Fluorinated double-carbon synergistically-coated modified ferromanganese polyanionic positive electrode material as well as preparation method and application thereof
By using a fluorinated double-carbon synergistic coating modification method, the problem of insufficient electron transport pathways in polyanionic cathode materials for sodium-ion batteries was solved, improving electronic conductivity and cycle stability, reducing preparation costs, and laying the foundation for the industrialization of sodium-ion batteries.
Patent Information
- Application Number
- CN202411052316.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-15
AI Technical Summary
The lack of electron transport pathways in existing sodium-ion battery polyanion cathode materials leads to poor electrochemical kinetic performance, and existing modification methods are costly and difficult to prepare on a large scale.
A fluorinated dual-carbon synergistic coating modification method is adopted, which combines inorganic and organic carbon sources and uses dry and wet processes to synergistically coat the material surface and bulk phases, forming one-dimensional and three-dimensional conductive carbon network crosslinks to construct a uniform coating layer, and then fluorinates the outer carbon material with NF3 gas.
This significantly improves the electronic conductivity and cycle stability of the material, reduces the manufacturing cost, and enables the widespread application of high-performance sodium-ion battery cathode materials.
Smart Images

Figure CN118954464A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium ion batteries, and specifically relates to a fluorinated double-carbon synergistically coated modified manganese iron polyanion type positive electrode material, and a preparation method and application thereof. Background Art
[0002] Sodium ion battery polyanion compounds refer to compounds with a three-dimensional network structure formed by strong covalent bonds between polyanion polyhedra and transition metal ion polyhedra. This structure enables the material to have excellent ion transmission rate and higher redox voltage than other types of positive electrode materials. Among them, the introduction of some manganese groups enables polyanion-type positive electrode materials to have open three-dimensional channels of polyanion positive electrode materials. At the same time, due to the relatively high redox potential of manganese ions, the material has a wider voltage window.
[0003] However, due to the lack of electron transmission paths caused by phosphate and unstable Mn3+, the electrochemical kinetic performance of this material is poor. Therefore, the existing technology often uses some materials that can significantly improve the kinetic performance to modify it. The existing methods to improve electronic conductivity often use expensive carbon materials for coating, such as rGO, Mxene, carbon nanofibers, single-walled carbon nanotubes, etc. At the same time, the commonly used coating methods are also relatively cumbersome, such as chemical vapor deposition, sol-gel method, solvothermal method, etc., which are costly and cannot be prepared on a large scale. Summary of the invention
[0004] The purpose of the present invention is to provide a fluorinated double-carbon synergistically coated modified manganese iron polyanion positive electrode material and a preparation method and application thereof, so as to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing a fluorinated double-carbon synergistically coated modified manganese iron polyanion positive electrode material comprises the following steps:
[0007] S1. placing an inorganic carbon source in water, stirring and ultrasonically treating the water to obtain a uniform dispersion;
[0008] S2, uniformly mixing the phosphate salt, iron salt, sodium salt and manganese salt according to a certain molar ratio;
[0009] S3, mixing, stirring and ultrasonically treating the solutions in steps S1 and S2 to obtain a uniform and stable solution;
[0010] S4, drying the raw materials obtained in S3 to obtain a powdery mixed precursor;
[0011] S5, heat treating the powdery mixed precursor obtained in S4 under an inert reducing atmosphere;
[0012] S6. Evenly mix the sample heat-treated in S5 with an organic carbon source, perform a secondary heat treatment under an inert atmosphere, collect the heat-treated product, and obtain a powder sample.
[0013] Preferably, in S6, the secondary heat treatment is specifically a fluorination treatment, and the material is placed in a NF3 atmosphere for annealing, the annealing temperature is 250-330°C, and the annealing time is 5-25min.
[0014] Preferably, in S1, the inorganic carbon source is at least one of carbon nanotubes, graphene, carbon spheres, carbon nanofibers, and acetylene black.
[0015] Preferably, in S2, the phosphate salt is at least one of sodium dihydrogen phosphate, sodium pyrophosphate, sodium hydrogen phosphate, and sodium phosphate, preferably sodium dihydrogen phosphate;
[0016] The iron salt is one or a mixture of two or more of reduced iron powder, ferric nitrate, and ferrous oxalate, preferably ferric nitrate;
[0017] The sodium salt is one or a mixture of two or more of sodium dihydrogen phosphate, sodium pyrophosphate, sodium hydrogen phosphate, and sodium phosphate, preferably sodium dihydrogen phosphate;
[0018] The manganese salt is one or a mixture of two or more of manganese nitrate hydrate, manganese acetate and manganese dioxide, and is preferably manganese nitrate hydrate.
[0019] Preferably, in S2, the molar ratio of sodium element, iron element and phosphorus element in the sodium source, iron source, manganese source and phosphorus source is 2:0-3:0-3:4, preferably 2:1:2:4.
[0020] Preferably, in S3, the ultrasonic treatment is performed using a cell crusher for 15-45 min, preferably 30 min.
[0021] Preferably, in S4, the drying method is spray drying, room temperature solvent evaporation and ball milling, preferably spray drying; the feed temperature is 230-290°C, preferably 260°C.
[0022] Preferably, in said S5, the inert reducing atmosphere is one or more of argon, hydrogen, and argon-hydrogen mixed gas (95:5), preferably argon-hydrogen mixed gas (95:5);
[0023] The heat treatment is divided into three steps: pre-sintering, high temperature calcination and organic carbon source coating:
[0024] Pre-sintering process: heating rate 2℃ / min, pre-sintering temperature 250-400℃, preferably 350℃; heat preservation time 3-10h, preferably 6h; cooling is furnace cooling;
[0025] High temperature calcination process: heating rate 1-5°C / min, preferably 5°C / min; temperature 500-650°C, preferably 620°C; insulation time 10-14h, preferably 12h; cooling is furnace cooling;
[0026] Organic carbon source coating calcination process: heating rate 1-5°C / min, preferably 2°C / min; temperature 450-650°C, preferably 500°C.
[0027] Preferably, in S6, the organic carbon source is at least one of glucose, starch, ascorbic acid, sucrose, tannic acid, biomass carbon, methanol, acetic acid, sodium acetate, methanol, preferably ascorbic acid;
[0028] The total carbon source accounts for 5-15 wt.% in the material, preferably 10%.
[0029] A fluorinated double carbon synergistically coated modified manganese iron polyanion type positive electrode material, wherein the fluorinated double carbon synergistically coated modified manganese iron polyanion type positive electrode material is prepared by the fluorinated double carbon synergistically coated modified manganese iron polyanion type positive electrode material preparation method as described in any one of the above items, and its molecular formula is Na4Mn x Fe 3-x (PO4)2(P2O7)@CNTs@CF.
[0030] Preferably, the positive electrode material is particles with an average particle size of 50 nm-10 μm, preferably 3-5 μm.
[0031] Application of a fluorinated double-carbon synergistically coated modified manganese iron polyanion positive electrode material in the preparation of a sodium ion battery positive electrode sheet comprises the following steps:
[0032] (1) Weigh the following components by mass: 70 parts of fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material, 20 parts of acetylene black, and 10 parts of a binder, wherein the mass ratio of fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material: conductive carbon black: binder is 7:2:1;
[0033] (2) dissolving the fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material, acetylene black and a binder in N-methylpyrrolidone, controlling the solid content to 12%-14%, preferably 14%, to adjust the slurry viscosity, and mixing them evenly under dry conditions to prepare a fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode slurry;
[0034] (3) coating on treated aluminum foil and drying at 120° C. for 12 h to obtain a fluorinated double carbon synergistically coated modified manganese iron polyanion type positive electrode material positive electrode sheet;
[0035] In an argon glove box, the dried electrode was cut into discs with a diameter of 12 mm and assembled into a button-type half-cell. In this assembly, the metal sodium sheet was used as the negative electrode. Subsequently, the electrochemical performance of the obtained fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode sheet was tested, in which the sodium sheet was used as the negative electrode. The electrolyte used was 1 molL -1 The sodium salt of NaClO4 was dissolved in a solution of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1, and an additional 5% fluoroethylene carbonate (FEC) additive was added. During the electrochemical performance test, the charge and discharge temperature was room temperature (25°C) and the current 1C was 129mA / g.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] (1) By combining organic carbon sources with inorganic dual carbon sources and dry methods with wet methods, the material is synergistically coated in both the bulk and surface phases, effectively improving the electronic conductivity of the polyanion positive electrode material.
[0038] (2) The preparation method of the present invention does not use expensive conductive carbon materials as modified materials, and the process used does not require high-energy consumption and high-demand equipment and processes. It has high economic cost performance, the entire reaction is easy to control and environmentally friendly, the product does not require post-processing, and large-scale production does not need to consider environmental impact.
[0039] (3) The present invention strictly and synergistically controls the concentration ratio of the two carbon sources, reaction temperature and other parameters, and fully utilizes the cross-linking of one-dimensional and three-dimensional conductive carbon networks to construct an all-round, three-dimensional uniform coating layer, providing a "high-speed channel" for the transmission of electrons and significantly improving the electronic conductivity of the material.
[0040] (4) The calcination temperature affects the graphitization degree of the carbon source, and the carbon coating with higher graphitization is beneficial to inhibit the agglomeration and agglomeration of the microparticles, while inhibiting the corrosion of the electrolyte on the electrolytic surface material under high pressure, improving the thermal stability and chemical stability of the iron-based phosphate composite particles, and effectively improving the cycle performance and rate performance of the iron-phosphate composite material.
[0041] (5) The addition ratio of organic and inorganic carbon sources has no effect on the structure of the material, but the conductive network coating layer formed by it directly affects the electronic conductivity and ionic conductivity of the material, further affecting its performance as a positive electrode material for sodium ion batteries.
[0042] (6) The outer carbon coating layer is tightly coated on the surface of the material through electrostatic coupling, which effectively buffers the volume expansion during the charge and discharge process, and further inhibits the Jahn-Te ller effect of the manganese iron phosphate polyanion / carbon composite material. It also effectively inhibits the corrosion of the electrolyte on the electrode material and the dissolution of manganese, reduces capacity loss, and significantly improves the cycle stability.
[0043] (7) The outer carbon coating layer is fluorinated by using fluorine gas produced by high-temperature decomposition of NF3 gas. Since fluorine has the strongest electronegativity, its introduction into carbon materials can further improve the conductivity of carbon materials and further improve the electrochemical activity of carbon materials.
[0044] (8) The material prepared by the present invention can exhibit excellent performance when used as a positive electrode material for sodium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 is the XRD pattern of the present invention;
[0046] Figure 2 It is a low-power scanning electron microscope image of the present invention;
[0047] Figure 3 It is a low-magnification transmission electron microscope image of the present invention;
[0048] Figure 4 This is a cycle curve diagram of the button cell in Example 4 of the present invention at a rate of 0.5C;
[0049] Figure 5 This is a charge and discharge curve diagram of the button cell in Example 4 of the present invention at a rate of 0.1C. DETAILED DESCRIPTION
[0050] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0051] Embodiment 1:
[0052] See also Figure 1-Figure 5 As shown, a method for preparing a fluorinated double carbon synergistically coated modified manganese iron polyanion type positive electrode material comprises the following steps:
[0053] S1. placing an inorganic carbon source in water, stirring and ultrasonically treating the water to obtain a uniform dispersion;
[0054] S2, uniformly mixing the phosphate salt, iron salt, sodium salt and manganese salt according to a certain molar ratio;
[0055] S3, mixing, stirring and ultrasonically treating the solutions in steps S1 and S2 to obtain a uniform and stable solution;
[0056] S4, drying the raw materials obtained in S3 to obtain a powdery mixed precursor;
[0057] S5, heat treating the powdery mixed precursor obtained in S4 under an inert reducing atmosphere;
[0058] S6. Evenly mix the sample heat-treated in S5 with an organic carbon source, perform a secondary heat treatment under an inert atmosphere, collect the heat-treated product, and obtain a powder sample.
[0059] As can be seen from the above, when preparing the fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material, first prepare 30ml of 5mg / ml uniform graphene dispersion, take 1.5mmol ferric nitrate nine hydrate, 1mol citric acid, 2mmol anhydrous sodium dihydrogen phosphate, dissolve in the dispersion and ultrasonicate until the solution is uniform. After spray drying, the precursor powder is obtained. The precursor powder is placed in a tubular furnace, and an argon hydrogen mixture (95:5) is passed through the furnace. It is heated to 300℃ at a heating rate of 2℃ / min, kept warm for 6 hours, and then heated to 500℃ and kept warm for 10 hours. After cooling with the furnace, take 100mg of the material and 5mg of glucose (C6H 12 After being uniformly mixed with O6), the mixture was heated to 500°C in the above atmosphere and kept at this temperature for 2 hours, then cooled with the furnace, and NF3 gas was introduced and heated to 300°C for 10 minutes to obtain the desired Na4Fe3(PO4)2P2O7@rGO@CF positive electrode composite material.
[0060] Embodiment 2:
[0061] When preparing the modified manganese iron polyanion positive electrode material with fluorinated double carbon synergistic coating, prepare 30 ml of 5 mg / ml uniform carbon ball dispersion, take 1.125 mmol ferric nitrate nine hydrate, 0.375 mol manganese acetate, 1 mol citric acid, 2 mmol anhydrous sodium dihydrogen phosphate, dissolve in the dispersion and ultrasonicate until the solution is uniform. After spray drying, the precursor powder is obtained. The precursor powder is placed in a tubular furnace, and an argon-hydrogen mixed gas (95:5) is passed through the furnace. It is heated to 320°C at a heating rate of 2°C / min, and then heated to 550°C for 10 hours after being kept warm for 6 hours. After cooling with the furnace, the obtained material is mixed with 5wt.% starch (C6H 10 O5) n After uniform mixing, the mixture was heated to 500°C in the above atmosphere again, kept at this temperature for 2 hours, cooled with the furnace, and then NF3 gas was introduced and heated to 250°C for 5 minutes to obtain the desired Na4Fe 2.25 Mn 0.75 (PO4)2P2O7@Carbonspheres@CF positive electrode composite material.
[0062] Embodiment three:
[0063] When preparing the modified manganese iron polyanion positive electrode material with fluorinated double carbon synergistic coating, prepare 30ml of 5mg / ml uniform Mxene dispersion, prepare 30ml of 5mg / ml uniform carbon ball dispersion, take 0.75mmo l ferric nitrate nine hydrate, 0.75mmo l manganese acetate, 1mmo l citric acid, 2mmo l anhydrous sodium dihydrogen phosphate, and disperse the solution and ultrasonicate until the solution is uniform. After spray drying, the precursor powder is obtained. The precursor powder is placed in a tubular furnace, and an argon-hydrogen mixed gas (95:5) is passed through the furnace. It is heated to 330℃ at a heating rate of 2℃ / min, kept warm for 6 hours, and then heated to 600℃ and kept warm for 10 hours. After cooling with the furnace, the obtained material is mixed with 5wt.% sucrose (C 12 H 22 O 11 ) were uniformly mixed and heated to 500°C in the above atmosphere again, kept warm for 2 hours, and then cooled with the furnace, and then NF3 gas was introduced and heated to 300°C for 15 minutes to obtain the desired Na4Fe 1.5 Mn 1.5 (PO4)2P2O7@MXene@CF positive electrode composite material.
[0064] Embodiment 4:
[0065] When preparing the modified manganese iron polyanion positive electrode material with fluorinated double carbon synergistic coating, prepare 30ml of 5mg / ml uniform CNTs dispersion, take 0.375mmol ferric nitrate nine hydrate, 1.125mol manganese acetate, 1mol citric acid, 2mmol anhydrous sodium dihydrogen phosphate, and disperse the solution and ultrasonicate until the solution is uniform. After spray drying, the precursor powder is obtained. The precursor powder is placed in a tubular furnace, and an argon-hydrogen mixed gas (95:5) is passed through the furnace. It is heated to 350℃ at a heating rate of 2℃ / min, kept warm for 6 hours, and then heated to 620℃ and kept warm for 10 hours. After cooling with the furnace, the obtained material is uniformly mixed with 5wt.% ascorbic acid (C6H8O6) and heated to 500℃ in the above atmosphere again. After keeping warm for 2 hours, it is cooled with the furnace, and then NF3 gas is passed through and heated to 300℃ for reaction for 20min to obtain the required Na4Fe 0.75 Mn 2.25 (PO4)2P2O7@CNTs@CF positive electrode composite material.
[0066] Embodiment five:
[0067] When preparing the modified manganese iron polyanion positive electrode material with fluorinated double carbon synergistic coating, prepare 30 ml of 5 mg / ml uniform CNFs dispersion, take 1.5 mol manganese acetate, 1 mol citric acid, 2 mmol anhydrous sodium dihydrogen phosphate, and dissolve them in deionized water. After spray drying, the precursor powder is obtained. The precursor powder is placed in a tubular furnace, and an argon-hydrogen mixture (95:5) is passed through the furnace. It is heated to 400°C at a heating rate of 2°C / min, and then heated to 650°C for 10 hours. After cooling with the furnace, the obtained material is mixed with 5wt.% tannic acid (C 76 H 52 O 46 ) were uniformly mixed and heated to 500°C in the above atmosphere again, kept warm for 2 hours, and then cooled with the furnace. NF3 gas was introduced and heated to 320°C for reaction for 25 minutes to obtain the desired Na4Mn3(PO4)2P2O7@CNFs@CF positive electrode composite material.
[0068] Embodiment six:
[0069] When preparing the modified manganese iron polyanion positive electrode material with fluorinated double carbon synergistic coating, prepare 30ml of 5mg / ml uniform CNTs dispersion, take 0.375mmo l ferric nitrate nine hydrate, 1.125mmo l manganese acetate, 1mmo l citric acid, 2mmo l anhydrous sodium dihydrogen phosphate, and disperse the solution and ultrasonicate until the solution is uniform. After spray drying, the precursor powder is obtained. The precursor powder is placed in a tubular furnace, and an argon-hydrogen mixed gas (95:5) is passed through the furnace. It is heated to 350℃ at a heating rate of 2℃ / min, kept warm for 6 hours, and then heated to 620℃ and kept warm for 10 hours. After cooling with the furnace, the obtained material is uniformly mixed with 5wt.% ascorbic acid (C6H8O6) and heated to 500℃ in the above atmosphere again. After keeping warm for 2 hours, it is cooled with the furnace to obtain the required Na4Fe 0.75 Mn 2.25 (PO4)2P2O7@CNTs@C positive electrode composite material.
[0070] Embodiment seven:
[0071] When preparing the modified manganese iron polyanion positive electrode material with fluorinated double carbon synergistic coating, prepare 30 ml of 5 mg / ml uniform carbon ball dispersion, take 1.125 mmol ferric nitrate nine hydrate, 0.375 mol manganese acetate, 1 mol citric acid, 2 mmol anhydrous sodium dihydrogen phosphate, dissolve in the dispersion and ultrasonicate until the solution is uniform. After spray drying, the precursor powder is obtained. The precursor powder is placed in a tubular furnace, and an argon-hydrogen mixed gas (95:5) is passed through the furnace. It is heated to 320°C at a heating rate of 2°C / min, and then heated to 550°C for 10 hours after being kept warm for 6 hours. After cooling with the furnace, the obtained material is mixed with 5wt.% starch (C6H 10O5) n After uniform mixing, the mixture was heated to 500°C in the above atmosphere again and kept at this temperature for 2 hours, and then cooled in the furnace to obtain the desired Na4Fe 2.25 Mn 0.75 (PO4)2P2O7@Carbon spheres@C positive electrode composite material.
[0072] Comparative Example 1:
[0073] Take 0.375 mmol of ferric nitrate nonahydrate, 1.125 mol of manganese acetate, 1 mol of citric acid, 2 mmol of anhydrous sodium dihydrogen phosphate, and disperse the solution by ultrasound until the solution is uniform. After spray drying, the precursor powder is obtained. The precursor powder is placed in a tubular furnace, and an argon-hydrogen mixture (95:5) is passed through the furnace. It is heated to 350°C at a heating rate of 2°C / min, kept warm for 6 hours, and then heated to 620°C and kept warm for 10 hours. After cooling with the furnace, the obtained material is evenly mixed with 5wt.% ascorbic acid (C6H8O6) and heated to 500°C in the above atmosphere again. After keeping warm for 2 hours, it is cooled with the furnace, and then NF3 gas is passed through and heated to 300°C for reaction for 20 minutes to obtain the required Na4Fe 0.75 Mn 2.25 (PO4)2P2O7@CF positive electrode composite material.
[0074] Comparative Example 2:
[0075] Prepare 30ml of 5mg / ml uniform CNTs dispersion, take 0.375mmol iron nitrate nonahydrate, 1.125mol manganese acetate, 1mol citric acid, 2mmol anhydrous sodium dihydrogen phosphate, and disperse the solution and ultrasonicate until the solution is uniform. After spray drying, the precursor powder is obtained. The precursor powder is placed in a tubular furnace, and an argon-hydrogen mixture (95:5) is passed through the furnace. It is heated to 350℃ at a heating rate of 2℃ / min, kept warm for 6 hours, and then heated to 620℃ and kept warm for 10 hours. After cooling with the furnace, NF3 gas is passed and heated to 300℃ for reaction for 20min to obtain the required Na4Fe 0.75 Mn 2.25 (PO4)2P2O7@CF positive electrode composite material.
[0076] Test example 1:
[0077] The composite positive electrode materials prepared in Example 1, Example 4, Example 6 and Comparative Example 1 and Comparative Example 2 were subjected to X-ray diffraction test. The XRD spectrum is shown in FIG. Figure 1 As shown. Figure 1It can be seen from the XRD spectrum in that all the above positive electrode composite materials correspond to the Pn21a space group, and all diffraction peaks can be well matched with the PDF standard card: PDF#89-0579. No obvious impurity diffraction peaks are observed, and the crystallinity is good, which indicates that the Mn element partially replaces the Fe position, a certain carbon layer is coated, and fluorination does not affect the crystal structure of the material. This result shows that this experimental method can prepare a single-phase and well-crystalline fluorinated double-carbon synergistically coated modified manganese iron polyanion positive electrode material.
[0078] Test Example 2:
[0079] The Na4Fe 0.75 Mn 2.25 The morphology of (PO4)2P2O7@CNTs@CF composite cathode material was observed by scanning electron microscopy. Figure 2 As shown, the material appears as hollow spherical particles with a size between 3-5 μm and an obvious carbon coating layer outside the sphere, indicating that the preparation method can synthesize a fluorinated double-carbon synergistically coated modified manganese iron polyanion positive electrode material with a relatively uniform and concentrated carbon layer coating.
[0080] Test Example 3:
[0081] The Na4Fe 0.75 Mn 2.25 The morphology of (PO4)2P2O7@CNTs@CF composite cathode material was observed by transmission electron microscopy. Figure 3 As shown, except for Figure 2 In addition to the same hollow spherical structure, CNTs can be clearly observed in the outer carbon coating layer, indicating that the preparation method can synthesize a fluorinated double-carbon synergistically coated modified manganese iron polyanion positive electrode material uniformly coated with a one-dimensional combined with a three-dimensional conductive network.
[0082] Test Example 4:
[0083] The battery prepared in Example 4 was subjected to charge and discharge tests. The button-type half-cell was used as the main battery, the current 1C was 129 mA / g, and the charge and discharge temperature was room temperature (25° C.). Figure 4 The figure shows the 0.5C cycle curve of the button cell assembled in Example 4. The test voltage range is 1.8-4.2V. The initial discharge capacity of the cycle is 118.7mAh / g. After 50 cycles, the discharge capacity is 106.1mAh / g, and the capacity retention rate is 90.1%.
[0084] Test Example 5:
[0085] The button cell prepared in Example 4 was subjected to a charge and discharge test, with a current of 1C of 129 mA / g and a charge and discharge temperature of room temperature. Figure 5The figure shows the charge and discharge curve of the button cell assembled in Example 4. The charge and discharge current is 0.1C, and the charge and discharge voltage range is 1.8-4.2V. As can be seen from the figure, during the entire charge and discharge process, the charge and discharge curve is smooth and complete, indicating that the battery can be charged and discharged well; the discharge specific capacity can be as high as 128.75mAh / g. The above data show that the fluorinated double-carbon synergistically coated modified manganese iron polyanion positive electrode material has a discharge specific capacity close to the theoretical capacity.
[0086] Test Example 6:
[0087] The button cell prepared in Example 4 was subjected to charge and discharge tests. The current 1C was 129mA / g, and the charge and discharge temperature was room temperature. The charge and discharge current was 0.1C, and the charge and discharge voltage range was 1.8-4.2V. The discharge energy density can be as high as 389.4mWh / g. The above data show that the fluorinated double-carbon synergistically coated modified manganese iron polyanion positive electrode material has a higher energy density.
[0088] The specific test results are as follows:
[0089]
[0090] From the above, it can be seen that the fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material provided by the present invention effectively improves the electronic conductivity of the material while ensuring that the material structure and performance are not affected. Among them, the organic carbon source is combined with the inorganic double carbon source, and the dry method is combined with the wet method to synergistically coat the material in the bulk and surface phases, effectively improving the electronic conductivity of the polyanion positive electrode material; taking the improvement of the electrochemical performance of the battery as the starting point, the coating thickness and type are regulated, so that the obtained positive electrode material can improve the cycle stability while meeting the conventional performance of sodium ion batteries, providing a new idea for the development of high-performance, long-life, high-energy density polyanion sodium ion battery positive electrode materials;
[0091] The present invention provides a method for preparing the above-mentioned fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material. In the method, an inorganic carbon source is introduced in the precursor raw material mixing stage, and after electrostatic pre-adsorption and uniform cross-linking with the material, a precursor is prepared by spray drying, and low-temperature sintering is performed to form a pure phase compound, and then after mechanical mixing with an organic carbon source, heat treatment and carbonization are performed to form a surface core-shell coating layer. The preparation method does not use expensive conductive carbon materials as modified materials, and the process used does not set high-energy consumption and high-demand equipment and processes, and has high economic cost performance;
[0092] The present invention provides a method for fluorinating the carbon layer on the surface of the modified manganese iron polyanion positive electrode material by using fluorine gas generated by high-temperature decomposition of NF3 gas. Since the electronegativity of fluorine element is the strongest, its introduction into carbon material can further improve the conductivity of carbon material, change the electronic configuration and atomic structure of carbon atoms and their surrounding atoms, and improve the electrochemical activity of carbon material. Since the sodium ion battery prepared based on the above material has been tested, its operating voltage can reach about 4.2V, its capacity and energy density are high, and its cycle stability is good, which lays a foundation for promoting the industrialization of sodium ion batteries.
[0093] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material, characterized in that: The following steps are involved: S1. placing an inorganic carbon source in water, stirring and ultrasonically treating the water to obtain a uniform dispersion; S2, uniformly mixing the phosphate salt, iron salt, sodium salt and manganese salt according to a certain molar ratio; S3, mixing, stirring and ultrasonically treating the solutions in steps S1 and S2 to obtain a uniform and stable solution; S4, drying the raw materials obtained in S3 to obtain a powdery mixed precursor; S5, heat treating the powdery mixed precursor obtained in S4 under an inert reducing atmosphere; S6. Evenly mix the sample heat-treated in S5 with an organic carbon source, perform a secondary heat treatment under an inert atmosphere, collect the heat-treated product, and obtain a powder sample.
2. The method for preparing a fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material according to claim 1, characterized in that: In S6, the secondary heat treatment is specifically a fluorination treatment, and the material is placed in a NF3 atmosphere for annealing, the annealing temperature is 250-330°C, and the annealing time is 5-25min.
3. The method for preparing a fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material according to claim 1, characterized in that: In S1, the inorganic carbon source is at least one of carbon nanotubes, graphene, carbon spheres, carbon nanofibers, and acetylene black.
4. The method for preparing a fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material according to claim 1, characterized in that: In S2, the phosphate salt is at least one of sodium dihydrogen phosphate, sodium pyrophosphate, sodium hydrogen phosphate, and sodium phosphate; The iron salt is one or a mixture of two or more of reduced iron powder, ferric nitrate and ferrous oxalate; Sodium salt is one or a mixture of two or more of sodium dihydrogen phosphate, sodium pyrophosphate, sodium hydrogen phosphate, and sodium phosphate; The manganese salt is one or a mixture of two or more of manganese nitrate hydrate, manganese acetate and manganese dioxide.
5. The method for preparing a fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material according to claim 1, characterized in that: In S2, the molar ratio of sodium element, iron element and phosphorus element in the sodium source, iron source, manganese source and phosphorus source is 2:0-3:0-3:
4.
6. The method for preparing a fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material according to claim 1, characterized in that: In said S5, the inert reducing atmosphere is one or more of argon, hydrogen, and argon-hydrogen mixed gas (95:5); The heat treatment is divided into three steps: pre-sintering, high temperature calcination and organic carbon source coating: Pre-burning process: heating rate 2℃ / min, pre-burning temperature 250-400℃, insulation time 3-10h, cooling with the furnace; High temperature calcination process: heating rate 1-5℃ / min, temperature 500-650℃, insulation time 10-14h, cooling with the furnace; Organic carbon source coating calcination process: heating rate 1-5°C / min, temperature 450-650°C.
7. The method for preparing a fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material according to claim 1, characterized in that: In S6, the organic carbon source is at least one of glucose, starch, ascorbic acid, sucrose, tannic acid, biomass carbon, methanol, acetic acid, sodium acetate, methanol, etc.; The total carbon source accounts for 5-15 wt.% in the material.
8. A fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material, characterized in that: The fluorinated double carbon synergistically coated modified manganese iron polyanion type positive electrode material is prepared by the fluorinated double carbon synergistically coated modified manganese iron polyanion type positive electrode material preparation method according to any one of claims 1 to 7, and its molecular formula is Na4Mn x Fe 3-x (PO4)2(P2O7)@CNTs@CF.
9. The fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material according to claim 7, characterized in that: The positive electrode material is particles with an average particle size of 50nm-10μm.
10. An application of the fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material as claimed in claim 7 in the preparation of a positive electrode sheet for a sodium ion battery, characterized in that: The following steps are involved: (1) Weigh the following components by mass: 70 parts of fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material, 20 parts of acetylene black, and 10 parts of a binder, wherein the mass ratio of fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material: conductive carbon black: binder is 7:2:1; (2) dissolving the fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material, acetylene black and a binder in N-methylpyrrolidone, controlling the solid content to 12%-14%, preferably 14%, to adjust the slurry viscosity, and mixing them evenly under dry conditions to prepare a fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode slurry; (3) The mixture is coated on treated aluminum foil and dried at 120° C. for 12 h to obtain a fluorinated double carbon synergistically coated modified manganese iron polyanion positive electrode material positive electrode sheet.
Citation Information
Patent Citations
Carbon-coated sodium ferrous fluorophosphate material, preparation thereof and application of carbon-coated sodium ferrous fluorophosphate material in sodium ion battery
CN114914413A
Dual-carbon modified iron-manganese-based mixed phosphate microsphere material as well as preparation method and application thereof
CN117613227A
Polyanionic sodium ion battery positive electrode material, preparation method thereof and sodium ion battery
CN118213494A
Cited By
Composite carbon-coated sodium ferrous sulfate positive electrode material as well as preparation method and application thereof
CN120413642A
Sodium ion positive electrode material and preparation method and application thereof
CN120497314A