Modification method of recycled aggregate

By using a specific formula modification method on the regenerated aggregate, the modified slurry is formed, which solves the problem of low mechanical properties and durability of the regenerated aggregate concrete, and achieves rapid coagulation and efficient modification of the modified slurry, which is significantly It improves the compressive strength and crack resistance of the aggregate, while reducing production costs.

CN118930105APending Publication Date: 2024-11-12中交一公局绿建(厦门)科技有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411159003.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The mechanical properties and durability of existing recycled coarse aggregate concrete are lower than those of natural aggregate concrete, and commonly used surface modified materials such as polymer emulsions and volcanic mortars have the ability to improve durability but reduce mechanical properties, cost and low modification efficiency. question.

Method used

A modification method is adopted to form a mixed solution by dissolving water, water reducing agent, retarder, premature strength agent, defoaming agent and thickening agent in a heating container, and then stirring the cement and blending material evenly and slowly The regenerated aggregate is added and soaked for 5-10 minutes to form a modified slurry, and the preferred formulation includes specific ratios of cement, admixture, water reducing agent, retarder, defoaming agent and thickening agent.

Benefits of technology

The rapid condensation of the modified slurry is achieved, the compressive strength, motion modulus and sulfur aluminate corrosion resistance of the regenerated aggregate are improved, and the surface cracks are significantly reduced, crack resistance is enhanced, and production costs are reduced.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a modification method of recycled aggregate, which comprises the following steps: adding water into a heating container, respectively adding a water reducing agent, a retarder, an early strength agent, a defoaming agent and a thickening agent, dissolving to obtain a mixed solution, adding cement and an admixture into a stirring container, stirring, and uniformly mixing to obtain the recycled aggregate. Slowly adding the mixed solution in the heating container into a stirring container, stirring until the mixed solution is uniformly mixed to obtain modified slurry, adding recycled aggregate into the stirring container, infiltrating for 5-10 minutes, and then taking out to obtain modified recycled aggregate; according to the scheme, the modified slurry is short in setting time, the modification time can be shortened, the modification efficiency is high, the raw materials are low in price and easy to obtain, after the aggregate is modified, the compressive strength is improved by 40%, the dynamic elastic modulus is improved by 15%, the crushing value is reduced by 30%, the sulphoaluminate erosion resistance is improved by 50%, surface cracks are obviously reduced under aggregate microscopic observation, and the crack resistance is obviously enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aggregate modification, in particular to a method for modifying recycled aggregate. Background Art

[0002] The most common recycled coarse aggregate is made from waste concrete. The mechanical properties and durability of recycled aggregate concrete prepared with recycled coarse aggregate are lower than those of natural aggregate concrete prepared with natural aggregate. Therefore, in order to improve the durability and mechanical properties of recycled coarse aggregate concrete, researchers have proposed a large number of aggregate modification technologies, among which surface modification (RA) has attracted more and more attention. The commonly used materials for RA surface treatment can be divided into three categories: polymer emulsion, volcanic ash slurry and sodium silicate solution. However, these three materials also have certain limitations. For example, polymer emulsion can improve the durability of recycled aggregate concrete but reduce its mechanical properties, volcanic ash slurry is expensive and has low modification efficiency and long processing time.

[0003] Therefore, those skilled in the art provide a method for modifying recycled aggregate to solve the problem raised. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a method for modifying recycled aggregate.

[0005] The present invention provides a method for modifying recycled aggregates using the following technical solution:

[0006] A method for modifying recycled aggregate, comprising:

[0007] (1) adding water into a heating container, and then respectively adding a water reducing agent, a retarder, an early strength agent, a defoaming agent and a thickener to dissolve them to obtain a mixed solution;

[0008] (2) Add cement and admixture into a mixing container and stir to mix them evenly;

[0009] (3) slowly adding the mixed solution in the heating container into the stirring container, and stirring until the mixture is uniformly mixed to obtain a modified slurry;

[0010] (4) Add the recycled aggregate into a stirring container, soak for 5-10 minutes, and then take it out to obtain the modified recycled aggregate;

[0011] Wherein, the modified liquid comprises, by weight:

[0012] 190-220 parts of water, 880-920 parts of cement, 95-105 parts of admixture, 4.4-4.6 parts of water reducer, 7.5-8.5 parts of retarder, 0.35-0.45 parts of defoamer, 1.9-2.1 parts of early strength agent, 0.01-0.025 parts of thickener;

[0013] Preferably, the cement is sulphoaluminate cement and silicate cement or ordinary silicate cement, and the mass ratio is 8:1.

[0014] Preferably, the cement is sulphoaluminate cement, aluminate cement and silicate cement or ordinary silicate cement, and the mass ratio is 6:2:1.

[0015] Preferably, the thickener is one or more of cellulose ether, polyethylene oxide, polyvinyl alcohol, hydroxyethyl cellulose, sodium polyacrylate, and polyacrylamide.

[0016] Preferably, the defoaming agent is one or more of ethylene glycol stearate, distearyl ethylenediamine, polyoxypropylene glycerol, dimethylsiloxane, and pentaerythritol ether.

[0017] Preferably, the retarder is one or more of trisodium phosphate, trisodium polyphosphate, borax, zinc chloride, zinc carbonate, sodium sulfite, ferrous sulfate, calcium lignin sulfonate, sucrose, and tartaric acid.

[0018] Preferably, the early strength agent is one or more of lithium carbonate, sodium nitrate, calcium nitrate, silicate, potassium sulfate, sodium sulfate, potassium sulfate, lithium sulfate, calcium chloride, sodium chloride, and triethanolamine.

[0019] Preferably, the admixture is one or more of fly ash, granulated blast furnace slag, silica fume, limestone powder, steel slag powder, phosphorus slag powder, and zeolite powder.

[0020] Preferably, the water reducer is one or more of a lignin sulfonate water reducer, a naphthalenesulfonic acid formaldehyde condensate high efficiency water reducer, an aminosulfonate high efficiency water reducer, and a polycarboxylic acid high performance water reducer.

[0021] Preferably, the heating temperature in step (1) is 40-60° C. and the heating time is 3-5 minutes.

[0022] In summary, the present invention includes the following beneficial technical effects:

[0023] The modified slurry has a short setting time, which can shorten the modification time. The modification efficiency is high, the raw materials are cheap and easy to obtain, and the production cost is reduced. The initial setting time of the modified slurry is 90-110min, and the slurry fluidity is ≥300mm. The working performance of the modified liquid is fully maintained and the operating time is increased. The modified cement slurry with a size of 40mm×40mm×160mm is ≥55Mpa for 3h after testing according to the cement mortar strength test method (ISO method). After the aggregate is modified, the compressive strength is increased by 40%, the dynamic elastic modulus is increased by 15%, the crushing value is reduced by 30%, the resistance to sulphoaluminate erosion is increased by 50%, and the surface cracks of the aggregate are significantly reduced under microscopic observation, which significantly enhances the crack resistance. DETAILED DESCRIPTION

[0024] The embodiment of the invention discloses a method for modifying recycled aggregate.

[0025] Embodiment 1

[0026] A method for modifying recycled aggregate, comprising:

[0027] (1) adding water into a heating container, and then respectively adding a water reducing agent, a retarder, an early strength agent, a defoaming agent and a thickener to dissolve them to obtain a mixed solution;

[0028] (2) Add cement and admixture into a mixing container and stir to mix them evenly;

[0029] (3) slowly adding the mixed solution in the heating container to the stirring container, and stirring until the mixture is uniformly mixed to obtain a modified slurry;

[0030] (4) Add the recycled aggregate into a stirring container, soak for 5 minutes, and then take it out to obtain the modified recycled aggregate;

[0031] Wherein, the modified liquid includes, by weight:

[0032] 200 parts of water, 800 parts of sulphoaluminate cement, 100 parts of silicate cement, 100 parts of admixture, 4.5 parts of water reducer, 8 parts of retarder, 0.4 parts of defoamer, 2 parts of early strength agent, 0.02 parts of thickener;

[0033] Among them, the retarder is borax.

[0034] The early strength agent is lithium sulfate.

[0035] The defoaming agent is dimethylsiloxane.

[0036] The thickener is 100,000 molecular weight cellulose ether.

[0037] The admixture is slag powder.

[0038] The water reducing agent is a polycarboxylic acid-based high-performance water reducing agent.

[0039] The heating temperature in step (1) is 45° C. and the heating time is 4 minutes.

[0040] Embodiment 2

[0041] A method for modifying recycled aggregate, comprising:

[0042] (1) adding water into a heating container, and then respectively adding a water reducing agent, a retarder, an early strength agent, a defoaming agent and a thickener to dissolve them to obtain a mixed solution;

[0043] (2) Add cement and admixture into a mixing container and stir to mix them evenly;

[0044] (3) slowly adding the mixed solution in the heating container into the stirring container, and stirring until the mixture is uniformly mixed to obtain a modified slurry;

[0045] (4) Add the recycled aggregate into a stirring container, soak for 5 minutes, and then take it out to obtain the modified recycled aggregate;

[0046] The modified slurry comprises, by weight:

[0047] 210 parts of water, 600 parts of sulphoaluminate cement, 200 parts of aluminate cement, 100 parts of Portland cement, 100 parts of admixture, 4.5 parts of water reducer, 8 parts of retarder, 0.7 parts of defoamer, 2 parts of early strength agent, 0.01 parts of thickener;

[0048] Among them, the retarder is borax.

[0049] The early strength agent is lithium sulfate.

[0050] The thickener is 100,000 cellulose ether.

[0051] The defoaming agent is dimethylsiloxane.

[0052] The admixture is slag powder.

[0053] The water reducing agent is a polycarboxylic acid-based high-performance water reducing agent.

[0054] The heating temperature in step (1) is 45° C. and the heating time is 4 minutes.

[0055] The initial setting time of the modified slurry is 90-110min, and the final setting time is less than 120min, which fully maintains the working performance of the modified slurry and increases the operating time. It is tested according to the standard of cement mortar strength test method (ISO method). The 3h compressive strength of the modified cement slurry with a size of 40mm×40mm×160mm is ≥55Mpa.

[0056] After aggregate modification, the compressive strength increased by 40%, the dynamic elastic modulus increased by 15%, the crushing value decreased by 30%, the resistance to sulphoaluminate erosion increased by 50%, and the surface cracks of the aggregate under microscopic observation were significantly reduced, which significantly enhanced the crack resistance.

[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for modifying recycled aggregate, characterized in that: include: (1) adding water into a heating container, and then respectively adding a water reducing agent, a retarder, an early strength agent, a defoaming agent and a thickener to dissolve them to obtain a mixed solution; (2) Add cement and admixture into a mixing container and stir to mix them evenly; (3) slowly adding the mixed solution in the heating container into the stirring container, and stirring until the mixture is uniformly mixed to obtain a modified slurry; (4) Add the recycled aggregate into a stirring container, soak for 5-10 minutes, and then take it out to obtain the modified recycled aggregate; Wherein, the modified slurry comprises, by weight: 190-220 parts of water, 880-920 parts of cement, 95-105 parts of admixture, 4.4-4.6 parts of water reducer, 7.5-8.5 parts of retarder, 0.35-0.45 parts of defoamer, 1.9-2.1 parts of early strength agent, and 0.01-0.025 parts of thickener.

2. The method for modifying recycled aggregate according to claim 1, characterized in that: The cement is sulphoaluminate cement and silicate cement or ordinary silicate cement, and the mass ratio is 8:

1.

3. The method for modifying recycled aggregate according to claim 1, characterized in that: The cement is sulphoaluminate cement, aluminate cement and silicate cement or ordinary silicate cement, and the mass ratio is 6:2:

1.

4. The method for modifying recycled aggregate according to claim 1, characterized in that: The thickener is one or more of cellulose ether, polyethylene oxide, polyvinyl alcohol, hydroxyethyl cellulose, sodium polyacrylate, and polyacrylamide.

5. The method for modifying recycled aggregate according to claim 1, characterized in that: The nano admixture is one or more of fly ash, granulated blast furnace slag, silica fume, limestone powder, steel slag powder, phosphorus slag powder and zeolite powder.

6. The method for modifying recycled aggregate according to claim 1, characterized in that The defoaming agent is one or more of ethylene glycol stearate, distearyl ethylenediamine, polyoxypropylene glycerol, dimethylsiloxane, and pentaerythritol ether.

7. The method for modifying recycled aggregate according to claim 1, characterized in that The retarder is one or more of trisodium phosphate, trisodium polyphosphate, borax, zinc chloride, zinc carbonate, sodium sulfite, ferrous sulfate, calcium lignin sulfonate, sucrose, and tartaric acid.

8. The method for modifying recycled aggregate according to claim 1, characterized in that The early strength agent is one or more of lithium carbonate, sodium nitrate, calcium nitrate, silicate, potassium sulfate, sodium sulfate, potassium sulfate, lithium sulfate, calcium chloride, sodium chloride, and triethanolamine.

9. The method for modifying recycled aggregate according to claim 1, characterized in that The water reducer is one or more of lignin sulfonate water reducer, naphthalenesulfonic acid formaldehyde condensate high-efficiency water reducer, aminosulfonate high-efficiency water reducer, and polycarboxylic acid high-performance water reducer.

10. The method for modifying recycled aggregate according to claim 1, characterized in that: The heating temperature in step (1) is 40-60° C. and the heating time is 3-5 minutes.

Citation Information

Cited By

  • Modified recycled coarse aggregate, preparation method and self-compacting concrete

    CN121758089A