Metal halide luminescent material and preparation method and application thereof
By heating the reaction of tetraethylammonium halide and cuprous halide in the polytetrafluoroethylene inner liner, a metal halide luminescent material of (TEA) 2Cu2Xy type was prepared, which solved the difference in color development index and materials in existing solid-state lighting devices. The high cost problem achieves high color rendering index and low cost single-component white light emission, suitable for natural white LED applications.
Patent Information
- Application Number
- CN202410964341.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-18
AI Technical Summary
Among existing solid-state lighting devices, the color rendering index of phosphor is poor, the emission efficiency is low, and it relies on rare earth dopants and high-temperature sintering processes, resulting in high cost, supply difficulties and environmental problems, making it difficult to achieve a single group with high color rendering index. Split white light emitting material.
By heating and reacting tetraethylammonium halide with cuprous halide in a polytetrafluoroethylene inner liner, a metal halide luminescent material of (TEA) 2Cu2Xy type is prepared, and the emission spectrum is adjustable in the visible light area is achieved, and the A single component white light crystal (TEA) 2Cu2Br2Cl2 with excellent color development index is used to prepare white light emitting devices.
It achieves ultra-wideband single-component white light emission with a high color rendering index (CRI up to 95). The material does not contain rare earth elements. It has a simple preparation process and low cost. It is suitable for large-scale industrial production and has good thermal stability.
Smart Images

Figure CN118930440A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of luminescent materials, and in particular relates to a metal halide luminescent material and a preparation method and application thereof. Background Art
[0002] It is estimated that artificial lighting accounts for about 20% of global electricity consumption and is a significant contributor to carbon dioxide (CO2) emissions, accounting for about 6% of global CO2 emissions. With the development of urbanization worldwide, emissions are further increasing. Therefore, the development of efficient and energy-saving light-emitting materials and devices is imminent. Current solid-state lighting (SSL) devices are usually composed of blue InGaN light-emitting diode (LED) chips combined with (YAG:Ce 3+ ) yellow phosphor or ultraviolet (UV) LED chips combined with a mixture of blue, green and red phosphors. Although these strategies have become mainstream in the lighting market, there are still serious bottlenecks in practical applications. 3+ Due to the lack of red emission in the phosphors, the white light emitted by the blue LEDs they are coated with has a poor color rendering index (CRI) (CRI < 80). Although multi-component phosphors have a high color rendering index, their emission efficiency is low due to the influence of self-absorption. In addition, the degradation rates of phosphors are different, causing the emission spectra of multi-phosphors to change over time. In addition, almost all commercial phosphors rely on rare earth dopants and high-temperature sintering processes, which leads to potential cost, supply and environmental issues. Therefore, exploring new single-component white light emitting materials based on earth-abundant elements is of great significance for next-generation SSL applications.
[0003] In recent years, single-component white-light emitters have emerged as promising alternatives. These emitters have many advantages, such as no self-absorption, simple device structure, and high color stability, triggering significant interest in the field of artificial lighting. The broadband white-light emission of organic-inorganic lead halide hybrids has attracted widespread attention in energy-efficient solid-state lighting (SSL) applications, however, the toxicity of lead in these hybrid materials has hampered their commercial prospects. A key parameter in lighting is the color rendering index (CRI), which reflects the ability of a light source to accurately reproduce the color of the illuminated sample. Indoor lighting requires a CRI greater than 80, however, for specific industries with strict color requirements, such as jewelry, museum galleries, photography, and surgery, white light emission with a color rendering index as high as 90 is required. In order to accurately represent colors, the light source must emit photons covering the entire visible spectrum, but such broadband emission is difficult to achieve in single-component white-light emitters. Generally, a light-emitting diode (LED) chip is covered with a single or multiple phosphors to produce white-light emission. However, since the emission of a single phosphor is generally relatively narrow, the resulting white light has poor color rendering. However, mixed phosphors will cause efficiency loss due to self-absorption, and the different aging rates of individual phosphors will cause the emission spectrum to change over time. Therefore, finding ultra-broadband single-component white light emitting materials with excellent color rendering index (CRI) is of great significance to the development of white light diodes. Summary of the invention
[0004] In order to solve the above technical problems, the present invention proposes a metal halide luminescent material and a preparation method and application thereof.
[0005] In order to achieve the above object, the present invention is achieved through the following technical solutions:
[0006] In a first aspect, the present invention provides a metal halide luminescent material, the chemical formula of which is (TEA)2Cu2X y , wherein TEA is a tetraethylammonium halide compound, and X is composed of one or more of the halogens chlorine (Cl) and bromine (Br).
[0007] In a second aspect, the present invention provides a method for preparing the above-mentioned metal halide luminescent material, comprising:
[0008] Tetraethylammonium halide compound TEA and cuprous halide are added to a polytetrafluoroethylene liner and mixed with an organic solvent. After heating and reaction, the product is cooled to room temperature and then the crystal product is taken out. After washing and drying, the crystal (TEA)2Cu2X is obtained. y .
[0009] Preferably, the molar ratio of the tetraethylammonium halide compound TEA to cuprous halide is 1:1.
[0010] Preferably, the tetraethylammonium halide compound TEA is tetraethylammonium bromide TEABr, and the cuprous halide is cuprous chloride CuCl.
[0011] Preferably, the organic solvent is isopropanol.
[0012] Preferably, the tetraethylammonium bromide TEABr and cuprous chloride CuCl are added to a polytetrafluoroethylene liner and mixed with isopropanol, and then heated at 100° C. for 10 hours, cooled to room temperature, and then the crystal product is taken out, washed and dried to obtain a single-component white light crystal (TEA)2Cu2Br2Cl2.
[0013] In a third aspect, the present invention provides the use of the metal halide luminescent material prepared by the above method in a single-component white light emitting device.
[0014] Preferably, the method for preparing the single-component white light emitting device comprises:
[0015] The (TEA)2Cu2Br2Cl2 crystals were ground into powder, evenly mixed with UV curing adhesive, and then coated on 310nm UV lamp beads to prepare a white light emitting device, which emits white light after power is turned on.
[0016] The beneficial effects of the present invention are:
[0017] The present invention reacts cuprous halide with tetraethylammonium halide to synthesize a series of crystals including crystals emitting blue light, white light and yellow light, thus completing the (TEA)2Cu2X y The preparation of the crystal realizes that the emission spectrum is adjustable in the visible light region, and a crystal (TEA)2Cu2Br2Cl2 emitting ultra-wideband single-component white light with excellent color rendering index (CRI) is obtained; its single-component white light crystal has ultra-wideband emission characteristics, a half-maximum width (FWHM) of 300nm, and a CIE chromaticity coordinate of (0.32, 0.32), which is very close to the pure white light CIE chromaticity coordinate (0.33, 0.33), all of which make it an ideal choice for natural white light LED applications, and when prepared into a white light emitting device, the color rendering index (CRI) is as high as 95; and the present invention does not contain rare earth elements, is an environmentally friendly material, and its preparation process and preparation technology are simple, low cost, and can realize large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0019] Figure 1is a molecular structure diagram of crystal 1-9 in Example 1;
[0020] Figure 2 is the fluorescence spectrum of crystal 1-9 in Example 1;
[0021] Figure 3 is the CIE chromaticity diagram of crystal 1-9 in Example 1;
[0022] Figure 4 This is a photo of the light emitting device made of No. 5 as a single-component white light emitting material in Example 1 shining on a colored pencil;
[0023] Figure 5 This is the thermogravimetric curve of crystals 1-9 in Example 1. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0025] Example 1
[0026] Metal halide luminescent material, its chemical formula is (TEA)2Cu2X y , wherein TEA is a tetraethylammonium halide compound, and X is composed of one or more of the halogens chlorine (Cl) and bromine (Br). Preparation of metal halide luminescent materials: Add the raw materials to polytetrafluoroethylene liners No. 1-9 according to the corresponding component amounts of No. 1-9 in Table 1, wherein TEABr is tetraethylammonium bromide and TEACl is tetraethylammonium chloride. Except for the No. 9 liner, which adds 7.5 ml of isopropanol and 7.5 ml of cyclohexane, 15 ml of isopropanol is added to the other liners respectively. The liners are sealed with a stainless steel reactor outer liner and placed in an oven and heated at 100°C for 10 hours. After cooling to room temperature, take out the crystalline product, wash it three times, and then put it in a vacuum drying oven for five hours to obtain dry (TEA)2Cu2X y Crystal samples, whose crystal molecular structure is as follows Figure 1 As shown, the structures are similar, but the halogen ratios are different, among which No. 5 is a single-component white light crystal.
[0027] Table 1 Synthesis information of compounds 1-9
[0028] Serial number Chemical formula CuBr(g) TEABr(g) CuCl(g) TEACl(g) 1 <![CDATA[(TEA)2Cu2Br4]]> 0.287 0.420 2 <![CDATA[(TEA)2Cu2Br 3.5 Cl 0.5 ]]> 0.214 0.420 0.050 3 <![CDATA[(TEA)2Cu2Br3Cl]]> 0.143 0.420 0.099 4 <![CDATA[(TEA)2Cu2Br 2.5 Cl 1.5 ]]> 0.072 0.420 0.148 5 <![CDATA[(TEA)2Cu2Br2Cl2]]> 0.420 0.198 6 <![CDATA[(TEA)2Cu2Br 1.5 Cl 2.5 ]]> 0.315 0.198 0.083 7 <![CDATA[(TEA)2Cu2BrCl3]]> 0.210 0.198 0.166 8 <![CDATA[(TEA)2Cu2Br 0.5 Cl 3.5 ]]> 0.105 0.198 0.2485 9 <![CDATA[(TEA)2Cu2Cl4]]> 0.198 0.331
[0029] (1) Fluorescence spectroscopy analysis
[0030] Fluorescence spectra of 1-9 crystals were analyzed at room temperature using an Edinburgh Instruments FLS1000 fluorescence spectrophotometer. Figure 2It can be seen that the emission spectrum is adjustable in the visible light region, from blue light to white light to yellow light, and the spectrum range of crystal No. 5 is wide, with ultra-wideband emission characteristics, half-peak width (FWHM) of 300nm, CIE coordinates of (0.32, 0.32), very close to the pure white light CIE coordinates (0.33, 0.33). All these characteristics make it an ideal choice for natural white light LED applications.
[0031] (2) Luminescence performance test
[0032] Grind the No. 5 crystal into powder, mix it evenly with UV curing glue, and then apply it to 310nm UV lamp beads (excitation wavelength 310nm, voltage 5-6.5V, power 0.5-1W) to prepare a white light device, which emits white light after power is turned on. Figure 3 The chromaticity coordinate diagram shows that the luminous color is very close to pure white light. When the white light device is powered on and shined on colored pencils, it can be seen that the white light can clearly display and restore the bright colors of the colored pencils ( Figure 4 ), CRI is 95, indicating that the white light has a high color rendering index.
[0033] (3) Thermal stability analysis
[0034] The thermal gravimetric analysis of 1-9 crystals was performed in the range of 30-800°C. Figure 5 It can be seen from the thermogravimetric curve that the phosphor prepared in the present invention does not lose mass and decompose until about 200° C., indicating that the crystal has good thermal stability.
[0035] Example 2
[0036] Preparation of single-component white light emitting devices:
[0037] Grind No. 5 crystal into powder, mix it evenly with UV curing glue, and then apply it to 310nm UV lamp beads (excitation wavelength 310nm, voltage 5-6.5V, power 0.5-1W) to prepare a white light device, which emits white light after power is turned on.
[0038] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all details in detail, nor do they limit the invention to only the specific embodiments described. Obviously, many modifications and changes can be made according to the content of this specification.
Claims
1. A metal halide luminescent material, characterized in that: Its chemical formula is (TEA)2Cu2X y , wherein TEA is a tetraethylammonium halide compound, and X is composed of one or more of the halogens chlorine and bromine.
2. The method for preparing the metal halide luminescent material according to claim 1, characterized in that: include: Tetraethylammonium halide compound TEA and cuprous halide are added to a polytetrafluoroethylene liner and mixed with an organic solvent. After heating and reaction, the product is cooled to room temperature and then the crystal product is taken out. After washing and drying, the crystal (TEA)2Cu2X is obtained. y .
3. The method for preparing the metal halide luminescent material according to claim 2, characterized in that: The molar ratio of the tetraethylammonium halide compound TEA to cuprous halide is 1:
1.
4. The method for preparing the metal halide luminescent material according to claim 3, characterized in that: The tetraethylammonium halide compound TEA is tetraethylammonium bromide TEABr, and the cuprous halide is cuprous chloride CuCl.
5. The method for preparing the metal halide luminescent material according to claim 4, characterized in that: The organic solvent is isopropanol.
6. The method for preparing the metal halide luminescent material according to claim 5, characterized in that: The tetraethylammonium bromide TEABr and cuprous chloride CuCl are added to a polytetrafluoroethylene liner and mixed with isopropanol, and then heated at 100° C. for 10 hours, cooled to room temperature, and then the crystal product is taken out, washed and dried to obtain a single-component white light crystal (TEA)2Cu2Br2Cl2.
7. Use of the metal halide luminescent material prepared according to claim 6 in a single-component white light emitting device.
8. The method for preparing a single-component white light emitting device according to claim 7, characterized in that: include: The (TEA)2Cu2Br2Cl2 crystals were ground into powder, evenly mixed with UV curing adhesive, and then coated on 310nm UV lamp beads to prepare a white light emitting device, which emits white light after power is turned on.
Citation Information
Patent Citations
Preparation method of a class of copper (I) halogen cluster compounds capable of emitting different fluorescence
CN109666035A
Ultrasonic preparation method of fluorescent copper halogen cluster compound
CN109666036A
Grinding preparation method of copper (I)-bromine hybrid fluorescent materials
CN111205860A
Organic-inorganic hybrid halide luminescent material as well as preparation method and application thereof
CN112521938A
White light amine copper halide single crystal as well as low-temperature preparation method and application thereof
CN115385804A