Preparation method of tough bionic structure ceramic material for fused deposition 3D printing

By introducing graphene and ionic polymers on the surface of ceramic powder and using roller pressing and laser beam heating in melt deposition 3D printing, the problem of preparation of complex structures and high toughness in ceramic melt deposition 3D printing is solved, achieving high flexibility The preparation of ceramic materials with density and complex structures improves the toughness and processing integrity of the material.

CN118930285AActive Publication Date: 2024-11-12CHENGDU AIRCRAFT INDUSTRY GROUP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410980628.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The existing ceramic melt deposition 3D printing technology is difficult to prepare complex structures and high toughness ceramic materials, with low density and complex processes, which limits its application.

Method used

By introducing graphene and ionic polymer on the surface of the sheet ceramic powder, the in-situ covalent bond grafting method is used to modify, and the ceramic materials are arranged in a direction along the rolling direction using a rolling device during the melt deposition 3D printing process. Combined with laser beam heating and sintering treatment, a high toughness ceramic material is formed.

Benefits of technology

It significantly improves the toughness and density of ceramic materials, realizes the preparation of complex structures, overcomes the problems of brittleness and structural singleness of traditional methods, and enhances the strength and toughness and processing integrity of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930285A_ABST
    Figure CN118930285A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a tough bionic structure ceramic material for fused deposition 3D printing, and belongs to the technical field of additive manufacturing. Graphene and an ionic polymer are modified on the surface of flaky ceramic powder, so that the agglomeration and accumulation tendency among the flaky ceramic powder can be inhibited, and the toughness of the ceramic material is improved; the dispersity of the flaky ceramic powder among the alkane printing bonding aids can also be improved, so that the flaky ceramic powder can be oriented under the action of an external field; and meanwhile, graphene introduced in situ is beneficial to improving the strength and toughness of the flaky ceramic powder, the structural integrity of the raw materials in the processing process and the obdurability of the finally sintered ceramic are improved, and the problem that complex components are not easy to prepare in existing ceramic fused deposition 3D printing is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of additive manufacturing and relates to a method for preparing a tough bionic structural ceramic material for fused deposition 3D printing. Background Art

[0002] Ceramics have excellent properties such as high hardness, high strength and high modulus, and are widely used in energy, medical, aerospace and other fields. However, their intrinsic brittleness and crack sensitivity limit their service environment and service life. In recent years, due to the development of bionic technology, various bionic materials prepared based on the microstructure of organisms have emerged. By studying the "brick-mud" multi-level microstructure of shells, crustaceans and other organisms with good impact performance in nature, layered composite ceramics with similar interface structure design have been prepared using bionic technology. Its microstructure is composed of alternating hard layers and soft layers, which prolongs the crack extension path and significantly improves the fracture toughness and energy absorption level of the material. Different from the traditional strengthening and toughening mechanism, the toughening mechanism of layered composite ceramics belongs to the energy absorption and dissipation mechanism. This structural design will reduce the sensitivity of the mechanical properties of the material to defects, making it a defect-resistant material, and greatly improving the fracture toughness of the material. Compared with the traditional strengthening mechanism, the design of layered composite ceramics avoids the problems of the toughening effect being limited by the working environment and the uniform dispersion of the first phase. The toughening effect is much better than the traditional strengthening mechanism, and the fracture work can even be increased by 2-3 orders of magnitude. At present, the hard and soft interlayers of layered composite ceramics are usually prepared by processes such as tape casting, gel injection molding, and rolling film molding. After the hard and soft interlayers are dried, they are stacked together and sintered to prepare layered ceramic composite materials. Although the layered composite ceramics prepared by the above method have high toughness, their structure is usually relatively simple, and it is difficult to prepare ceramic components with complex structures, which greatly limits their application.

[0003] In recent years, emerging additive manufacturing, such as 3D printing technology, is based on the principle of discrete stacking, using automatic control to stack materials layer by layer to achieve rapid manufacturing of complex parts. It has the advantages of flexible structural design, integrated processing and molding, high preparation accuracy, and short preparation cycle, providing a new way to prepare high-performance ceramic parts with complex structures. Among them, fused deposition 3D printing technology is a method of melting various fusible wires or granules by heating, solidifying and molding them layer by layer on the machine printing table to finally obtain a three-dimensional ceramic blank, and then high-temperature degreasing and sintering to obtain the final ceramic part.

[0004] In the additive manufacturing process of ceramic fused deposition 3D printing technology, spherical ceramic powders with higher fluidity are usually selected as raw materials, but this usually ignores the crushing effect of ball milling and other processing processes on the spherical raw materials and the large stacking gaps between spherical particles. Therefore, the prepared ceramics are usually low in densification and brittle. In addition, the preparation process of ceramic materials with high toughness using traditional methods is often complicated and not convenient for preparing ceramic materials with complex and fine structures, so its practical application is often limited.

[0005] Therefore, in view of the above-mentioned defects of the existing ceramic fused deposition 3D printing technology, the present invention discloses a method for preparing a tough bionic structural ceramic material for fused deposition 3D printing. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing tough bionic structural ceramic materials for fused deposition 3D printing. Based on the in-situ covalent bond grafting method, a modification strategy of graphene and ionic polymers is introduced to modify the surface of flaky ceramics. Through the high in-plane toughness of graphene and the repulsive effect between ionic polymers, the orientation degree and toughness of flaky ceramics are further improved, thereby overcoming the difficulty of preparing complex components in existing ceramic fused deposition 3D printing.

[0007] The present invention is achieved through the following technical solutions: The method for preparing a tough bionic structural ceramic material for fused deposition 3D printing comprises the following steps: Step 1: Introducing graphene and ionic polymer on the surface of the flaky ceramic powder by in-situ covalent bond grafting to modify the flaky ceramic powder; Step 2: Mix the modified flaky ceramic powder, sintering aid, printing adhesive, and plasticizer to obtain a wire material, evenly disperse the wire material by solution dispersion, and extrude the wire material to form a printing wire material; Step 3: Using a fused deposition 3D printing device to melt-print the printing filament onto the surface of the part to obtain a primary embryo, and rolling the molten printing filament during the melt printing process so that the flaky ceramic material in the molten printing filament is oriented along the rolling direction; Step 4, defatting the primary embryo to remove the ionic polymer used to assist molding in the primary embryo to obtain a brown body; Step 5: Sintering the brown body to densify the brown body to form a ceramic material.

[0008] In order to better implement the present invention, further, the step 1 specifically includes: Step 1.1, using a silane coupling agent to carry out a condensation reaction with a hydroxyl group on the surface of the flaky ceramic powder, so that the silane coupling agent is grafted onto the surface of the flaky ceramic powder; Step 1.2, adding the flaky ceramic powder to the evenly dispersed graphene oxide solution, so that the graphene oxide is grafted onto the surface of the flaky ceramic powder; Step 1.3, reacting the flaky ceramic powder with a silane coupling agent to introduce vinyl groups on the surface of the flaky ceramic powder, so as to graft double covalent bonds on the surface of the flaky ceramic powder; Step 1.4, adding the flake ceramic powder grafted with double covalent bonds into a solution containing an ionic polymer monomer to perform free radical copolymerization; Step 1.5, reducing the graphene oxide on the surface of the flaky ceramic powder to graphene, and dissociating the flaky ceramic powder in an acidic or alkaline environment to form a polyelectrolyte with positive or negative charge on the surface of the flaky ceramic powder, thereby completing the modification of the flaky ceramic powder.

[0009] In order to better implement the present invention, further, the step 2 specifically includes: Step 2.1, using an organic solvent to dissolve the printing adhesive; Step 2.2, mixing the modified flaky ceramic powder, sintering aid, printing adhesive, and plasticizer to obtain a raw material solution, and ultrasonically dispersing the raw material solution; Step 2.3, filtering, drying, and crushing the dispersed raw material solution to obtain a wire raw material, and refining the wire raw material; Step 2.4: Use a screw extruder to extrude the mixed wire raw material to prepare the printing wire.

[0010] In order to better realize the present invention, further, the volume fraction of the flaky ceramic powder in the raw material solution is 10vol%-70vol%, the ratio of the sintering aid, printing adhesive and plasticizer is 2:1:1; the thickness of the flaky ceramic powder is 10nm-1000nm, the width is 5μm-100μm, and the length is 5μm-100μm.

[0011] In order to better implement the present invention, further, the volume fraction of the flaky ceramic powder in the raw material solution is 50 vol%.

[0012] In order to better implement the present invention, further, the printing adhesive includes any one monomer of polyethylene, polyvinyl acetate, polyethylene glycol, and polyoxyethylene, or a mixture of any two of them.

[0013] In order to better implement the present invention, further, the step 3 specifically includes: Step 3.1, using a laser beam as a heating source, half of the laser beam acts on the printing filament until the printing filament is in a semi-molten state; the other half of the laser beam acts on the surface of the part, and then a fused deposition 3D printing device is used to print the semi-molten printing filament onto the surface of the part; Step 3.2: During the process of laying the printing filament on the surface of the part, a rolling device is used to roll the semi-molten printing filament to roll the printing filament into a flat strip, so that the printing filament is oriented along the rolling direction to obtain a primary embryo.

[0014] In order to better implement the present invention, further, the step 4 specifically includes: Step 4.1, firing the preform in air for a time greater than or equal to 2 hours, a heating rate of 0.5°C / min during the firing process, and a final firing temperature greater than or equal to 600°C; Step 4.2: Continue to increase the temperature at a rate of 2°C / min until the firing temperature is greater than or equal to 1000°C and the firing time is greater than or equal to 2h.

[0015] In order to better implement the present invention, further, in step 5, the temperature is continued to be increased at a heating rate of 4°C / min until the sintering temperature is greater than or equal to 1600°C and the sintering time is greater than or equal to 2h.

[0016] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) The present invention modifies the surface of the flaky ceramic powder with graphene and ionic polymer, which can not only inhibit the agglomeration and accumulation tendency between the flaky ceramic powders, but also improve the dispersibility of the flaky ceramic powders between the alkane printing adhesive additives, thereby facilitating the orientation of the flaky ceramic powders under the action of an external field; at the same time, the in-situ introduced graphene helps to improve the strength and toughness of the flaky ceramic powders, improve the structural integrity of the raw materials during the processing process and the toughness of the final sintered ceramics; (2) The present invention uses a laser beam as a heating source. Half of the laser beam spot acts on the printing filament to make it reach a semi-molten state, and the other half acts on the surface of the formed part, which promotes the penetration of the ends of the resin molecular chains of the formed part between adjacent layers and increases the fluidity of the printing filament. (3) The present invention adds a roller pressing device during the melt printing process, which can make the semi-molten printing wire material be flattened into a strip under the pressure of the roller and bonded to the formed parts. The roller pressing pressure enhances the bonding effect between adjacent wire materials, and is also conducive to the orientation of the sheet ceramics in the molten printing material along the rolling direction, thereby reducing the shrinkage rate in the subsequent sintering, and thus improving the density of the component; (4) The layered composite ceramic materials prepared by the principle of melt 3D additive printing not only have higher toughness, but also can be designed with various complex structures according to service requirements, thereby achieving flexible and efficient customization of target components. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of the steps of the present invention; Figure 2 Schematic diagram of the processing flow of flaky ceramics. DETAILED DESCRIPTION

[0018] The following detailed descriptions are all illustrative and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0019] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the present invention explicitly states otherwise, singular forms are also intended to include plural forms. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0020] For the convenience of description, if the words "up", "down", "left" and "right" appear in the present invention, they only indicate that they are consistent with the up, down, left and right directions of the drawings themselves, and do not limit the structure. They are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present invention.

[0021] Terminology explanation section: The terms "install", "connect", "connect", "fixed" and the like in the present invention should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integrated connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be an internal connection between two elements, or an interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances.

[0022] Embodiment 1: The method for preparing tough bionic structural ceramic materials for fused deposition 3D printing of this embodiment is as follows: Figure 1 As shown, the following steps are included: Step 1: Introducing graphene and ionic polymer on the surface of the flaky ceramic powder by in-situ covalent bond grafting to modify the flaky ceramic powder; Step 2: Mix the modified flaky ceramic powder, sintering aid, printing adhesive, and plasticizer to obtain a wire material, evenly disperse the wire material by solution dispersion, and extrude the wire material to form a printing wire material; Step 3: Using a fused deposition 3D printing device to melt-print the printing filament onto the surface of the part to obtain a primary embryo, and rolling the molten printing filament during the melt printing process so that the flaky ceramic material in the molten printing filament is oriented along the rolling direction; Step 4, defatting the primary embryo to remove the ionic polymer used to assist molding in the primary embryo to obtain a brown body; Step 5: Sintering the brown body to densify the brown body to form a ceramic material.

[0023] Embodiment 2: The method for preparing tough bionic structural ceramic materials for fused deposition 3D printing is improved on the basis of Example 1, wherein step 1 specifically comprises: Step 1.1, using a silane coupling agent to carry out a condensation reaction with a hydroxyl group on the surface of the flaky ceramic powder, so that the silane coupling agent is grafted onto the surface of the flaky ceramic powder; Step 1.2, adding the flaky ceramic powder to the evenly dispersed graphene oxide solution, so that the graphene oxide is grafted onto the surface of the flaky ceramic powder; Step 1.3, reacting the flaky ceramic powder with a silane coupling agent to introduce vinyl groups on the surface of the flaky ceramic powder, so as to graft double covalent bonds on the surface of the flaky ceramic powder; Step 1.4, adding the flake ceramic powder grafted with double covalent bonds into a solution containing an ionic polymer monomer to perform free radical copolymerization; Step 1.5, reducing the graphene oxide on the surface of the flaky ceramic powder to graphene, and dissociating the flaky ceramic powder in an acidic or alkaline environment to form a polyelectrolyte with positive or negative charge on the surface of the flaky ceramic powder, thereby completing the modification of the flaky ceramic powder.

[0024] The other parts of this embodiment are the same as those of Embodiment 1, and thus will not be described in detail.

[0025] Embodiment 3: The method for preparing a tough bionic structural ceramic material for fused deposition 3D printing is improved on the basis of Example 1 or 2, wherein step 2 specifically comprises: Step 2.1, using an organic solvent to dissolve the printing adhesive; Step 2.2, mixing the modified flaky ceramic powder, sintering aid, printing adhesive, and plasticizer to obtain a raw material solution, and ultrasonically dispersing the raw material solution; Step 2.3, filtering, drying, and crushing the dispersed raw material solution to obtain a wire raw material, and refining the wire raw material; Step 2.4: Use a screw extruder to extrude the mixed wire raw material to prepare the printing wire.

[0026] Furthermore, the volume fraction of the flaky ceramic powder in the raw material solution is 10vol%-70vol%, the ratio of the sintering aid, printing adhesive and plasticizer is 2:1:1; the thickness of the flaky ceramic powder is 10nm-1000nm, the width is 5μm-100μm, and the length is 5μm-100μm.

[0027] Furthermore, the volume fraction of the flaky ceramic powder in the raw material solution is 50 vol%.

[0028] Furthermore, the printing adhesive includes any one monomer of polyethylene, polyvinyl acetate, polyethylene glycol, and polyoxyethylene, or a mixture of any two of them.

[0029] The other parts of this embodiment are the same as those of Embodiment 1 or 2, and thus will not be described in detail.

[0030] Embodiment 4: The method for preparing a tough bionic structural ceramic material for fused deposition 3D printing is improved on the basis of any one of embodiments 1-3, wherein step 3 specifically comprises: Step 3.1, using a laser beam as a heating source, half of the laser beam acts on the printing filament until the printing filament is in a semi-molten state; the other half of the laser beam acts on the surface of the part, and then a fused deposition 3D printing device is used to print the semi-molten printing filament onto the surface of the part; Step 3.2: During the process of laying the printing filament on the surface of the part, a rolling device is used to roll the semi-molten printing filament to roll the printing filament into a flat strip, so that the printing filament is oriented and arranged along the rolling direction to obtain a primary embryo. The rolling direction is set along the 3D printing direction, and the rolling particle size is determined by the relative distance between the rolling wheel and the printed part, and the relative distance is determined by the printing layer height in the path planning.

[0031] The other parts of this embodiment are the same as any one of Embodiments 1-3, so they are not described again.

[0032] Embodiment 5: The method for preparing a tough bionic structural ceramic material for fused deposition 3D printing is improved on the basis of any one of embodiments 1-4, wherein step 4 specifically comprises: Step 4.1, firing the preform in air for a time greater than or equal to 2 hours, a heating rate of 0.5°C / min during the firing process, and a final firing temperature greater than or equal to 600°C; Step 4.2: Continue to increase the temperature at a rate of 2°C / min until the firing temperature is greater than or equal to 1000°C and the firing time is greater than or equal to 2h.

[0033] In the step 5, the temperature is continuously increased at a heating rate of 4° C. / min until the sintering temperature is greater than or equal to 1600° C. and the sintering time is greater than or equal to 2 hours.

[0034] The other parts of this embodiment are the same as any one of Embodiments 1-4, so they are not described again.

[0035] Embodiment 6: Preparation method of tough bionic structural ceramic materials for fused deposition 3D printing, such as Figure 2 As shown: Modified flaky ceramic powder: The flaky ceramic powder is made of flaky alumina, and a silane coupling agent (KH550) is used to react with the hydroxyl groups on the surface of the flaky alumina (FC), and the ungrafted silane coupling agent is removed by ultrasonic solvent cleaning. Then, the flaky alumina (FC-KH550) grafted with the silane coupling agent is added to a uniformly dispersed graphene oxide solution to react, so that the graphene oxide is grafted to the surface of the flaky alumina, thereby realizing the grafting of graphene oxide on the surface of the flaky alumina. Then, the flaky alumina (FC-G) grafted with graphene oxide is reacted with a silane coupling agent (KH570), and a reactive vinyl group is introduced on the surface of the flaky alumina (FC-G) grafted with graphene oxide. The flaky alumina grafted with a double covalent bond is added to a solution containing ethyleneimine for free radical copolymerization, so that a large amount of polyethyleneimine is introduced on the surface of the flaky alumina to obtain a flaky alumina (FC-G-PEI) with an ionic polymer on the surface. The graphene oxide on the surface of the flaky alumina with ionic polymer on the surface is partially ionized and reduced to graphene, and the polyethyleneimine is ionized into polyethyleneimine salt using an acidic solution, and finally a modified flaky ceramic powder (FC-G-PEI+) is obtained.

[0036] The solution of the wire raw material includes paraffin wax, polyethylene, and polyvinyl acetate, and the ratio of paraffin wax: polyethylene: polyvinyl acetate is 2:1:1; the volume fraction of the flaky aluminum oxide in the raw material solution is 50 vol%.

[0037] Flake aluminum oxide may also refer to a mixture, in which the ratio of flake aluminum oxide, nano-magnesium oxide, nano-titanium oxide, nano-zirconium oxide and nano-silicon oxide is 1:1:1:1:1. 10% polyvinyl acetate is dissolved in acetone, and flake aluminum oxide is added to the raw material solution for ultrasonic dispersion for 1 hour, and then the dispersion is filtered, dried and crushed; finally, the above raw materials are mixed at 190°C for 2 hours to be fully mixed, and then a twin-screw extruder is used to prepare a printing filament with a diameter of 1.75 mm.

[0038] The prepared printing filaments are converted into embryos using fused deposition 3D printing equipment. The model to be printed is obtained by drawing with MaterialiseMagics software, and then the model is sliced ​​with Cura software. Before printing, the printing filaments need to be tested for printability to determine the appropriate laser beam power and slice thickness. When laying the material, the laser beam is used as the heating source. Half of the laser beam spot acts on the printing filament to make it semi-molten, and half acts on the surface of the formed part, which promotes the penetration of the ends of the resin molecular chains of the formed parts between adjacent layers and increases fluidity. At the same time, the added roller pressing device can make the semi-molten printing filaments flattened into strips under the pressure of the roller and bonded to the formed parts. The pressure of the roller also enhances the bonding effect between adjacent filaments, which is conducive to the orientation of the flake aluminum oxide along the rolling direction, reducing the shrinkage rate in the subsequent sintering and improving the density of the component.

[0039] Degreasing the preform: preferably solvent degreasing followed by high temperature degreasing. First, sinter in air at 600°C for 2 hours, with a heating rate of 0.5°C / min; then, increase the temperature to 1000°C at a rate of 2°C / min, and keep at 1000°C for 2 hours.

[0040] The degreased embryo is sintered at a rate of 4°C / min to 1600°C and maintained for 2 hours. After cooling in the furnace, the target layered alumina ceramics can be obtained.

[0041] The bending strength and fracture toughness of the obtained alumina ceramics are shown in Table 1 below: Table 1. Flexural strength and fracture toughness The above are only preferred embodiments of the present invention and are not intended to limit the present invention in any form. Any simple modifications or equivalent changes made to the above embodiments based on the technical essence of the present invention fall within the protection scope of the present invention.

Claims

1. A method for preparing tough bionic structural ceramic materials for fused deposition 3D printing, characterized in that: The following steps are involved: Step 1: Introducing graphene and ionic polymer on the surface of the flaky ceramic powder by in-situ covalent bond grafting to modify the flaky ceramic powder; Step 2: Mix the modified flaky ceramic powder, sintering aid, printing adhesive, and plasticizer to obtain a wire material, evenly disperse the wire material by solution dispersion, and extrude the wire material to form a printing wire material; Step 3: Using a fused deposition 3D printing device to melt-print the printing filament onto the surface of the part to obtain a primary embryo, and rolling the molten printing filament during the melt printing process so that the flaky ceramic material in the molten printing filament is oriented along the rolling direction; Step 4, defatting the primary embryo to remove the ionic polymer used to assist molding in the primary embryo to obtain a brown body; Step 5: Sintering the brown body to densify the brown body to form a ceramic material.

2. The method for preparing tough bionic structural ceramic material for fused deposition 3D printing according to claim 1, characterized in that: The step 1 specifically includes: Step 1.1, using a silane coupling agent to carry out a condensation reaction with a hydroxyl group on the surface of the flaky ceramic powder, so that the silane coupling agent is grafted onto the surface of the flaky ceramic powder; Step 1.2, adding the flaky ceramic powder to the evenly dispersed graphene oxide solution, so that the graphene oxide is grafted onto the surface of the flaky ceramic powder; Step 1.3, reacting the flaky ceramic powder with a silane coupling agent to introduce vinyl groups on the surface of the flaky ceramic powder, so as to graft double covalent bonds on the surface of the flaky ceramic powder; Step 1.4, adding the flake ceramic powder grafted with double covalent bonds into a solution containing an ionic polymer monomer to perform free radical copolymerization; Step 1.5, reducing the graphene oxide on the surface of the flaky ceramic powder to graphene, and dissociating the flaky ceramic powder in an acidic or alkaline environment to form a polyelectrolyte with positive or negative charge on the surface of the flaky ceramic powder, thereby completing the modification of the flaky ceramic powder.

3. The method for preparing tough bionic structural ceramic material for fused deposition 3D printing according to claim 2, characterized in that: The step 2 specifically includes: Step 2.1, using an organic solvent to dissolve the printing adhesive; Step 2.2, mixing the modified flaky ceramic powder, sintering aid, printing adhesive, and plasticizer to obtain a raw material solution, and ultrasonically dispersing the raw material solution; Step 2.3, filtering, drying, and crushing the dispersed raw material solution to obtain a wire raw material, and refining the wire raw material; Step 2.4: Use a screw extruder to extrude the mixed wire raw material to prepare the printing wire.

4. The method for preparing tough bionic structural ceramic material for fused deposition 3D printing according to claim 3, characterized in that: The volume fraction of the flaky ceramic powder in the raw material solution is 10vol%-70vol%, and the ratio of the sintering aid, printing adhesive, and plasticizer is 2:1:1; the thickness of the flaky ceramic powder is 10nm-1000nm, the width is 5μm-100μm, and the length is 5μm-100μm.

5. The method for preparing tough bionic structural ceramic material for fused deposition 3D printing according to claim 4, characterized in that: The volume fraction of the flaky ceramic powder in the raw material solution is 50 vol%.

6. The method for preparing tough bionic structural ceramic material for fused deposition 3D printing according to claim 5, characterized in that: The printing adhesive includes any one monomer or a mixture of any two of polyethylene, polyvinyl acetate, polyethylene glycol, and polyoxyethylene.

7. The method for preparing a tough bionic structural ceramic material for fused deposition 3D printing according to any one of claims 1 to 6, characterized in that: The step 3 specifically includes: Step 3.1, using a laser beam as a heating source, half of the laser beam acts on the printing filament until the printing filament is in a semi-molten state; the other half of the laser beam acts on the surface of the part, and then a fused deposition 3D printing device is used to print the semi-molten printing filament onto the surface of the part; Step 3.2: During the process of laying the printing filament on the surface of the part, a rolling device is used to roll the semi-molten printing filament to roll the printing filament into a flat strip, and the printing filament is oriented along the rolling direction to obtain a primary embryo.

8. The method for preparing a tough bionic structural ceramic material for fused deposition 3D printing according to any one of claims 1 to 6, characterized in that: The step 4 specifically includes: Step 4.1, firing the preform in air for a time greater than or equal to 2 hours, a heating rate of 0.5°C / min during the firing process, and a final firing temperature greater than or equal to 600°C; Step 4.2: Continue to increase the temperature at a rate of 2°C / min until the firing temperature is greater than or equal to 1000°C and the firing time is greater than or equal to 2h.

9. The method for preparing tough bionic structural ceramic material for fused deposition 3D printing according to claim 8, characterized in that: In the step 5, the temperature is continuously increased at a heating rate of 4° C. / min until the sintering temperature is greater than or equal to 1600° C. and the sintering time is greater than or equal to 2 hours.

Citation Information

Patent Citations

  • Method for making hybrid ceramic / metal, ceramic / ceramic body by using 3D printing process

    CN113526963A

  • Method for preparing high-toughness ceramic material based on photocuring 3D printing

    CN117567139A

  • Layered ceramic based on fused deposition modeling and preparation method thereof

    CN118146002A

  • Three-dimensional (3D) printing

    US20190009465A1