Zinc tin oxide ceramic target material and preparation method thereof
Through sand grinding, spray granulation, molding, cold isostatic molding, normal pressure sintering, and hot isostatic sintering, tin and zinc oxide ceramic targets with high density, low resistivity and high uniformity are prepared to solve the problem of The problem of poor performance of tin oxide zinc targets in the prior art is provided, and solutions for indium alternative materials are provided, and preparation efficiency and stability are improved.
Patent Information
- Application Number
- CN202411112348.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
AI Technical Summary
It is difficult to prepare tin zinc oxide targets with high density, low resistivity and high uniformity, and the indium resources are tight, resulting in an increase in demand for indium, and alternative materials with similar photoelectric properties are needed.
The super-pressure sintering isostatic sintering isostatic sintering isostatic sintering isostatic sintering by optimizing the mixing ratio, particle size and process parameters of tin dioxide and zinc oxide powders. Tin-zinc ceramic target with high density, low resistivity and high uniformity.
The high density, low resistivity and high uniformity of tin oxide zinc targets are achieved, the preparation efficiency and production stability are improved, the adverse costs are reduced, and the solution to replace indium is provided.
Smart Images

Figure BDA0004992602550000081 
Figure BDA0004992602550000091 
Figure BDA0004992602550000092
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semiconductor target materials, and in particular to a tin zinc oxide ceramic target material and a preparation method thereof. Background Art
[0002] As a good semiconductor material, transparent conductive oxide (TCO) films represented by indium tin oxide (ITO) are widely used in liquid crystal displays, solar cells, gas sensors, energy-saving windows, antistatic coatings, modern fighter jets and cruise missile windows, etc. In recent years, with the vigorous development of the electronics industry, the demand for indium has increased, resulting in a shortage of indium resources and a surge in the price of indium. Therefore, the development of new alternative materials with photoelectric properties comparable to those of ITO films has become an important research topic in the field of materials. SnO2 has stable physical and chemical properties and is easy to form a uniform, dense and chemically stable film. It is an n-type wide bandgap semiconductor with good chemical stability, high optical transmittance and low resistivity. It is widely used in transparent conductive films, solar cells, gas sensors and other related fields.
[0003] Chinese patent application 202410286062.7 discloses a method for preparing a tin oxide zinc target, comprising the following steps: first, mixing, dispersing and grinding zinc oxide powder with a first dispersant to obtain slurry one; then adding tin dioxide powder to the obtained slurry one and mixing, dispersing and grinding with a second dispersant to obtain slurry two; then adding a binder to the obtained slurry two, dispersing and grinding to obtain slurry three; finally, molding, drying, dehydrating, curing, degreasing and sintering slurry three to obtain a tin oxide zinc target.
[0004] In this case, the uniformity of dispersion of various components inside the target material was improved through multiple dispersions of zinc oxide and tin dioxide in the process of preparing the slurry and optimization of the dispersant. At the same time, the density of the target material was improved and the defects inside the target material were reduced through the rational use of the binder.
[0005] Patent CN97108322.3 discloses a method for manufacturing indium oxide / tin oxide sputtering targets, in which isostatic pressing is used during the sintering process, wherein the cold isostatic pressure is 200-280 MPa, the holding time is 10 minutes, the cold isostatic pressing medium is oil, and the rough blank density after cold isostatic pressing is 45-55% of the theoretical density; the hot isostatic pressing temperature is 1100-1300°C, the holding time is 0.5-6 hours, the atmosphere pressure is 100-120 MPa, the hot isostatic pressing medium is argon, and the maximum density of the target material is 96%.
[0006] The technical problem to be solved in this case is: how to propose a method for preparing a high-density tin zinc oxide target. Summary of the invention
[0007] The purpose of the present invention is to provide a method for preparing a tin zinc oxide ceramic target material, and to prepare a sputtering target material with excellent properties such as ultra-high density, low resistivity, high uniformity and stable process through a sand grinding-spray granulation-compression molding-cold isostatic pressing-normal pressure sintering-hot isostatic pressing sintering process.
[0008] To achieve the above object, the present application discloses a method for preparing a tin zinc oxide ceramic target, comprising the following steps:
[0009] Step 1: After mixing tin dioxide powder and zinc oxide powder, pure water, dispersant and binder are added, mixed, stirred and ground to obtain a mixed slurry;
[0010] Step 2: spray-drying and homogenizing the mixed slurry to obtain tin zinc oxide powder;
[0011] Step 3: molding and cold isostatic pressing the tin oxide zinc powder to obtain a tin oxide zinc target blank;
[0012] Step 4: sintering the tin oxide zinc target blank at high temperature to obtain a tin oxide zinc target material;
[0013] Step 5: Load the tin oxide zinc target into the mold, seal, degas, and perform hot isostatic pressing. After removing the mold, the tin oxide zinc ceramic target is obtained.
[0014] Wherein, in step 1, the mass ratio of tin dioxide powder to zinc oxide powder is 90-95:5-10;
[0015] The particle size D50 of the tin zinc oxide powder in step 2 is 0.5-2 μm.
[0016] Preferably, the particle size of the tin dioxide and zinc oxide powders in step 1 is 100 to 300 nm.
[0017] Preferably, the solid content of the mixed slurry in step 1 is 50-70%.
[0018] Preferably, the dispersant in step 1 is selected from at least one of polyvinyl pyrrolidone, polycarboxylic acid compounds, and polyvinyl salts, and the amount of the dispersant added is 5 to 15% of the total mass of the tin dioxide powder and the zinc oxide powder;
[0019] The binder is selected from at least one of polyvinyl alcohol, carboxymethyl cellulose, polyacrylamide, polyacrylic acid salt and polyethylene glycol, and the added amount of the binder is 5-15% of the total mass of the tin dioxide powder and the zinc oxide powder.
[0020] Preferably, the median particle size D50 of the mixed slurry in step 1 is 0.1-0.5 μm.
[0021] Preferably, the molding pressure in step 3 is 30-100 MPa, and the holding time is 10-100 s;
[0022] The cold isostatic pressing pressure in step 3 is 200-400 MPa, and the holding time is 1-10 minutes.
[0023] Preferably, the high temperature sintering operation in step 4 is: firstly heating to 300-600°C at a heating rate of 0.1-0.5°C / min, then heating to 700-1200°C at a heating rate of 1-3°C / min, then heating to 1300-1400°C at a heating rate of 0.5-1°C / min, and keeping warm for 2-15h; finally, cooling to 100°C at a cooling rate of 5-10°C / min, and then naturally cooling to room temperature.
[0024] Preferably, the degassing treatment in step 5 is performed at a temperature of 300 to 700° C. and for a time of 2 to 10 hours;
[0025] The hot isostatic pressing temperature is 1150-1300° C., the pressure is 80-170 MPa, and the heat preservation and pressure holding time is 3-10 hours.
[0026] In addition, a tin-zinc oxide ceramic target is also disclosed, which is prepared by any of the above-mentioned methods for preparing the tin-zinc oxide ceramic target.
[0027] The beneficial effects of the present invention are:
[0028] The present invention provides a method for preparing a tin-zinc oxide ceramic target material. By performing hot isostatic pressing on the tin-zinc oxide target material after normal pressure high-temperature sintering, the problem of poor uniformity of the target material prepared by normal pressure sintering is further improved, thereby achieving the effect of improving preparation efficiency, production stability and reducing bad cost. DETAILED DESCRIPTION
[0029] In the description of the present invention, it should be noted that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0030] Example 1
[0031] Step 1: After mixing tin dioxide powder and zinc oxide powder with a particle size of 200 nm in a mass ratio of 92.5:7.5, pure water, polyvinyl pyrrolidone accounting for 10% of the total mass of the oxide powder, and polyvinyl alcohol accounting for 10% of the total mass of the oxide powder are added, mixed, stirred, and ground to obtain a mixed slurry with a particle size D50 of 0.3 μm and a solid content of 60%;
[0032] Step 2: spray-drying and homogenizing the mixed slurry to obtain tin zinc oxide powder with a median particle size of 1.25 μm;
[0033] Step 3: The tin oxide zinc powder is molded by molding at a molding pressure of 65 MPa and a holding time of 55 seconds, and then is cold isostatically pressed at a pressure of 300 MPa and a holding time of 5 minutes to obtain a tin oxide zinc target blank;
[0034] Step 4: sintering the tin oxide zinc target blank at high temperature, heating it to 450°C at a heating rate of 0.3°C / min, then heating it to 950°C at a heating rate of 2°C / min, and then heating it to 1350°C at a heating rate of 0.7°C / min, and keeping it at this temperature for 8 hours; finally cooling it to 100°C at a cooling rate of 7°C / min, and then naturally cooling it to room temperature to obtain a tin oxide zinc target;
[0035] Step 5: The tin oxide zinc target is loaded into the mold, sealed, degassed at 500°C for 7 hours, and hot isostatically pressed at a temperature of 1225°C and a pressure of 125 MPa for 7 hours. After removing the mold, the tin oxide zinc ceramic target is obtained.
[0036] Example 2
[0037] Step 1: After mixing tin dioxide powder and zinc oxide powder with a particle size of 100 nm in a mass ratio of 92.5:7.5, pure water, polyvinyl pyrrolidone accounting for 15% of the total mass of the oxide powder, and polyvinyl alcohol accounting for 5% of the total mass of the oxide powder are added, mixed, stirred, and ground to obtain a mixed slurry with a particle size D50 of 0.1 μm and a solid content of 50%;
[0038] Step 2: spray-drying and homogenizing the mixed slurry to obtain tin zinc oxide powder with a median particle size of 1.25 μm;
[0039] Step 3: The tin oxide zinc powder is molded by molding at a molding pressure of 30 MPa and a holding time of 100 seconds, and then is cold isostatically pressed at a pressure of 200 MPa and a holding time of 10 minutes to obtain a tin oxide zinc target blank;
[0040] Step 4: sintering the tin oxide zinc target blank at high temperature, heating it to 300°C at a heating rate of 0.1°C / min, then heating it to 700°C at a heating rate of 1°C / min, and then heating it to 1300°C at a heating rate of 0.5°C / min, and keeping it at this temperature for 15 hours; finally cooling it to 100°C at a cooling rate of 5°C / min, and then naturally cooling it to room temperature to obtain a tin oxide zinc target;
[0041] Step 5: The tin oxide zinc target is loaded into the mold, sealed, degassed at 300°C for 10 hours, and hot isostatically pressed at a temperature of 1150°C and a pressure of 80 MPa for 10 hours. After removing the mold, the tin oxide zinc ceramic target is obtained.
[0042] Example 3
[0043] Step 1: After mixing tin dioxide powder and zinc oxide powder with a particle size of 300 nm in a mass ratio of 92.5:7.5, pure water, polyvinyl pyrrolidone accounting for 5% of the total amount of oxide powder, and polyvinyl alcohol accounting for 15% of the total amount of oxide powder are added, mixed, stirred, and ground to obtain a mixed slurry with a particle size of D50 = 0.5 μm and a solid content of 70%;
[0044] Step 2: spray drying and homogenizing the mixed slurry to obtain tin zinc oxide powder with a particle size of 1.25 μm;
[0045] Step 3: The tin oxide zinc powder is molded by molding at a molding pressure of 100 MPa and a holding time of 10 seconds, and then is cold isostatically pressed at a pressure of 400 MPa and a holding time of 1 minute to obtain a tin oxide zinc target blank;
[0046] Step 4: sintering the tin oxide zinc target blank at high temperature, heating it to 600°C at a heating rate of 0.5°C / min, then heating it to 1200°C at a heating rate of 3°C / min, and then heating it to 1400°C at a heating rate of 1°C / min, and keeping it at this temperature for 2 hours; finally cooling it to 100°C at a cooling rate of 10°C / min, and then naturally cooling it to room temperature to obtain a tin oxide zinc target;
[0047] Step 5: The tin oxide zinc target is loaded into the mold, sealed, degassed at 700°C for 2 hours, and hot isostatically pressed at a temperature of 1300°C and a pressure of 170 MPa for 3 hours. After removing the mold, the tin oxide zinc ceramic target is obtained.
[0048] Example 4
[0049] The method is basically the same as Example 1, except that the mass ratio of tin dioxide to zinc oxide powder in step 1 is 90:10.
[0050] Example 5
[0051] The method is basically the same as Example 1, except that the mass ratio of tin dioxide to zinc oxide powder in step 1 is 95:5.
[0052] Example 6
[0053] The method is basically the same as Example 1, except that the mass ratio of tin dioxide to zinc oxide powder in step 1 is 89:11.
[0054] Example 7
[0055] The method is basically the same as Example 1, except that the mass ratio of tin dioxide to zinc oxide powder in step 1 is 96:4.
[0056] Example 8
[0057] The method is basically the same as Example 1, except that the particle size D50 of the tin zinc oxide powder in step 2 is 0.5 μm.
[0058] Example 9
[0059] The method is basically the same as Example 1, except that the particle size D50 of the tin zinc oxide powder in step 2 is 2 μm.
[0060] Example 10
[0061] The method is basically the same as Example 1, except that the particle size D50 of the tin zinc oxide powder in step 2 is 0.4 μm.
[0062] Embodiment 11
[0063] The method is basically the same as Example 1, except that the particle size D50 of the tin zinc oxide powder in step 2 is 2.1 μm.
[0064] Example 12
[0065] It is basically the same as Example 1, except that the maximum temperature of high-temperature sintering in step 4 is 1450°C.
[0066] Example 13
[0067] It is basically the same as Example 1, except that the temperature of hot isostatic pressing in step 5 is 1400°C.
[0068] Comparative Example 1
[0069] Step 1: After mixing tin dioxide powder and zinc oxide powder with a particle size of 200 nm in a mass ratio of 92.5:7.5, pure water, polyvinyl pyrrolidone accounting for 10% of the total amount of oxide powder, and polyvinyl alcohol accounting for 10% of the total amount of oxide powder are added, mixed, stirred, and ground to obtain a mixed slurry with a particle size of D50 = 0.3 μm and a solid content of 60%;
[0070] Step 2: spray drying and homogenizing the mixed slurry to obtain tin zinc oxide powder with a particle size of 1.25 μm;
[0071] Step 3: The tin oxide zinc powder is molded by molding at a molding pressure of 65 MPa and a holding time of 55 seconds, and then is cold isostatically pressed at a pressure of 300 MPa and a holding time of 5 minutes to obtain a tin oxide zinc target blank;
[0072] Step 4: The tin oxide zinc target blank is loaded into a mold, sealed, degassed at 500°C for 7 hours, and hot isostatically pressed at a temperature of 1225°C and a pressure of 125 MPa for 7 hours. After removing the mold, the tin oxide zinc ceramic target is obtained.
[0073] Comparative Example 2
[0074] Step 1: After mixing tin dioxide powder and zinc oxide powder with a particle size of 200 nm in a mass ratio of 92.5:7.5, pure water, polyvinyl pyrrolidone accounting for 10% of the total amount of oxide powder, and polyvinyl alcohol accounting for 10% of the total amount of oxide powder are added, mixed, stirred, and ground to obtain a mixed slurry with a particle size of D50 = 0.3 μm and a solid content of 60%;
[0075] Step 2: spray drying and homogenizing the mixed slurry to obtain tin zinc oxide powder with a particle size of 1.25 μm;
[0076] Step 3: The tin oxide zinc powder is molded by molding at a molding pressure of 65 MPa and a holding time of 55 seconds, and then is cold isostatically pressed at a pressure of 300 MPa and a holding time of 5 minutes to obtain a tin oxide zinc target blank;
[0077] Step 4: sinter the tin oxide zinc target blank at high temperature, heat it to 450°C at a heating rate of 0.3°C / min, then heat it to 950°C at a heating rate of 2°C / min, and then heat it to 1375°C at a heating rate of 0.7°C / min, and keep it at this temperature for 8 hours; finally, cool it to 100°C at a cooling rate of 7°C / min, and then naturally cool it to room temperature to obtain a tin oxide zinc ceramic target.
[0078] Performance Test:
[0079] Test method:
[0080] Density: Archimedean drainage method;
[0081] Resistivity: four-probe measurement method;
[0082] Grain size: metallographic microscopy.
[0083] The test results are shown in Table 1:
[0084] Table 1
[0085]
[0086]
[0087] Conclusion analysis:
[0088] 1. From Examples 1-3, 12-13 and the data in Table 2, it can be seen that:
[0089] Table 2
[0090]
[0091]
[0092] In Examples 1-3, the particle sizes of tin oxide powder and zinc oxide powder, the temperature and holding time during high-temperature sintering and hot isostatic pressing operations were changed during the preparation of tin oxide zinc ceramic targets, which had little effect on the density and conductivity of the target. However, it can be seen from Examples 12 and 13 that when the maximum temperature during high-temperature sintering exceeds 1400°C or the maximum temperature during hot isostatic pressing exceeds 1300°C, the performance of the target is greatly affected, and its relative density is reduced by at least 1.12%, and the resistivity and average grain size are increased by at least 426.827 μΩ·cm and 8.014 μm, respectively.
[0093] 2. It can be seen from Examples 1 and 4-7 that the mass ratio of tin dioxide powder to zinc oxide powder in step 1 in Example 1 is 92.5:7.5;
[0094] In Example 4, the mass ratio of tin dioxide powder to zinc oxide powder in step 1 is 90:10;
[0095] In Example 5, the mass ratio of tin dioxide powder to zinc oxide powder in step 1 is 95:5;
[0096] In Example 6, the mass ratio of tin dioxide powder to zinc oxide powder in step 1 is 89:11;
[0097] In Example 7, the mass ratio of tin dioxide powder to zinc oxide powder in step 1 is 96:4. The experimental data are shown in Table 3:
[0098] Table 3
[0099] Group Relative density / % Resistivity (μΩ·cm) Average grain size (μm) Example 1 99.8 198.721 5.573 Example 4 99.75 241.648 6.019 Example 5 99.73 249.307 6.102 Example 6 97.30 1171.561 25.006 Example 7 97.09 1014.428 21.211
[0100] From the experimental data in Table 3, it can be seen that when the doping amount of zinc oxide is between 5% and 10%, due to the 2+ Radius larger than Sn 4+ radius and the Zn in ZnO during sintering 2+ It will also replace Sn in SnO2 4+ This makes the material sintered densely, further improving the conductive properties of the target material.
[0101] 3. It can be seen from Examples 1 and 8-11 that the particle size D50 of the tin zinc oxide powder in step 2 in Example 1 is 1.25 μm;
[0102] The particle size D50 of the tin zinc oxide powder in step 2 in Example 8 is 0.5 μm;
[0103] The particle size D50 of the tin zinc oxide powder in step 2 of Example 9 is 2 μm;
[0104] The particle size D50 of the tin zinc oxide powder in step 2 of Example 10 is 0.4 μm;
[0105] The particle size D50 of the tin zinc oxide powder in step 2 of Example 11 is 2.5 μm. Combined with the data in Table 4, it can be seen that:
[0106] Table 4
[0107] Group Relative density / % Resistivity (μΩ·cm) Average grain size (μm) Example 1 99.80 198.721 5.573 Example 8 99.70 247.381 5.987 Example 9 99.69 238.269 6.201 Example 10 99.35 461.801 9.422 Embodiment 11 99.27 482.763 9.311
[0108] It can be seen from the data in Table 4 that when the particle size D50 of the tin zinc oxide powder is less than 0.5 μm, the powder particle size is too fine, the smaller particles cannot move freely and have a lower loose density, the friction between the particles is large, and it is difficult to press and form, resulting in poor target density and conductivity. At the same time, when the particle size D50 of the tin zinc oxide powder is greater than 2.0 μm, the powder particle size is larger and the activity is poor, which hinders the sintering process, causes stress concentration at the grain boundary, increases the risk of cracking, and the density of the produced target is lower and the performance is poor.
[0109] 4. It can be seen from Example 1 and Comparative Examples 1-2 that, relative to Example 1, Comparative Example 1 did not perform high-temperature sintering, but only performed hot isostatic pressing;
[0110] In Comparative Example 2, only high temperature sintering was performed, and no hot isostatic pressing was performed. Combining the data in Table 5, it can be seen that:
[0111] Table 5
[0112] Group Relative density / % Resistivity (μΩ·cm) Average grain size (μm) Example 1 99.8 198.721 5.573 Comparative Example 1 98.36 1086.147 21.234 Comparative Example 2 98.18 1198.98 25.332
[0113] It can be seen from the data in Table 5 that in the preparation process of tin zinc oxide ceramic targets, the combination of high temperature sintering operation and hot isostatic pressing operation can greatly improve the relative density and conductivity of the target.
[0114] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a tin zinc oxide ceramic target, characterized in that: The preparation method comprises the following steps: Step 1: After mixing tin dioxide powder and zinc oxide powder, pure water, dispersant and binder are added, mixed, stirred and ground to obtain a mixed slurry; Step 2: spray-drying and homogenizing the mixed slurry to obtain tin zinc oxide powder; Step 3: molding and cold isostatic pressing the tin oxide zinc powder to obtain a tin oxide zinc target blank; Step 4: Sintering the tin oxide zinc target blank at high temperature to obtain a tin oxide zinc target material; Step 5: Load the tin oxide zinc target into the mold, seal, degas, and perform hot isostatic pressing, and remove the mold to obtain the tin oxide zinc ceramic target; Wherein, in step 1, the mass ratio of tin dioxide powder to zinc oxide powder is 90-95:5-10; The particle size D50 of the tin zinc oxide powder in step 2 is 0.5-2 μm.
2. The method for preparing a tin zinc oxide ceramic target according to claim 1, characterized in that: The particle size of the tin dioxide and zinc oxide powders is 100-300 nm.
3. The method for preparing a tin zinc oxide ceramic target according to claim 1, characterized in that: The solid content of the mixed slurry in step 1 is 50-70%.
4. The method for preparing a tin zinc oxide ceramic target according to claim 1, characterized in that: The dispersant in step 1 is selected from at least one of polyvinyl pyrrolidone, polycarboxylic acid compounds, and polyvinyl salts, and the amount of the dispersant added is 5-15% of the total mass of the tin dioxide powder and the zinc oxide powder; The binder is selected from at least one of polyvinyl alcohol, carboxymethyl cellulose, polyacrylamide, polyacrylic acid salt and polyethylene glycol, and the added amount of the binder is 5-15% of the total mass of the tin dioxide powder and the zinc oxide powder.
5. The method for preparing a tin zinc oxide ceramic target according to claim 1, characterized in that: The median particle size D50 of the mixed slurry in step 1 is 0.1-0.5 μm.
6. The method for preparing a tin zinc oxide ceramic target according to claim 1, characterized in that: During the molding process of step 3, the pressure is 30-100 MPa and the holding time is 10-100 s; During the cold isostatic pressing process of step 3, the pressure is 200-400 MPa and the holding time is 1-10 min.
7. The method for preparing a tin zinc oxide ceramic target according to claim 1, characterized in that: The high temperature sintering operation in step 4 is as follows: firstly, the temperature is increased to 300-600°C at a heating rate of 0.1-0.5°C / min, then the temperature is increased to 700-1200°C at a heating rate of 1-3°C / min, then the temperature is increased to 1300-1400°C at a heating rate of 0.5-1°C / min, and the heat preservation time is 2-15h; finally, the temperature is decreased to 100°C at a cooling rate of 5-10°C / min, and then naturally cooled to room temperature.
8. The method for preparing a tin zinc oxide ceramic target according to claim 1, characterized in that: The temperature of the degassing treatment in step 5 is 300-700°C and the time is 2-10h; The hot isostatic pressing temperature is 1150-1300° C., the pressure is 80-170 MPa, and the heat preservation and pressure holding time is 3-10 hours.
9. A tin zinc oxide ceramic target, characterized in that: The target is prepared by the method for preparing the tin zinc oxide ceramic target according to any one of claims 1 to 8.
Citation Information
Patent Citations
Sputtering target and manufacturing method thereof, film obtained by utilizing the target, film sheet and laminating sheet
CN102965628A
High-density AZO target and preparation method thereof
CN104418592A
High-density fine-grain zinc oxide doped tin oxide-based ceramic target material and preparation method thereof
CN113563063A
Preparation method of ITO ceramic target material
CN113735568A
ZTO target material and preparation method thereof
CN116751032A
Cited By
Preparation method of cerium, tantalum and zinc co-doped tin oxide target material
CN120025164A