Method for developing alloy furnace tailings for building cement production

Through the mixing of the ratio of tailslag and calcium oxide slag of acid-lined steelmaking alloy furnace, inspection and neutralizing agent adjustment of the X-ray fluorescence spectrometer, the problems of low mass coefficient of tailslag and unstable magnesium oxide content in traditional methods are solved. It has achieved high-quality development of alloy furnace tailings, met the standards of building cement production, and improved the stability and resource utilization efficiency of cement.

CN118930092APending Publication Date: 2024-11-12DEQING ZHENGBO ENVIRONMENTAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411214145.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-31
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The traditional alloy furnace tailslag development method fails to fully utilize the useful components in the furnace tailslag, resulting in waste of resources, uneven cement performance, unstable quality control, and difficult to meet the standards for building cement production.

Method used

By obtaining the alloy furnace tailslag produced by acidic furnace lining steelmaking, it is scientifically mixed with the slag using calcium oxide as the slag-making agent, and using X-ray fluorescence spectrometer to perform batch component inspection and neutralizing agent adjustment to ensure that the mass coefficient is greater than 1.4 The magnesium oxide content is less than 10%, followed by drying to control the moisture content.

Benefits of technology

It effectively improves the mass coefficient and composition uniformity of the tailings of the alloy furnace, ensures that it meets the standards of building cement production, enhances the stability and safety of cement, and realizes efficient utilization of resources and environmental protection benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930092A_ABST
    Figure CN118930092A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of alloy furnace tailings development, and discloses an alloy furnace tailings development method for building cement production, which comprises the following steps: S1, alloy furnace tailings generated by acid furnace lining steelmaking are obtained, the alloy furnace tailings contain calcium oxide, magnesium oxide and aluminum oxide, but the mass coefficient is lower than 1.4, and the alloy furnace tailings are obtained; according to the method, the alloying furnace tailings generated by acid lining steelmaking and the slag using calcium oxide as a slag former are scientifically proportioned and mixed, so that the quality coefficient of the alloying furnace tailings can be stably improved and is stabilized to be greater than 1.4, and the method effectively overcomes the problem that the quality coefficient of the alloying furnace tailings is too low in a traditional method, and improves the quality coefficient of the alloying furnace tailings. According to the present invention, the alloy furnace tailings are used as the raw material, such that the application performance of the alloy furnace tailings in the building cement production meets the standard requirement, the cement quality and the cement stability are enhanced, and the components of the alloy furnace tailings are accurately analyzed through the batch sampling inspection and the X-ray fluorescence spectrometer so as to real-timely monitor and adjust the components of the alloy furnace tailings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy furnace tailings development, in particular to a method for developing alloy furnace tailings for building cement production. Background Art

[0002] In the process of steel smelting, especially in furnaces using alkaline lining materials such as aluminum silicate and magnesium silicate, alloy furnace tailings are generated. These furnace tailings are mainly composed of metal oxides and silicates. Due to the effect of alkaline lining materials, these furnace tailings usually have a lower mass coefficient and a lower magnesium oxide content. The preparation of building cement requires high-quality raw materials, which should have a suitable mass coefficient and chemical composition to ensure the strength, durability and other performance requirements of cement. Common cement raw materials include limestone, clay, iron ore and gypsum. Although alloy furnace tailings can be used as potential raw materials for cement production, their composition usually does not fully meet the standards for cement production. For example, furnace tailings may contain high magnesium oxide or other unfavorable components, and further processing is required to adjust their chemical composition to meet the requirements of cement raw materials. In the production of modern building materials, resource reuse and environmental protection are emphasized. By optimizing the composition of alloy furnace tailings, waste emissions can be reduced while reducing the cost of raw material procurement. This requires the development of an effective treatment method to improve the quality of furnace tailings so that it meets the requirements of cement production.

[0003] Traditional methods have significant drawbacks in the utilization of alloy furnace tailings, mainly due to the following problems: First, the useful components in the tailings are not fully utilized, resulting in resource waste and low-quality raw materials; second, the slag quality control is unstable, affecting the uniformity of cement performance. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a method for developing alloy furnace tailings for building cement production, which solves the problems of failure to fully utilize the useful components in the furnace tailings and unstable slag quality control, which affects the uniformity of cement performance.

[0005] To achieve the above objectives, the present invention is implemented by the following technical scheme: A method for developing alloy furnace tailings for building cement production, comprising the following steps: S1: Obtain alloy furnace tailings produced by acidic furnace lining steelmaking, which contains calcium oxide, magnesium oxide and aluminum oxide, but the mass coefficient is less than 1.4; S2: Obtain slag using calcium oxide as a slag-making agent, with a mass coefficient greater than 1.4, a magnesium oxide content that meets the requirements for building cement production, and an appropriate calcium oxide content; S3: Mix the acidic furnace lining slag obtained in S1 with the slag obtained in step 1.2 according to the following ratio: Acidic furnace lining slag: 50%-70% Using calcium oxide slag: 30%-50% To form alloy furnace tailings, ensure that the mass coefficient of the mixed alloy furnace tailings is stably greater than 1.4, and the magnesium oxide content is controlled below 10%; S4: sampling and testing the mixed alloy furnace tailings in batches, using an X-ray fluorescence spectrometer to determine its composition, including the content of calcium oxide, magnesium oxide, aluminum oxide, silicon dioxide, manganese dioxide and titanium dioxide, and recording and analyzing the composition data of each batch of slag; S5: According to the test results in S4, the mixing ratio is adjusted, and a neutralizing agent is added to adjust the composition of the alloy furnace tailings to ensure that the quality coefficient of the final product is greater than 1.4 and the magnesium oxide content is less than 10%; S6: Re-test the adjusted mixed slag to verify whether its mass coefficient and magnesium oxide content meet the requirements. If not, repeat step 1.5 until the standards are met; S7: Dry the alloy furnace tailings that meet the requirements to control their moisture content to prevent excessive moisture from affecting the uniformity of the composition and improve its stability through drying.

[0006] Preferably, the neutralizing agent is calcium oxide, and the amount added is determined according to the test results of the alloy furnace tailings after mixing to reduce the magnesium oxide content to less than 10%.

[0007] Preferably, in S4, the inspection method used includes an X-ray fluorescence spectrometer to ensure that the analysis results of each component are accurate.

[0008] Preferably, the alloy furnace tailings mixed in S5 are fully stirred to ensure uniform composition.

[0009] Preferably, in S7, the temperature range of the drying treatment is 60°C to 120°C, and the time is 24 hours to 48 hours to ensure that the moisture content is controlled within a specified range.

[0010] Preferably, in S6, if the standard is still not met after the initial adjustment, the mixing ratio and the amount of the neutralizer added are readjusted according to the test results, and re-tested until it is qualified.

[0011] Preferably, the ratio of calcium oxide, magnesium oxide and aluminum oxide in the alloy furnace tailings is precisely controlled to meet the component requirements of building cement production and ensure that the magnesium oxide content does not exceed the standard. Beneficial Effects

[0012] The present invention provides a method for developing alloy furnace tailings for building cement production. Compared with the prior art, it has the following beneficial effects: By scientifically mixing the alloy furnace tailings produced by acidic furnace lining steelmaking with slag using calcium oxide as a slag-forming agent, the present invention can stably improve the quality coefficient of the alloy furnace tailings to make it stably greater than 1.4. This method effectively overcomes the problem of too low quality coefficient of alloy furnace tailings in traditional methods, thereby ensuring that its application performance in the production of building cement meets the standard requirements and enhances the quality and stability of cement. Secondly, the present invention can monitor and adjust the composition of the alloy furnace tailings in real time by batch sampling and testing and using an X-ray fluorescence spectrometer to accurately analyze the composition of the alloy furnace tailings to ensure that its magnesium oxide content is controlled below 10%. This measure effectively avoids the situation where the magnesium oxide content exceeds the standard, ensures that the chemical composition of the alloy furnace tailings meets the standard requirements for the production of building cement, and improves the safety and stability of cement. In addition, the present invention introduces a neutralizing agent (calcium oxide) and, based on the inspection of the mixed alloy furnace tailings The test results are adjusted to accurately control the ratio of calcium oxide to magnesium oxide in the alloy furnace tailings. This method effectively solves the problem of too high or too low magnesium oxide content in the traditional treatment process, further optimizes the quality of the alloy furnace tailings, and provides a more reliable raw material for the production of building cement. Finally, the present invention dries the alloy furnace tailings that meet the requirements and controls its moisture content, thereby preventing excessive moisture from affecting the uniformity of the composition. This drying treatment measure improves the stability and consistency of the final product, ensures the reliability and long-term stability of the alloy furnace tailings in practical applications, provides high-quality raw materials for the production of building cement, and meets the requirements of modern environmental protection and resource recycling. In summary, the method of the present invention effectively solves the problems existing in the traditional method by accurately controlling and optimizing the composition and quality of the alloy furnace tailings, provides a more stable and efficient raw material for the production of building cement, and has significant economic and environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 A schematic diagram of a process for developing alloy furnace tailings for building cement production proposed by the present invention; Figure 2 A detection diagram of the alloy furnace tailings composition of a method for developing alloy furnace tailings for building cement production proposed by the present invention; Figure 3 The present invention provides a detailed table of the composition of the slag after steelmaking in the method for developing alloy furnace tailings for building cement production proposed by the present invention. DETAILED DESCRIPTION

[0014] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0015] See also Figure 1-Figure 3 , specifically including the following embodiments: Embodiment 1

[0016] A method for developing alloy furnace tailings for building cement production comprises the following steps: S1: Obtain the alloy furnace tailings produced by acid lining steelmaking, which contains calcium oxide, magnesium oxide and aluminum oxide, but the mass coefficient is lower than 1.4. The alloy furnace tailings produced in the acid lining steelmaking process usually contain calcium oxide, magnesium oxide and aluminum oxide. Since the mass coefficient of the slag is lower than 1.4, its application performance in the production of building cement is poor. The main sources of acid lining slag include waste slag produced in the blast furnace and electric arc furnace steelmaking processes. In order to ensure the effect of its subsequent treatment, it is necessary to collect a sufficient amount of acid lining slag from the steel plant and conduct preliminary physical and chemical analysis to confirm its composition and quality standards; S2: Obtain slag using calcium oxide as a slag-forming agent, whose quality coefficient is greater than 1.4, the magnesium oxide content meets the requirements of construction cement production, and the calcium oxide content is appropriate. The slag using calcium oxide as a slag-forming agent is usually improved by adding calcium oxide during the steelmaking process to improve the quality coefficient of the slag. The quality coefficient of this slag is greater than 1.4, which meets the requirements of construction cement production. The characteristics of the required slag include appropriate calcium oxide content and magnesium oxide content that meets cement production. When selecting these slags, it is necessary to ensure that they are derived from a steelmaking process with appropriate composition and conduct detailed chemical analysis to ensure that they meet the quality standards for construction cement production; S3: Mix the acidic furnace lining slag obtained in S1 with the slag obtained in step 1.2 according to the following ratio: Acidic furnace lining slag: 50%-70% Using calcium oxide slag: 30%-50% In order to form alloy furnace tailings and ensure that the mass coefficient of the mixed alloy furnace tailings is stably greater than 1.4, and the magnesium oxide content is controlled below 10%, the acidic furnace lining slag and the slag using calcium oxide are mixed in proportion according to the component analysis and quality requirements. The mixing ratio is 50%-70% for the acidic furnace lining slag and 30%-50% for the slag using calcium oxide. This ratio is optimized to ensure that the mixed alloy furnace tailings has a stable mass coefficient greater than 1.4 and the magnesium oxide content is controlled below 10%. The mixing process needs to be carried out in a dedicated mixing equipment to ensure uniform mixing and avoid uneven components affecting the quality of the final product; S4: Take samples in batches for inspection of the mixed alloy furnace tailings, use an X-ray fluorescence spectrometer to determine its composition, including the content of calcium oxide, magnesium oxide, aluminum oxide, silicon dioxide, manganese dioxide and titanium dioxide, record and analyze the composition data of each batch of slag, and use an X-ray fluorescence spectrometer to determine the chemical composition of each batch of samples when sampling and inspecting the mixed alloy furnace tailings in batches. The test items include components such as calcium oxide, magnesium oxide, aluminum oxide, silicon dioxide, manganese dioxide and titanium dioxide. This step ensures that the composition of each batch of slag meets the requirements. The inspection data needs to be recorded and analyzed in detail to confirm whether the quality of the alloy furnace tailings meets the standards; S5: According to the test results in S4, adjust the mixing ratio and add neutralizer to adjust the composition of the alloy furnace tailings to ensure that the quality coefficient of the final product is greater than 1.4 and the magnesium oxide content is less than 10%. According to the test results, if the quality coefficient or magnesium oxide content of the alloy furnace tailings does not meet the requirements, it is necessary to adjust the mixing ratio and add neutralizer (such as calcium oxide) as needed. The amount of neutralizer added needs to be determined based on the specific test results of the mixed alloy furnace tailings to ensure that the quality coefficient of the final product is greater than 1.4 and the magnesium oxide content is less than 10%. This adjustment process may need to be performed multiple times to achieve the optimal mixing ratio and amount of neutralizer added; S6: Re-test the adjusted mixed slag to verify whether its mass coefficient and magnesium oxide content meet the requirements. If not, repeat step 1.5 until the standards are met. The adjusted mixed slag needs to be re-tested to confirm whether its mass coefficient and magnesium oxide content meet the standards. If the mixed slag after the initial adjustment still does not meet the standards, it is necessary to readjust the mixing ratio and the amount of neutralizer added, and re-test. This step may need to be repeated several times until the quality of the alloy furnace tailings fully meets the standards for construction cement production; S7: Dry the alloy furnace tailings that meet the requirements to control their moisture content, prevent excessive moisture from affecting the uniformity of the composition, and improve their stability through drying. The drying process aims to reduce the moisture content in the alloy furnace tailings to prevent excessive moisture from affecting the uniformity of the composition and the stability of the final product. The temperature range of the drying process is 60°C to 120°C, and the processing time is 24 hours to 48 hours. The drying process needs to be carried out in a controlled environment to ensure that the moisture content remains within the specified range, thereby improving the stability and consistency of the alloy furnace tailings.

[0017] The neutralizing agent is calcium oxide, and the amount of addition is determined according to the test results of the alloy furnace tailings after mixing to reduce the magnesium oxide content to below 10%. The choice of neutralizing agent is calcium oxide, and its main function is to reduce the magnesium oxide content in the alloy furnace tailings. The amount of addition needs to be determined according to the test results of each batch of alloy furnace tailings after mixing to ensure that the magnesium oxide content is less than 10%. The amount of calcium oxide added and the way it is used should be calculated and adjusted in detail to achieve the best treatment effect.

[0018] In S4, the inspection methods used include X-ray fluorescence spectrometer to ensure the accuracy of the analysis results of each component. X-ray fluorescence spectrometer is a high-precision analytical instrument used to determine the content of various elements in alloy furnace tailings. The instrument can provide accurate component analysis results to ensure that the chemical composition of each batch of samples meets the requirements. Its use method includes sample preparation, instrument calibration, and recording and analysis of measurement data.

[0019] The alloy tailings after mixing in S5 are fully stirred to ensure uniform composition. The alloy tailings after mixing need to be fully stirred in the stirring equipment to ensure uniform distribution of each component. The stirring time and speed need to be controlled during the stirring process to avoid uneven distribution of components. Full stirring helps to achieve more accurate mixing ratio and composition control, and improve the quality of the final product.

[0020] In S7, the temperature range of the drying treatment is 60°C to 120°C, and the time is 24 hours to 48 hours to ensure that the moisture content is controlled within the specified range. The temperature range of the drying treatment is 60°C to 120°C. According to different moisture contents and processing requirements, select appropriate drying temperature and time. The drying time is 24 hours to 48 hours to ensure that the moisture in the alloy furnace tailings is effectively removed and the stable moisture content requirements are achieved. The temperature and humidity need to be monitored during the drying process to prevent over-drying or incomplete drying.

[0021] In S6, if the standard is still not met after the initial adjustment, the mixing ratio and the amount of neutralizer added are readjusted according to the test results, and re-tested until qualified. After the initial adjustment of the mixing ratio and the amount of neutralizer added, re-testing is required to confirm whether the standard is met. If the alloy furnace tailings still do not meet the quality requirements after the initial adjustment, the mixing ratio and the amount of neutralizer added are readjusted according to the test results for further optimization. This process may need to be carried out multiple times until the quality of the alloy furnace tailings meets the standards for construction cement production.

[0022] The ratio of calcium oxide, magnesium oxide and aluminum oxide in the alloy furnace tailings is precisely controlled to meet the composition requirements of construction cement production and ensure that the magnesium oxide content does not exceed the standard.

[0023] Working principle: By precisely controlling and optimizing the chemical composition of alloy furnace tailings, it is ensured that it meets the quality standards for construction cement production. The core steps of this method include material acquisition, mixing ratio, component detection, adjustment and optimization, and drying. First, alloy furnace tailings are obtained from the acidic furnace lining steelmaking process. These slags usually contain calcium oxide, magnesium oxide and aluminum oxide, but their mass coefficient is less than 1.4. In addition, slag using calcium oxide as a slag-making agent is obtained, and its mass coefficient is greater than 1.4, and the magnesium oxide content meets the requirements of construction cement production. Then, the two slags are mixed according to a predetermined ratio (acidic furnace lining slag accounts for 50%-70%, and slag using calcium oxide accounts for 30%-50%) to form alloy furnace tailings. The goal of this step is to ensure that the mass coefficient of the mixed alloy furnace tailings is stably greater than 1.4 and the magnesium oxide content is controlled below 10%. The mixed alloy furnace tailings need to be sampled and inspected in batches, and their chemical composition is determined using an X-ray fluorescence spectrometer. These components include calcium oxide, magnesium oxide, aluminum oxide, and aluminum oxide. Aluminum dioxide, silicon dioxide, manganese dioxide and titanium dioxide. The inspection results are used to evaluate whether the quality of each batch of slag meets the requirements. If it is found that the magnesium oxide content exceeds the standard or the quality coefficient does not meet the standard, it is necessary to adjust the mixing ratio and add a neutralizer (calcium oxide) to further adjust the composition to ensure that the quality of the final product meets the standard. After adjusting the mixing ratio and adding the neutralizer, the alloy furnace tailings are re-inspected to verify whether its quality coefficient and magnesium oxide content meet the standard. If it still does not meet the standard after the initial adjustment, continue to adjust the mixing ratio and the amount of neutralizer added, and re-inspect until it is qualified. Finally, the alloy furnace tailings that meet the requirements are dried to control the moisture content to prevent excessive moisture from affecting the uniformity of the composition. The drying temperature range is 60°C to 120°C, and the processing time is 24 hours to 48 hours. Through this process, the stability and consistency of the final product are ensured, making the alloy furnace tailings a high-quality raw material that meets the requirements of building cement production, realizing the effective utilization of waste and maximization of resources.

[0024] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the application should be included in the protection scope of the present application.

Claims

1. A method for developing alloy furnace tailings for building cement production, characterized in that: The following steps are involved: S1: Obtain alloy furnace tailings produced by acidic furnace lining steelmaking, which contains calcium oxide, magnesium oxide and aluminum oxide, but the mass coefficient is less than 1.4; S2: Obtain slag using calcium oxide as a slag-making agent, with a mass coefficient greater than 1.4, a magnesium oxide content that meets the requirements for building cement production, and an appropriate calcium oxide content; S3: Mix the acidic furnace lining slag obtained in S1 with the slag obtained in step 1.2 according to the following ratio: Acidic furnace lining slag: 50%-70% Using calcium oxide slag: 30%-50% To form alloy furnace tailings, ensure that the mass coefficient of the mixed alloy furnace tailings is stably greater than 1.4, and the magnesium oxide content is controlled below 10%; S4: sampling and testing the mixed alloy furnace tailings in batches, using an X-ray fluorescence spectrometer to determine its composition, including the content of calcium oxide, magnesium oxide, aluminum oxide, silicon dioxide, manganese dioxide and titanium dioxide, and recording and analyzing the composition data of each batch of slag; S5: According to the test results in S4, the mixing ratio is adjusted, and a neutralizing agent is added to adjust the composition of the alloy furnace tailings to ensure that the quality coefficient of the final product is greater than 1.4 and the magnesium oxide content is less than 10%; S6: Re-test the adjusted mixed slag to verify whether its mass coefficient and magnesium oxide content meet the requirements. If not, repeat step 1.5 until the standards are met; S7: Dry the alloy furnace tailings that meet the requirements to control their moisture content to prevent excessive moisture from affecting the uniformity of the composition and improve its stability through drying.

2. The method for developing alloy furnace tailings for building cement production according to claim 1, characterized in that: The neutralizing agent is calcium oxide, and the amount of addition is determined according to the test results of the mixed alloy furnace tailings to reduce the magnesium oxide content to less than 10%.

3. The method for developing alloy furnace tailings for building cement production according to claim 1, characterized in that: In S4, the inspection method used includes an X-ray fluorescence spectrometer to ensure that the analysis results of each component are accurate.

4. The method for developing alloy furnace tailings for building cement production according to claim 1, characterized in that: The alloy furnace tailings mixed in S5 are fully stirred to ensure uniform composition.

5. The method for developing alloy furnace tailings for building cement production according to claim 1, characterized in that: In S7, the temperature range of the drying treatment is 60°C to 120°C, and the time is 24 hours to 48 hours to ensure that the moisture content is controlled within the specified range.

6. The method for developing alloy furnace tailings for building cement production according to claim 1, characterized in that: In S6, if the standard is still not met after the initial adjustment, the mixing ratio and the amount of the neutralizer added are readjusted according to the test results, and the test is performed again until it is qualified.

7. The method for developing alloy furnace tailings for building cement production according to claim 1, characterized in that: The ratio of calcium oxide, magnesium oxide and aluminum oxide in the alloy furnace tailings is precisely controlled to meet the component requirements of building cement production and ensure that the magnesium oxide content does not exceed the standard.