Preparation method of magnesium aluminum silicate adsorbent

Through the preparation method of magnesium aluminum silicate adsorbent, the existing silicate adsorbent has solved the problem of small specific surface area and complex preparation, and efficient removal of transition metal ions is achieved, simplified the process flow, and is suitable for industrial production.

CN118929681APending Publication Date: 2024-11-12ZHEJIANG HUANGMA TECH CO LTD +4
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411092216.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing silicate adsorbent has a small specific surface area, poor adsorption effect of transition metal ions, and a complex preparation process. Some processes require acid treatment to lead to waste acid contamination.

Method used

The preparation method of magnesium aluminum silicate adsorbent is adopted to synthesize inorganic silicate, magnesium salt and aluminum salt under hydrothermal reaction, and control the reaction conditions and raw material ratio to prepare a large specific surface area and strong adsorption capacity of transition metal ions. magnesium aluminum silicate adsorbent without acidification.

Benefits of technology

The specific surface area and transition metal ion removal rate of magnesium aluminum silicate adsorbent are improved to reach 99.9%, the preparation process is simplified, the equipment requirements are reduced, and it is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929681A_ABST
    Figure CN118929681A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of adsorbents and the technical field of inorganic silicate material preparation, and discloses a preparation method of a magnesium aluminum silicate adsorbent. The preparation method comprises the following steps: dissolving inorganic silicate in water, then adding an inorganic magnesium salt aqueous solution, and reacting to obtain a white turbid liquid I; adding an inorganic aluminum salt aqueous solution into the white turbid liquid I, and reacting to obtain a white turbid liquid II; and finally, carrying out hydrothermal reaction on the white turbid liquid II to prepare the magnesium aluminum silicate adsorbent. The prepared magnesium aluminum silicate is large in specific surface area and can efficiently adsorb transition metal ions within a short time; and meanwhile, new impurities are not introduced, metal transition ions can be removed to the level of 1 ppm or below, and the removal rate of the transition metal ion impurities reaches up to 99.9%. The preparation method provided by the invention is simple in process, does not need acid liquor treatment, has low requirements on instruments and equipment, and can adapt to large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adsorbents and the technical field of inorganic silicate material preparation, and particularly relates to a method for preparing a magnesium aluminum silicate adsorbent. Background Art

[0002] Transition metal ions can cause certain harm or impact on the human body and the production of some industrial products. With the rapid development of industry, transition metal ions are widely present in our daily environment and enter our body through our daily diet, thus causing a variety of diseases in the human body. At the same time, transition metal ions as impurities can cause a greater impact in the production process of some industrial products. For example, the most important thing in the development process is to ensure the cleanliness of the product manufacturing process. Surfactants are usually used for cleaning. The most commonly used surfactant is distyrylphenol polyoxyethylene ether (DSP polyether). However, DSP polyether will introduce transition metal ion impurities during the development process, thereby affecting the development process and causing irreversible effects on the product.

[0003] Methods for removing transition metal ions include adsorption, ion exchange, oxidation-reduction, flocculation, electrochemical, membrane separation, etc. Adsorption is widely used due to its low cost, environmental friendliness, and good effect in removing transition metal ions. Adsorbents can effectively adsorb transition metal ions through chelation, electrostatic action, physical adsorption or chemical adsorption, with high removal rate and good adsorption effect.

[0004] An adsorbent is a solid substance or material that can adsorb specific impurities in a liquid or gas environment. The adsorbent should have the following characteristics: (1) It has a large specific surface area, can fully contact with the adsorbate, and promote the adsorption of the adsorbate; (2) It has excellent chemical stability and will not react chemically with the adsorbate to produce new substances or introduce new impurities; (3) It is simple to manufacture and the raw materials are easy to obtain; (4) It has good directional adsorption performance for the adsorbate. Silicate adsorbents are widely used due to their high pore volume, high specific surface area, good stability, relatively simple preparation process, and relatively low raw material prices.

[0005] In recent years, silicate adsorbents have been widely used in the adsorbent field. They can be used to adsorb a variety of impurities, such as alkali metals, transition metal ions, impurities in crude oil, and trace pesticides in soil. Silicate adsorbents include magnesium silicate (talc), aluminum silicate (kaolinite) adsorbents, etc. However, the silicate adsorbents currently prepared still have problems such as small specific surface area, poor adsorption effect on transition metal ions, complex preparation process, and acid treatment (causing waste acid pollution) in some processes.

[0006] Therefore, there is an urgent need to provide a silicate adsorbent that has a simple preparation method, does not require acidification, and has a strong adsorption capacity for transition metal ions. Summary of the invention

[0007] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a method for preparing a magnesium aluminum silicate adsorbent. The magnesium aluminum silicate adsorbent prepared by the present invention has a large specific surface area and a strong adsorption capacity for transition metal ions, and its preparation method is simple and does not require acidification.

[0008] The invention provides a method for preparing a magnesium aluminum silicate adsorbent.

[0009] Specifically, a method for preparing a magnesium aluminum silicate adsorbent comprises the following steps:

[0010] (1) dissolving an inorganic silicate in water to obtain a white aqueous solution;

[0011] (2) adding an inorganic magnesium salt aqueous solution to the white aqueous solution 1 prepared in step (1), stirring and reacting to obtain a white suspension 1;

[0012] (3) adding an inorganic aluminum salt aqueous solution to the white suspension 1 prepared in step (2), stirring and reacting to obtain a white suspension 2;

[0013] (4) subjecting the white suspension prepared in step (3) to a hydrothermal reaction. After the reaction is completed, the filtrate is separated by solid-liquid separation, dried, and ground to obtain a magnesium aluminum silicate adsorbent.

[0014] In some embodiments of the present invention, the inorganic silicate is selected from one of sodium silicate, calcium silicate and iron silicate.

[0015] In some embodiments of the present invention, the inorganic magnesium salt is selected from one of magnesium sulfate, magnesium chloride, magnesium nitrate and magnesium carbonate.

[0016] In some embodiments of the present invention, the inorganic aluminum salt is selected from one of aluminum sulfate, aluminum chloride and aluminum nitrate.

[0017] In some embodiments of the present invention, the concentration of the aqueous solution 1 is 0.1-1.2 mol / L; preferably, the concentration of the aqueous solution 1 is 0.3-0.8 mol / L.

[0018] In some embodiments of the present invention, the concentration of the inorganic magnesium salt aqueous solution is 0.1-1 mol / L; preferably, the concentration of the inorganic magnesium salt aqueous solution is 0.3-0.7 mol / L.

[0019] In some embodiments of the present invention, the concentration of the inorganic aluminum salt aqueous solution is 0.1-1 mol / L; preferably, the concentration of the inorganic aluminum salt aqueous solution is 0.3-0.7 mol / L.

[0020] The concentration of each material solution in the reaction will determine the solid content in the reaction. A higher solid content will result in a lower reaction conversion rate and a higher particle hardness of the magnesium aluminum silicate adsorbent finally prepared. By controlling the concentrations of the aqueous solution 1, the inorganic magnesium salt aqueous solution and the inorganic aluminum salt aqueous solution, the reaction conversion rate and the particle quality of the final product can be effectively improved.

[0021] In some embodiments of the present invention, in the magnesium aluminum silicate adsorbent, the molar ratio of the silicon element to the magnesium element is (1-2):1; preferably, the molar ratio of the silicon element to the magnesium element is (1.5-2):1.

[0022] In some embodiments of the present invention, in the magnesium aluminum silicate adsorbent, the molar ratio of the magnesium element to the aluminum element is (1-6):1; preferably, the molar ratio of the magnesium element to the aluminum element is (4-6):1; further preferably, the molar ratio of the magnesium element to the aluminum element is (4.5-5.5):1.

[0023] In some embodiments of the present invention, in step (2), the inorganic magnesium salt aqueous solution is added to the white aqueous solution prepared in step (1) in a segmented or dropwise manner. Preferably, the addition time is 5 to 60 minutes; more preferably, the addition time is 10 to 30 minutes.

[0024] In some embodiments of the present invention, the reaction temperature in step (2) is 15-80°C, and the reaction time is 15-100 min. Preferably, the reaction temperature in step (2) is 25-50°C, and the reaction time is 30-60 min.

[0025] In some embodiments of the present invention, in step (3), the inorganic aluminum salt aqueous solution is added to the white suspension prepared in step (2) in a segmented or dropwise manner. Preferably, the addition time is 10 to 60 minutes; more preferably, the addition time is 15 to 40 minutes.

[0026] In some embodiments of the present invention, the reaction temperature in step (3) is 15-80°C, and the reaction time is 15-100 min. Preferably, the reaction temperature in step (3) is 25-60°C, and the reaction time is 20-60 min.

[0027] In some embodiments of the present invention, the temperature of the hydrothermal reaction is 110-130° C., and the time of the hydrothermal reaction is 14-20 hours. Preferably, the temperature of the hydrothermal reaction is 115-125° C., and the time of the hydrothermal reaction is 18-20 hours.

[0028] In some embodiments of the present invention, the drying method includes oven heating drying and hot air drying. The temperature of the oven heating drying is 60-240°C, preferably, the temperature of the oven heating drying is 120-160°C. The inlet air temperature of the hot air drying is 160-280°C; the inlet air temperature of the hot air drying is 210-240°C.

[0029] The invention provides a magnesium aluminum silicate adsorbent.

[0030] Specifically, a magnesium aluminum silicate adsorbent is prepared by the above preparation method; the specific surface area of ​​the magnesium aluminum silicate adsorbent is greater than 570m 2 / g.

[0031] Preferably, the specific surface area of ​​the magnesium aluminum silicate adsorbent is greater than 585m 2 / g; Further preferably, the specific surface area of ​​the magnesium aluminum silicate adsorbent is greater than 600m 2 / g.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The present invention optimizes the preparation process and controls the raw material ratio and reaction conditions to prepare magnesium aluminum silicate, which has a large specific surface area and can efficiently adsorb transition metal ions in a short time (30 minutes); at the same time, it does not introduce new impurities and can remove metal transition ions to below 1 ppm. The removal rate of transition metal ion impurities is as high as 99.9%.

[0034] (2) The preparation method provided by the present invention has simple steps and is easy to operate. The magnesium aluminum silicate synthesized by high-temperature hydrothermal synthesis does not need to be treated with acid or other treatment processes, and has low requirements for instruments and equipment. The production process can adapt to large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a comparison chart of the adsorption effects of magnesium silicate, aluminum silicate and magnesium aluminum silicate. DETAILED DESCRIPTION

[0036] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be noted that the following embodiments do not limit the protection scope of the present invention.

[0037] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0038] Example 1

[0039] This embodiment provides a method for preparing a magnesium aluminum silicate adsorbent, which is as follows:

[0040] 0.35 mol magnesium chloride is added to 1 L deionized water, and stirred continuously to obtain a magnesium chloride aqueous solution with a concentration of 0.35 mol / L. 0.45 mol sodium silicate is added to 1 L deionized water, and stirred continuously to obtain a sodium silicate aqueous solution with a concentration of 0.45 mol / L. 0.35 mol aluminum chloride is added to 1 L deionized water, and stirred continuously to obtain an aluminum chloride aqueous solution with a concentration of 0.35 mol / L. 100mL of magnesium chloride aqueous solution was added dropwise to 140mL of sodium silicate aqueous solution, the addition time was 10min, the stirring reaction temperature was room temperature (20-25℃), the stirring reaction time was 30min, and after the reaction, a white suspension was obtained, n(Si) / n(Mg)=9:5; 50mL of aluminum chloride aqueous solution was added dropwise to the white suspension, the addition time was 15min, the stirring reaction temperature was room temperature (20-25℃), the stirring time was 20min, and after the reaction, a white suspension was obtained; the white suspension was transferred into a synthesis reactor, and placed in an oven for hydrothermal reaction, the oven temperature was 120℃, and the oven reaction time was 18h. After the reaction, a white block solid was obtained after centrifugation and drying, and the white powder obtained by grinding was n(Mg) / n(Al)=2:1 magnesium aluminum silicate adsorbent.

[0041] Example 2

[0042] This embodiment provides a method for preparing a magnesium aluminum silicate adsorbent, which is as follows:

[0043] 0.35 mol magnesium chloride is added to 1 L deionized water, and stirred continuously to obtain a magnesium chloride aqueous solution with a concentration of 0.35 mol / L. 0.45 mol sodium silicate is added to 1 L deionized water, and stirred continuously to obtain a sodium silicate aqueous solution with a concentration of 0.45 mol / L. 0.35 mol aluminum chloride is added to 1 L deionized water, and stirred continuously to obtain an aluminum chloride aqueous solution with a concentration of 0.35 mol / L. 100mL of magnesium chloride aqueous solution was added dropwise to 140mL of sodium silicate aqueous solution, the addition time was 10min, the stirring reaction temperature was room temperature (20-25℃), the stirring reaction time was 30min, and after the reaction, a white suspension was obtained, n(Si) / n(Mg)=9:5; 33.33mL of aluminum chloride aqueous solution was added dropwise to the white suspension, the addition time was 15min, the stirring reaction temperature was room temperature (20-25℃), the stirring time was 20min, and after the reaction, a white suspension was obtained; the white suspension was transferred into a synthesis reactor, and placed in an oven for hydrothermal reaction, the oven temperature was 120℃, and the oven reaction time was 18h. After the reaction, a white block solid was obtained after centrifugation and drying, and a white powder was obtained by grinding, which was n(Mg) / n(Al)=3:1 magnesium aluminum silicate adsorbent.

[0044] Example 3

[0045] This embodiment provides a method for preparing a magnesium aluminum silicate adsorbent, which is as follows:

[0046] 0.35 mol magnesium chloride is added to 1 L deionized water, and stirred continuously to obtain a magnesium chloride aqueous solution with a concentration of 0.35 mol / L. 0.45 mol sodium silicate is added to 1 L deionized water, and stirred continuously to obtain a sodium silicate aqueous solution with a concentration of 0.45 mol / L. 0.35 mol aluminum chloride is added to 1 L deionized water, and stirred continuously to obtain an aluminum chloride aqueous solution with a concentration of 0.35 mol / L. 100mL of magnesium chloride aqueous solution was added dropwise to 140mL of sodium silicate aqueous solution, the addition time was 10min, the stirring reaction temperature was room temperature (20-25℃), the stirring reaction time was 30min, and after the reaction, a white suspension was obtained, n(Si) / n(Mg)=9:5; 25mL of aluminum chloride aqueous solution was added dropwise to the white suspension, the addition time was 15min, the stirring reaction temperature was room temperature (20-25℃), the stirring time was 20min, and after the reaction, a white suspension was obtained; the white suspension was transferred into a synthesis reactor, and placed in an oven for hydrothermal reaction, the oven temperature was 120℃, and the oven reaction time was 18h. After the reaction, a white block solid was obtained after centrifugation and drying, and the white powder obtained by grinding was n(Mg) / n(Al)=4:1 magnesium aluminum silicate adsorbent.

[0047] Example 4

[0048] This embodiment provides a method for preparing a magnesium aluminum silicate adsorbent, which is as follows:

[0049] 0.35 mol magnesium chloride is added to 1 L deionized water, and stirred continuously to obtain a magnesium chloride aqueous solution with a concentration of 0.35 mol / L. 0.45 mol sodium silicate is added to 1 L deionized water, and stirred continuously to obtain a sodium silicate aqueous solution with a concentration of 0.45 mol / L. 0.35 mol aluminum chloride is added to 1 L deionized water, and stirred continuously to obtain an aluminum chloride aqueous solution with a concentration of 0.35 mol / L. 100mL of magnesium chloride aqueous solution was added dropwise to 140mL of sodium silicate aqueous solution, the addition time was 10min, the stirring reaction temperature was room temperature (20-25℃), the stirring reaction time was 30min, and after the reaction, a white suspension was obtained, n(Si) / n(Mg)=9:5; 20mL of aluminum chloride aqueous solution was added dropwise to the white suspension, the addition time was 15min, the stirring reaction temperature was room temperature (20-25℃), the stirring time was 20min, and after the reaction, a white suspension was obtained; the white suspension was transferred into a synthesis reactor, and placed in an oven for hydrothermal reaction, the oven temperature was 120℃, and the oven reaction time was 18h. After the reaction, a white block solid was obtained after centrifugation and drying, and the white powder obtained by grinding was n(Mg) / n(Al)=5:1 magnesium aluminum silicate adsorbent.

[0050] Adsorption test: add 30 mg of magnesium aluminum silicate, magnesium silicate, and aluminum silicate adsorbents respectively to 30 mL of a solution with an iron ion concentration of 15 ppm, stir at 25°C and 300 r / min, and take 2.5 mL of sample for detection after 30 minutes. The test method is o-phenanthroline ultraviolet spectrophotometry. The specific implementation method is: take 2.5 mL of the upper clear liquid of the sample, filter it with a filter head, and add hydroxylamine hydrochloride, o-phenanthroline, and sodium acetate solution in turn, wherein hydroxylamine hydrochloride can oxidize divalent iron ions to trivalent iron ions, and o-phenanthroline reacts with trivalent iron ions to turn the solution orange-red. Sodium acetate acts as an acidic buffer, and the value at a wavelength of 510 nm is taken. The test results are as follows: Figure 1 As shown. The test results show that the removal rate of iron ions by magnesium aluminum silicate adsorbent can reach 99.9%, and the removal rate of iron ions by magnesium silicate and aluminum silicate adsorbents is between 75% and 80%. The adsorption effect of magnesium aluminum silicate adsorbent on metal ions is significantly better than that of magnesium silicate adsorbent and aluminum silicate adsorbent on metal ions.

[0051] The specific surface area and pore structure of the magnesium aluminum silicate, magnesium silicate and aluminum silicate prepared in Example 4 were tested. The test results are shown in Table 1.

[0052] Table 1 Pore structure parameters of magnesium aluminum silicate, magnesium silicate, and magnesium aluminum silicate

[0053]

[0054] It can be seen from Table 1 that the specific surface area of ​​magnesium aluminum silicate is 618.8m 2 / g is significantly greater than magnesium silicate 27.8m 2 / g and aluminum silicate 17.2m 2 / g specific surface area, when magnesium and aluminum appear at the same time, the specific surface area of ​​silicate is significantly increased. Compared with magnesium silicate adsorbent and aluminum silicate adsorbent, the magnesium aluminum silicate adsorbent prepared in this patent has a larger specific surface area and can efficiently adsorb transition metal ions in a shorter time (30min).

[0055] Example 5

[0056] This embodiment provides a method for preparing a magnesium aluminum silicate adsorbent, which is as follows:

[0057] 0.35 mol magnesium chloride is added to 1 L deionized water, and stirred continuously to obtain a magnesium chloride aqueous solution with a concentration of 0.35 mol / L. 0.45 mol sodium silicate is added to 1 L deionized water, and stirred continuously to obtain a sodium silicate aqueous solution with a concentration of 0.45 mol / L. 0.35 mol aluminum chloride is added to 1 L deionized water, and stirred continuously to obtain an aluminum chloride aqueous solution with a concentration of 0.35 mol / L. 100mL of magnesium chloride aqueous solution was added dropwise to 140mL of sodium silicate aqueous solution, the addition time was 10min, the stirring reaction temperature was room temperature (20-25℃), the stirring reaction time was 30min, and after the reaction, a white suspension was obtained, n(Si) / n(Mg)=9:5; 16.67mL of aluminum chloride aqueous solution was added dropwise to the white suspension, the addition time was 15min, the stirring reaction temperature was room temperature (20-25℃), the stirring time was 20min, and after the reaction, a white suspension was obtained; the white suspension was transferred into a synthesis reactor, and placed in an oven for hydrothermal reaction, the oven temperature was 120℃, and the oven reaction time was 18h. After the reaction, a white block solid was obtained after centrifugation and drying, and a white powder was obtained by grinding, which was a magnesium aluminum silicate adsorbent with n(Mg) / n(Al)=6:1.

[0058] Adsorption test: 30 mg of magnesium aluminum silicate adsorbent with n(Mg) / n(Al)=2:1~6:1 was added to 30 mL of solution with iron ion concentration of 15 ppm, stirred at 25°C and 300 r / min, and the iron ion concentration was tested at 30 minutes. The test method is o-phenanthroline ultraviolet spectrophotometry, and the specific implementation method is: take 2.5 mL of the upper clear liquid of the sample, filter it with a filter head, and add hydroxylamine hydrochloride, o-phenanthroline, and sodium acetate aqueous solution in sequence, wherein hydroxylamine hydrochloride can oxidize divalent iron ions to trivalent iron ions, o-phenanthroline and trivalent iron ions undergo complexation reaction to turn the solution orange-red, and sodium acetate acts as an acidic buffer, and the value at a wavelength of 510 nm is taken. From the test results, it can be seen that with the increase of magnesium content, the removal rate of iron ions by magnesium aluminum silicate adsorbent gradually increases. When n(Mg) / n(Al)=6:1, the adsorption performance of magnesium aluminum silicate begins to decrease. It can be concluded that when n(Mg) / n(Al)=5:1, the adsorption effect of magnesium aluminum silicate is the best.

[0059] Example 6

[0060] This embodiment provides a method for preparing a magnesium aluminum silicate adsorbent, which is as follows:

[0061] 0.35 mol magnesium chloride is added to 1 L deionized water, and stirred continuously to obtain a magnesium chloride aqueous solution with a concentration of 0.35 mol / L. 0.45 mol sodium silicate is added to 1 L deionized water, and stirred continuously to obtain a sodium silicate aqueous solution with a concentration of 0.45 mol / L. 0.35 mol aluminum chloride is added to 1 L deionized water, and stirred continuously to obtain an aluminum chloride aqueous solution with a concentration of 0.35 mol / L. 100mL of magnesium chloride aqueous solution was added dropwise to 140mL of sodium silicate aqueous solution, the addition time was 10min, the stirring reaction temperature was room temperature (20-25℃), the stirring reaction time was 30min, and a white suspension was obtained after the reaction, n(Si) / n(Mg)=9:5; 20mL of aluminum chloride aqueous solution was added dropwise to the white suspension, the addition time was 15min, the stirring reaction temperature was room temperature (20-25℃), the stirring time was 20min, and a white suspension was obtained after the reaction; the white suspension was transferred into a synthesis reactor and placed in an oven for hydrothermal reaction, the oven temperature was 120℃, and the oven reaction time was 14h. After the reaction, a white block solid was obtained after centrifugation and drying, and a white powder was obtained by grinding, which was a magnesium aluminum silicate adsorbent with n(Mg) / n(Al)=5:1.

[0062] Example 7

[0063] This embodiment provides a method for preparing a magnesium aluminum silicate adsorbent, which is as follows:

[0064] 0.35 mol magnesium chloride is added to 1 L deionized water, and stirred continuously to obtain a magnesium chloride aqueous solution with a concentration of 0.35 mol / L. 0.45 mol sodium silicate is added to 1 L deionized water, and stirred continuously to obtain a sodium silicate aqueous solution with a concentration of 0.45 mol / L. 0.35 mol aluminum chloride is added to 1 L deionized water, and stirred continuously to obtain an aluminum chloride aqueous solution with a concentration of 0.35 mol / L. 100mL of magnesium chloride aqueous solution was added dropwise to 140mL of sodium silicate aqueous solution, the addition time was 10min, the stirring reaction temperature was room temperature (20-25℃), the stirring reaction time was 30min, and after the reaction, a white suspension was obtained, n(Si) / n(Mg)=9:5; 20mL of aluminum chloride aqueous solution was added dropwise to the white suspension, the addition time was 15min, the stirring reaction temperature was room temperature (20-25℃), the stirring time was 20min, and after the reaction, a white suspension was obtained; the white suspension was transferred into a synthesis reactor, and placed in an oven for hydrothermal reaction, the oven temperature was 120℃, and the oven reaction time was 16h. After the reaction, a white block solid was obtained after centrifugation and drying, and the white powder obtained by grinding was n(Mg) / n(Al)=5:1 magnesium aluminum silicate adsorbent.

[0065] Example 8

[0066] This embodiment provides a method for preparing a magnesium aluminum silicate adsorbent, which is as follows:

[0067] 0.35 mol magnesium chloride is added to 1 L deionized water, and stirred continuously to obtain a magnesium chloride aqueous solution with a concentration of 0.35 mol / L. 0.45 mol sodium silicate is added to 1 L deionized water, and stirred continuously to obtain a sodium silicate aqueous solution with a concentration of 0.45 mol / L. 0.35 mol aluminum chloride is added to 1 L deionized water, and stirred continuously to obtain an aluminum chloride aqueous solution with a concentration of 0.35 mol / L. 100mL of magnesium chloride aqueous solution was added dropwise to 140mL of sodium silicate aqueous solution, the addition time was 10min, the stirring reaction temperature was room temperature (20-25℃), the stirring reaction time was 30min, and a white suspension was obtained after the reaction, n(Si) / n(Mg)=9:5; 20mL of aluminum chloride aqueous solution was added dropwise to the white suspension, the addition time was 15min, the stirring reaction temperature was room temperature (20-25℃), the stirring time was 20min, and a white suspension was obtained after the reaction; the white suspension was transferred into a synthesis reactor and placed in an oven for hydrothermal reaction, the oven temperature was 120℃, and the oven reaction time was 20h. After the reaction, a white block solid was obtained after centrifugation and drying, and a white powder was obtained by grinding, which was a magnesium aluminum silicate adsorbent with n(Mg) / n(Al)=5:1.

[0068] Example 9

[0069] This embodiment provides a method for preparing a magnesium aluminum silicate adsorbent, which is as follows:

[0070] 0.35 mol magnesium chloride is added to 1 L deionized water, and stirred continuously to obtain a magnesium chloride aqueous solution with a concentration of 0.35 mol / L. 0.45 mol sodium silicate is added to 1 L deionized water, and stirred continuously to obtain a sodium silicate aqueous solution with a concentration of 0.45 mol / L. 0.35 mol aluminum chloride is added to 1 L deionized water, and stirred continuously to obtain an aluminum chloride aqueous solution with a concentration of 0.35 mol / L. 180mL magnesium chloride aqueous solution was added dropwise to 140mL sodium silicate aqueous solution, the addition time was 10min, the stirring reaction temperature was room temperature (20-25℃), the stirring reaction time was 30min, and a white suspension 1 was obtained after the reaction was completed; 20mL aluminum chloride aqueous solution was added dropwise to the white suspension 1, n(Mg) / n(Al)=5:1, the addition time was 15min, the stirring reaction temperature was room temperature (20-25℃), the stirring time was 20min, and a white suspension 2 was obtained after the reaction was completed; the white suspension 2 was transferred to a synthesis reactor and placed in an oven for hydrothermal reaction, the oven temperature was 120℃, and the oven reaction time was 18h. After the reaction was completed, a white block solid was obtained after centrifugation and drying, and a white powder was obtained by grinding, which was a magnesium aluminum silicate adsorbent with n(Si) / n(Mg)=1:1.

[0071] Example 10

[0072] This embodiment provides a method for preparing a magnesium aluminum silicate adsorbent, which is as follows:

[0073] 0.35 mol magnesium chloride is added to 1 L deionized water, and stirred continuously to obtain a magnesium chloride aqueous solution with a concentration of 0.35 mol / L. 0.45 mol sodium silicate is added to 1 L deionized water, and stirred continuously to obtain a sodium silicate aqueous solution with a concentration of 0.45 mol / L. 0.35 mol aluminum chloride is added to 1 L deionized water, and stirred continuously to obtain an aluminum chloride aqueous solution with a concentration of 0.35 mol / L. 138.5mL magnesium chloride aqueous solution was added dropwise to 140mL sodium silicate aqueous solution, the addition time was 10min, the stirring reaction temperature was room temperature (20-25℃), the stirring reaction time was 30min, and a white suspension 1 was obtained after the reaction was completed; 20mL aluminum chloride aqueous solution was added dropwise to the white suspension 1, n(Mg) / n(Al)=5:1, the addition time was 15min, the stirring reaction temperature was room temperature (20-25℃), the stirring time was 20min, and a white suspension 2 was obtained after the reaction was completed; the white suspension 2 was transferred to a synthesis reactor and placed in an oven for hydrothermal reaction, the oven temperature was 120℃, and the oven reaction time was 18h. After the reaction was completed, a white block solid was obtained after centrifugation and drying, and a white powder was obtained by grinding, which was a magnesium aluminum silicate adsorbent with n(Si) / n(Mg)=13:10.

[0074] Comparative Example 1

[0075] In Example 1 of Patent CN117138742A, magnesium sulfate, aluminum nitrate and sodium silicate are reacted to obtain a precipitate, and the precipitate is added to a 70% sulfuric acid solution to obtain an acidic modified magnesium aluminum silicate. The optimal specific surface area of ​​the adsorbent is 559 m 2 / g, the sodium ions in the aqueous solution can be reduced to 1.03ppm. However, the specific surface area of ​​magnesium aluminum silicate in Comparative Example 1 is significantly smaller than that of the present application, and its preparation process is complicated and requires acidification. The preparation process of the magnesium aluminum silicate adsorbent provided by the present invention is simpler and does not require acidification. At the same time, the ion concentration can be reduced to below 1ppm after adsorption for 30min, and the adsorption efficiency is relatively high.

[0076] Adsorption test: Take 30 mg of the adsorbent provided in each embodiment and comparative example, add 30 mL of a solution with an iron ion concentration of 15 ppm, stir at 25 ° C, 300 r / min, and test the iron ion concentration at 30 min. The test method is o-phenanthroline ultraviolet spectrophotometry, and the specific implementation method is: take 2.5 mL of the upper clear liquid of the sample, filter it with a filter head, and add hydroxylamine hydrochloride, o-phenanthroline, and sodium acetate aqueous solution in sequence, wherein hydroxylamine hydrochloride can oxidize divalent iron ions to trivalent iron ions, o-phenanthroline and trivalent iron ions undergo a complex reaction to turn the solution orange-red, and sodium acetate acts as an acidic buffer, taking the value at a wavelength of 510 nm. The test results are shown in Table 2.

[0077] Table 2 Specific surface area of ​​adsorbents and ion concentration and removal rate after adsorption

[0078] Magnesium aluminum silicate adsorbent <![CDATA[Specific surface area m 2 / g]]> Ion concentration after adsorption Ion removal rate Example 1 570 3.15 79.0% Example 2 586 2.55 83.0% Example 3 592 1.2 92.0% Example 4 618 0.015 99.9% Example 5 601 1.05 93.0% Example 6 560 1.605 89.3% Example 7 589 1.350 91.0% Example 8 617 0.15 99.9% Example 9 593 1.5 90.0% Example 10 598 1.26 91.6% Comparative Example 1 559 1.030 99.9%

[0079] In summary, the magnesium aluminum silicate adsorbent provided by the present invention has excellent adsorption performance, and the removal rate of transition metal ions is as high as 99.9%, and the transition metal ion content in the product can be reduced to below 0.02 ppm; the adsorbent has stable and efficient adsorption performance, does not introduce new impurities, and the production process is simplified and energy-efficient.

[0080] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a magnesium aluminum silicate adsorbent, characterized in that: The following steps are involved: (1) dissolving an inorganic silicate in water to obtain a white aqueous solution; (2) adding an inorganic magnesium salt aqueous solution to the white aqueous solution 1 prepared in step (1), stirring and reacting to obtain a white suspension 1; (3) adding an inorganic aluminum salt aqueous solution to the white suspension 1 prepared in step (2), stirring and reacting to obtain a white suspension 2; (4) subjecting the white suspension prepared in step (3) to a hydrothermal reaction. After the reaction is completed, the filtrate is separated by solid-liquid separation and dried to obtain a magnesium aluminum silicate adsorbent.

2. The preparation method according to claim 1, characterized in that: The inorganic silicate is selected from one of sodium silicate, calcium silicate and iron silicate; the inorganic magnesium salt is selected from one of magnesium sulfate, magnesium chloride, magnesium nitrate and magnesium carbonate; the inorganic aluminum salt is selected from one of aluminum sulfate, aluminum chloride and aluminum nitrate.

3. The preparation method according to claim 1 or 2, characterized in that: The concentration of the aqueous solution 1 is 0.1-1.2 mol / L; the concentration of the inorganic magnesium salt aqueous solution is 0.1-1 mol / L; the concentration of the inorganic aluminum salt aqueous solution is 0.1-1 mol / L.

4. The preparation method according to claim 3, characterized in that: In the magnesium aluminum silicate adsorbent, the molar ratio of the silicon element to the magnesium element is (1-2):1; preferably, the molar ratio of the silicon element to the magnesium element is (1.5-2):

1.

5. The preparation method according to claim 4, characterized in that: In the magnesium aluminum silicate adsorbent, the molar ratio of the magnesium element to the aluminum element is (1-6):

1.

6. The preparation method according to claim 1 or 2, characterized in that: The reaction temperature in step (2) is 15 to 80° C., and the reaction time is 15 to 100 minutes.

7. The preparation method according to claim 1 or 2, characterized in that: The reaction temperature in step (3) is 15 to 80° C., and the reaction time is 15 to 100 min.

8. The preparation method according to claim 1 or 2, characterized in that: The temperature of the hydrothermal reaction is 110-130° C., and the time of the hydrothermal reaction is 14-20 hours.

9. A magnesium aluminum silicate adsorbent, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8; the specific surface area of ​​the magnesium aluminum silicate adsorbent is greater than 570m 2 / g.

10. The magnesium aluminum silicate adsorbent according to claim 9, characterized in that: The specific surface area of ​​the magnesium aluminum silicate adsorbent is greater than 585m 2 / g; Preferably, the specific surface area of ​​the magnesium aluminum silicate adsorbent is greater than 600m 2 / g.

Citation Information

Patent Citations

  • Preparation method and application of magnesium silicate adsorbent

    CN113694878A

  • Acid-modified magnesium aluminum silicate adsorbent as well as preparation method and application thereof

    CN117138742A

  • Adsorbent material and method of preparing same

    GB1349409A

  • Improvements in magnesium aluminium silicates and in their preparation

    GB873506A

  • Busbar assembly and battery pack including the same

    KR1020240177975A