Prebaked anode anti-oxidation ceramic coating for electrolytic aluminum and preparation method of prebaked anode anti-oxidation ceramic coating

By using the slurry method to prepare alumina and silicon carbide ceramic coatings prepared in electrolytic aluminum production, combined with water glass binder, the problems of high consumption of prebaked anode and low coating strength are solved, and high-strength and dense coatings are achieved The formation and adaptability of large-scale production significantly reduce anode consumption and production costs.

CN118930218AActive Publication Date: 2024-11-12XI AN JIAOTONG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411208686.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The consumption of prebaked anodes in the existing electrolytic aluminum production is high, and the common sol-gel preparation methods have problems such as low coating strength, high cost, and difficulty in large-scale industrial production.

Method used

Using electrolytic aluminum pre-baked anode anti-oxidation ceramic coating based on the slurry method, using ceramic aggregates such as alumina and silicon carbide, combined with sodium water glass and potassium water glass as binders, and at a lower temperature by spraying or brushing. Dry and cure under the ground to form a coating with good adhesion, dense and high strength, reducing the contact between the anode and the oxidation atmosphere.

Benefits of technology

The formation of high-strength, dense ceramic coatings at lower temperatures are achieved, which reduces anode consumption, simplifies the preparation process, is suitable for large-scale industrial production, and shows good oxidation resistance under high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930218A_ABST
    Figure CN118930218A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of coatings, and discloses a prebaked anode anti-oxidation ceramic coating for electrolytic aluminum and a preparation method of the prebaked anode anti-oxidation ceramic coating. The coating comprises the following raw materials in percentage by mass: 45-55% of ceramic aggregate, 40-50% of a binder, 0.5-5% of a suspending agent, 0.2-5% of a functional additive and 0.5-6% of water, the ceramic aggregate is composed of at least two of aluminum oxide, silicon carbide, zirconium oxide and silica powder, and the ceramic aggregate at least contains aluminum oxide and silicon carbide; the binder is a mixture of sodium water glass and potash water glass. The anti-oxidation ceramic coating for the electrolytic aluminum prebaked anode is prepared by a two-step curing method. The binder interacts with the ceramic aggregate and undergoes a chemical reaction at a high temperature to generate a substance capable of improving the performance of the ceramic coating, so that the strength of the coating is improved. The ceramic coating is kept at 900 DEG C for 72 hours, the weight loss ratio of an oxidation experiment is lower than 1%, and it is shown that the ceramic coating has good oxidation resistance at the high temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a prebaked anode anti-oxidation ceramic coating in the electrolytic aluminum industry and a preparation method thereof. Background Art

[0002] my country's electrolytic aluminum production leads the world. As of July 2023, my country's electrolytic aluminum production accounts for 59.3% of the world's total. During the electrolysis process, alumina acts as a solute and carbonaceous bodies act as anodes to carry out electrochemical reactions in aluminum electrolytic cells. Among them, prebaked anodes, as consumable materials, account for a large part of the cost. The theoretical minimum amount of carbon anodes consumed is 333kg / t-Al. However, due to the loss of anodes during the electrolysis process, the actual electrolysis consumption of prebaked anodes is about 410kg / t-Al. A large part of the prebaked anodes react chemically with air and carbon dioxide during the electrolysis process and are consumed. The oxidation of prebaked anodes not only increases the cost of electrolytic aluminum, but also produces a large amount of CO and CO 2 , which is not conducive to achieving the "dual carbon" goal. Therefore, it is urgent to develop a prebaked anode coating that is cost-effective and easy to operate.

[0003] The common method for preparing the prebaked anode anti-oxidation coating is the sol-gel method, which has serious shrinkage during the drying process, low coating strength, and a cumbersome preparation process. The high cost is not conducive to large-scale industrial production. Therefore, it is necessary to provide a new prebaked anode anti-oxidation ceramic-based coating and its coating method to overcome the above technical problems. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of existing coatings and to provide a prebaked anode anti-oxidation coating, ceramic coating and preparation method for electrolytic aluminum based on a slurry method. The coating is sprayed or brushed on the surface of the prebaked anode, dried and cured at a relatively low temperature to form a dense, high-strength coating with good adhesion, which effectively avoids the contact between the oxidizing atmosphere and the prebaked anode during the electrolytic aluminum process, thereby reducing the consumption of the anode.

[0005] The technical solution adopted by the present invention is:

[0006] A prebaked anode anti-oxidation ceramic coating for electrolytic aluminum, the coating comprising the following raw materials in percentage by mass: 45-55% ceramic aggregate, 40-50% binder, 0.5-5% suspending agent, 0.2-5% functional additive, and 0.5-6% water; wherein the ceramic aggregate is composed of at least two of aluminum oxide, silicon carbide, zirconium oxide, and silicon micropowder, wherein the ceramic aggregate contains at least aluminum oxide and silicon carbide, the mass percentage of aluminum oxide in the ceramic aggregate is 50%-80%, and the mass percentage of silicon carbide in the ceramic aggregate is 20%-40%; the binder is sodium water glass (Na2 O·nSiO 2 ) and potassium water glass (K 2 O·nSiO 2 ).

[0007] In some embodiments, the aluminum oxide is α-aluminum oxide.

[0008] In some of the embodiments, the silicon carbide is green silicon carbide.

[0009] In some embodiments, the modulus of the sodium water glass and potassium water glass in the binder is 2.3-3.4.

[0010] In some embodiments, the suspending agent is one or both of sodium bentonite and fumed silica.

[0011] In some embodiments, the functional additive is at least one of yttrium oxide, sodium hydroxide, and potassium hydroxide.

[0012] In some of the embodiments, the mass ratio of sodium water glass to potassium water glass in the binder is 1:(0.2-1).

[0013] A method for preparing a prebaked anode anti-oxidation ceramic coating for electrolytic aluminum comprises the following steps: weighing the raw materials as described above,

[0014] (1) uniformly mixing a binder and half of the ceramic aggregate to obtain a first mixed slurry;

[0015] (2) uniformly mixing the first mixed slurry with the suspending agent and the functional additive to obtain a second mixed slurry;

[0016] (3) adding the remaining ceramic aggregate and water to the second mixed slurry and stirring evenly to obtain a prebaked anode anti-oxidation ceramic coating for electrolytic aluminum;

[0017] (4) applying a coating on the surface of the prebaked anode;

[0018] (5) Wait until the coating is dried and solidified to form a pre-baked anode anti-oxidation ceramic coating for electrolytic aluminum.

[0019] Adding raw materials at one time may cause agglomeration, thereby affecting the effect of raw material mixing and the quality of the ceramic coating prepared subsequently. However, the method of the present invention can obtain a mixed slurry that is evenly mixed and does not agglomerate by adjusting the process, and obtain a prebaked anode anti-oxidation ceramic coating for electrolytic aluminum.

[0020] In some of the embodiments, the method of applying the coating includes spraying or brushing.

[0021] In some of the embodiments, the brush coating method can be used to first paint the side and top surfaces of the prebaked anode as needed, and then paint the bottom surface after drying. The drying temperature is 45-55°C, the drying time is 25-35 minutes, and the coating is repeated 2-4 times to control the coating thickness to 0.2 to 0.5 mm.

[0022] In some embodiments, the drying and curing is a two-step drying and curing method, comprising the following steps:

[0023] The prebaked anode coated with the coating is heated at 65°C to 85°C for 1.5 to 2.5 hours; and then heated at 120°C to 150°C for 6.5 to 9.5 hours.

[0024] The beneficial effects of the present invention are:

[0025] (1) In the electrolytic aluminum prebaked anode anti-oxidation ceramic coating of the present invention, the binder is water glass, and the main component is silicate. It has good stability in a high temperature environment, a short curing time of the coating, high strength, and can be dried and cured at a relatively low temperature without the need for high-temperature sintering, thereby reducing the difficulty of coating preparation.

[0026] (2) In the anti-oxidation ceramic coating of the electrolytic aluminum prebaked anode of the present invention, silicate binders such as water glass can interact with the ceramic aggregate used in the present invention and can undergo chemical reactions at high temperatures to generate substances that can improve the performance of the ceramic coating, thereby further increasing the strength of the coating.

[0027] (3) In the anti-oxidation ceramic coating of the prebaked anode of electrolytic aluminum of the present invention, the main component of the aggregate is aluminum oxide, which can minimize the increase of impurities in the aluminum electrolytic cell and basically will not affect the electrolysis process and the purity of the product.

[0028] (4) The electrolytic aluminum prebaked anode anti-oxidation ceramic coating of the present invention is prepared by a slurry method. The coating overcomes the problem of easy shrinkage of conventional coatings during the drying process, and the obtained coating has high strength. The method is easy to operate, the equipment is simple, and it is not limited by environmental and site conditions. The coating composition is simple and cheap, suitable for mass production, and easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The preparation flow chart of the coating.

[0030] Figure 2 The following are Fourier transform infrared spectra of the coating prepared in Example 1 after drying and curing under different conditions.

[0031] Figure 3 This is a 100x SEM image of the surface of the coating prepared in Example 1 after drying and curing.

[0032] Figure 4This is a 1500x SEM image of the surface of the coating prepared in Example 1 after drying and curing.

[0033] Figure 5 The left side is untreated, and the right side is coated with the coating prepared according to Example 1 before and after the oxidation experiment.

[0034] Figure 6 These are photos of the untreated test pieces before and after the oxidation test.

[0035] Figure 7 This is a photograph of a test block coated with the coating prepared in Example 2 after an oxidation test.

[0036] Figure 8 This is a photograph of the test block coated with the coating prepared in Comparative Example 2 after the oxidation test.

[0037] Fig. 9 This is a photograph of the test block coated with the coating prepared in Comparative Example 3 after the oxidation test.

[0038] Fig.10 This is a photograph of a test block coated with the coating prepared in Comparative Example 4 after an oxidation test.

[0039] Fig.11 This is a 100x SEM image of the surface of the coating prepared in Comparative Example 4 after drying and curing.

[0040] Fig.12 This is a 1500x SEM image of the surface of the coating prepared in Comparative Example 4 after drying and curing. DETAILED DESCRIPTION

[0041] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0042] The slurry method mentioned in the present invention is a technology in which ceramic aggregate, binder, etc. are mixed in a certain slurry ratio to prepare a slurry, the uniform slurry is evenly applied on the surface of the substrate by spraying or brushing, and a coating is obtained after a certain period of drying and curing.

[0043] Prebaked anode for electrolytic aluminum, also known as aluminum carbon, is one of the indispensable and irreplaceable core raw materials for the production of electrolytic aluminum. It has good electrical conductivity and high temperature corrosion resistance and is called the heart of the electrolytic cell. At present, the coating of the present invention can be used for conventional prebaked anodes for electrolytic aluminum. The coating is dried and cured at a relatively low temperature to form a dense and high-strength coating with good adhesion. The coating effectively avoids the contact between the oxidizing atmosphere and the prebaked anode during the electrolytic aluminum process, thereby reducing the consumption of the anode.

[0044] The present invention provides an anti-oxidation coating and ceramic coating for prebaked anode of electrolytic aluminum based on a slurry method and a preparation method thereof. The technical scheme is to use powders such as aluminum oxide and silicon carbide as ceramic aggregates, and to prepare an anti-oxidation ceramic coating for prebaked anode of electrolytic aluminum through a slurry process under the action of a binder, a suspending agent, a functional additive, water, etc.

[0045] A prebaked anode anti-oxidation ceramic coating for electrolytic aluminum, the components and their mass percentages of the coating are: 45-55% ceramic aggregate, 40-50% binder, 0.5-5% suspending agent, 0.2-5% functional additive, and 0.5-6% water.

[0046] The ceramic aggregate is composed of at least two of alumina, silicon carbide, zirconium oxide and silicon powder, and the ceramic aggregate contains at least alumina and silicon carbide.

[0047] That is, the ceramic aggregate can be composed of alumina and silicon carbide, or the ceramic aggregate can be composed of alumina, silicon carbide, and zirconium oxide, or the ceramic aggregate can be composed of alumina, silicon carbide, and silicon powder, or the ceramic aggregate can be composed of alumina, silicon carbide, zirconium oxide, and silicon powder.

[0048] The binder is a mixture of sodium water glass and potassium water glass.

[0049] Water glass is a silicate that is soluble in water. It is composed of alkali metals and silicon dioxide in different proportions. The most commonly used are sodium water glass and potassium water glass. Sodium water glass is an aqueous solution of sodium silicate, and its chemical formula is Na 2 O·nSiO 2 Potassium water glass is an aqueous solution of potassium silicate, with the molecular formula K 2 O·nSiO 2 .

[0050] In some of the embodiments, sodium water glass and potassium water glass can be prepared and used immediately, and the mass of the binder defined in the ceramic coating formulation of the present invention is the mass of the prepared sodium water glass and potassium water glass.

[0051] In the prebaked anode anti-oxidation coating for electrolytic aluminum of the present invention, silicate binders such as water glass can interact with the ceramic aggregate used in the present invention, and can undergo chemical reactions at high temperatures to generate substances that can improve the performance of the ceramic coating, thereby further improving the strength of the coating, thereby overcoming the problem of phosphate binders in the prior art that contaminate the original aluminum, and the problem of organic binders such as methyl cellulose and resins that are not resistant to high temperatures.

[0052] Because the binder is water glass, the main component of which is silicate, it has good stability in high temperature environments, the coating has a short curing time, high strength, and can be dried and cured at a lower temperature without the need for high-temperature sintering, reducing the difficulty of coating preparation.

[0053] In some of the embodiments, the mass percentage of aluminum oxide in the ceramic aggregate is controlled to be 50% to 80%.

[0054] Alumina and water glass in the aggregate can generate substances that improve the performance of the ceramic coating and further increase the strength of the coating. Therefore, the proportion of alumina needs to be limited. If the proportion of alumina is less than 50% or greater than 80%, the coating is prone to defects such as reduced mechanical properties and density of the coating, and too low alumina proportion will introduce too many other elements into the electrolytic cell.

[0055] In some preferred embodiments, the alumina is α-alumina.

[0056] Alumina can be divided into two main types: α-alumina and γ-alumina. The present invention prefers α-alumina. The anti-oxidation ceramic coating obtained by coating the coating prepared by α-alumina on the pre-baked anode of electrolytic aluminum has better comprehensive performance.

[0057] In some preferred embodiments, the silicon carbide is green silicon carbide.

[0058] Silicon carbide is generally divided into black silicon carbide and green silicon carbide. The present invention preferably uses green silicon carbide to prepare the coating, and the ceramic coating obtained by coating the coating has higher strength.

[0059] In some embodiments, the mass percentage of silicon carbide in the ceramic aggregate is controlled to be 20% to 40%.

[0060] Silicon carbide can improve the hardness, toughness and wear resistance of ceramic coatings.

[0061] In some embodiments, the average particle size of the ceramic aggregate is 1.3-18 μm.

[0062] In some embodiments, the mass ratio of sodium water glass to potassium water glass is 1: (0.2-1). The significance lies in that the composite water glass has better anti-aging performance of the coating, is more conducive to preservation, and the coating cures faster during use.

[0063] In some embodiments, the modulus of the sodium water glass and potassium water glass in the binder is 2.3-3.4.

[0064] The modulus of sodium water glass refers to the SiO 2 and Na 2O molar ratio, this parameter has an important influence on the performance and application of sodium water glass. The modulus of sodium water glass is usually between 1.5 and 3.5, which reflects the molar ratio of SiO 2 and Na 2 The relative content of O. The present invention prefers sodium water glass and potassium water glass with a modulus of 2.3 to 3.4.

[0065] In some embodiments, the suspending agent is one or both of sodium bentonite and fumed silica.

[0066] The main function of the suspending agent is to evenly disperse the solid particles in the liquid, achieve liquid mixing and solid dispersion, and form a stable suspension system. When the coating of the present invention is used to coat the surface of the prebaked anode for electrolytic aluminum, the ordinary brushing method requires 2-4 times of brushing, which generally takes 2-5 hours. The mixed coating can continuously maintain a stable suspension system.

[0067] In some embodiments, the functional additive is one, two, or three of yttrium oxide, sodium hydroxide, and potassium hydroxide.

[0068] The functional additives improve the stability of the coating and enhance the mechanical properties of the coating.

[0069] The present invention also provides a method for preparing the anti-oxidation ceramic coating of the electrolytic aluminum prebaked anode based on the slurry method. The preparation flow chart of the coating is shown in Figure 1 .

[0070] The specific steps are as follows:

[0071] Weigh the raw materials as described in any of the above items,

[0072] (1) Prepare a first mixed slurry by uniformly mixing a binder with half of the ceramic aggregate to obtain a first mixed slurry.

[0073] (2) preparing a second mixed slurry by uniformly mixing the first mixed slurry with the suspending agent and the functional additive to obtain the second mixed slurry.

[0074] (3) adding the remaining ceramic aggregate and water to the second mixed slurry and stirring evenly to obtain an electrolytic aluminum prebaked anode anti-oxidation ceramic coating;

[0075] (4) applying a coating on the surface of the prebaked anode;

[0076] (5) Wait until the coating is dried and solidified to form a pre-baked anode anti-oxidation ceramic coating for electrolytic aluminum.

[0077] In some of these embodiments, the adhesive is prepared and used immediately, so temporary preparation is required. Those skilled in the art can handle it according to common sense.

[0078] In some embodiments, the sodium water glass in the binder is prepared by dissolving instant sodium silicate in deionized water, heating to 35-45° C., and stirring until the instant sodium silicate is completely melted. The potassium water glass in the binder is prepared by dissolving instant potassium silicate in deionized water, heating to 35-45° C., and stirring until the instant potassium silicate is completely melted.

[0079] In some of the embodiments, the method of applying the coating on the surface of the test block includes spraying or brushing.

[0080] The specific operation of the brush coating method is as follows: brush the side and top surface of the prebaked anode → dry at 45-55°C for 25-35 minutes → cool to room temperature (about 12-18 minutes to cool to room temperature in the embodiment) → brush the bottom surface → dry at 45-55°C for 25-35 minutes → cool to room temperature, and apply 2 to 4 times according to this process. Ensure that the coating thickness is 0.2-0.5 mm.

[0081] Technical personnel in this industry can also adopt the spraying method as needed, and optimize and adjust the spraying parameters in the spraying method.

[0082] In step (5), the coating is dried and cured. The technical personnel in the industry can dry and cure the coating according to conventional operations, such as drying and curing at room temperature for 24 hours.

[0083] In some preferred embodiments, the coating is dried and cured in two steps, the first step of curing is to heat the test piece at 65°C-85°C for 1.5-2.5 hours, and the second step of curing is to heat at 120°C-150°C for 6.5-9.5 hours. The first step of curing can ensure that the free water in the coating is fully evaporated and will not evaporate too quickly, which can effectively avoid defects such as bubbling, cracks, and pores. The second step of curing can ensure that the coating is fully dried and cured, and that most of the -Si-OH groups are converted into high-bond energy Si-O-Si structures.

[0084] The application scenario of the ceramic coating of the present invention and the formed ceramic coating is prebaked anode for electrolytic aluminum. In the anti-oxidation ceramic coating of the prebaked anode for electrolytic aluminum of the present invention, the main component of the aggregate is aluminum oxide, which can minimize the increase of impurities in the aluminum electrolytic cell and basically does not affect the electrolysis process and the purity of the product.

[0085] Modern electrolytic aluminum industry production adopts cryolite-alumina molten salt electrolysis. Molten cryolite is the solvent, alumina is the solute, carbonite is the anode, and aluminum liquid is the cathode. After a strong direct current is passed, an electrochemical reaction (electrolysis) is carried out at the two poles in the electrolytic cell at 950℃~970℃. Therefore, the anti-oxidation ceramic coating is coated on the prebaked anode for electrolytic aluminum to form a ceramic coating, which needs to withstand high temperatures above 800℃ for a long time. The present invention uses a 900℃ insulation treatment for 72h and air as an oxidizing gas to detect and evaluate the protective isolation effect of the ceramic coating on the prebaked anode.

[0086] The prebaked anode test block used in the embodiment is cut from the actual prebaked anode for electrolytic aluminum, and the experimental effect is equivalent to using the prebaked anode for industrial electrolytic aluminum.

[0087] The alumina used in the following examples is α-alumina, the silicon carbide is green silicon carbide, and other raw materials are all commercially available products.

[0088] The following is a description with reference to specific embodiments.

[0089] Example 1

[0090] 65 g of 3.3 mold instant sodium silicate and 65 g of deionized water were heated to 40°C and stirred until a translucent viscous liquid was formed to prepare 130 g of sodium water glass (Na 2 O·nSiO 2 40 g of 3.3 mold instant potassium silicate and 60 g of deionized water were heated to 40°C and stirred until a translucent viscous liquid was formed to prepare 100 g of potassium water glass (K 2 O·nSiO 2 ). The prepared sodium water glass and potassium water glass were stirred for 10 minutes to obtain a binder. 70 grams of aluminum oxide, 32 grams of silicon carbide, 12 grams of zirconium oxide, and 10 grams of silicon powder were added to the prepared 230g binder, and stirred for 10 minutes to obtain a first slurry. 6 grams of sodium bentonite and 11 grams of yttrium oxide were added, and stirred for 10 minutes to obtain a second mixed slurry. 70 grams of aluminum oxide, 32 grams of silicon carbide, 12 grams of zirconium oxide, 10 grams of silicon powder, and 5 grams of deionized water were added, and stirred for 10 minutes to obtain an electrolytic aluminum prebaked anode anti-oxidation ceramic coating.

[0091] Paint the side and top of the test block → dry at 50°C for 30 minutes → cool to room temperature → paint the bottom → dry at 50°C for 30 minutes → cool to room temperature. Apply the paint three times to obtain a pre-baked anode test block coated with the paint, and the thickness of the coating is between 0.2 and 0.5 mm.

[0092] The coating is dried and cured using a two-step curing method, the specific operations are as follows:

[0093] The first curing step was to heat the test piece at 85°C for 2.5 hours, and the second curing step was to heat the test piece at 150°C for 7.5 hours. The ceramic coating of the prebaked anode was prepared.

[0094] Among them, the first step of curing can ensure that the free water in the coating is fully evaporated and will not evaporate too quickly, which can effectively avoid defects such as bubbling, cracks, pores, etc. The second step of curing can ensure that the coating is fully dried and cured, and that most of the -Si-OH groups are converted into high-bond energy Si-O-Si structures.

[0095] As a comparison, the prebaked anode test block coated with the coating was dried and cured at room temperature for 24 hours to obtain a ceramic coating of the prebaked anode.

[0096] The coating obtained by drying and curing according to Example 1 and the coating obtained by drying and curing at room temperature for 24 hours were subjected to infrared spectroscopy analysis. The Fourier transform infrared spectra after drying and curing under different conditions are shown in the figure below. Figure 2 shown.

[0097] Depend on Figure 2 It can be seen that the coating solidifies at 1644cm at room temperature. -1 and 990cm -1 There are obvious peaks at 3200cm -1 There is a broad peak. 1644cm -1 The sharp peak at 990 cm is related to the H-OH bond in free water. -1 There is a clear peak at 3200cm -1 The broad peak is related to the -Si-OH group in the binder. After the coating was dried and cured at room temperature for 24 hours, there were still a lot of free water and -Si-OH groups, proving that the coating was not completely dried and cured at room temperature. The coating was 1644cm after the first step of curing. -1 The peak at 0.0447 W basically disappeared, indicating that the free water in the coating had been completely evaporated after the first step of curing. No obvious peak appeared after the second step of curing, indicating that the -Si-OH groups in the coating were converted into high-bond energy Si-O-Si structures after the second step of curing, and the coating had been fully cured.

[0098] The ceramic coating obtained by the two-step curing method in Example 1 was analyzed by electron microscope. Figure 3 and Figure 4 . Figure 3 This is a 100x SEM image of the surface of the ceramic coating obtained by the two-step curing method of the coating prepared in Example 1. Figure 3 It shows that the surface of the ceramic coating is smooth and has no obvious defects. Figure 4 This is a 1500x SEM image of the surface of the ceramic coating obtained by the two-step curing method of the coating prepared in Example 1. Figure 4It shows that the aggregate and binder in the ceramic coating are fully combined.

[0099] The prebaked anode test block with an anti-oxidation ceramic coating prepared in Example 1 was weighed M1 after drying and curing. The test block was placed in a tube furnace and kept at 900°C for 72 hours. Heating was stopped, and the test block was taken out and weighed M2 after cooling to room temperature. The weight loss rate was calculated, and the weight loss rate = (M1-M2) / M1×100%. The weight loss rate of the test block was 0.54%.

[0100] The weight loss rate can reflect the anti-oxidation performance of the coating. The weight loss rate of the test block protected by the coating was only 0.54% under the condition of 900℃ for 72h, showing excellent anti-oxidation performance.

[0101] The test block with no treatment on the left side and coating protection on the right side (Example 1) was placed in a tube furnace and kept at 900°C for 20 hours. The heating was stopped and the test block was taken out after cooling to room temperature. The photos of the test block before and after the oxidation experiment are as follows: Figure 5 shown.

[0102] Figure 5 In the figure, the untreated part on the left side is severely oxidized, and the height of the test block decreases by about 40%. The part protected by the coating on the right side has no obvious oxidation phenomenon, which shows that the ceramic coating of the present invention has good anti-oxidation performance at high temperature.

[0103] Example 2

[0104] Heat 80 grams of 2.7 molds of instant sodium silicate and 80 grams of deionized water to 40°C, stir until it becomes a translucent viscous liquid, and prepare sodium water glass. Heat 24 grams of 3.3 molds of instant potassium silicate and 36 grams of deionized water to 40°C, stir until it becomes a translucent viscous liquid, and prepare potassium water glass. Stir the prepared sodium water glass and potassium water glass for 10 minutes to prepare a binder. Add 72 grams of aluminum oxide, 40 grams of silicon carbide, and 14 grams of zirconium oxide to the binder and stir for 10 minutes to obtain a first slurry. Add 6 grams of fumed silica, 5 grams of sodium bentonite, 3 grams of sodium hydroxide, and 4 grams of yttrium oxide, and stir for 10 minutes to obtain a second mixed slurry. Add 72 grams of aluminum oxide, 40 grams of silicon carbide, 14 grams of zirconium oxide, and 10 grams of deionized water and stir for 10 minutes to obtain an electrolytic aluminum prebaked anode anti-oxidation ceramic coating.

[0105] Paint the side and top surface of the prebaked anode test block → dry at 55°C for 25 minutes → cool to room temperature → paint the bottom surface → dry at 55°C for 25 minutes → cool to room temperature. Apply this process 4 times to obtain a prebaked anode test block coated with the coating, and the thickness of the coating is between 0.2 and 0.5 mm.

[0106] The coating is dried and cured using a two-step curing method, the specific operations are as follows:

[0107] The first curing step was to heat the test piece at 85°C for 2 hours, and the second curing step was to heat at 150°C for 8 hours.

[0108] A ceramic coating of a prebaked anode is prepared.

[0109] The untreated test block and the test block with coating protection (Example 2) were placed in a tube furnace and kept at 900°C for 72 hours. The heating was stopped and the test blocks were taken out after cooling to room temperature. The weight loss of the two test blocks was compared under the same conditions. Figure 6 The untreated test piece was completely oxidized, with a weight loss of 100%. Figure 7 The results show that the test block coated with the protective coating has no obvious oxidation phenomenon, the weight loss rate is 0.64%, and the coating has no obvious defects, indicating that the coating of the present invention has good anti-oxidation performance at high temperatures.

[0110] Example 3

[0111] Heat 80 grams of 3-mold instant sodium silicate and 80 grams of deionized water to 40°C, stir until it becomes a translucent viscous liquid, and obtain sodium water glass. Heat 16 grams of 3.3-mold instant potassium silicate and 24 grams of deionized water to 40°C, stir until it becomes a translucent viscous liquid, and obtain potassium water glass. Stir the obtained sodium water glass and potassium water glass for 10 minutes to obtain a binder. Add 110 grams of aluminum oxide and 27.5 grams of silicon carbide to the binder and stir for 10 minutes to obtain a first slurry. Add 6 grams of fumed silica, 4 grams of sodium bentonite, and 3 grams of potassium hydroxide, and stir for 10 minutes to obtain a second mixed slurry. Add 110 grams of aluminum oxide, 27.5 grams of silicon carbide, and 12 grams of deionized water, and stir for 10 minutes to obtain an electrolytic aluminum prebaked anode anti-oxidation ceramic coating.

[0112] Paint the side and top of the prebaked anode test block → dry at 50°C for 25 minutes → cool to room temperature → paint the bottom → dry at 50°C for 25 minutes → cool to room temperature. Apply twice according to this process to obtain a prebaked anode test block coated with the coating, and the thickness of the coating is between 0.2 and 0.5 mm.

[0113] The coating is dried and cured using a two-step curing method, the specific operations are as follows:

[0114] The first curing step was to heat the test piece at 85°C for 2 hours, and the second curing step was to heat at 150°C for 8 hours.

[0115] A ceramic coating of a prebaked anode is prepared.

[0116] The test block with coating protection (Example 3) was placed in a tube furnace and kept at 900°C for 72 hours. The heating was stopped and the block was taken out after cooling to room temperature. The weight loss was measured to be 0.88%.

[0117] Example 4

[0118] Heat 62.5 grams of 3.3 mold instant sodium silicate and 62.5 grams of deionized water to 40°C, stir until it becomes a translucent viscous liquid, and prepare sodium water glass. Heat 50 grams of 3.3 mold instant potassium silicate and 75 grams of deionized water to 40°C, stir until it becomes a translucent viscous liquid, and prepare potassium water glass. Stir the prepared sodium water glass and potassium water glass for 10 minutes to prepare a binder. Add 56.25 grams of aluminum oxide, 45 grams of silicon carbide, and 11.25 grams of silicon powder to the binder, stir for 10 minutes, and obtain the first slurry. Add 12.5 grams of yttrium oxide and 10 grams of sodium bentonite, stir for 10 minutes to obtain the second mixed slurry. Add 56.25 grams of aluminum oxide, 45 grams of silicon carbide, 11.25 grams of silicon powder, and 2.5 grams of deionized water, stir for 10 minutes, and obtain an electrolytic aluminum prebaked anode anti-oxidation ceramic coating.

[0119] Paint the side and top of the pre-baked anode test block → dry at 55°C for 30 minutes → cool to room temperature → paint the bottom surface → dry at 55°C for 30 minutes → cool to room temperature. Follow this process for 4 times to obtain a pre-baked anode test block coated with paint.

[0120] The coating is dried and cured using a two-step curing method, the specific operations are as follows:

[0121] The first curing step was to heat the test piece at 85°C for 2.5 hours, and the second curing step was to heat at 140°C for 7.5 hours.

[0122] A ceramic coating of a prebaked anode is prepared.

[0123] The test block with coating protection (Example 4) was placed in a tube furnace and kept at 900°C for 72 hours. The heating was stopped and the block was taken out after cooling to room temperature. The weight loss was measured to be 0.92%.

[0124] Comparative Example 1

[0125] Chinese patent application number 201911337979.0, "A ceramic-based high-temperature antioxidant coating for electrolytic aluminum prebaked carbon anode and its preparation method" (publication number CN 111039662A). "The antioxidant coating is brushed on the graphite rod, dried at room temperature for 1 day, and then placed in a muffle furnace together with the graphite rod not coated with the antioxidant coating, first heated to 500°C, kept warm for 1 hour, and then continued to heat to 970°C and kept warm for 8 hours. Stop heating, cool to room temperature, take out, and compare the weight loss of the graphite rod coated with the antioxidant coating and the graphite rod not coated with the antioxidant coating under the same conditions."

[0126] The results showed that the weight loss rate of Example 1 was 2.76%, and the weight loss rate of Example 2 was 3.14%.

[0127] The ceramic coating formed by the prebaked anode anti-oxidation ceramic coating and the coating method of the present invention is kept at 900°C for 72 hours, and the weight loss rate in the oxidation experiment is less than 1%, indicating that the ceramic coating of the present invention has good anti-oxidation performance at high temperatures.

[0128] Comparative Example 2

[0129] 40% of the binder in the original Example 1 was replaced with water. The specific binder was 78g of sodium water glass + 60g of potassium water glass (130g of sodium water glass + 100g of potassium water glass in Example 1), 97g of water, and other raw materials and preparation methods were the same as those in Example 1.

[0130] After drying and curing, the coating was found to have cracked. Figure 8 .

[0131] Comparative Example 3

[0132] Add half of the binder, specifically 195g of sodium water glass + 150g of potassium water glass (130g of sodium water glass + 100g of potassium water glass in Example 1), and other raw materials and preparation methods are the same as in Example 1.

[0133] After the test piece was kept at 900℃ for 72 hours, it was found that the coating had obvious bulging phenomenon. Fig. 9 .

[0134] This indicates that the amount of binder added should not be too low or too high. The preparation of a surface defect-free, dense anti-oxidation coating requires strict control of the amount of binder added.

[0135] Comparative Example 4

[0136] The ceramic aggregate only uses 275 g of alumina (220 g of alumina + 55 g of silicon carbide in Example 3), and the other raw materials and preparation method are the same as in Example 3.

[0137] The obtained prebaked anode test block was taken out after being kept at 900℃ for 72 hours, and it was found that obvious cracks appeared on the coating surface. Fig.10 . Fig.11 In the 100x SEM image of the surface of the coating after drying and curing, it is shown that after the coating prepared in Comparative Example 4 is dried and cured, the surface of the coating obtained is uneven and has obvious defects such as pores and cracks. Fig.12 In the 1500x SEM image of the surface of the coating after drying and curing, it is shown that after the coating prepared in Comparative Example 4 is dried and cured, the aggregate and the binder are not fully combined together, and defects such as pores and cracks are more obvious.

[0138] By comparison, it can be seen that ceramic aggregate cannot only be made of alumina. The preparation of a defect-free, dense, anti-oxidation coating requires the use of ceramic aggregates with a suitable ratio.

[0139] The parameters of the above embodiments and comparative examples are compared, and the results are shown in Table 1.

[0140] Table 1 Weight loss rate of samples in antioxidant experiment

[0141] Mass before oxidation / g Mass after oxidation / g Weight loss rate / % Untreated test block 109.26 0 100% Example 1 117.57 116.93 0.54% Example 2 116.82 116.07 0.64% Example 3 116.70 115.67 0.88% Example 4 117.31 116.23 0.92% Comparative Example 1 2.76% Comparative Example 2 110.41 101.55 8.02% Comparative Example 3 115.13 111.94 2.77% Comparative Example 4 113.17 106.38 6.00%

[0142] By comparison, it can be seen that the ceramic coating prepared by the coating obtained according to the formula of the present invention has a lower weight loss rate and has no obvious defects after the oxidation test, which shows that the ceramic coating of the present invention has good high-temperature oxidation resistance at high temperatures.

[0143] The above is a further detailed description of the present invention, which should not be regarded as a limitation on the specific implementation of the present invention. For ordinary technicians in the technical field to which the present invention belongs, simple deduction or replacement without departing from the concept of the present invention is within the protection scope of the present invention.

Claims

1. A prebaked anode anti-oxidation ceramic coating for electrolytic aluminum, characterized in that: The coating comprises the following raw materials in percentage by mass: 45-55% of ceramic aggregate, 40-50% of binder, 0.5-5% of suspending agent, 0.2-5% of functional additive and 0.5-6% of water; wherein the ceramic aggregate is composed of at least two of alumina, silicon carbide, zirconium oxide and silicon micropowder, wherein the ceramic aggregate contains at least alumina and silicon carbide, the mass percentage of alumina in the ceramic aggregate is 50%-80%, and the mass percentage of silicon carbide in the ceramic aggregate is 20%-40%; and the binder is a mixture of sodium water glass (Na2O·nSiO2) and potassium water glass (K2O·nSiO2).

2. The prebaked anode anti-oxidation ceramic coating for electrolytic aluminum according to claim 1, characterized in that: The aluminum oxide is α-aluminum oxide.

3. The prebaked anode anti-oxidation ceramic coating for electrolytic aluminum according to claim 1, characterized in that: The silicon carbide is green silicon carbide.

4. The prebaked anode anti-oxidation ceramic coating for electrolytic aluminum according to claim 1, characterized in that: The modulus of the sodium water glass and potassium water glass in the binder is 2.3-3.

4.

5. The prebaked anode anti-oxidation ceramic coating for electrolytic aluminum according to claim 1, characterized in that: The suspending agent is one or both of sodium bentonite and fumed silica.

6. The prebaked anode anti-oxidation ceramic coating for electrolytic aluminum according to claim 1, characterized in that: The functional additive is at least one of yttrium oxide, sodium hydroxide and potassium hydroxide.

7. The prebaked anode anti-oxidation ceramic coating for electrolytic aluminum according to claim 1, characterized in that: The mass ratio of sodium water glass to potassium water glass in the binder is 1:(0.2-1).

8. A method for preparing a prebaked anode anti-oxidation ceramic coating for electrolytic aluminum, characterized in that: The method comprises the following steps: weighing the raw materials according to any one of claims 1 to 7, (1) uniformly mixing a binder and half of the ceramic aggregate to obtain a first mixed slurry; (2) uniformly mixing the first mixed slurry with the suspending agent and the functional additive to obtain a second mixed slurry; (3) adding the remaining ceramic aggregate and water to the second mixed slurry and stirring evenly to obtain a prebaked anode anti-oxidation ceramic coating for electrolytic aluminum; (4) coating the surface of the prebaked anode; (5) Wait until the coating is dried and solidified to form a pre-baked anode anti-oxidation ceramic coating for electrolytic aluminum.

9. The preparation method according to claim 8, characterized in that: The coating application method includes spraying or brushing.

10. The preparation method according to claim 8, characterized in that: Drying and curing includes the following steps: The prebaked anode coated with the coating is heated at 65°C to 85°C for 1.5-2.5 hours; and then heated at 120°C to 150°C for 6.5-9.5 hours.

Citation Information

Patent Citations

  • Method for preparing ceramic coating on surface of porous ceramic matrix by slurry spraying

    CN102942385A

  • Ceramic alloy coating and coating layer

    CN108793929A

  • Electrolytic aluminum prebaked carbon anode ceramic-based high-temperature oxidation-resistant coating and preparation method thereof

    CN111039662A

  • Anti-sparking high-temperature-resistant insulating anode hook for aluminum electrolysis cell

    CN217556314U

  • Cerium oxycompound, stable anode for molten salt electrowinning and method of production

    WO1988001312A1