Method and device for producing spherical nickel hydroxide
By using a new jacketed reactor and a special stirring device in the production of spherical nickel hydroxide, combined with ultrasonic vibration, the problem of long reaction time and poor liquid phase mixing effect is solved, and the uniformity of product morphology and particle size is achieved. Improved the performance of nickel-hydrogen batteries.
Patent Information
- Application Number
- CN202411064022.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing spherical nickel hydroxide production technology, the reaction time of the reactor is long and the liquid phase mixing effect is poor, resulting in uneven product morphology and uneven particle size.
A new jacketed reactor is used, combined with a special "U" stirring paddle and ultrasonic vibrator, to ensure the homogeneous reaction of the solution by adjusting the temperature and pH, and to ensure the maximum material by adopting specific feeding methods and washing processes. Good nucleation and growth.
The problem of long reaction time and poor liquid phase mixing effect is effectively overcome. The prepared spherical nickel hydroxide product has good morphology and uniform particle size, which improves the bulk density, thereby improving the performance of nickel-hydrogen batteries.
Smart Images

Figure CN118929792A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nickel hydroxide production, and in particular to a method and device for producing spherical nickel hydroxide. Background Art
[0002] Spherical nickel hydroxide is the positive electrode material of nickel-hydrogen batteries and nickel-hydrogen power batteries. It can also be used as a precursor material for the positive electrode active material (lithium nickel cobalt oxide) of lithium-ion batteries. The preparation of spherical nickel hydroxide is of great significance to promoting the development of domestic batteries.
[0003] At present, the production of spherical nickel hydroxide adopts the nickel sulfate solution-sodium hydroxide solution direct precipitation method. The reactor used has the problems of long reaction time, poor liquid phase mixing effect and uneven product morphology. Summary of the invention
[0004] In view of the above problems, the present invention provides a method and device for producing spherical nickel hydroxide, which overcomes the problems of long reaction time in the reactor and poor liquid phase mixing effect, and the prepared product has good morphology and uniform particle size.
[0005] To solve the above problems, the technical solution adopted by the present invention is: A method for producing spherical nickel hydroxide comprises the following steps: S1, assembling a novel jacketed reactor, adding deionized water into the novel jacketed reactor, and adjusting the temperature and pH value in the novel jacketed reactor to a predetermined range; S2, starting a stirring device and an ultrasonic vibrating rod in the novel jacketed reactor to disturb and vibrate the solution in the novel jacketed reactor, wherein the stirring device adopts a special "U"-shaped stirring paddle, and the "U"-shaped paddle is also equipped with a plurality of spoiler plates for homogenous reaction of the liquid phase; S3, starting a metering pump to convey an organic amine solution, a nickel salt solution and an alkali solution into the reactor in proportion; S4, stopping conveying after the raw materials are sufficiently replenished, discharging the materials from the bottom, and placing them in an aging kettle with stirring for aging; washing, filtering, drying and screening the aged materials to obtain spherical nickel hydroxide.
[0006] The present invention can effectively prepare spherical nickel hydroxide products, overcome the problems of long reaction time in the reactor and poor liquid phase mixing effect, and the prepared products have good morphology and uniform particle size; the specific stirring device and the specific feeding method ensure the optimal nucleation and growth of the material.
[0007] Preferably, in step S1, deionized water is added to the novel jacketed reactor until the liquid level is more than 3 cm above the temperature sensor.
[0008] Preferably, in step S1, an organic amine solution and an alkali solution are pumped into the novel jacketed reactor to control the pH value of the solution in the reactor to be 11.4-11.7; the organic amines include formamide and acetamide, and the concentration is 4.2-8.4 mol / L; the nickel salts include nickel sulfate, nickel chloride, and nickel nitrate, and the concentration is 2.0-4.0 mol / L; the alkali solution includes sodium hydroxide and potassium hydroxide, and the concentration is 4.0-8.0 mol / L.
[0009] When the pH value is low, the crystal growth rate in the system is too large compared to the crystal nucleation rate, and it is easy to obtain larger and more irregular crystals, which makes the sample packing density too small. When the pH value is high, the crystal nucleation rate in the system is too large compared to the crystal growth rate, making the product grains smaller, which makes the packing density too small.
[0010] Preferably, in step S1, the oil bath is turned on for heating until the temperature of the solution in the kettle is constant at 50-60°C.
[0011] The temperature of the solution in the kettle is set at 50~60℃. As the reaction temperature increases, the supersaturation in the solution decreases, and the nucleation rate of nickel hydroxide is sensitive to the change of supersaturation. Therefore, although the reaction rate of various processes generally increases with the increase of reaction temperature, the decrease of supersaturation weakens the increase of nucleation rate accordingly, so increasing the temperature is more conducive to the nucleation rate of nickel hydroxide. However, too high a temperature will increase the kinetic energy of the reactant molecules too quickly, which is not conducive to the formation of stable crystal nuclei. Then the small particle nuclei will dissolve and re-deposit on the surface of large particles. At the same time, since the precipitant used is organic amine, too high a reaction temperature will increase the volatilization of organic amine, causing amine loss, and will also increase energy consumption. The evaporation of the solution system during the reaction will also have a significant impact on the accurate and continuous measurement of the reaction pH value.
[0012] Preferably, in step S2, an ultrasonic vibrator is started to vibrate the solution, with an ultrasonic frequency of 20 KHz and a power of 1000-2000 W.
[0013] Through ultrasonic vibration technology, the attraction between spherical nickel hydroxide can be effectively broken, the occurrence of agglomeration can be reduced, and the stacking density can be increased.
[0014] Preferably, in step S3, the pH value of the system is constantly monitored to maintain a constant pH value of the solution.
[0015] Preferably, in step S4, the aged material is washed with deionized water for multiple times and then filtered, and dried after the conductivity of the filtrate is lower than 5 μS / cm. The dried material is crushed into powder and then sieved to obtain spherical nickel hydroxide.
[0016] Preferably, in step S3, the positions where the organic amine solution, the nickel salt solution and the alkali solution are added are all close to the inner side of the stirring paddle blades, so as to accelerate the mutual reaction time of the materials.
[0017] Organic amines include formamide and acetamide, and the concentration is 4.2~8.4mol / L. If the concentration is too low, the growth rate of the crystal will be too slow, so that the bulk density of the product is too low. When the concentration is too high, it is easy to cause local supersaturation during the dropwise addition process, so that the nucleation rate is too fast, and fine grains or even colloids are generated, so that the bulk density is too low. Nickel salts include nickel sulfate, nickel chloride, and nickel nitrate, and the concentration is 2.0~4.0mol / L. If the nickel-amine ratio is too large, the particles will be irregular or spherical, and if the nickel-amine ratio is too small, the particles will be agglomerated. Alkali solutions include sodium hydroxide and potassium hydroxide, and the concentration is 4.0~8.0mol / L. If the concentration is too low, the growth rate of the crystal will be too slow, so that the bulk density of the product is too low. When the concentration is too high, it is easy to cause local supersaturation during the dropwise addition process, so that the nucleation rate is too fast, and fine grains or even colloids are generated, so that the bulk density is too low.
[0018] A spherical nickel hydroxide production device comprises a novel jacketed reactor, wherein a feeding device is arranged at the upper end of the novel jacketed reactor, and a stirring device is arranged inside the novel jacketed reactor, wherein the stirring device adopts a special "U"-shaped stirring paddle, and the "U"-shaped paddle is also equipped with a plurality of spoiler plates for homogenizing the liquid phase; an ultrasonic vibrating rod located outside the stirring device is also arranged inside the novel jacketed reactor, and during the feeding process, the solution in the novel jacketed reactor is continuously disturbed and vibrated to reduce the occurrence of agglomeration and improve the stacking density.
[0019] Preferably, the feeding device comprises an alkali solution feeding pipe, an organic amine solution feeding pipe and a nickel salt feeding pipe, and the alkali solution feeding pipe, the organic amine solution feeding pipe and the nickel salt feeding pipe are all located inside the "U"-shaped stirring paddle blade.
[0020] It should be noted that: since organic amines are oily substances, their viscosity and specific gravity are relatively large compared to aqueous solutions, and conventional reaction devices are difficult to mix materials in a short time. At the same time, due to the hysteresis of solution rotation, different vectors exist at different heights of the solution, and the speed is inconsistent. Basically, the absolute velocity vector at the bottom of the solution is large, and the middle and upper parts are small. The prepared nickel hydroxide has poor particle size uniformity and unstable morphology. When the material is passed into the bottom of the reactor, due to the preparation of ultrasonic waves, the special paddle type and the multiple groups of spoilers installed on the "U"-shaped paddle, it can be ensured that the absolute velocity vector in the middle and upper parts is still large, and the shear force of the fluid is large, which will enhance the collision between particles, so that the nickel hydroxide particles are combined with each other through van der Waals forces, solvation forces, etc., and the material can be mixed quickly, and the liquid phase can react homogeneously. In summary, the absolute velocity vector of this set of devices is evenly distributed, which can effectively ensure that the prepared spherical nickel hydroxide has uniform particle size and stable morphology, which is conducive to improving the packing density of spherical nickel hydroxide, thereby greatly improving the performance of nickel-hydrogen batteries.
[0021] The beneficial effects of the present invention are: Compared with the prior art, the present invention can effectively prepare spherical nickel hydroxide products, overcome the problems of long reaction time in the reactor and poor liquid phase mixing effect, and the prepared products have good morphology and uniform particle size. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic structural diagram of the spherical nickel hydroxide production device of the present invention.
[0023] Figure 2 This is a high-magnification scanning electron microscope image of the spherical nickel hydroxide of the present invention.
[0024] In the figure: 1. Oil bath inlet; 2. Ultrasonic vibrator; 3. Alkaline solution feeding pipeline; 4. Organic amine solution feeding pipeline; 5. Stirring device; 6. Nickel salt feeding pipeline; 7. pH sensor; 8. Spoiler; 9. Discharge port; 10. Oil bath outlet; 11. Temperature sensor. DETAILED DESCRIPTION
[0025] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0026] Spherical nickel hydroxide is the positive electrode material of nickel-hydrogen batteries and nickel-hydrogen power batteries. It can also be used as a precursor material for the positive electrode active material (lithium nickel cobalt oxide) of lithium-ion batteries. The preparation of spherical nickel hydroxide is of great significance to promoting the development of domestic batteries.
[0027] At present, the production of spherical nickel hydroxide adopts the nickel sulfate solution-sodium hydroxide solution direct precipitation method. The reactor used has the problems of long reaction time, poor liquid phase mixing effect and uneven product morphology.
[0028] In order to solve the above problems, a method for producing spherical nickel hydroxide comprises the following steps: Step 1: Assemble the new jacketed reactor and ensure stable operation of all components.
[0029] Step 2: Add deionized water to the new jacketed reactor until the liquid level is more than 3 cm above the temperature sensor.
[0030] Step 3: Pump organic amine solution and alkali solution into the new jacketed reactor to control the pH value of the solution in the reactor to 11.4~11.7.
[0031] Step 4: Turn on the oil bath heating and wait until the temperature of the solution in the kettle is constant at 50~60℃.
[0032] Step 5: Start the stirring device to disturb the solution.
[0033] Step 6: Start the ultrasonic vibrator to vibrate the solution. The ultrasonic frequency is 20KHz and the power is adjustable from 1000 to 2000W.
[0034] Step 7: Turn on the metering pump to deliver the organic amine solution, nickel salt solution and alkali solution into the kettle in proportion, and constantly check the pH value of the system to maintain a constant pH value of the solution.
[0035] Step 8: After the raw materials are replenished sufficiently, stop conveying, release the materials from the bottom, and put them into an aging kettle with stirring for aging.
[0036] Step 9: Wash the aged material with deionized water for several times and then filter it. Dry it after the conductivity of the filtrate is lower than 5μS / cm.
[0037] Step 10: The dried material is crushed into powder and then sieved to obtain spherical nickel hydroxide. Figure 2 .
[0038] Specifically, the pH value of the solution in the kettle is controlled to be 11.4~11.7. When the pH value is low, the crystal growth rate in the system is too large compared to the crystal nucleation rate, and it is easy to obtain larger and more irregular crystals, which makes the sample packing density too small. When the pH value is high, the crystal nucleation rate in the system is too large compared to the crystal growth rate, so that the product grains are smaller, and the packing density is too small.
[0039] Specifically, the temperature of the solution in the kettle is set at 50-60°C. As the reaction temperature increases, the supersaturation in the solution decreases, and the nucleation rate of nickel hydroxide is sensitive to changes in supersaturation. Therefore, although the reaction rates of various processes generally increase with increasing reaction temperature, the decrease in supersaturation weakens the increase in nucleation rate, so increasing the temperature is more conducive to the nucleation rate of nickel hydroxide. However, too high a temperature will increase the kinetic energy of the reactant molecules too quickly, which is not conducive to the formation of stable crystal nuclei. Then the small particle nuclei will dissolve and re-deposit on the surface of the large particles. At the same time, since the precipitant used is an organic amine, a too high reaction temperature will increase the volatilization of the organic amine, causing amine loss, and will also increase energy consumption. The evaporation of the solution system during the reaction will also have a significant impact on the accurate and continuous measurement of the reaction pH value.
[0040] Specifically, the ultrasonic frequency is 20KHz, and the power is adjustable from 1000 to 2000W. Through ultrasonic vibration technology, the attraction between spherical nickel hydroxide can be effectively broken, the occurrence of agglomeration can be reduced, and the stacking density can be increased.
[0041] Specifically, organic amines include formamide and acetamide, and the concentration is 4.2-8.4 mol / L. If the concentration is too low, the growth rate of the crystal will be too slow, so that the bulk density of the product will be too low. If the concentration is too high, it is easy to cause local supersaturation during the dropwise addition process, so that the nucleation rate is too fast, and fine grains or even colloids are generated, so that the bulk density is too low.
[0042] Specifically, nickel salts include nickel sulfate, nickel chloride, and nickel nitrate, with a concentration of 2.0-4.0 mol / L. A nickel-amine ratio that is too large will result in irregular or spherical particles, and a nickel-amine ratio that is too small will result in agglomerated particles.
[0043] Specifically, the alkali solution includes sodium hydroxide and potassium hydroxide, and the concentration is 4.0~8.0 mol / L. If the concentration is too low, the growth rate of the crystal will be too slow, so that the bulk density of the product will be too low. If the concentration is too high, it is easy to cause local supersaturation during the dropwise addition process, so that the nucleation rate is too fast, and fine grains or even colloids are generated, so that the bulk density is too low.
[0044] Specifically, the reactor is equipped with a high-precision temperature sensor and a pH sensor, which can accurately detect changes in system temperature and pH. It is also equipped with a specific stirring device and a specific feeding method to ensure optimal nucleation and growth of the material.
[0045] The reactor adopts jacket heating, and the temperature inside the reactor is more uniform.
[0046] The stirring device adopts a special "U"-shaped stirring paddle, and the "U"-shaped paddle is also equipped with multiple groups of spoilers for homogenous reaction of the liquid phase. When the material is passed into the bottom of the reactor, it can be quickly mixed. The nickel ions will quickly form a complex with the organic amine, inhibiting the rapid formation of nickel hydroxide precipitation by nickel ions and hydroxide ions, which is conducive to the formation of crystal nuclei and the growth of crystals to achieve a mutually restrained stable state.
[0047] The reactor is equipped with an ultrasonic vibrator. Turning on the vibrator during the product preparation process can effectively break the attraction between spherical nickel hydroxides, reduce the occurrence of agglomeration, and increase the packing density.
[0048] The organic amine solution, nickel salt solution and alkali solution are quantitatively added into the reaction kettle through three pipes without interfering with each other.
[0049] The positions where the organic amine solution, nickel salt solution and alkali solution are added are all close to the inner side of the stirring paddle blades, so as to accelerate the mutual reaction time of the materials and make the formation and growth of crystal nuclei better.
[0050] The present invention can effectively prepare spherical nickel hydroxide products, overcome the problems of long reaction time in the reactor and poor liquid phase mixing effect, and the prepared products have good morphology and uniform particle size.
[0051] See attached Figure 1 A spherical nickel hydroxide production device, the reactor is equipped with a high-precision temperature sensor 11 and a pH sensor 7, which can accurately detect the temperature and pH changes of the system, and is equipped with a specific stirring device 5. The stirring device 5 adopts a special stirring paddle, and the paddle is also equipped with multiple groups of spoilers 8 for homogenous reaction of the liquid phase. At the same time, it is equipped with an ultrasonic vibrator 2 to effectively break the attraction between the spherical nickel hydroxides, reduce the occurrence of agglomeration, and increase the packing density; organic amine solution, nickel salt solution and alkali solution are quantitatively added to the reactor through three pipes without interfering with each other. The addition positions are close to the inner side of the stirring paddle blades, which are used to accelerate the mutual reaction time of the materials and ensure the optimal nucleation and growth of the materials.
[0052] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for producing spherical nickel hydroxide, characterized in that: The steps include: S1, assembling a new jacketed reactor, adding deionized water into the new jacketed reactor, and adjusting the temperature and pH value in the new jacketed reactor to a predetermined range; S2. Start the stirring device and ultrasonic vibrator in the new jacketed reactor to disturb and vibrate the solution in the new jacketed reactor. The stirring device adopts a special "U"-shaped stirring paddle, and the "U"-shaped paddle is also equipped with multiple groups of spoilers for homogenous reaction of the liquid phase. S3, start the metering pump to deliver the organic amine solution, nickel salt solution and alkali solution into the kettle in proportion; S4. After the raw materials are sufficiently replenished, the conveying is stopped, the materials are discharged from the bottom, and are placed in an aging kettle with stirring for aging; the aged materials are washed, filtered, dried, and sieved to obtain spherical nickel hydroxide.
2. The method for producing spherical nickel hydroxide according to claim 1, characterized in that: In step S1, deionized water is added to the novel jacketed reactor until the liquid level is more than 3 cm above the temperature sensor.
3. The method for producing spherical nickel hydroxide according to claim 1, characterized in that: In step S1, an organic amine solution and an alkaline solution are pumped into the novel jacketed reactor to control the pH value of the solution in the reactor to be 11.4-11.7; the organic amines include formamide and acetamide with a concentration of 4.2-8.4 mol / L; the nickel salts include nickel sulfate, nickel chloride and nickel nitrate with a concentration of 2.0-4.0 mol / L; the alkaline solution includes sodium hydroxide and potassium hydroxide with a concentration of 4.0-8.0 mol / L.
4. The method for producing spherical nickel hydroxide according to claim 1, characterized in that: In step S1, the oil bath is turned on for heating until the temperature of the solution in the kettle is constant at 50-60°C.
5. The method for producing spherical nickel hydroxide according to claim 1, characterized in that: In step S2, an ultrasonic vibrator is started to vibrate the solution, with an ultrasonic frequency of 20 KHz and a power of 1000-2000 W.
6. The method for producing spherical nickel hydroxide according to claim 1, characterized in that: In step S3, the pH value of the system is constantly monitored to maintain a constant pH value of the solution.
7. The method for producing spherical nickel hydroxide according to claim 1, characterized in that: In step S4, the aged material is washed with deionized water for multiple times and then filtered. After the conductivity of the filtrate is lower than 5 μS / cm, it is dried. The dried material is crushed into powder and then sieved to obtain spherical nickel hydroxide.
8. The method for producing spherical nickel hydroxide according to claim 1, characterized in that: In step S3, the positions where the organic amine solution, the nickel salt solution and the alkali solution are added are all close to the inner side of the stirring paddle blades, so as to accelerate the mutual reaction time of the materials.
9. A spherical nickel hydroxide production device, comprising a novel jacketed reactor, wherein a feeding device is provided at the upper end of the novel jacketed reactor, characterized in that: The novel jacketed reactor is provided with a stirring device inside. The stirring device adopts a special "U"-shaped stirring paddle. The "U"-shaped paddle is also equipped with multiple groups of spoilers for homogenous reaction of the liquid phase. The novel jacketed reactor is also provided with an ultrasonic vibrator located outside the stirring device. During the feeding process, the solution in the novel jacketed reactor is continuously disturbed and vibrated to reduce the occurrence of agglomeration and increase the stacking density.
10. A spherical nickel hydroxide production device according to claim 9, characterized in that: The feeding device comprises an alkali solution feeding pipeline, an organic amine solution feeding pipeline and a nickel salt feeding pipeline, and the alkali solution feeding pipeline, the organic amine solution feeding pipeline and the nickel salt feeding pipeline are all located inside the "U"-shaped stirring paddle blade.