamic frequency sweep results of dispersions of milled graphene carbon nanoparticles containing different loading amounts showing the storage modulus (G'), loss modulus (G") and complex viscosity, respectively.
[0019] Fig.18 Included is a graph of viscosity versus shear rate for aqueous dispersions of graphene carbon nanoparticles containing 8 wt % unmilled graphene carbon nanoparticles versus 20 wt % milled graphene carbon nanoparticles.
[0020] Fig.19 The viscosity of aqueous graphene carbon nanoparticle dispersions at a shear rate of 10 Hz is shown for a dispersion containing 8 wt % unground graphene carbon nanoparticles versus 20 wt % ground graphene carbon nanoparticles.
[0021] Fig. 20 Included are plots of viscosity versus shear rate for dispersions of graphene carbon nanoparticles in organic solvents containing 5 wt % of unmilled graphene carbon nanoparticles, 10 wt % of milled graphene carbon nanoparticles, and 15 wt % of graphene carbon nanoparticles.
[0022] Fig.21 The viscosity of the graphene carbon nanoparticle dispersion in the organic solvent at a shear rate of 10 Hz is shown for dispersions in the organic solvent containing 5 wt % of unground graphene carbon nanoparticles, 10 wt % of ground graphene carbon nanoparticles, and 15 wt % of graphene carbon nanoparticles.
[0023] Figure 22 to Figure 24 is a graph of the instability index versus time for a dispersion containing a milled graphene carbon nanoparticle dispersion and an unmilled graphene carbon nanoparticle dispersion.
[0024] Fig.25 The instability index values of graphene nanoparticle dispersions in different types of organic solvents including N-methyl-2-pyrrolidone (NMP), SAR acrylic resin, and copolymers of lauryl methacrylate and vinyl pyrrolidone (LMA-VP) having different LMA contents are shown.
[0025] Fig.26 Shown is the viscosity of graphene carbon nanoparticle dispersions in PVP of LMA-VP dispersant resin with increasing lauryl methacrylate content at 10 Hz shear rate.
[0026] Fig. 27 Shown is the viscosity of graphene carbon nanoparticle dispersions in PVP of LMA-VP dispersant resin with increasing lauryl methacrylate content at 10 Hz shear rate.
[0027] Fig.28 Shown is the viscosity of graphene carbon nanoparticle dispersions in PVP of LMA-VP dispersant resin with increasing lauryl methacrylate content at 10 Hz shear rate.
[0028] Fig.29 is a graph of D50 particle size versus lauryl methacrylate content in the slurry as a weight percent of the total solids in the slurry.
[0029] Fig.30 is a graph of viscosity and D50 particle size versus the lauryl methacrylate content in the slurry as a weight percent of the total solids in the slurry.
[0030] Figures 31 to 38A scanning electron microscope image of a lithium-ion cathode film prepared using a dispersion of graphene carbon nanoparticles.
[0031] Fig.39 is a graph of the capacity retention versus cycle number at various C rates for lithium-ion cathode films prepared using graphene carbon nanoparticle dispersions.
[0032] Fig.40 is a graph of the capacity retention versus cycle number at various C rates for lithium-ion cathode films prepared using graphene carbon nanoparticle dispersions. DETAILED DESCRIPTION
[0033] The present invention provides graphene carbon nanoparticle dispersions that are stable during storage and use. The stable dispersions can be used in a variety of different applications, including conductive inks, battery anode and / or cathode coatings, supercapacitors, EMI shielding, RFI shielding, thermally conductive coatings, conductive coatings, lubricants, coolants, composite materials, 3D printing, etc. Conductive inks can include silver inks, medical electrode inks, silver mixed inks, carbon inks, dielectric inks, zinc electrode battery inks, manganese battery inks, thermosetting carbon battery inks, IR transparent anti-counterfeiting inks, and low resistance UV inks. Applications of conductive inks include smartphones, tablets, interactive and electrochromic displays, biomedical sensors, printed keyboards, industrial membrane switch controls, RFID tags, and other products with printed circuits.
[0034] As used herein, the term "dispersed" refers to graphene carbon nanoparticles dispersed in a medium (such as a solvent containing a polymer dispersant) to form a substantially uniform dispersion of graphene carbon nanoparticles throughout the medium without a large amount of aggregation of particles. As described more fully below, the uniformity of the dispersion can be measured by an "instability index". The presence of aggregation can be determined by standard methods, such as visual analysis of TEM micrographs. Aggregation can also be detected by standard particle size measurement techniques and measurements of electrical conductivity or optical properties of materials containing graphene carbon particles such as color, haze, blackness, reflectivity, and transmission characteristics.
[0035] The graphene carbon nanoparticles can be ground to improve their dispersibility and / or stability in the composition. Various different types of grinding techniques can be used, such as solid state grinding, ball milling, dry ball milling, Eiger grinding, LAU grinding, Cowles grinding, etc.
[0036] In addition to graphene carbon nanoparticles, the dispersion also includes various types of resin dispersants. The resin can improve the dispersibility and / or stability of graphene carbon nanoparticles in the dispersion. For example, the resin dispersant can include a combination of lauryl methacrylate (LMA) and vinyl pyrrolidone (VP) resins. The LMA-VP copolymer can be synthesized using conventional free radical polymerization chemistry. In such a formulation, LMA can generally account for 10 to 90 weight %, and VP can generally account for 10 to 90 weight %. For example, the range of LMA can be 40 or 50 to 85 weight %, and the range of VP can be 15 to 50 or 60 weight %. In certain embodiments, LMA can account for about 75 weight %, and VP can account for about 25 weight %. The resin dispersant can promote the dispersion and stability in the ground and unground graphene carbon nanoparticle dispersion.
[0037] For example, the resin dispersant may include an addition copolymer comprising stearyl acrylate (SA) and vinyl pyrrolidone (VP) residues. SA-VP copolymers may be synthesized using conventional free radical polymerization chemistry. In such formulations, SA may typically account for 10 to 90% by weight, and VP may typically account for 10 to 90% by weight. For example, SA may range from 40 or 50 to 85% by weight, while VP may range from 15 to 50 or 60% by weight. In certain embodiments, SA may account for about 75% by weight, while VP may account for about 25% by weight.
[0038] For example, the resin dispersant may include an addition polymer containing a vinyl pyrrolidone residue, such as, for example, polyvinyl pyrrolidone (PVP). The weight average molecular weight of PVP may be at least 1,000 g / mol, such as at least 3,000 g / mol, such as at least 5,000 g / mol. The weight average molecular weight of PVP may be no more than 2,000,000 g / mol, such as no more than 1,000,000 g / mol, such as no more than 500,000 g / mol, such as no more than 100,000 g / mol, such as no more than 50,000 g / mol, such as no more than 20,000 g / mol, such as no more than 15,000 g / mol. The weight average molecular weight of PVP may be 1,000 to 2,000,000 g / mol, such as 1,000 to 1,000,000 g / mol, such as 1,000 to 500,000 g / mol, such as 1,000 to 100,000 g / mol, such as 3,000 to 50,000 g / mol, such as 5,000 to 20,000 g / mol, such as 5,000 to 15,000 g / mol.
[0039] The weight ratio of graphene carbon nanoparticles to resin dispersant may generally be in the range of 0.1:1 to 20:1, for example 0.5:1 to 15:1, 1:1 to 10:1, or 3:1 to 6:1, such as 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, or 10:1.
[0040] The dispersant resin enhances the dispersion stability of graphene carbon nanoparticles and can expand the use of such nanoparticles in applications such as conductive inks, battery manufacturing, thermal conductive coatings, conductive coatings, EMI and RFI shielding coatings, lubricants, composite materials, 3D printing, etc. The dispersant of the present invention may include the following advantages: extended shelf life, high graphene carbon nanoparticle loading, and a dispersion that remains stable at room temperature and elevated temperatures.
[0041] Graphene carbon nanoparticles and resin dispersants can be added to various types of solvents to prepare the dispersion of the present invention. Suitable solvents include aqueous solvents and organic solvents, such as N-methyl-2-pyrrolidone (NMP), oil, benzyl alcohol, diethylene glycol monoethyl ester (DE) acetate, triethyl phosphate, etc.
[0042] Compared with conventional graphene carbon particle dispersion, graphene carbon nanoparticle of the present invention can be dispersed in various types of aqueous and organic solvents relatively in large quantities to produce dispersion with relatively high graphene carbon particle loading.For example, the graphene carbon particle of grinding can account for at least 5 weight % of the gross weight of solvent and graphene carbon particle.For example, the graphene carbon particle of grinding can account for at least 8 weight % or at least 10 weight % or at least 12 weight % or at least 15 weight % of dispersion.For example, in water-based solvent dispersion, the graphene carbon particle of grinding can be dispersed with 20 weight % or 23 weight % or 25 weight % or higher amount at the most.In organic solvent dispersion such as NMP, the graphene carbon particle of grinding can exist with 10 weight % or 12 weight % or 15 weight % or 20 weight % or higher amount at the most. Alternatively, the loading of the milled grapheme carbon particles can be relatively low, such as less than 5 or 3 wt%, or less than 2 or 1 wt%, or less than 0.5 or 0.1 wt%.
[0043] Compared with conventional additives, graphene carbon nanoparticles can be added to the basic formula at a relatively low loading. For example, the graphene carbon nanoparticle dispersion of the present invention can be added to the basic formula or material at a particle loading of less than 5 wt %, or less than 2 wt %, or less than 1 wt %, or less than 0.5 wt %, while meeting or exceeding the performance of conventional graphene-containing formulas or materials. For example, a loading of 0.05 to 1 wt % or 0.1 to 0.5 wt % can be used in lubricant formulations.
[0044] The instability index analysis can be used to accelerate the assessment of long-term stability, which measures the dispersion sedimentation at a specific centrifugal speed and temperature. Unless otherwise specified in the specification or claims, the measurement of the "instability index" is as follows: the dispersion sample is loaded into a centrifuge and a pulsed near-infrared light of 865nm is transmitted through the sample. During the centrifugation process, the near-infrared light transmitted through the sample is measured using a dispersion analyzer sold by LuM GmbH under the name LUMiSizer Model 611. The measurement is carried out at 25 ° C and 4000rpm centrifuge speed, and the relative centrifugal acceleration (RCA) is 2202 during the 20-minute centrifugation process. The transmission level at the beginning of the centrifugation is compared with the transmission level at the end of the 20-minute period, and the instability index is calculated by normalizing the recorded transmission level changes. The reported instability index is a dimensionless number between 0 and 1, where "0" means that the particle concentration has not changed, and "1" means that the dispersion has been completely phase separated. A relatively unstable dispersion will show a higher increase in transmittance due to significant phase separation of the graphene carbon nanoparticles and the solvent, while a relatively stable dispersion will show a lower increase in transmittance due to less phase separation. The software tool calculates the instability index. The article entitled "Instability Index" (T. Detloff, T. Sobisch, D. Lerche, Instability Index, Dispersion Letters Technical, T4 (2013) 1-4, updated 2014) describes How the software tool determines the instability index, which is incorporated herein by reference. The instability index of the ground graphene carbon nanoparticle aqueous dispersion can generally be less than 0.7, for example, less than 0.6, or less than 0.5, or less than 0.4, or less than 0.3, or less than 0.1. The instability index of the ground graphene carbon nanoparticle dispersion in the oil solvent is generally less than 0.5, for example, less than 0.4, or less than 0.3, or less than 0.2 or less than 0.1.
[0045] The instability index can be at least 10% less than a similar dispersion containing unmilled grapheme carbon particles, for example, at least 50% less, or at least 100% less, or at least 300% less, or at least 500% less.
[0046] Compared with similar solvent mixtures containing unground graphene carbon nanoparticles, solvent mixtures containing ground graphene carbon particles can have lower viscosity. For example, at a loading of 1 wt % of graphene carbon nanoparticles, ground graphene carbon particles can cause the viscosity of solvent dispersions to be at least 10% or 20% lower than the viscosity of similar solvent dispersions with unground graphene carbon particles. Viscosity can be measured by standard techniques, wherein rheological measurements are collected using Anton Paar MCR 302 and CP50-1 / TG measuring cones. Viscosity measurements at 10 Hz shear rates can be used for comparative dispersion rheology.
[0047] The ground graphene carbon nanoparticle dispersion can be added to various base formulations, such as by stirring, shaking, grinding, milling, etc. As described above, the base formulation to which the graphene carbon nanoparticle dispersion can be added can include various types of inks, coatings, lubricants, etc.
[0048] The graphene carbon particles used in the present invention can be obtained from commercial sources, such as from Raymor, Angstron, XGSciences and other commercial sources. As discussed in detail below, the graphene carbon particles can be produced according to the method and equipment described in U.S. Patents No. 8,486,363, No. 8,486,364 and No. 9,221,688, which are incorporated herein by reference. Carbon nanotubes or other carbonaceous materials such as conductive carbon black, graphite, etc. can be used in combination with graphene carbon particles or in place of graphene carbon particles.
[0049] As used herein, the term "graphene carbon particle" refers to a carbon particle having one or more layers of sp 2 Carbon particles of the structure of bonded carbon atom plane sheets, which are densely packed in a honeycomb lattice. The average number of stacked layers may be less than 100, for example less than 50. In certain embodiments, the average number of stacked layers is 30 or less, such as 20 or less, 10 or less, or in some cases 5 or less. The average number of stacked layers may be greater than 2, for example, greater than 3, or greater than 4. At least a portion of the graphene carbon particles may be in the form of substantially bent, curled, wrinkled or buckled flakes. The graphene carbon nanoparticles may be turbo-stationary, i.e., adjacent stacked atomic layers do not exhibit the ordered ABABernal stacking associated with conventional exfoliated graphene, but exhibit disordered or non-ABABAB stacking. Alternatively, the graphene carbon particles may be in the form of nanotubes. Particles generally do not have a spherical or equiaxed morphology.
[0050] Measured in the direction perpendicular to the carbon atom layer, graphene carbon nanoparticles may have a thickness of no more than 10 nanometers, no more than 5 nanometers, or no more than 4 or 3 or 2 or 1 nanometers in certain embodiments, such as no more than 3.6 nanometers. Graphene carbon particles can be from 1 atomic layer to 3, 6, 9, 12, 20 or 30 atomic layers or thicker. The width and length of the graphene carbon particles present in the composition of the present invention measured in the direction parallel to the carbon atom layer are at least 50 nanometers, such as greater than 100 nanometers, greater than 100 nanometers until 500 nanometers, or greater than 100 nanometers until 200 nanometers. Graphene carbon particles can be provided in the form of ultrathin flakes, lamellae or sheets, having a relatively high aspect ratio greater than 3: 1, such as greater than 10: 1 (aspect ratio is defined as the ratio of the longest dimension of the particle to the shortest dimension of the particle). Alternatively, when the graphene carbon particles are in the form of nanotubes, they may have an outer diameter of 0.3 to 100 nm, or 0.4 to 40 nm, a length of 0.3 nm to 50 cm, or 500 nm to 500 μm, and an aspect ratio of 1:1 to 100,000,000:1, or 10:1 to 10,000:1.
[0051] The graphene carbon particles may have a relatively low oxygen content. For example, even when having a thickness of no more than 5 nanometers or no more than 2 nanometers, the graphene carbon particles may have an oxygen content of no more than 2 atomic weight percent, such as no more than 1.5 or 1 atomic weight percent, or no more than 0.6 atomic weight percent, such as about 0.5 atomic weight percent. The oxygen content of the graphene carbon particles can be measured using an X-ray photoelectron spectrometer, such as described in DR Dreyer et al., Chem. Soc. Rev. 39, 228-240 (2010).
[0052] The graphene carbon particles may have a BET specific surface area of at least 50 m2 / g, such as 70 to 1000 m2 / g, or in some cases, 200 to 1000 m2 / g or 200 to 400 m2 / g. As used herein, the term "BET specific surface area" refers to a specific surface area measured by nitrogen adsorption according to the Brunauer-Emmett-Teller method described in the journal "The Journal of the American Chemical Society", 60, 309 (1938) according to the ASTM D3663-78 standard.
[0053] The graphene carbon particles may have a Raman spectrum 2D / G peak ratio of at least 0.9:1, or 0.95:1, or 1:1, such as at least 1.2:1 or 1.3:1. As used herein, the term "2D / G peak ratio" refers to the peak at 2692 cm -1The 2D peak intensity at 1,580 cm -1 Such a 2D / G peak ratio may exist in graphene carbon nanoparticles having an average stacking layer number greater than 2, such as 3 or more stacking layers.
[0054] The graphene carbon particles may have a relatively low bulk density. For example, the graphene carbon particles used in certain embodiments of the present invention are characterized by having a bulk density of less than 0.2 g / cm 3 , such as not more than 0.1 g / cm 3 The bulk density (tapped density) of the ground graphene carbon particles is determined for the purposes of the present invention by placing 0.4 grams of graphene carbon particles in a glass measuring cylinder with a readable scale. The cylinder is raised about 1 inch and tapped 100 times by hitting the bottom of the cylinder against a hard surface to allow the graphene carbon particles to settle within the cylinder. The volume of the particle is then measured and the bulk density is calculated by dividing 0.4 grams by the measured volume, where the bulk density is expressed in g / cm 3 express.
[0055] The compression density and densification percentage of the graphene carbon particles may be less than the compression density and densification percentage of graphite powder and certain types of substantially flat graphene carbon particles. Lower compression density and lower densification percentage are currently considered to be more conducive to better dispersion and / or rheological properties than graphene carbon particles exhibiting higher compression density and higher densification percentage. In certain embodiments, the compression density of the graphene carbon particles is 0.9 or less, such as less than 0.8, less than 0.7, such as 0.6 to 0.7. In certain embodiments, the densification percentage of the graphene carbon particles is less than 40%, such as less than 30%, such as 25% to 30%.
[0056] For the purposes of the present invention, the compression density of the graphene carbon particles is calculated by the measured thickness of a given mass of particles after compression. Specifically, the measured thickness is determined by cold pressing 0.1 grams of graphene carbon particles in a 1.3 cm mold at 15,000 pounds for 45 minutes, with a contact pressure of 500 MPa. The compression density of the graphene carbon particles is then calculated from the measured thickness according to the following equation:
[0057]
[0058] The densification percentage of the graphene carbon particles was then determined as the calculated compressed density of the graphene carbon particles determined above divided by the graphite density of 2.2 g / cm 3 ratio.
[0059] Immediately after mixing and at a later time point, such as 10 minutes, or 20 minutes, or 30 minutes or 40 minutes later, the measured volume liquid conductivity of the graphene carbon particles may be at least 100 microSiemens, such as at least 120 microSiemens, such as at least 140 microSiemens. For the purposes of the present invention, the volume liquid conductivity of the graphene carbon particles is determined as follows. First, a sample of a 0.5% solution of graphene carbon particles in butyl cellosolve is sonicated for 30 minutes with a bath sonicator. Immediately after sonication, the sample is placed in a standard calibrated conductivity cell (K=1). A Fisher Scientific AB 30 conductivity meter is introduced into the sample to measure the conductivity of the sample. Conductivity is plotted over the course of about 40 minutes.
[0060] The graphene carbon particles can be substantially free of unwanted or harmful materials. For example, the graphene carbon particles can contain zero or only trace amounts of polycyclic aromatic hydrocarbons (PAHs), such as less than 2 wt% PAH, less than 1 wt% PAH, or zero PAH.
[0061] The starting graphene carbon nanoparticles used in the present invention can be manufactured, for example, by heat treatment. According to an embodiment of the present invention, the thermally produced graphene carbon particles are made from a carbon-containing precursor material heated to a high temperature in a hot zone such as a plasma. A carbon-containing precursor, such as a hydrocarbon provided in a gaseous or liquid form, is heated in a hot zone to produce graphene carbon particles in or downstream of the hot zone. For example, the thermally produced graphene carbon particles can be manufactured by the systems and methods disclosed in U.S. Patents Nos. 8,486,363, 8,486,364, and 9,221,688.
[0062] Graphene carbon particles can be prepared by using the apparatus and method described in U.S. Pat. No. 8,486,363, wherein (i) one or more hydrocarbon precursor materials capable of forming dicarbon fragment species (such as n-propanol, ethane, ethylene, acetylene, vinyl chloride, 1,2-dichloroethane, allyl alcohol, propionaldehyde and / or vinyl bromide) are introduced into a hot zone (such as a plasma), and (ii) the hydrocarbon is heated to a temperature of at least 1,000° C. in the hot zone to form graphene carbon particles. Graphene carbon particles can be made by using the apparatus and method described in U.S. Pat. No. 8,486,364, wherein (i) a methane precursor material (such as a material comprising at least 50% methane, or in some cases, gaseous or liquid methane of at least 95% or 99% or more purity) is introduced into a hot zone (such as a plasma), and (ii) the methane precursor is heated in the hot zone to form graphene carbon particles. Such methods can produce graphene carbon particles having at least some, and in some cases all, of the above-described characteristics.
[0063] During the production of graphene carbon particles by the above-mentioned thermal production method, a carbon-containing precursor is provided as a feed that can be contacted with an inert carrier gas. The carbon-containing precursor material can be heated in a hot zone, for example, by a plasma system, such as a DC plasma, an RF plasma, a microwave plasma, etc. In certain embodiments, the precursor material is heated to a temperature greater than 2,000°C to 20,000°C or higher, such as 3,000°C to 15,000°C. For example, the temperature range of the hot zone can be 3,500°C to 12,000°C, such as 4,000°C to 10,000°C. Although the hot zone can be generated by a plasma system, it should be understood that any other suitable heating system can be used to create the hot zone, such as various types of furnaces, including electrically heated tubular furnaces, etc.
[0064] The gas stream may be contacted with one or more quench streams injected into the plasma chamber through at least one quench stream injection port. The quench stream may cool the gas stream to promote the formation of graphene carbon particles or control their particle size or morphology. In certain embodiments of the present invention, after the gaseous product stream is contacted with the quench stream, the ultrafine particles may pass through a converging member. After the graphene carbon particles leave the plasma system, they may be collected. The graphene carbon particles may be separated from the gas stream using any suitable means, such as a bag filter, a cyclone separator, or deposited on a substrate.
[0065] Without being limited by any theory, it is currently believed that the aforementioned method of manufacturing graphene carbon nanoparticles is particularly suitable for producing graphene carbon nanoparticles with relatively low thickness and relatively high aspect ratio and relatively low oxygen content as described above. In addition, contrary to the main production of particles with basic two-dimensional (or planar) morphology, it is currently believed that such methods can produce a large number of graphene carbon nanoparticles with basic bending, curling, wrinkling or buckling morphology (referred to as "3D" morphology herein). This characteristic is considered to be reflected in the compressed density characteristics described above, and is considered to be beneficial to the present invention, because it is currently believed that when a considerable portion of the graphene carbon particles have a 3D morphology, "edge to edge" and "edge to edge" contact between the graphene carbon particles in the composition can be promoted. This is considered to be because particles with 3D morphology are less likely to aggregate in the composition (due to lower van der Waals forces) than particles with two-dimensional morphology. Furthermore, it is currently believed that even in the case of "face-to-face" contact between particles having 3D morphology, since the particles may have more than one face plane, the entire particle surface will not have a single "face-to-face" interaction with another single particle, but may participate in interactions with other particles in other planes, including other "face-to-face" interactions. Therefore, graphene carbon particles having 3D morphology can provide good conductive and / or thermal conductive paths in dispersions and can be used to obtain conductive and / or thermal conductive properties. In addition, the 3D morphology can provide super lubricity in certain formulations.
[0066] The dispersant resin may include an addition polymer. The addition polymer may be derived from and include a structural unit including one or more α,β-ethylenically unsaturated monomer residues, such as those discussed below, and may be prepared by polymerizing a reaction mixture of such monomers. The monomer mixture may include one or more ethylenically unsaturated monomers containing active hydrogen groups. The reaction mixture may also include ethylenically unsaturated monomers containing heterocyclic groups. As used herein, an ethylenically unsaturated monomer containing a heterocyclic group refers to a monomer having at least one α,β ethylenically unsaturated group and at least one cyclic portion, which has at least one atom, such as, for example, oxygen, nitrogen or sulfur, in addition to the carbon in the ring structure. Non-limiting examples of ethylenically unsaturated monomers containing heterocyclic groups include vinyl pyrrolidone and vinyl caprolactam, etc. The reaction mixture may additionally include other ethylenically unsaturated monomers, such as alkyl esters of (meth) acrylic acid and other monomers described below.
[0067] The addition polymer may include a (meth)acrylic acid polymer comprising structural units comprising one or more (meth)acrylic acid monomer residues. The (meth)acrylic acid polymer may be prepared by polymerizing a reaction mixture of α,β-ethylenically unsaturated monomers comprising one or more (meth)acrylic acid monomers and optionally other ethylenically unsaturated monomers. As used herein, the term "(meth)acrylic acid monomer" refers to acrylic acid, methacrylic acid, and monomers derived therefrom, including alkyl esters of acrylic acid and methacrylic acid, etc. As used herein, the term "(meth)acrylic acid polymer" refers to a polymer derived from or comprising structural units comprising one or more (meth)acrylic acid monomer residues. The monomer mixture may include one or more (meth)acrylic acid monomers containing active hydrogen groups, ethylenically unsaturated monomers containing heterocyclic groups, and other ethylenically unsaturated monomers. The (meth)acrylic polymers may also be prepared using epoxy-functional ethylenically unsaturated monomers such as glycidyl methacrylate in a reaction mixture and the epoxy functional groups on the resulting polymer may be post-reacted with a β-hydroxy functional acid such as citric acid, tartaric acid and / or 3-hydroxy-2-naphthoic acid to produce hydroxyl functional groups on the (meth)acrylic polymer.
[0068] The addition polymer may include a structural unit that is included in the (meth) alkyl acrylate residue containing 8 to 22 carbon atoms in the alkyl group. The non-limiting examples of the (meth) alkyl acrylate containing 8 to 22 carbon atoms in the alkyl group include octyl (meth) acrylate, isodecyl (meth) acrylate, stearyl (meth) acrylate, 2-ethylhexyl (meth) acrylate, decyl (meth) acrylate, behenyl (meth) acrylate, octadecyl (meth) acrylate and lauryl (meth) acrylate. As a specific example, lauryl methacrylate may be used. By the gross weight of the addition polymer, the structural unit that includes the (meth) alkyl acrylate residue containing 8 to 22 carbon atoms in the alkyl group may account for at least 5 weight %, such as at least 10 weight %, such as at least 20 weight %, such as at least 30 weight %, such as at least 50 weight %, such as at least 70 weight %.
[0069] Addition polymer can include the structural unit comprising hydroxyalkyl ester residue.The limiting examples of hydroxyalkyl ester include hydroxyethyl (meth) acrylate and hydroxypropyl (meth) acrylate.By the gross weight of addition polymer, the structural unit comprising hydroxyalkyl ester residue can account for at least 0.5 weight %, such as at least 1 weight %, such as at least 2 weight %, and can be no more than 30 weight %, such as no more than 20 weight %, such as no more than 10 weight %, such as no more than 5 weight %.By the gross weight of addition polymer, the structural unit comprising hydroxyalkyl ester residue can account for 0.5 weight % to 30 weight %, such as 1 weight % to 20 weight %, such as 2 weight % to 20 weight %, 2 weight % to 10 weight %, such as 2 weight % to 5 weight %.By the gross weight of the polymerizable monomer used in the reaction mixture, addition polymer can be derived from the reaction mixture comprising 0.5 weight % to 30 weight %, such as 1 weight % to 20 weight %, such as 2 weight % to 20 weight %, 2 weight % to 10 weight %, such as 2 weight % to 5 weight % of hydroxyalkyl ester. Including a structural unit comprising a hydroxyalkyl ester residue in the dispersant results in the dispersant comprising at least one hydroxyl group (although the hydroxyl group may be included by other methods).
[0070] The addition polymer may include the structural unit that comprises the vinyl heterocyclic amide residue. The non-limiting examples of vinyl heterocyclic amides include vinyl pyrrolidone and vinyl caprolactam etc. By the gross weight of the addition polymer, the structural unit that includes the ethylenically unsaturated monomer residue that comprises the heterocyclic group may account for at least 0.5 wt %, such as at least 1 wt %, such as at least 10 wt %, such as at least 20 wt %, such as at least 40 wt %, such as at least 50 wt %, and may be not more than 90 wt %, such as not more than 85 wt %, such as not more than 60 wt %, such as not more than 50 wt %, such as not more than 40 wt %, such as not more than 30 wt %, such as not more than 20 wt %. The structural units comprising the residue of an ethylenically unsaturated monomer comprising a heterocyclic group may account for 0.5 wt % to 99 wt %, such as 0.5 wt % to 50 wt %, such as 1 wt % to 40 wt %, such as 5 wt % to 30 wt %, 8 wt % to 27 wt %, such as 10 wt % to 90 wt %, such as 15 wt % to 60 wt %, such as 15 wt % to 50 wt %, such as 40 wt % to 85 wt %, such as 50 wt % to 85 wt %. The addition polymer can be derived from a reaction mixture comprising ethylenically unsaturated monomers containing 0.5 to 50 wt % of heterocyclic groups, such as 1 to 40 wt %, such as 5 to 30 wt %, 8 to 27 wt %, such as 10 to 90 wt %, such as 15 to 60 wt %, such as 15 to 50 wt %, such as 40 to 85 wt %, such as 50 to 85 wt %, based on the total weight of polymerizable monomers used in the reaction mixture.
[0071] The addition polymer may contain structural units containing other α,β-ethylenically unsaturated monomer residues. Non-limiting examples of other α,β-ethylenically unsaturated monomers include vinyl aromatic compounds such as styrene, α-methylstyrene, α-chlorostyrene and vinyltoluene; organic nitriles such as acrylonitrile and methacrylonitrile; allyl monomers such as allyl chloride and allyl cyanide; monomer dienes such as 1,3-butadiene and 2-methyl-1,3-butadiene; and acetoacetoxyalkyl (meth) acrylates such as ethylene glycol acetoacetate methacrylate (AAEM) (which may be self-crosslinking). Based on the total weight of the addition polymer, the structural units containing other α,β-ethylenically unsaturated monomer residues may account for at least 0.5% by weight, such as at least 1% by weight, such as at least 2% by weight, and may be no more than 30% by weight, such as no more than 20% by weight, such as no more than 10% by weight, such as no more than 5% by weight. Structural units comprising residues of other α,β-ethylenically unsaturated monomers may account for 0.5 to 30 wt%, such as 1 to 20 wt%, such as 2 to 20 wt%, 2 to 10 wt%, such as 2 to 5 wt%, based on the total weight of the addition polymer. The addition polymer may be derived from a reaction mixture comprising 0.5 to 30 wt%, such as 1 to 20 wt%, such as 2 to 20 wt%, 2 to 10 wt%, such as 2 to 5 wt%, based on the total weight of the polymerizable monomers used in the reaction mixture.
[0072] Addition polymers can be prepared by conventional free radical initiated solution polymerization techniques, wherein polymerizable monomers are dissolved in a second organic medium comprising a solvent or a solvent mixture and polymerized in the presence of a free radical initiator until conversion is complete. The second organic medium for preparing the addition polymer can be the same as the organic medium present in the dispersion composition, so that the composition of the organic medium will not change due to the addition of the addition polymer solution. For example, the second organic medium can include the same primary solvent and cosolvent in the same proportion as the organic medium of the dispersion composition. Alternatively, the second organic medium for preparing the addition polymer can be different from and distinguished from the organic medium of the dispersion composition. The second organic medium for producing the addition polymer can include any suitable organic solvent or solvent mixture, including those discussed above about the organic medium, such as, for example, Aromatic 200, Solvesso 200, etc.
[0073] Examples of free radical initiators are those that are soluble in the monomer mixture, such as azobisisobutyronitrile, azobis(α,γ-methylvaleronitrile), t-butyl perbenzoate, t-butyl peracetate, benzoyl peroxide, di-t-butyl peroxide, and t-amyl peroxy-2-ethylhexyl carbonate.
[0074] Optionally, a chain transfer agent soluble in the monomer mixture may be used, such as an alkyl mercaptan, for example tert-dodecyl mercaptan; a ketone such as methyl ethyl ketone, a chlorinated hydrocarbon such as chloroform. The chain transfer agent provides control over the molecular weight so that the product has the desired viscosity for various coating applications. Tert-dodecyl mercaptan is preferred because it results in a high conversion of monomer to polymer product.
[0075] Addition polymers may be prepared with other structures as well as random and alternating copolymer structures including, but not limited to, block copolymers, graft copolymers, brush copolymers, star copolymers, and telechelic copolymers.
[0076] Block copolymers used herein can generally be described by the structure [A]-b-[B], where "b" represents a block structure and "r" represents a random structure. Although many block copolymers, including the one proposed in the present invention, are diblock copolymers, it is not uncommon to have additional blocks. The blocks of the block copolymer can be synthesized in any order (sequence) to achieve resin properties. However, there may be some comprehensive restrictions on the selection of block sequence. The individual blocks of the block copolymer can be homopolymers or can be copolymers of two or more monomers. Complete conversion of the first monomer is not required before synthesizing the second block, so the second block can be a copolymer of residual monomers from the first block and monomers from the second block (i.e., [A]-b-[ArB]). This is sometimes referred to as a "gradient" or "tapered" copolymer.
[0077] Block copolymers (e.g., diblock or triblock) can be produced by controlled radical polymerization of at least one ethylenically unsaturated monomer by the following reactions: reverse addition-fragmentation chain transfer (RAFT) mechanism, atom transfer radical polymerization (ATRP), nitroxide-mediated polymerization technology and organometallic mediated radical polymerization (OMRP), most notably cobalt-mediated radical polymerization (CMRP). Other methods include iodine-mediated polymerization, group transfer polymerization (GTP), anionic polymerization, cationic polymerization. The choice of method depends on many parameters, such as cost, compatibility with the selected monomers, tolerance to functional groups, operating temperature, whether the presence of catalysts (e.g., metals) is undesirable in the final product, etc. It should be understood that the first, second and (if used) third blocks of the block copolymer can be produced in any order (sequence), and one of the blocks can react with the first and / or second components.
[0078] As used herein, the term "controlled radical polymerization" and related terms such as "controlled radical polymerization process" include, but are not limited to, ATRP, single electron transfer (SET) polymerization, RAFT, and nitroxide-mediated polymerization.
[0079] Controlled radical polymerizations, such as RAFT and other polymerizations listed above, are often described as "living polymerizations," i.e., chain growth polymerizations that propagate substantially without chain transfer and substantially without chain termination. The molecular weight of polymers prepared by controlled radical polymerization can be controlled by the stoichiometry of the reactants, such as the initial concentrations of one or more monomers and one or more initiators. Controlled radical polymerization techniques allow a polymer of one monomer to be chain extended with a second type of polymer to produce a block copolymer. In addition, controlled radical polymerization also provides polymers having properties including narrow molecular weight distributions, such as polydispersity index (PDI) values within a desired range; and / or well-defined polymer chain structures, such as block copolymers and alternating copolymers.
[0080] The ATRP process can generally be described as comprising: polymerizing one or more free radical polymerizable monomers in the presence of an initiating system and forming a polymer. The initiating system can include an initiator having at least one free radical transferable atom or group; a transition metal compound, such as a catalyst, which participates in a reversible redox cycle with the initiator; and a ligand coordinated to the transition metal compound. U.S. Patents Nos. 5,763,548, 5,789,487, 5,807,937, 6,538,091, 6,887,962, 7,572,874, 7,893,173, 7,893,174, and 8,404,788 further describe the ATRP process in detail.
[0081] Reversible addition-fragmentation chain transfer, or RAFT polymerization, is one of several reversible-deactivation free radical polymerizations that utilizes chain transfer agents in the form of thiocarbonyl sulfides or similar compounds (such as dithioesters, thiocarbamates, and xanthates; also known as RAFT agents) to mediate polymerization via a reversible chain transfer process, thereby controlling the molecular weight, structure, and polydispersity of the resulting free radical polymerization process.
[0082] Nitroxide-mediated free radical polymerization is a free radical polymerization method that utilizes alkoxyamine initiators to produce polymers with well-controlled stereochemistry and very low polydispersity index. It is a reversibly deactivated free radical polymerization.
[0083] Graphene carbon nanoparticle dispersion of the present invention can be used for producing various types of material compositions. Composition can comprise any one of multiple thermoplastic and / or thermosetting compositions known in the art. For example, coating composition can comprise and be selected from epoxy resin, acrylic polymer, polyester polymer, polyurethane polymer, polyamide polymer, polyether polymer, epoxy polymer based on bisphenol A, polysiloxane polymer, styrene, ethylene, butylene, its copolymer and its mixture. Usually, these polymers can be any polymer of these types prepared by any method known to those skilled in the art. Such polymer can be solvent-based, water-soluble or water-dispersible, emulsifiable or have limited water solubility. In addition, polymer can be provided in sol-gel system, can provide in core-shell polymer system, or can provide in powder form. In certain embodiments, polymer is a dispersion in the continuous phase comprising water and / or organic solvent, such as emulsion polymer or non-aqueous dispersion.
[0084] In addition to the resin and graphene carbon nanoparticle components, coatings or other materials according to certain embodiments of the present invention may include additional components conventionally added to coating or ink compositions, such as crosslinkers, pigments, colorants, flow aids, defoamers, dispersants, solvents, UV absorbers, catalysts, and surfactants.
[0085] Thermosetting or curable coating compositions typically include a film-forming polymer or resin having functional groups reactive with itself or a crosslinking agent. The functional groups on the film-forming resin may be selected from any of a variety of reactive functional groups, including, for example, carboxylic acid groups, amine groups, epoxy groups, hydroxyl groups, thiol groups, carbamate groups, amide groups, urea groups, isocyanate groups (including blocked isocyanate groups and tri-alkylcarbamoyl triazines) mercaptan groups, styrene groups, anhydride groups, acetoacetate acrylates, uretdione groups, and combinations thereof.
[0086] The thermosetting coating composition generally comprises a crosslinking agent, which may be selected from, for example, aminoplasts, polyisocyanates including blocked isocyanates, polyepoxides, β-hydroxyalkylamides, polyacids, anhydrides, organometallic acid functional materials, polyamines, polyamides, and mixtures of any of the foregoing. Suitable polyisocyanates include polyfunctional isocyanates. Examples of polyfunctional polyisocyanates include aliphatic diisocyanates such as hexamethylene diisocyanate and isophorone diisocyanate, and aromatic diisocyanates such as toluene diisocyanate and 4,4'-diphenylmethane diisocyanate. Polyisocyanates may be blocked or unblocked. Examples of other suitable polyisocyanates include isocyanurate trimers, allophanates, and cyclic diureas of diisocyanates. Examples of commercially available polyisocyanates include DESMODUR N3390 sold by Bayer and TOLONATE HDT90 sold by Rhodia. Suitable aminoplasts include condensates of amines and / or amides with aldehydes. For example, condensates of melamine with formaldehyde are suitable aminoplasts. Suitable aminoplasts are well known in the art. Suitable aminoplasts are disclosed, for example, in U.S. Pat. No. 6,316,119, Col. 5, Lines 45-55, which is incorporated herein by reference. In certain embodiments, the resin may be self-crosslinking. Self-crosslinking means that the resin contains functional groups capable of reacting with itself, such as alkoxysilane groups, or the reaction product contains co-reactive functional groups, such as hydroxyl groups and blocked isocyanate groups.
[0087] The dry film thickness of the cured coating can generally be in the range of less than 0.5 micron to 100 microns or more, such as 1 to 50 microns. As a specific example, the thickness of the cured coating can be in the range of 1 to 15 microns. However, significantly greater coating thicknesses and significantly greater material sizes of non-coating materials are within the scope of the present invention.
[0088] As used herein, molecular weights are determined by gel permeation chromatography using polystyrene standards. Unless otherwise indicated, molecular weights are on a weight average basis.
[0089] In certain aspects of the invention, the graphene carbon nanoparticle dispersion can be used to prepare a lithium ion battery cathode and anode. The lithium ion battery may include an anode, a cathode, a separator between the anode and the cathode, and an electrolyte in contact with the anode and the cathode. The housing is in electrical contact with the anode, and the terminal is in electrical contact with the cathode.
[0090] The electrolyte of a lithium-ion battery may generally include a lithium-containing electrolyte salt dissolved in an organic solvent. Examples of lithium-containing electrolyte salts include LiClO4, LiAsF6, LiPF6, LiBF4, LiB(C6H5)4, LiB(C2O4)2, CH3SO3Li, CF3SO3Li, LiCl, LiBr, etc. Examples of organic solvents include propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, 1,2-dimethoxyethane, 1,2-diethoxyethane, γ-butyrolactone, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, ether, cyclopentane, methyl cyclopentane, acetonitrile, propionitrile, anisole, acetate, butyrate, propionate, etc. Cyclic carbonates such as propylene carbonate or chain carbonates such as dimethyl carbonate and diethyl carbonate may be used. These organic solvents may be used alone or in combination of two or more. In certain embodiments, the electrolyte may also include additives or stabilizers such as VC (ethylene carbonate), VEC (vinyl ethylene carbonate), FEC (fluoroethylene carbonate), EA (ethylene acetate), TPP (triphenyl phosphate), phosphazene, LiBOB, LiBETI, LiTFSI, BP (biphenyl), PS (propylene sulfite), ES (ethylene sulfite), AMC (allyl methyl carbonate) and APV (adipate divinyl ester).
[0091] Graphene carbon nanoparticle dispersions can be used to prepare lithium ion battery cathode materials, as disclosed in U.S. Patent No. 9,761,903, which is incorporated herein by reference. Graphene carbon nanoparticle dispersions can be used to prepare lithium ion battery anode materials as disclosed in U.S. Patent Application Publication No. 2014 / 0272591, which is incorporated herein by reference.
[0092] The cathode of a lithium ion battery may include a lithium-containing active material, graphene carbon nanoparticles from the present dispersion, and a binder. The cathode may include a conductive substrate, such as a metal foil containing Al, a carbon-coated aluminum foil, an aluminum porous metal body, etc. A coating of the cathode material may be deposited and cured on the substrate to form a coating having a typical dry film thickness of 5 or 10 to 500 microns, such as 20 or 25 to 200 microns, such as 50 to 100 microns.
[0093] The lithium-containing active material of the cathode coating may include LiFePO4, carbon-coated lithium iron phosphate, lithium cobaltate, lithium nickel cobalt aluminum oxide, lithium manganate, lithium nickel cobalt manganate, etc. For example, the lithium-containing active material accounts for 50-99.9% by weight of the solidified cathode coating material, such as 80-99.5% by weight, or 87-99% by weight. The graphene carbon nanoparticles may generally contain 0.25 to 25% by weight of the solidified cathode coating material, such as 0.5 to 10% by weight, or 1 or 2 to 8% by weight.
[0094] The binder may typically include polyvinylidene fluoride (PVDF), acrylic resins, cellulosics such as carboxymethyl cellulose, etc. The binder may comprise 0.25 to 25 wt % of the cured cathode coating material, such as 0.5 to 10 wt %, or 1 or 2 to 8 wt %.
[0095] The anode of the lithium-ion battery may include a conductive substrate, such as a copper foil or other metal foil, with a coating containing graphene carbon nanoparticles deposited on one or both sides thereof. The anode material containing graphene carbon particles may include a mixture of graphene carbon nanoparticles with lithium reactive particles such as Si and / or Sn and a binder.
[0096] The anode material may include 15 to 85 wt % of lithium reactive metal particles, 3 to 75 wt % of graphene carbon nanoparticles, and 3 to 60 wt % of a binder. For example, the lithium reactive metal particles may account for 25 to 70 wt %, or 30 to 50 wt %. For example, the graphene carbon nanoparticles may account for 10 to 60 wt %, or 30 to 50 wt %.
[0097] The lithium-reactive metal particles may include Si, Sn, or a combination thereof. The lithium-reactive metal particles may generally have an average particle size of less than 1,000 nanometers, such as 5 to 200 nanometers, or 10 to 120 nanometers.
[0098] The binder of the anode material may comprise a polymer. For example, the polymer binder may include poly(acrylic acid) (PAA), an acrylate polymer containing greater than 5 wt % acrylic acid, carboxymethyl cellulose, polymethacrylic acid, an acrylate polymer containing greater than 5 wt % methacrylic acid, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), acrylic latex dispersion, and the like.
[0099] In view of the foregoing, the present invention therefore relates to but is not limited to the following aspects:
[0100] Aspect 1. A dispersion comprising a solvent; graphene carbon nanoparticles; and a polymer dispersant resin.
[0101] Aspect 2. The dispersion according to aspect 1, wherein the graphene carbon nanoparticles have an average aspect ratio greater than 3:1 and a Raman 2D:G peak ratio of at least 1:1.
[0102] Aspect 3. The dispersion according to aspect 1 or 2, wherein the polymeric dispersant resin comprises an addition polymer comprising a vinyl heterocyclic amide residue.
[0103] Aspect 4. The dispersion according to aspect 3, wherein the vinyl heterocyclic amide comprises vinyl pyrrolidone.
[0104] Aspect 5. The dispersion according to any of the preceding aspects, wherein the dispersion has an instability index of less than 0.7.
[0105] Aspect 6. The dispersion according to any one of the preceding aspects, wherein the graphene carbon nanoparticles account for greater than 5 wt % based on the total weight of the dispersion.
[0106] Aspect 7. The dispersion according to aspect 6, wherein the dispersion has an instability index of less than 0.7.
[0107] Aspect 8. The dispersion according to aspect 6, wherein the instability index is less than 0.3.
[0108] Aspect 9. The dispersion according to any one of the preceding aspects, wherein the instability index of the dispersion is less than the instability index of the same dispersion containing graphene carbon nanoparticles having a Raman 2D:G peak ratio less than 0.9:1.
[0109] Aspect 10. The dispersion according to any of the preceding aspects, wherein the polymeric dispersant comprises polyvinylpyrrolidone.
[0110] Aspect 11. The dispersion according to aspect 10, wherein the polyvinyl pyrrolidone has a weight average molecular weight of 1,000 to 2,000,000.
[0111] Aspect 12. The dispersion according to any of the preceding aspects, wherein the graphene carbon nanoparticles are thermally produced at a temperature of at least 3,500°C.
[0112] Aspect 13. The dispersion according to any one of the preceding aspects, wherein the graphene carbon nanoparticles are ground.
[0113] Aspect 14. The dispersion of any of the preceding aspects, wherein the grapheme carbon particles are turbostratic and have a BET specific surface area of at least 70 m2 / g.
[0114] Aspect 15. The dispersion of any preceding aspect, wherein the solvent comprises water.
[0115] Aspect 16. The dispersion of any preceding aspect, wherein the solvent comprises an organic solvent.
[0116] Aspect 17. The dispersion according to aspect 16, wherein the organic solvent comprises oil, N-methyl-2-pyrrolidone, benzyl alcohol, diethylene glycol monoethyl (DE) acetate and / or triethyl phosphate.
[0117] Aspect 18. The dispersion of aspect 16, wherein the organic solvent comprises oil.
[0118] Aspect 19. The dispersion according to aspect 16, wherein the organic solvent comprises N-methyl-2-pyrrolidone.
[0119] Aspect 20. The dispersion according to any one of the preceding aspects, wherein the weight ratio of the graphene carbon nanoparticles to the dispersant resin is from 0.5:1 to 15:1.
[0120] Aspect 21 A dispersion according to Aspect 1, wherein the polymer dispersant resin comprises an addition polymer, and the addition polymer comprises a homopolymer, a block (co)polymer, a random (co)polymer, an alternating (co)polymer, a graft (co)polymer, a brush (co)polymer, a star (co)polymer, a telechelic (co)polymer or a combination thereof.
[0121] Aspect 22. The dispersion according to aspect 21, wherein the dispersion has an instability index of less than 0.5.
[0122] Aspect 23. The dispersion according to aspect 21 or 22, wherein the graphene carbon nanoparticles account for greater than 3 weight percent based on the total weight of the dispersion.
[0123] Aspect 24. The dispersion according to any one of aspects 21-23, wherein the instability index is less than 0.3.
[0124] Aspect 25. The dispersion according to any of aspects 21-24, wherein the polymeric dispersant is an addition polymer comprising an alkyl (meth)acrylate residue having 8 to 22 carbon atoms in the alkyl group, a vinyl heterocyclic amide residue, or a combination thereof.
[0125] Aspect 26. The dispersion according to aspect 25, wherein the alkyl (meth)acrylate containing 8 to 22 carbon atoms in the alkyl group comprises lauryl methacrylate or stearyl acrylate.
[0126] Aspect 27. The dispersion according to any of aspects 26-26, wherein the vinyl heterocyclic amide comprises vinyl pyrrolidone.
[0127] Aspect 28. The dispersion according to any one of aspects 21-27, wherein the graphene carbon nanoparticles are thermally produced at a temperature of at least 3,500°C.
[0128] Aspect 29. The dispersion of any one of aspects 21-28, wherein the graphene carbon nanoparticles have an average aspect ratio greater than 3:1 and a Raman 2D:G peak ratio of at least 1:1.
[0129] Aspect 30. The dispersion of any one of aspects 21-29, wherein the grapheme carbon particles are turbostratic and have a BET specific surface area of at least 70 m2 / g.
[0130] Aspect 31. The dispersion according to any one of aspects 21-30, wherein the graphene carbon nanoparticles are ground.
[0131] Aspect 32. The dispersion according to any one of aspects 21-31, wherein the organic solvent comprises oil, N-methyl-2-pyrrolidone, benzyl alcohol, diethylene glycol monoethyl (DE) acetate and / or triethyl phosphate.
[0132] Aspect 33. The dispersion of any one of aspects 21-31, wherein the organic solvent comprises an oil.
[0133] Aspect 34. The dispersion of any one of aspects 21-31, wherein the organic solvent comprises N-methyl-2-pyrrolidone.
[0134] Aspect 35. The dispersion according to any one of aspects 21-34, wherein the weight ratio of the graphene carbon nanoparticles to the dispersant resin is from 0.5:1 to 15:1.
[0135] Aspect 36. A method for dispersing graphene carbon nanoparticles in a solvent, comprising mixing a dispersant resin into the solvent, wherein the dispersant resin comprises an addition polymer, and the addition polymer comprises a homopolymer, a block (co)polymer, a random (co)polymer, an alternating (co)polymer, a graft (co)polymer, a brush (co)polymer, a star (co)polymer, a telechelic (co)polymer or a combination thereof; and mixing the graphene carbon nanoparticles into the solvent and dispersant resin mixture.
[0136] Aspect 37. The method according to aspect 36, wherein the addition polymer comprises a vinyl heterocyclic amide residue.
[0137] Aspect 38. The method according to aspect 36 or 37, further comprising grinding the graphene carbon nanoparticles before mixing the graphene carbon nanoparticles into the solvent and dispersant resin mixture.
[0138] Aspect 39. The method according to any one of aspects 36-38, wherein the graphene carbon nanoparticles have an average aspect ratio greater than 3:1 and a Raman 2D:G peak ratio of at least 1:1.
[0139] Aspect 40 A dispersion prepared by the method of any one of aspects 36-39.
[0140] Aspect 41. The dispersion according to aspect 40, wherein the dispersion comprises the dispersion according to any one of aspects 1-35.
[0141] Aspect 42. A lubricant comprising the dispersion according to any one of aspects 1-36.
[0142] Aspect 43. A lubricant according to Aspect 42, wherein the lubricant comprises a base oil, a dispersant resin and graphene carbon nanoparticles dispersed in the base oil; the dispersant resin comprises an addition polymer, and the addition polymer comprises a homopolymer, a block (co)polymer, a random (co)polymer, an alternating (co)polymer, a graft (co)polymer, a brush (co)polymer, a star (co)polymer, a telechelic (co)polymer or a combination thereof.
[0143] Aspect 44. A lithium-ion battery electrode slurry comprising lithium-containing active materials or lithium-reactive particles; and the dispersion according to any one of aspects 1-35.
[0144] Aspect 45. A lithium ion battery electrode, wherein the lithium ion battery electrode is made of the lithium ion battery electrode slurry according to Aspect 44.
[0145] The following examples are intended to illustrate various aspects of the present invention and are not intended to limit the scope of the present invention.
[0146] Example 1
[0147] 2 grams of graphene carbon nanoparticles (GNP) powder commercially available from Raymor produced according to the teachings of U.S. Patent No. 8,486,364 were added to a 100 mL plastic cup (FlackTek Company) with 6 zirconium oxide beads (5 mm, very high density zirconium oxide, 95% ZrO2, 5% Y2O3, Glen Mills). The sample was mixed for 8 minutes at 2350 rpm at 2 minute intervals on a FlackTek fast mixer (DAC600.1FVZ). The grinding beads were then removed from the container. For larger quantities, 25 grams of graphene carbon nanoparticles were added to a 500 mL plastic cup with 20 beads and mixed for 8 minutes at 2350 rpm at 2 minute intervals on a fast mixer. Powder samples were then collected for analytical characterization and dispersion preparation. Deionized water can be optionally added to the graphene carbon nanoparticles in the container, for example, a deionized water mist can be sprayed onto the graphene carbon nanoparticle powder in a plastic cup, wherein the water level is 0% to 99.9%. The water-wetted GNP sample can then be mixed on a rapid mixer with grinding beads under the same conditions as above.
[0148] After preparing the GNP samples by speed mixer mixing as described in Example 1, the samples were formulated as dispersions in various aqueous and organic solvents. Milled Graphene Carbon Nanoparticle Dispersions can be prepared using various milling techniques including speed mixer, Cowles blade, and Eiger mill milling.
[0149] Example 2
[0150] In the rapid mixer dispersion, 0.34% dispersant resin (50% solids) listed in Table 1 was first added to the base oil solvent in a plastic cup. The sample was mixed with 6 zirconium oxide beads on a rapid mixer for 4 minutes, or longer as needed, until the resin was completely dissolved. Afterwards, 0.50% of the pre-ground graphene powder prepared in Example 1 was added to the cup of the resin-solvent mixture and mixed for another 8 minutes at 2350rpm on a rapid mixer. The process was repeated, except that the graphene carbon nanopowder of Example 1 was replaced by commercially available exfoliated graphene sold by XG Sciences under the name M25. The weight percentages of each component in the standard base oil dispersion formula are listed in Table 1. Using LUMiSizer, the instability index of each dispersion was measured to be 0.201 at 1500rpm, 313RCA (relative centrifugal acceleration), 25°C, and 5 minutes. Figure 1 is a graph of the instability index versus time for the oil dispersion of Table 1 containing ground plasma graphene carbon particles and ground exfoliated graphene carbon particles with a graphene loading of 0.5% and a graphene to resin ratio of 10. Figure 1 It is shown that under the same formulation, the milled plasma graphene dispersion exhibits a significantly lower instability index and better stability than the milled commercial exfoliated graphene dispersion.
[0151] Table 1 Composition of GNP dispersion in oil (wt%)
[0152] Components GNP 0.50 0 M25 Graphene 0 0.50 Dispersant resin* 0.17 0.17 Oil solvent** 99.33 99.33
[0153] *Dispersant resin: Copolymer of lauryl methacrylate and vinyl pyrrolidone
[0154] **Oil solvents: various types of oil solvents, including but not limited to bar chain oil, cutting oil, gear oil, hydraulic oil, air compressor oil, pneumatic tool oil, etc.
[0155] While the solid-state pre-grinding process is effective in improving the dispersion quality of thermally produced turbostratic graphene carbon nanoparticles, no significant improvement in dispersion quality was observed when the same grinding process was applied to commercially available exfoliated graphene M25.
[0156] Example 3
[0157] In the speed mixer dispersion, 7.7% polyvinyl pyrrolidone (PVP) was first added to deionized water in a plastic cup. The sample was mixed with 6 zirconium oxide beads on the speed mixer for 4 minutes, or longer if necessary, until the resin was completely dissolved. After that, 23% of the pre-ground GNP powder prepared in Example 1 was added to the cup along with the PVP dispersant and solvent mixture and mixed again on the speed mixer at 2350 rpm for another 8 minutes. The weight percentages of the components in the standard water dispersion formula are listed in Table 2.
[0158] Table 2 Aqueous graphene dispersion
[0159] Components weight% Deionized water 69.3% PVP* 7.7% GNP 23%
[0160] *PVP, polyvinylpyrrolidone, CAS#9003-39-8, Mw=10,000, Sigma Aldrich
[0161] Example 4
[0162] In the Cowles blade dispersion, 7.7% polyvinyl pyrrolidone (PVP) was first added to deionized water while mixing with a Cowles blade. Once the resin was completely dissolved, 23% of the pre-ground GNP powder prepared by Example 1 GNP was gradually added while stirring vigorously with a Cowles blade, starting at 500RPM and steadily increasing to 2000RPM as needed. The mixture was then mixed on the Cowles blade for 30 minutes, or longer if necessary. The weight percentages of the components in the standard aqueous dispersion formula are listed in Tables 3 and 4. The dispersion in Table 3 prepared using this process had an instability index of 0.335 measured using a LUMiSizer at 4000rpm, 2201RCA, 25°C, and 20 minutes. The instability index of the dispersion in Table 4 prepared using this process was measured to be 0.582.
[0163] Table 3 Aqueous graphene dispersion
[0164] Components weight% Deionized water 69.3% PVP* 7.7% GNP 23%
[0165] *PVP, polyvinylpyrrolidone, CAS#9003-39-8, Mw=10,000, Sigma Aldrich
[0166] Example 5
[0167] In the Eiger mill dispersion, the Cowles blade is first used for pre-dispersion. The resin is added to the water or solvent while mixing with a high lift or Cowles blade. Once the resin is completely dissolved, the GNPs are gradually added while stirring vigorously with a Cowles blade, starting at 500RPM and steadily increasing to 2000RPM as needed. The pre-dispersed formulation is then ground using an Eiger mill with 1-1.2mm Zirconox grinding media to a residence time of 20 minutes to further reduce the particle size. The weight percentages of the components in the standard water dispersion formulation are listed in Tables 3 and 4. The instability index of the dispersion in Table 3 measured using a LUMiSizer at 4000rpm, 2201RCA (relative centrifugal acceleration), 25°C, and 20 minutes is 0.080. The instability index of the dispersion in Table 4 measured using a LUMiSizer at 4000rpm, 2201RCA, 25°C, and 20 minutes is 0.511. Figure 2 is a plot of the instability index versus time for aqueous dispersions containing milled plasma graphene carbon particles (20% graphene loading) and milled exfoliated graphene carbon particles (8% graphene loading), wherein the graphene to resin ratio is 3. The graph shows that the 20% milled plasma graphene dispersion exhibits a significantly lower instability index and better stability than the 8% milled exfoliated graphene dispersion.
[0168] Table 4 Aqueous graphene dispersion
[0169] Components weight% Deionized water 89.3% PVP* 2.7% GNP 8%
[0170] *PVP, polyvinylpyrrolidone, CAS#9003-39-8, Mw=10,000, Sigma Aldrich
[0171] Example 6
[0172] The components listed in Table 5 were used to prepare the compositions.
[0173] Table 5
[0174]
[0175] 4 PVP, Polyvinylpyrrolidone, CAS#9003-39-8, from Sigma Aldrich
[0176] 5 Thermally produced graphene carbon particles produced according to the method disclosed in U.S. Pat. No. 8,486,364, having a measured BET specific surface area of at least 300 m 2 / g, an average number of layers of 7, and a flake size of 150-200 nm, and is commercially available as PureWave graphene (GNP) from Raymor NanoIntgris.
[0177] The components in Table 5 constitute the water-based (wb) graphene carbon nanoparticle pre-dispersion formulation. First, PVP was added to the water while mixing with a high lift or Cowles blade. Once PVP was completely dissolved in the water, GNPs were gradually added while stirring vigorously with a Cowles blade, starting at 500 RPM and steadily increasing to 2000 RPM as needed. The pre-dispersed formulation in Table 5 was ground to a residence time of 20 minutes using an Eiger mill with 1-1.2 mm Zirconox grinding media to reduce the particle size to less than 1 μm.
[0178] As shown in Table 6, the pre-dispersion and grind dispersion of Table 5 were analyzed for particle size, instability and rheology.
[0179] Table 6
[0180]
[0181] 6 Particle size - measured by Mastersizer 2000, an analytical technique for measuring particle size distribution, from Melvern Instruments
[0182] 7 Instability Index - measured by LUMiSizer, an analytical technique for accelerated instability, from LUM GmbH, measured at 4000 rpm for 60 seconds
[0183] 8 High and low shear viscosity - measured using the Anton Paar Rheometer from Anton Paar Example 7
[0184] In the Cowles blade dispersion, 40% of LMA-VP resin (50% solids) was first added to the base oil solvent while mixing with a Cowles blade. Once the resin was completely dissolved, 20% of the pre-ground graphene powder prepared in Example 1 was gradually added while stirring vigorously with a Cowles blade, starting at 500 RPM and steadily increasing to 2000 RPM as needed. The mixture was then mixed on the Cowles blade for 30 minutes, or longer if necessary. The weight percentages of the components in the standard dispersion formula are listed in Table 7.
[0185] Table 7 Composition of GNP dispersions in oil
[0186] Components weight% GNP 20 Dispersant resin* 20 Resin solvent 20 Oil solvent** 40
[0187] *Dispersant resin: Copolymer of lauryl methacrylate and vinyl pyrrolidone
[0188] **Oil solvents: various types of oil solvents, including but not limited to bar chain oil, cutting oil, gear oil, hydraulic oil, air compressor oil, pneumatic tool oil, etc.
[0189] Example 8
[0190] In a speed mixer dispersion, 0.5% of polyvinyl pyrrolidone (PVP) was first added to N-methyl-2-pyrrolidone (NMP) in a plastic cup. The sample was mixed with 6 zirconium oxide beads on a speed mixer for 4 minutes, or longer as needed, until the resin was completely dissolved. Afterwards, 5% of the pre-ground graphene powder prepared in Example 1 was added to the cup of the resin-solvent mixture and mixed again on the speed mixer at 2350 rpm for another 8 minutes. The weight percentages of the components in the standard aqueous dispersion formula are listed in Table 8.
[0191] Table 8 Composition of GNP dispersion in N-methyl-2-pyrrolidone (NMP)
[0192] Components weight% GNP 5% PVP* 0.5% NMP** 94.5%
[0193] *PVP, polyvinylpyrrolidone, CAS#9003-39-8, Mw=10,000, Sigma Aldrich
[0194] **NMP, N-methyl-2-pyrrolidone, CAS#872-50-4, anhydrous, 99.5%, Sigma Aldrich
[0195] Example 9
[0196] The compositions listed in Table 9 were prepared.
[0197] Table 9
[0198] weight% C D E 95% <![CDATA[ 9 NMP]]> NMP NMP 0.5% PVP <![CDATA[ 10 SAR resin]]> <![CDATA[ 11 PSII]]> 4.5% TGC TGC TGC
[0199] 9 NMP-N-methyl-2-pyrrolidone, CAS#872-50-4, from Sigma Aldrich
[0200] 10 SAR Resin - Acrylic Resin from PPG
[0201] 11 PSII - Acrylic resin from PPG
[0202] The components in samples C, D and E from Table 9 constitute the solvent-based graphene carbon nanoparticle dispersion formulation. For sample C, PVP was added to NMP while mixing with a Cowles blade. Once PVP was completely dissolved in NMP, TGC was gradually added while stirring vigorously with a Cowles blade, starting at 500RPM and steadily increasing to 2000RPM as needed. The pre-dispersed sample C formulation was ground using an Eiger grinder with 1-1.2mm Zirconox grinding media to a residence time of 20 minutes.
[0203] For Sample D, SAR resin was added to NMP and mixed on a FlackTek speed mixer at 2350 rpm for 5 minutes. TGC was then added to the mixture and mixed on a speed mixer at 2350 rpm for another 5 minutes. The mixing step was repeated as needed.
[0204] For Sample E, PSII resin was added to NMP and mixed on a FlackTek speed mixer at 2350 rpm for 5 minutes. TGC was then added to the mixture and mixed on a speed mixer at 2350 rpm for another 5 minutes. The mixing step was repeated as needed.
[0205] In order to better understand the dispersed material, in situ optical microscopy was used. In this case, the same concentration of graphene (0.5%) before and after grinding was dispersed using the same dispersant (PVP 10:1P / B) and solvent (NMP) similar to Example 8 above and was drop cast onto a glass slide. These were observed in situ during the solvent evaporation process. Two qualitative observations can be made. First, Figure 6 and Figure 7 Compared with the ball milling shown in Figure 4 and Figure 5 As shown in Figure 2, there are more micron-sized aggregates in the prepared graphene. As the solvent evaporates, Figure 4 and Figure 5 The size of the aggregates shown increases. Figure 3 This can also be easily seen with the naked eye when the same solution is drop cast onto a silicon wafer as shown.
[0206] Table 10 based on Figure 5 and Figure 7 The average particle area
[0207] picture sample Average particle area 5 Ball milling GNPs <![CDATA[0.6μm 2 ]]> 7 Unground GNPs <![CDATA[2.0μm 2 ]]>
[0208] A variety of analytical characterization techniques can be employed to monitor material quality and determine whether the desired thermal and electrical properties of graphene are retained after processing. In addition, tests can be performed to probe the physical changes caused by solid-state milling in order to understand the structure-property relationships that lead to improved dispersion quality and stability.
[0209] Raman, XPS and TEM can be used to monitor material quality. These can be used to test the graphite quality, purity and structure of the material. In the case of solid state grinding, Raman and XPS show defect density ( Fig. 9 ) and oxygen incorporation ( Figure 8 ) increases as a function of grinding time. In addition, high-magnification TEM shows that the morphology of individual graphene carbon nanoparticles before grinding ( Fig.10 ) and after grinding ( Fig.11 ) are the same.
[0210] The dispersion properties of solutions similar to those of Example 7 were analyzed using an Anton-Paar rheometer with parallel plate geometry (1 mm gap and 50 mm diameter), where the GNP loading was systematically varied. The two types of GNPs with and without solid-state grinding process were the main difference between the two series. NMP was used as solvent, while PVP (Mw-10000) was used as polymer binder, and the composition was kept at 10% (by weight) of the GNP weight in the solution. The samples were stabilized at 25°C for 5 minutes before measurement. Dynamic frequency sweep measurements were performed at a constant strain of 0.1% in the linear viscoelastic region (LVR) to study the dispersion structure as a function of GNP concentration, thereby accurately determining the GNP concentration at which the transition from fluid to strong gel behavior occurs.
[0211] Fig.12 and Fig.13 The frequency-dependent complex modulus (G' and G") and complex viscosity trends ( Fig.14 ). Classic strong gel behavior can be determined by dynamic frequency sweep measurements when the results are i) G' and G" values are independent of frequency and ii) the viscosity decreases with a gradient of ~(-1) on the double logarithmic plot for all applied frequencies. For the lowest concentration of 0.5%, the solution shows a viscoelastic response that is already close to strong gel behavior, and all solutions above 1% show strong gel behavior.
[0212] For the series with solid-state milled GNPs ( Fig.15 and Fig.16 ), the GNP concentration for strong gel behavior increased significantly by nearly 15% compared to the solution with pristine GNPs (<1%). It was found that G' and G" increased with concentration, frequency-independent complex modulus (G' and G") values, and viscosity ( Fig.17) increases with the increase of ), following a power law of ~(-1) in the double logarithmic plot, which is observed for the ball-milled GNP sample at a loading of nearly 15%.
[0213] A dramatic shift in the fluid-strong gel transition from about 1% to about 15% GNP loading was achieved by a solid phase grinding process. Conventional exfoliated graphene is known to have poor dispersibility even with polymer binders in organic and aqueous solutions, and strong gel behavior has been reported for similar systems with graphene loadings mostly below 1%. Dispersibility may be slightly improved by introducing structural defects (such as oxygen in graphene oxide), but the highest graphene loading in the strong gel state to date remains well below 5%.
[0214] Fig.18 Figure 1 is the flow curve of graphene aqueous dispersion. An 8% pristine graphene dispersion is compared to a 20% solid state milled graphene dispersion. The figure shows that the solid state milling process can significantly increase the solid content of the dispersion from 8% to 20% while maintaining comparable viscosity.
[0215] Fig.19 The viscosity of the graphene carbon nanoparticle dispersion at a shear rate of 10 Hz is shown for an 8% pristine graphene carbon nanoparticle dispersion and a 20% solid-state milled graphene carbon nanoparticle dispersion. The figure shows that the solid content of the dispersion can be significantly increased from 8% to 20% by the solid-state milling process while maintaining comparable viscosity.
[0216] Fig. 20 The curves for NMP dispersions comparing 5% pristine graphene carbon nanoparticle dispersions to 10%, 15% solid grind dispersions are shown. The graph shows that the 10% and 15% solid grind dispersions exhibit lower viscosities than the 5% standard dispersion.
[0217] Fig.21 The viscosity of the graphene carbon nanoparticle dispersion at 10 Hz shear rate is shown for 5% original graphene carbon nanoparticle dispersion and 10% and 15% solid ground graphene carbon nanoparticle dispersions. The figure shows that the 10% and 15% solid ground dispersions exhibit lower viscosity than the 5% standard dispersion.
[0218] It is obvious that the dispersion quality of solid-state milled GNPs is improved by an order of magnitude compared with the original unmilled GNPs.
[0219] The ground graphene carbon nanoparticles were dispersed in hydrocarbon oil. The results showed that solid-state grinding can not only increase the solid content of graphene carbon nanoparticles, but also significantly improve the quality and stability of graphene carbon nanoparticle dispersions.
[0220] like Fig. 22 , Fig.23and Fig.24 As shown in the instability index graph in , the solid state grinding process reduces the instability index compared to the original unground graphene carbon nanoparticle dispersion, making such dispersions more stable at room temperature and high temperature. The instability index of each dispersion was measured using a LUMiSizer at 1500 rpm, 313 RCA (relative centrifugal acceleration) and 25°C. Although Fig. 22 and Fig.23 Only times up to 10 minutes are shown, but the instability curve stabilizes at 10 minutes so that the instability index at 20 minutes will be essentially the same as shown at 10 minutes. The combination of grinding and resin addition provides a synergistic effect for the stabilization of the graphene carbon nanoparticle dispersion.
[0221] Solid-state grinding of graphene carbon can significantly increase the solid content and stability of graphene carbon nanoparticles in the dispersion, allowing the particles to be more effectively integrated into various solvent and water systems. Raman and XPS may show that defect density and oxygen incorporation increase with increasing grinding time, and rheological studies show that the fluid-strong gel transition increases from 1% of the dispersion made of original graphene carbon nanoparticles to 15% of the dispersion made of solid-state ground graphene carbon nanoparticles. Dispersions made with solid-state ground graphene carbon nanoparticles can achieve comparable battery performance in silicon anodes (2.5 times higher solid content) and better conductivity in LiFePO4 cathodes.
[0222] Alkyl-functionalized VP resins were evaluated as dispersants in NMP formulations suitable for lithium-ion battery electrode manufacturing. In a typical dispersion formulation, the dispersant resin (0.5 wt% of dispersion solids) was dissolved in NMP in a dual-pass asymmetric centrifuge (DAC) cup. GNP powder (5.0 wt% of dispersion solids) was added to the NMP solution and the cup was mixed for 8 minutes using a speed mixer DAC and six 5 mm ceramic mixing beads. The mixture was then stirred for 2-3 0 minutes using a 5% ethanol solution. The dispersion analyzer measures the instability index value to evaluate the room temperature stability of each dispersion. It should be noted that lower instability index values correspond to increased dispersion stability.
[0223] Copolymer resins with LMA contents ranging from 10 to 90 wt % were prepared using tert-amyl peroxy (2-ethylhexyl) carbonate (Trigonox 131) as a free radical initiator and targeting an initial [M]0:[I]0 ratio of 85:1. GNP dispersions were then prepared using the DAC mixing procedure described above and the instability index value of each resulting dispersion was measured. SAR dispersants were prepared by free radical polymerization of methyl methacrylate, 2-hydroxyethyl acrylate, methacrylic acid, 2-ethylhexyl acrylate and VP using NMP as a suitable polymerization solvent. SAR25 and SAR50 were prepared with VP incorporation levels of 25 wt % and 50 wt %, respectively. Fig.25 As shown, all LMA-VP copolymers provided dispersions with lower room temperature instability index values compared to the commercial PVP control (Mw ~ 10,000 g / mol) and SAR dispersants with 25 wt% or 50 wt% VP. Increasing the LMA content from 10 wt% to 70 wt% resulted in a decrease in the dispersion instability index, which reached a minimum when the dispersant contained 70 wt% or 75 wt% LMA. These results indicate that LMA-VP copolymers containing 70-75 wt% LMA are optimal for dispersing and stabilizing GNPs in NMP.
[0224] As described more fully in the following examples, graphene carbon nanoparticles were dispersed in an N-methyl-2-pyrrolidone (NMP) solution containing a polymer resin comprising N-vinyl pyrrolidone, N-vinyl pyrrolidone copolymerized with lauryl methacrylate (P(LMA-co-VP)) at various ratios of N-vinyl pyrrolidone to lauryl methacrylate ranging from 100:0 to 3:1, 1:1, and 1:3, and the viscosity of the graphene carbon nanoparticle dispersion decreased significantly with increasing lauryl methacrylate content, and the total solids of the dispersion remained constant at 6 wt%. In addition, it was generally observed that the particle size of the graphene carbon nanoparticles in the dispersion increased with increasing lauryl methacrylate content relative to the total solids content of the graphene carbon nanoparticle dispersion. This result indicates that the increased particle size due to lauryl methacrylate content varies with decreasing viscosity of the graphene carbon nanoparticle dispersion. The distribution of the lauryl methacrylate and N-vinyl pyrrolidone in the polymer resin as well as the molecular weight of the polymer resin may also be a factor in the overall particle size and viscosity of the dispersion.
[0225] Graphene carbon nanoparticle dispersions in NMP containing different amounts of lauryl methacrylate and N-vinyl pyrrolidone as a polymer resin dispersant were used as conductive additives for lithium-ion battery cathodes, where LiNi 0.5 Mn 0.3 Co 0.2O2 as the active material for Li-ion based energy storage and polyvinylidene fluoride as the binder, it is shown that when included in a lithium-ion battery electrode slurry composition, the graphene carbon dispersant resin has little effect on the rate performance and cycle life in button cell format. These results ensure that the graphene carbon nanoparticle dispersion with a lower viscosity using a certain ratio of lauryl methacrylate and N-vinyl pyrrolidone P(LMA-co-VP) can be used in electrochemically active Li-ion cathode films without significant observable degradation in the cycle life or rate performance of batteries in button cell format.
[0226] The increase of lauryl methacrylate in the dispersant resin allows an increase in the total solid content of the graphene carbon nanoparticle dispersion while achieving a desirable viscosity comparable to that using only poly(vinyl pyrrolidone) (abbreviated as PVP) as the dispersant.
[0227] Example 10
[0228] The compositions were prepared with the components listed in Table 11 under a N2 blanket to prevent moisture. In a speed mixer dispersion, the PVP dispersant resin was first added to NMP along with 10 zirconium oxide beads and mixed at 2000 rpm for 2 minutes until fully dissolved / dispersed. Then, graphene carbon nanoparticles (GNPs) were added and mixed at 2000 rpm for a total of 8 minutes or until fully dispersed. The weight percentages of the components in the standard dispersion formulation are listed in Table 11.
[0229] Table 11 GNP distribution in NMP with PVP
[0230] Components Dispersion A (wt%) Dispersion B (wt%) Dispersion C (wt%) NMP* 94.0 94.0 94.0 GNP 5.4 5.0 4.5 PVP 0.6 1.0 1.5
[0231] *NMP, N-methyl-2-pyrrolidone, CAS#872-50-4, anhydrous, 99.5%, Sigma Aldrich
[0232] **PVP, polyvinylpyrrolidone, CAS#9003-39-8, Mw=10,000 g / mol, Sigma Aldrich
[0233] Example 11
[0234] Compositions were prepared with the components listed in Table 12 under a N2 blanket to prevent moisture. In a speed mixer dispersion, P(LMA-co-VP) was first added to NMP along with 10 zirconium oxide beads and mixed at 2000 rpm for 2 minutes until fully dissolved / dispersed. Then, GNPs were added and mixed at 2000 rpm for a total of 8 minutes or until fully dispersed. The weight percentages of the components in the standard dispersion recipe are listed in Table 12.
[0235] Table 12 GNP distribution in NMP with P(LMA-co-VP)
[0236] Components Dispersion A (wt%) Dispersion B (wt%) Dispersion C (wt%) NMP* 94.0 94.0 94.0 GNP 5.4 5.0 4.5 Resin 1** 0.6 1.0 1.5
[0237] *NMP, N-vinylpyrrolidone, CAS#872-50-4, anhydrous, 99.5%, Sigma Aldrich
[0238] **Resin 1-Copolymer of lauryl methacrylate and N-vinyl pyrrolidone, P(LMA-co-VP) dispersed in NMP at a ratio of 1:3, Mw = ~16,000 g / mol
[0239] Example 12
[0240] Compositions were prepared with the components listed in Table 10 under a N2 blanket to prevent moisture. In a speed mixer dispersion, P(LMA-co-VP) was first added to NMP along with 10 zirconium oxide beads and mixed at 2000 rpm for 2 minutes until fully dissolved / dispersed. Then, GNPs were added and mixed at 2000 rpm for a total of 8 minutes or until fully dispersed. The weight percentages of the components in the standard dispersion recipe are listed in Table 13.
[0241] Table 13 GNP distribution in NMP with P(LMA-co-VP)
[0242]
[0243] *NMP, N-vinylpyrrolidone, CAS#872-50-4, anhydrous, 99.5%, Sigma Aldrich
[0244] **Resin 2-Lauryl methacrylate and N-vinyl pyrrolidone copolymer, P(LMA-co-VP) dispersed in NMP in a 1:1 ratio, Mw = ~31,000 g / mol
[0245] Example 13
[0246] Compositions were prepared with the components listed in Table 14 under a N2 blanket to prevent moisture. In a speed mixer dispersion, P(LMA-co-VP) was first added to NMP along with 10 zirconium oxide beads and mixed at 2000 rpm for 2 minutes until fully dissolved / dispersed. Then, GNPs were added and mixed at 2000 rpm for a total of 8 minutes or until fully dispersed. The weight percentages of the components in the standard dispersion recipe are listed in Table 14.
[0247] Table 14 GNP distribution in NMP with P(LMA-co-VP)
[0248]
[0249] *NMP, N-vinylpyrrolidone, CAS#872-50-4, anhydrous, 99.5%, Sigma Aldrich
[0250] **Resin 3-Copolymer of lauryl methacrylate and N-vinyl pyrrolidone, P(LMA-co-VP) dispersed in NMP at a ratio of 3:1, Mw = ~35,000 g / mol
[0251] Example 14
[0252] The compositions were prepared with the components listed in Table 15 under a N2 blanket to prevent moisture. In a speed mixer dispersion, P(LMA-co-VP) was first added to NMP along with 10 zirconium oxide beads and mixed at 2000 rpm for 2 minutes until fully dissolved / dispersed. Then, GNPs were added and mixed at 2000 rpm for a total of 8 minutes or 4 x 2 minute incremental mixing steps were used until fully dispersed. The weight percentages of the components in the standard dispersion formulation are listed in Table 15.
[0253] Table 15 GNP distribution in NMP with P(LMA-co-VP)
[0254]
[0255] *NMP, N-vinylpyrrolidone, CAS#872-50-4, anhydrous, 99.5%, Sigma Aldrich
[0256] **Resin 4-Lauryl methacrylate and N-vinyl pyrrolidone copolymer, P(LMA-co-VP) dispersed in n-pentyl propionate at a ratio of 3:1, Mw = ~43,000 g / mol
[0257] Example 15
[0258] In order to understand how changes in the lauryl methacrylate content will affect the viscosity of graphene carbon nanoparticle dispersions with low resin content, rheological measurements were collected using Anton Paar MCR 302 and CP50-1 / TG measuring cones. Viscosity measurements at a shear rate of 10 Hz were used to compare dispersion rheology. In each of Examples 10, 11, 12, and 13, the dispersion tested was described as Dispersion A, which contained a ratio of graphene to resin of 9. Fig.26 It is shown that at this particular resin content level, the resin has little effect on the rheological properties of the graphene carbon nanoparticle dispersion.
[0259] Example 16
[0260] To understand how changes in lauryl methacrylate content would affect the viscosity of graphene carbon nanoparticle dispersions with medium resin content, rheological measurements were collected at a shear rate of 10 Hz from the slurry described as Dispersion B in Examples 10, 11, 12, and 13, which contained a ratio of graphene carbon nanoparticles to resin of 5. Fig. 27 It is shown that when the lauryl methacrylate component is increased from 0% to 75% of the polymer resin at this particular resin content level, the viscosity of the graphene carbon nanoparticle dispersion is significantly reduced. Therefore, when using a ratio of graphene to resin >5, the increase in solids content may be less than about 30%.
[0261] Example 17
[0262] To understand how changes in lauryl methacrylate content would affect the viscosity of high resin content graphene carbon nanoparticle dispersions, rheological measurements were collected at a shear rate of 10 Hz from a slurry described as Dispersion C, which contained a ratio of graphene carbon nanoparticles to resin of 3. Fig.28 It is shown that the viscosity of the graphene carbon nanoparticle dispersion decreases significantly when the lauryl methacrylate component increases from 0% to 75% of the polymer resin at this particular resin content level. Therefore, when using a graphene to resin ratio of <5, the increase in solids content can be higher than about 30%.
[0263] Example 18
[0264] To determine the increased solids content achievable with resins containing high levels of lauryl methacrylate, graphene carbon dispersions were formulated at different total solids contents, but with a constant graphene carbon nanoparticle to resin ratio of 5. The compositions of the graphene carbon nanoparticle dispersions are shown in Table 16. Fig.29 and Fig.30It is shown that when Resin 3 is used to replace PVP in NMP-based graphene carbon nanoparticle dispersions, an increase in total solids up to and including about 30% can be achieved while maintaining similar viscosity at the same shear rate as when a graphene to resin ratio of 5 is used.
[0265] Table 16 GNP dispersion in NMP with PVP or resin 3
[0266]
[0267] *NMP, N-vinylpyrrolidone, CAS#872-50-4, anhydrous, 99.5%, Sigma Aldrich
[0268] **PVP, polyvinylpyrrolidone, CAS#9003-39-8, Mw=10,000 g / mol, Sigma Aldrich
[0269] ***Resin 3-Copolymer of lauryl methacrylate and N-vinyl pyrrolidone, P(LMA-co-VP) dispersed in NMP at a ratio of 3:1, Mw = ~35,000 g / mol
[0270] Example 19
[0271] To test the electrochemical stability of the dispersants when used in Li-ion cathode membranes, the graphene carbon nanoparticle dispersions listed above were used in a Li-ion cathode slurry formulation under a N2 blanket consisting of the components listed in Table 17. In a rapid mixer dispersion, the graphene carbon nanoparticle dispersion was added to the desired LiNi 0.5 Mn 0.3 Co 0.2 O2 active material and mixed at 2000 rpm for 30 seconds. Then add the required LiNi 0.5 Mn 0.3 Co 0.2 The other 1 / 2 of the O2 active material was mixed at 2000 rpm for a total of 60 seconds using 2×30 second incremental mixing steps. Before adding poly(vinylidene fluoride) (PVDF) to the Li-ion cathode slurry, PVDF was dissolved in NMP to prepare an 8 wt% solution. The resulting PVDF solution was then added to the LiNi 0.5 Mn 0.3 Co 0.2O2 and graphene carbon nanoparticle dispersions were added to a Li-ion cathode slurry and mixed at 2000 rpm for 30 seconds. The remaining amount of NMP was then added to the slurry and mixed at 2000 rpm in 30 second increments until fully mixed, with a total mixing time typically ranging from as low as 2 minutes to as high as 6 minutes. The film was then cast onto an aluminum foil substrate using a doctor blade method at a speed of 10 mm per second and then cured at 55°C for 2 minutes, followed by a second curing step at 120°C for 2 minutes. The film was then calendered to a desired porosity of about 25%-35%. Figure 31-Figure 38 Scanning electron microscope images of the final Li-ion cathode film are shown as cross-sections of the film. These images show that the 0.5 Mn 0.3 Co 0.2 Relatively uniform distribution of graphene carbon nanoparticles and binder within the larger secondary particle network of O2 particles.
[0272] Table 17 Li-ion cathode slurry composition
[0273] Components Weight percentage (%) <![CDATA[LiNi 0.5 Mn 0.3 What 0.2 O2]]> 45 GNP dispersion* 29 PVDF** 1 NMP*** 25
[0274] *GNP dispersions described in Example 8 Dispersion A and Dispersion B, Example 9 Dispersion A and Dispersion B, Example 10 Dispersion A and Dispersion B, and Example 11 Dispersion A and Dispersion B.
[0275] **PVDF-poly(vinylidene fluoride), Solvay 5130, Mw=1,000,000-1,100,000g / mol
[0276] ***NMP, N-vinylpyrrolidone, CAS#872-50-4, anhydrous, 99.5%, Sigma Aldrich
[0277] Example 20
[0278] To test the electrochemical stability of the dispersants when used in Li-ion cathode membranes, coin cells of the membranes described in Example 19 were assembled in a VAC Atmospheres Nexus II glove box under argon with an oxygen content of <2 ppm and a HO content of <0.5 ppm. Prior to coin cell fabrication, the films were punched into 1 cm 2The segments were used for button cell fabrication and vacuum dried at 110°C for 10 hours and then placed directly in a glove box without exposure to the outside atmosphere. 2032 button cells were used for fabrication, lithium metal was used as the counter electrode and reference electrode, and Celgard 2320 polypropylene / polyethylene / polypropylene (PP / PE / PP) was used as a separator. 75 μL of 1M LiPF6 solution dissolved in 3:7 ethylene carbonate / ethyl methyl carbonate and 2 wt % vinyl carbonate additive was used as an electrolyte. The button cells were charged and discharged at various rates described in Table 18 between 3.0 V and 4.3 V versus Li using a Bio-Logic BCS-805 or BCS-810 battery cycler, in order from top to bottom, for a total of 50 cycles.
[0279] Table 18 Charge and discharge rates of Li-ion button batteries
[0280] Charge / discharge C rate Cycle times 0.1C 3 0.2C 3 0.4C 3 0.8C 3 1.6C 3 1.0C 35
[0281] like Fig.39 and Fig.40 As shown, when the lauryl methacrylate content increases from 0% to 75% of the graphene carbon nanoparticle dispersion, and the ratio of graphene carbon nanoparticles to resin is 9 or 5, there seems to be little effect on capacity retention and cycle life. These results ensure that the graphene carbon nanoparticle dispersion that results in a reduced viscosity of the graphene carbon nanoparticle dispersion can be used for Li-ion cathode electrodes and has minimal impact on battery performance in button cell format, with the largest impact on rate capability at 1.6C compared to the Example 10 Dispersion A and B controls (no lauryl methacrylate in the graphene carbon nanoparticle dispersion resin) from Example 11 Dispersion A and B (dispersion with the highest lauryl methacrylate content).
[0282] Example 21
[0283] A dispersant resin having a random copolymer structure comprising lauryl acrylate and N-vinyl pyrrolidone monomers was prepared using free radical polymerization chemistry. In a typical preparation, Solvesso 200 (23.15 g) was charged to a reactor and heated to 110°C under a constant nitrogen atmosphere. A mixture of Solvesso 200 (3.56 g) and a free radical initiator, tert-amyl peroxy-2-ethylhexyl carbonate (0.46 g) was then added dropwise to the reactor from an initiator feed tank over 185 minutes. Five minutes after the free radical initiator solution was started, a mixture of lauryl acrylate (26.25 g) and N-vinyl pyrrolidone (8.75 g) was added to the reactor from a monomer feed tank over 180 minutes. After the free radical initiator and monomer feeds were completed, the monomer feed tank was rinsed with Solvesso 200 (3.56 g) and the solution was added to the reactor. A mixture of Solvesso 200 (3.56 g) and tert-amyl peroxy-2-ethylhexyl carbonate (0.15 g) was added to the reactor from the initiator tank over 60 minutes. The initiator feed tank was rinsed with Solvesso 200 (1.78 g) and the solution was added to the reactor. The reaction was then maintained at a constant temperature of 110° C. for 60 minutes.
[0284] Example 22
[0285] A dispersant resin having a random copolymer structure comprising lauryl methacrylate and N-vinyl pyrrolidone monomers was prepared using free radical polymerization chemistry. In a typical preparation, Solvesso 200 (20.00 grams) was charged to a reactor and heated to 120°C under a constant nitrogen atmosphere. A mixture of Solvesso 200 (3.60 grams) and a free radical initiator, tert-amyl peroxy-2-ethylhexyl carbonate (0.44 grams) was added dropwise to the reactor from an initiator feed tank over 185 minutes. Five minutes after the free radical initiator solution was started, a mixture of lauryl methacrylate (24.50 grams) and N-vinyl pyrrolidone (10.50 grams) was added to the reactor from a monomer feed tank over 180 minutes. After the free radical initiator and monomer feeds were completed, the monomer feed tank was rinsed with Solvesso 200 (4.80 grams) and the solution was added to the reactor. A mixture of Solvesso 200 (1.20 g) and tert-amyl peroxy-2-ethylhexyl carbonate (0.15 g) was added to the reactor from the initiator tank over 60 minutes. The reaction solution was then maintained at 120° C. for 30 minutes. A mixture of Solvesso 200 (1.20 g) and tert-amyl peroxy-2-ethylhexyl carbonate (0.15 g) was added to the reactor from the initiator tank over 60 minutes. The initiator feed tank was rinsed with Solvesso 200 (1.65 g) and the solution was added to the reactor. The reaction was then maintained at a constant temperature of 120° C. for 60 minutes.
[0286] Example 23
[0287] A dispersant resin having a random copolymer structure comprising stearyl acrylate and N-vinyl pyrrolidone monomers was prepared using free radical polymerization chemistry. In a typical preparation, Solvesso 200 (13.15 g) was charged to a reactor and heated to 110°C under a constant nitrogen atmosphere. A mixture of Solvesso 200 (3.56 g) and a free radical initiator, tert-amyl peroxy-2-ethylhexyl carbonate (0.46 g) was then added dropwise to the reactor from an initiator feed tank over 185 minutes. Five minutes after the start of the free radical initiator solution addition, a mixture of stearyl acrylate (26.25 g) and N-vinyl pyrrolidone (8.75 g), heated at 45°C to provide compatibility, was added to the reactor from a monomer feed tank over 180 minutes. After the free radical initiator and monomer feeds were completed, the monomer feed tank was rinsed with Solvesso 200 (1.56 g) and the solution was added to the reactor. A mixture of Solvesso 200 (3.56 g) and tert-amyl peroxy-2-ethylhexyl carbonate (0.15 g) was added to the reactor from the initiator tank over 60 minutes. The initiator feed tank was rinsed with Solvesso 200 (1.78 g) and the solution was added to the reactor. The reaction was then maintained at a constant temperature of 110° C. for 60 minutes.
[0288] Example 24
[0289] A dispersant resin having a random copolymer structure comprising stearyl methacrylate and N-vinyl pyrrolidone monomers was prepared using free radical polymerization chemistry. In a typical preparation, Solvesso 200 (23.15 g) was charged to a reactor and heated to 110° C. under a constant nitrogen atmosphere. A mixture of Solvesso 200 (3.87 g) and a free radical initiator, tert-amyl peroxy-2-ethylhexyl carbonate (0.50 g) was added dropwise to the reactor from an initiator feed tank over 185 minutes. Five minutes after the free radical initiator solution was started, a mixture of stearyl methacrylate (26.25 g) and N-vinyl pyrrolidone (8.75 g) was added to the reactor from a monomer feed tank over 180 minutes. After the free radical initiator and monomer feeds were completed, the monomer feed tank was rinsed with Solvesso 200 (3.56 g) and the solution was added to the reactor. A mixture of Solvesso 200 (3.56 g) and tert-amyl peroxy-2-ethylhexyl carbonate (0.15 g) was added to the reactor from the initiator tank over 60 minutes. The initiator feed tank was rinsed with Solvesso 200 (1.78 g) and the solution was added to the reactor. The reaction was then maintained at a constant temperature of 110° C. for 60 minutes.
[0290] Example 25
[0291] A dispersant resin having a random copolymer structure comprising stearyl acrylate and N-vinyl pyrrolidone monomers was prepared using free radical polymerization chemistry. In a typical preparation, n-pentyl propionate (18.18 g) was loaded into a reactor and heated to 120° C. under a constant nitrogen atmosphere. A mixture of n-pentyl propionate (3.66 g) and a free radical initiator, tert-pentyl peroxy-2-ethylhexyl carbonate (0.35 g) was added dropwise to the reactor from an initiator feed tank over 185 minutes. Five minutes after the free radical initiator solution was started, a mixture of stearyl acrylate (22.05 g), N-vinyl pyrrolidone (9.45 g) and Solvesso 200 (4.50 g) was added to the reactor from a monomer feed tank over 180 minutes. After the free radical initiator and monomer feeds were completed, the monomer feed tank was rinsed with n-pentyl propionate (1.80 g) and the solution was added to the reactor. A mixture of n-pentyl propionate (1.22 g) and tert-pentyl peroxy-2-ethylhexyl carbonate (0.12 g) was added to the reactor from the initiator tank over 60 minutes. The initiator feed tank was rinsed with n-pentyl propionate (2.25 g) and the solution was added to the reactor. The reaction was then maintained at a constant temperature of 120° C. for 60 minutes.
[0292] Example 26
[0293] A dispersant resin having a block copolymer structure comprising stearyl acrylate and N-vinyl pyrrolidone monomers was prepared using a reversible addition-fragmentation chain transfer (RAFT) polymerization reaction. In a typical preparation, n-pentyl propionate (70.2 g), 2-cyanobutane-2-yl-4-chloro-3,5-dimethyl-1H-pyrazole-1-dithiocarbonate (BM1565) (2.0724 g) and stearyl acrylate (100.8 g) were loaded into a reactor and heated to 85 ° C under a constant nitrogen atmosphere (covered and sprayed). A mixture of n-pentyl propionate (27.4 g) and a free radical initiator 2,2'-azobis(2-methylbutyronitrile) (0.2769 g) was sprayed with nitrogen for 15 minutes and then added dropwise to the reactor within 120 minutes. After the free radical initiator feed was completed, the reaction was kept at a constant temperature of 85 ° C for 60 minutes. Subsequently, a mixture of N-vinyl pyrrolidone (43.2 g) and n-pentyl propionate (21.6 g) was sparged with nitrogen for 15 minutes and then added dropwise to the reactor over 30 minutes. A mixture of n-pentyl propionate (27.4 g) and a free radical initiator 2,2'-azobis(2-methylbutyronitrile) (0.2769 g) was sparged with nitrogen for 15 minutes and then added dropwise to the reactor over 120 minutes. After the free radical initiator feed was completed, the reaction was maintained at a constant temperature of 85°C for 150 minutes.
[0294] For the purpose of detailed description, it should be understood that the present invention can envision various alternative changes and step sequences, unless there is an opposite explicit description. In addition, except in any operating example, or in the case of otherwise specified, all numerals, such as those representing values, quantities, percentages, ranges, sub-ranges and fractions, can be considered to start with "about", even if the term does not clearly appear. Therefore, unless there is an opposite indication, the numerical parameters set forth in the following specification and the appended claims are approximate values, which can change according to the desired characteristics to be obtained by the present invention. At least, and not intended to limit the application principle of the scope equivalent to the claims, each numerical parameter should be understood at least according to the numerical value with reported significant digits and using general rounding techniques. In the case of describing closed or open numerical ranges herein, all numerals, values, quantities, percentages, sub-ranges and fractions within or covered in the numerical range are considered to be specifically included in the original disclosure of the application and belong to the original disclosure of the application, as these numerals, values, quantities, percentages, sub-ranges and fractions have all been clearly written out.
[0295] Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the invention are approximations, the numerical values set forth in the specific examples are reported as precisely as possible. Any numerical value, however, inherently contains certain errors necessarily resulting from the standard deviation found in their respective testing measurements.
[0296] As used herein, "comprising," "containing," and similar terms are understood in the context of this application to be synonymous with "comprising," and are therefore open-ended and do not exclude the presence of additional undescribed or unlisted elements, materials, ingredients, or method steps. As used herein, "consisting of" is understood in the context of this application to exclude the presence of any unspecified elements, ingredients, or method steps. As used herein, "consisting essentially of" is understood in the context of this application to include the specified elements, materials, ingredients, or method steps, "as well as those that do not materially affect the basic and novel characteristics described."
[0297] As used herein, the terms "on", "onto", "applied on", "applied onto", "formed on", "deposited on", "deposited onto" refer to forming, covering, depositing or providing on but not necessarily in contact with a surface. For example, an electrodepositable coating composition "deposited onto" a substrate does not exclude the presence of one or more other intermediate coatings of the same or different composition located between the electrodepositable coating composition and the substrate.
[0298] While specific embodiments of the present invention have been described above for purposes of illustration, it will be apparent to those skilled in the art that various changes may be made in the details of the invention without departing from the invention as defined in the appended claims.
Claims
1. A dispersion comprising: Organic solvents; Graphene carbon nanoparticles; A polymer dispersant resin, wherein the polymer dispersant resin comprises an addition polymer, wherein the addition polymer comprises a homopolymer, a block (co)polymer, a random (co)polymer, an alternating (co)polymer, a graft (co)polymer, a brush (co)polymer, a star (co)polymer, a telechelic (co)polymer or a combination thereof.
2. The dispersion of claim 1, wherein the dispersion has an instability index of less than 0.
5.
3. The dispersion of claim 1, wherein the graphene carbon nanoparticles comprise greater than 3 wt % based on the total weight of the dispersion.
4. The dispersion of claim 3, wherein the instability index is less than 0.
3.
5. The dispersion of claim 1, wherein the polymeric dispersant comprises an addition polymer comprising an alkyl (meth)acrylate residue having from 8 to 22 carbon atoms in the alkyl group, a vinyl heterocyclic amide residue, or a combination thereof. 6 . The dispersion according to claim 5 , wherein the alkyl (meth)acrylate containing 8 to 22 carbon atoms in the alkyl group comprises lauryl methacrylate or stearyl acrylate.
7. The dispersion of claim 5, wherein the vinyl heterocyclic amide comprises vinyl pyrrolidone.
8. A method of preparing the dispersion of claim 1, wherein the graphene carbon nanoparticles are thermally produced at a temperature of at least 3,500°C.
9. The dispersion of claim 1, wherein the graphene carbon nanoparticles have an average aspect ratio greater than 3:1 and a Raman 2D:G peak ratio of at least 1:1, wherein the graphene carbon particles are turbostratic.
10. The dispersion of claim 1, wherein the graphene carbon nanoparticles are milled graphene carbon nanoparticles.
11. The dispersion of claim 1, wherein the graphene carbon particles are turbostratic and have a BET specific surface area of at least 70 m2 / g.
12. The dispersion of claim 1, wherein the organic solvent comprises oil, N-methyl-2-pyrrolidone, benzyl alcohol, diethylene glycol monoethyl (DE) acetate, and / or triethyl phosphate.
13. The dispersion of claim 12, wherein the organic solvent comprises an oil.
14. The dispersion of claim 12, wherein the organic solvent comprises N-methyl-2-pyrrolidone. 15 . The dispersion according to claim 1 , wherein the weight ratio of the graphene carbon nanoparticles to the dispersant resin is 0.5:1 to 15:
1.
16. A lubricant comprising the dispersion according to claim 1 dispersed in a base lubricating oil, wherein the graphene carbon nanoparticles account for 0.05 to 1 wt% based on the total weight of the lubricant.
17. A lithium ion battery electrode, comprising: lithium-containing active materials or lithium-reactive particles; and The dispersion according to claim 1.
Citation Information
Patent Citations
Method for stably dispersing graphene or / and carbon nanotubes in organic solvent
CN102911531A
Nanoplatelet dispersions, methods for their production and uses thereof
CN107922764A
Preparation method of graphene-containing lubricant additives and / or lubricating grease additives
CN107955671A
Method for producing composite material and composite molded product
JP2013071946A
Graphene-dispersed liquid and preparation method thereof
JP2014009104A