Ionomer resin as well as preparation method and application thereof

By controlling the addition of acid liquid, the precipitation rate of ionomer resin is slowed down, and the problem of metal salt impurity wrapping in saponification method is solved, and the preparation of ionomer resin with low metal residue, high transparency and low water absorption is achieved.

CN118930687APending Publication Date: 2024-11-12JIANGSU SAILBOAT PETROCHEMICAL CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410971091.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the ionomer resin preparation by the existing saponification method, improper addition of acid liquid causes metal salt impurities to be wrapped in polymer particles, making it difficult to clean, increasing water absorption and reducing transparency.

Method used

By controlling the addition of acid liquid, the combination of continuous addition, batch addition or spray addition is adopted to slow down the precipitation rate of ionomer resin, avoid metal salt impurities being wrapped, and reduce the content of metal salt impurities in the final product.

Benefits of technology

Effectively reduce the content of metal salt impurities in the ionomer resin, improve transparency and reduce water absorption, so that the metal residue in the final product is less than 100ppm, the light transmittance is higher than 91%, and white spots after tableting are avoided The appearance of

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides an ionomer resin and a preparation method and application thereof.The preparation method comprises the steps that firstly, an ethylene-unsaturated carboxylic ester copolymer, alkali and a mixed solvent react to obtain a polymer solution, then acid liquor is added into the obtained polymer solution for a reaction, and the ionomer resin is obtained. The method comprises the following steps: adding an acid solution into the ionomer resin, limiting the adding mode of the acid solution to be any one or a combination of at least two of continuous adding, fractional adding and spraying adding, and finally performing post-treatment to obtain the ionomer resin. According to the preparation method, the mode of adding the acid liquor is controlled, so that local enrichment of the acid liquor in the polymer solution is avoided, the precipitation rate of the ionomer resin is further slowed down, the wrapping rate of the precipitated ionomer resin on metal salt impurities is fundamentally reduced, the content of the metal salt impurities in the finally obtained ionomer resin is relatively low, and the service life of the ionomer resin is prolonged. Furthermore, the transparency is relatively high and the water absorption rate is relatively low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ionomer resins, and in particular relates to an ionomer resin and a preparation method and application thereof. Background Art

[0002] Ionomer resin refers to a class of polymers containing metal ions. The molecular structure is based on the copolymer of ethylene and unsaturated carboxylic acid as the main chain, on which metal ions are introduced. Ethylene-unsaturated carboxylic acid ester ionomer resin has excellent transparency, wear resistance, scratch resistance, low-temperature impact toughness and chemical resistance. It is widely used in sports equipment such as golf balls, bowling balls, sleds, surfing skateboards, cosmetics and perfume containers, food packaging (especially vacuum skin packaging), glass multilayers (high-rise, photovoltaic glass for construction), automotive parts, polar exploration equipment and other fields.

[0003] Saponification is one of the main methods for preparing ionomer resins. The ionomer resin prepared by the saponification method is prepared by using ethylene-unsaturated carboxylic acid ester copolymer as the base resin in the form of a solution through alkali saponification, acid demetallization, purification and desalting. Compared with the neutralization method, the saponification method has the advantages of easy availability of base resin and good product uniformity. However, in the acid demetallization step of the ionomer resin prepared by the saponification method, in general, when inorganic acids such as sulfuric acid and hydrochloric acid are added to generate impurity metal salts, partial precipitation of the polymer will occur. Some impurity metal salts are wrapped in the precipitated polymer particles, which are difficult to clean and will remain in the ionomer resin product, increasing its water absorption and reducing its transparency.

[0004] In order to achieve low residual metal salt impurities in the saponification process of ionomer resin provided in the prior art, the main method is to control the size of the precipitated ionomer particles. The smaller the precipitated ionomer particles are, the less metal salt impurities they contain, and the easier it is to clean. However, when the precipitated ionomer particles are too small, filtering is more difficult. Therefore, the particle size of the precipitated ionomer particles can generally only be controlled within a certain range, which results in the precipitated ionomer particles still containing a certain amount of metal salt impurities, resulting in a higher content of metal salt impurities in the final ionomer resin.

[0005] Therefore, in view of the above problems, it is urgent to develop a method for preparing an ionomer resin that can fundamentally avoid the precipitation of metal salt impurities wrapped in the ionomer resin. Summary of the invention

[0006] In view of the deficiencies in the prior art, the object of the present invention is to provide an ionomer resin and a preparation method and application thereof. The preparation method effectively reduces the local enrichment of the added acid solution in the polymer solution by controlling the addition mode of the acid solution to be any one of continuous addition, batch addition or spray addition or a combination of at least two of them, thereby slowing down the precipitation rate of the ionomer resin, avoiding the formed metal salt impurities from being wrapped by the precipitated ionomer resin, and thereby reducing the content of metal salt in the finally obtained ionomer resin.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a method for preparing an ionomer resin, the preparation method comprising the following steps:

[0009] (1) reacting an ethylene-unsaturated carboxylic acid ester copolymer, a base and a mixed solvent to obtain a polymer solution;

[0010] (2) adding an acid solution to the polymer solution obtained in step (1) to carry out a reaction, and performing post-treatment to obtain the ionomer resin;

[0011] The acid solution is added in a manner of continuous addition, batch addition or spray addition, or a combination of at least two of the above.

[0012] The preparation method of the ionomer resin provided by the present invention comprises the following steps: firstly subjecting an ethylene-unsaturated carboxylic acid ester copolymer and an alkali to a saponification reaction in a mixed solvent to obtain a polymer solution, and then adding an acid solution to the obtained polymer solution to carry out an acidification reaction. During the acidification reaction, metal salt impurities are generated and part of the ionomer resin is precipitated. By controlling the addition of the acid solution to be any one of continuous addition, batch addition or spray addition or a combination of at least two of them, local enrichment of the acid solution in the polymer solution is avoided, thereby slowing down the precipitation rate of the ionomer resin, fundamentally reducing the probability of encapsulation of the metal salt impurities, and making the finally obtained ionomer resin have a lower content of metal salt impurities, higher transparency and lower water absorption.

[0013] In the present invention, the “continuous addition” refers to adding at a constant flow rate without interruption.

[0014] In the present invention, the “adding in portions” refers to adding in multiple portions with a constant addition amount each time.

[0015] In the present invention, the "spray addition" refers to adding the acid solution by spraying it in the form of extremely fine water particles using high-pressure equipment.

[0016] Preferably, the mass percentage of the unsaturated carboxylate unit in the ethylene-unsaturated carboxylate copolymer in step (1) is 7-35%, for example, 7%, 10%, 15%, 20%, 25%, 30% or 35%.

[0017] Preferably, the melt index of the ethylene-unsaturated carboxylate copolymer in step (1) is 5 to 300 g / 10 min, for example 5 g / 10 min, 10 g / 10 min, 50 g / 10 min, 100 g / 10 min, 150 g / 10 min, 200 g / 10 min, 250 g / 10 min or 300 g / 10 min, the test temperature is 190° C., and the load is 2.16 kg.

[0018] Preferably, the ethylene-unsaturated carboxylic acid ester copolymer in step (1) comprises ethylene-butyl acrylate copolymer and / or ethylene-butyl methacrylate copolymer, and more preferably ethylene-butyl acrylate copolymer.

[0019] Preferably, based on the mass of all reaction raw materials in the preparation method as 100%, the mass of the ethylene-unsaturated carboxylate copolymer in step (1) is 10-50%, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50%, etc.

[0020] Preferably, the base in step (1) comprises sodium hydroxide.

[0021] Preferably, the molar ratio of the unsaturated carboxylate unit in the ethylene-unsaturated carboxylate copolymer of step (1) to the base of step (1) is 1:(1-1.5), for example, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4 or 1:1.5, etc., more preferably 1:(1-1.2), and even more preferably 1:(1.05-1.1).

[0022] Preferably, the mixed solvent in step (1) comprises an alcohol solvent and an aromatic solvent.

[0023] Preferably, the alcohol solvent is any one of methanol, ethanol, tert-butanol, n-butanol or isopropanol, or a combination of at least two thereof, and methanol is more preferred.

[0024] Preferably, the aromatic solvent includes p-xylene and / or xylene.

[0025] Preferably, the reaction temperature in step (1) is 150-200°C, for example, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C or 200°C, etc.

[0026] Preferably, the reaction time of step (1) is 1 to 5 h, for example, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h or 5 h.

[0027] Preferably, the acid solution is added in step (2) continuously for 10 to 120 min, such as 10 min, 20 min, 40 min, 60 min, 80 min, 100 min or 120 min.

[0028] Preferably, the acid solution is added in step (2) in batches, and the number of batches is not less than 3 times, such as 4 times, 5 times, 6 times, 7 times, 8 times, 9 times or 10 times. Preferably, the molar ratio of the base in step (1) to the acid in the acid solution in step (2) is 1:(0.1-0.9), such as 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8 or 1:0.9.

[0029] Preferably, the acid in the acid solution in step (2) comprises an inorganic acid.

[0030] Preferably, the inorganic acid comprises hydrochloric acid and / or sulfuric acid.

[0031] Preferably, the acid solution in step (2) also includes alcohol.

[0032] Preferably, based on 100 parts by weight of the inorganic acid, the amount of the alcohol is not more than 300 parts by weight, for example, 300 parts by weight, 280 parts by weight, 260 parts by weight, 240 parts by weight, 220 parts by weight, 200 parts by weight, 180 parts by weight, 160 parts by weight, 140 parts by weight, 120 parts by weight or 100 parts by weight, etc.

[0033] Preferably, the reaction temperature in step (2) is 60-120°C, for example, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C or 120°C.

[0034] Preferably, the reaction time of step (2) is 10 to 120 min, for example, 10 min, 20 min, 40 min, 60 min, 80 min, 100 min or 120 min.

[0035] Preferably, the post-treatment method in step (2) comprises: adding methanol to the reaction solution for precipitation, washing with water and drying to complete the post-treatment.

[0036] As a preferred technical solution, the preparation method comprises the following steps:

[0037] (1) saponification: reacting the ethylene-unsaturated carboxylic acid ester copolymer, a base and a mixed solvent at 150 to 200° C. for 1 to 5 hours to obtain a first polymer solution;

[0038] (2) Acidification: adding acid solution to the polymer solution obtained in step (1) and reacting at 60-120° C. for 10-120 min, wherein the acid solution is added by continuous addition, batch addition or spray addition, or a combination of at least two of the above, to obtain a second polymer solution;

[0039] (3) Post-treatment: adding methanol to the second polymer solution obtained in step (2) at 50-100° C. to precipitate, washing with water and drying to obtain the ionomer resin.

[0040] In a second aspect, the present invention provides an ionomer resin, which is prepared by the preparation method described in the first aspect.

[0041] In a third aspect, the present invention provides an ionomer resin prepared by the preparation method described in the first aspect or an ionomer resin described in the second aspect for use in preparing sports equipment, cosmetic containers, perfume containers, food packaging, glass composite layers, automotive parts or polar exploration equipment.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] (1) The preparation method of the ionomer resin provided by the present invention first reacts an ethylene-unsaturated carboxylic acid ester copolymer, a base and a mixed solvent to obtain a polymer solution, then adds an acid solution to the obtained polymer solution for reaction, and the method of adding the acid solution is limited to any one of continuous addition, batch addition or spray addition or a combination of at least two of them, and finally obtains the ionomer resin through post-treatment; the preparation method avoids local enrichment of the acid solution in the polymer solution by controlling the method of adding the acid solution, thereby slowing down the precipitation rate of the ionomer resin, fundamentally reducing the encapsulation rate of the precipitated ionomer resin on the metal salt impurities, so that the metal salt impurity content in the final ionomer resin is low, and thus the transparency is high and the water absorption rate is low;

[0044] (2) By controlling the addition method of the acid solution, the present invention can make the metal residue in the prepared ionomer resin less than 100 ppm, the light transmittance greater than 91%, and no white spots appear after tableting. DETAILED DESCRIPTION

[0045] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0046] Some of the raw material information involved in the following examples and comparative examples are as follows:

[0047] (1) Ethylene-butyl acrylate copolymer (EnBA):

[0048] EnBA20020, melt index of 20 g / 10 min, 190°C, butyl acrylate unit content of 20%, purchased from Repsol, brand E20020;

[0049] EnBA2715, melt index of 150 g / 10 min, 190°C, butyl acrylate unit content of 27%, purchased from Repsol, brand E27150;

[0050] EnBA33150, with a melt index of 150 g / 10 min, 190° C., and a butyl acrylate unit content of 33% by mass, is purchased from Repsol with a brand name of E33150.

[0051] (2) Alkali:

[0052] Sodium hydroxide, NaOH, AR grade, was purchased from Sinopharm.

[0053] (3) Solvent:

[0054] Anhydrous methanol, p-xylene, and xylene, AR grade, were purchased from Sinopharm Pharmaceuticals.

[0055] (4) Acid:

[0056] Hydrochloric acid, 37% by mass, AR grade, purchased from Sinopharm;

[0057] Sulfuric acid, 30% by mass, AR grade, purchased from Sinopharm Pharmaceuticals.

[0058] Example 1

[0059] A method for preparing an ionomer resin comprises the following steps:

[0060] (1) Saponification: 60 g EnBA20020, 4.1 g NaOH, 28 g methanol and 112 g p-xylene were placed in a container, heated to 180° C. and reacted for 1.5 h to obtain a first polymer solution;

[0061] (2) Acidification: The first polymer solution obtained in step (1) was cooled to 90° C., and 7.4 g of hydrochloric acid was added continuously for 30 min. After the addition was completed, the reaction was allowed to proceed for 1 h to obtain a second polymer solution;

[0062] (3) Post-treatment: adding methanol to the second polymer solution obtained in step (2) at 65° C. to precipitate the ionomer, washing with water three times and drying to obtain the ionomer resin.

[0063] Example 2

[0064] A method for preparing an ionomer resin, which differs from Example 1 in that the amount of hydrochloric acid added in step (2) is 5.1 g, and other substances, amounts and steps are the same as those in Example 1.

[0065] Example 3

[0066] A method for preparing an ionomer resin comprises the following steps:

[0067] (1) Saponification: 60 g EnBA20020, 4.1 g NaOH, 28 g methanol and 112 g p-xylene were placed in a container, heated to 180° C. and reacted for 1.5 h to obtain a first polymer solution;

[0068] (2) Acidification: The first polymer solution obtained in step (1) was cooled to 120° C., and 1 g of hydrochloric acid was added continuously for 30 min. After the addition was completed, the reaction was allowed to proceed for 1 h to obtain a second polymer solution;

[0069] (3) Post-treatment: adding methanol to the second polymer solution obtained in step (2) at 65° C. to precipitate the ionomer, washing with water three times and drying to obtain the ionomer resin.

[0070] Example 4

[0071] A method for preparing an ionomer resin comprises the following steps:

[0072] (1) Saponification: 60 g EnBA20020, 4.1 g NaOH, 28 g methanol and 112 g p-xylene were placed in a container, heated to 180° C. and reacted for 1.5 h to obtain a first polymer solution;

[0073] (2) Acidification: The first polymer solution obtained in step (1) was cooled to 90° C., and 16.8 g of sulfuric acid was added continuously for 30 min. After the addition was completed, the reaction was continued for 0.2 h to obtain a second polymer solution;

[0074] (3) Post-treatment: adding methanol to the second polymer solution obtained in step (2) at 65° C. to precipitate the ionomer, washing with water three times and drying to obtain the ionomer resin.

[0075] Example 5

[0076] A method for preparing an ionomer resin comprises the following steps:

[0077] (1) Saponification: 60 g EnBA27150, 5.6 g NaOH, 84 g methanol and 56 g p-xylene were placed in a container, heated to 180° C. and reacted for 2 h to obtain a first polymer solution;

[0078] (2) Acidification: The first polymer solution obtained in step (1) was cooled to 90° C., and 10.1 g of hydrochloric acid was added continuously for 30 min. After the addition was completed, the mixture was reacted for 2 h to obtain a second polymer solution.

[0079] (3) Post-treatment: adding methanol to the second polymer solution obtained in step (2) at 65° C. to precipitate the ionomer, washing with water three times and drying to obtain the ionomer resin.

[0080] Example 6

[0081] A method for preparing an ionomer resin comprises the following steps:

[0082] (1) Saponification: 60 g EnBA33150, 6.8 g (about 0.17 mol) NaOH, 84 g methanol and 56 g p-xylene were placed in a container, heated to 180° C. and reacted for 2 h to obtain a first polymer solution;

[0083] (2) Acidification: The first polymer solution obtained in step (1) was cooled to 90° C., and 12.2 g of hydrochloric acid was added continuously for 30 min. After the addition was completed, the reaction was allowed to proceed for 1 h to obtain a second polymer solution;

[0084] (3) Post-treatment: adding methanol to the second polymer solution obtained in step (2) at 65° C. to precipitate the ionomer, washing with water three times and drying to obtain the ionomer resin.

[0085] Example 7

[0086] A method for preparing an ionomer resin comprises the following steps:

[0087] (1) Saponification: 60 g EnBA20020, 4.1 g NaOH, 28 g methanol and 112 g xylene were placed in a container, heated to 180° C. and reacted for 1.5 h to obtain a first polymer solution;

[0088] (2) Acidification: The first polymer solution obtained in step (1) was cooled to 90° C., and a mixture of 7.4 g of hydrochloric acid and 20 g of methanol was added continuously for 30 min. After the addition was completed, the mixture was reacted for 1 h to obtain a second polymer solution;

[0089] (3) Post-treatment: adding methanol to the second polymer solution obtained in step (2) at 65° C. to precipitate the ionomer, washing with water three times and drying to obtain the ionomer resin.

[0090] Example 8

[0091] A method for preparing an ionomer resin, which differs from Example 1 in that hydrochloric acid is added in step (2) in four portions, with 1.85 g of hydrochloric acid added each time, and other substances, amounts and steps are the same as those in Example 1.

[0092] Example 9

[0093] A method for preparing an ionomer resin, which differs from Example 1 in that hydrochloric acid is added in step (2) in three portions, with 2.47 g of hydrochloric acid added each time, and other substances, amounts and steps are the same as those in Example 1.

[0094] Example 10

[0095] A method for preparing an ionomer resin, which differs from Example 1 in that in step (2), hydrochloric acid is added in two portions, 3.7 g of hydrochloric acid is added each time, and other substances, amounts and steps are the same as those in Example 1.

[0096] Embodiment 11

[0097] A method for preparing an ionomer resin, which differs from Example 1 in that in step (2), hydrochloric acid is added in a spraying manner, and a total of 7.4 g of hydrochloric acid is added, and other substances, amounts and steps are the same as those in Example 1.

[0098] Example 12

[0099] A method for preparing an ionomer resin, which differs from Example 1 in that the continuous addition time in step (2) is 5 minutes, and other substances, amounts and steps are the same as those in Example 1.

[0100] Comparative Example 1

[0101] A method for preparing an ionomer resin is different from Example 1 in that 7.4 g of hydrochloric acid is directly added at one time, and other substances, amounts and steps are the same as those in Example 1.

[0102] Comparative Example 2

[0103] A method for preparing an ionomer resin is different from Example 2 in that 5.1 g of hydrochloric acid is directly added at one time, and other substances, amounts and steps are the same as those in Example 2.

[0104] Comparative Example 3

[0105] A method for preparing an ionomer resin is different from Example 4 in that 16.8 g of sulfuric acid is directly added at one time, and other substances, amounts and steps are the same as those in Example 4.

[0106] Performance Testing:

[0107] (1) Metal residue: The metal residue in the ionomer resin was tested using an ion chromatograph (CIC-D160), specifically the anion content of the metal compound, such as chloride ion, sulfate ion, etc.

[0108] (2) Light transmittance: The ionomer resin was tested using a Shimadzu UV-3600i Plus UV spectrophotometer with a test sample thickness of 0.5 mm.

[0109] (3) White spots on tablets: The ionomer resin was pressed at 180°C and 30 MPa for 3 min to form a 2 mm thin sheet. A tablet sample was obtained and its surface was visually observed for white spots.

[0110] The ionomer resins provided in Examples 1 to 12 and Comparative Examples 1 to 3 were tested according to the above test method. The test results are shown in Table 1:

[0111] Table 1

[0112] Metal residue / ppm Light transmittance / % White spots on tablets Example 1 <100 >91 No white spots Example 2 <100 >91 No white spots Example 3 <100 >91 No white spots Example 4 <100 >91 No white spots Example 5 <100 >91 No white spots Example 6 <100 >91 No white spots Example 7 <100 >91 No white spots Example 8 <100 >91 No white spots Example 9 <100 >91 No white spots Example 10 2200 70 A small amount of white spots Embodiment 11 <100 >91 No white spots Example 12 5000 60 A small amount of white spots Comparative Example 1 20000 30 Lots of white spots Comparative Example 2 1800 75 A small amount of white spots Comparative Example 3 25000 28 Lots of white spots

[0113] From the data in Table 1, we can see that:

[0114] (1) The metal residues in the ionomer resins provided in Examples 1 to 9 and 11 were all less than 100 ppm, the light transmittances were all greater than 91%, and no white spots appeared after tableting.

[0115] (2) By comparing the data of Example 1 and Comparative Example 1, and Example 2 and Comparative Example 2, it can be seen that the metal residue in the ionomer resin obtained by directly adding hydrochloric acid for acidification at one time is as high as 20,000 ppm, the light transmittance is only 30-75%, and white spots appear after tableting.

[0116] (3) By comparing Example 4 and Comparative Example 3, it can be found that the ionomer resin obtained by directly adding sulfuric acid as the acid solution at one time also has the problems of high metal residue, low light transmittance and a large number of white spots on the pressed tablets.

[0117] (4) Further comparison of Example 1, Example 10 and Example 12 also shows that too few times of adding the acid solution in batches (Example 10) and too short a time of continuously adding the acid solution (Example 12) will also lead to a higher metal residue in the obtained ionomer resin, a lower transmittance, and white spots on the pressed sheet.

[0118] The applicant declares that the present invention illustrates an ionomer resin and its preparation method and application through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing an ionomer resin, It is characterized in that The preparation method comprises the following steps: (1) reacting an ethylene-unsaturated carboxylic acid ester copolymer, a base and a mixed solvent to obtain a polymer solution; (2) adding an acid solution to the polymer solution obtained in step (1) to carry out a reaction, and performing post-treatment to obtain the ionomer resin; The acid solution is added in a manner of continuous addition, batch addition or spray addition, or a combination of at least two of the above.

2. The preparation method according to claim 1, It is characterized in that The mass percentage of the unsaturated carboxylate unit in the ethylene-unsaturated carboxylate copolymer in step (1) is 7 to 35%; Preferably, the melt index of the ethylene-unsaturated carboxylic acid ester copolymer in step (1) is 5 to 300 g / 10 min; Preferably, the ethylene-unsaturated carboxylic acid ester copolymer in step (1) comprises ethylene-butyl acrylate copolymer and / or ethylene-butyl methacrylate copolymer, and more preferably ethylene-butyl acrylate copolymer; Preferably, based on the mass of all the reaction raw materials in the preparation method being 100%, the mass of the ethylene-unsaturated carboxylic acid ester copolymer in step (1) is 10-50%.

3. The preparation method according to claim 1 or 2, It is characterized in that The alkali in step (1) comprises sodium hydroxide; Preferably, the molar ratio of the unsaturated carboxylate unit in the ethylene-unsaturated carboxylate copolymer of step (1) to the base of step (1) is 1:(1-1.5), more preferably 1:(1-1.2), and even more preferably 1:(1.05-1.1).

4. The preparation method according to any one of claims 1 to 3, It is characterized in that The mixed solvent in step (1) comprises an alcohol solvent and an aromatic solvent; Preferably, the alcohol solvent is any one of methanol, ethanol, tert-butanol, n-butanol or isopropanol, or a combination of at least two thereof, and methanol is more preferably; Preferably, the aromatic solvent includes p-xylene and / or xylene.

5. The preparation method according to any one of claims 1 to 4, It is characterized in that The reaction temperature of step (1) is 150-200° C. and the reaction time is 1-5 hours.

6. The preparation method according to any one of claims 1 to 5, It is characterized in that The acid solution is added in step (2) by continuous addition, and the continuous addition time is 10 to 120 minutes; Preferably, the acid solution is added in step (2) in portions, and the number of portions added is not less than 3 times.

7. The preparation method according to any one of claims 1 to 6, It is characterized in that The molar ratio of the base in step (1) to the acid in the acid solution in step (2) is 1:(0.1-0.9); Preferably, the acid in the acid solution in step (2) comprises an inorganic acid; Preferably, the inorganic acid comprises hydrochloric acid and / or sulfuric acid; Preferably, the acid solution in step (2) further comprises alcohol; Preferably, based on 100 parts by weight of the inorganic acid, the amount of the alcohol used is not higher than 300 parts by weight.

8. The preparation method according to any one of claims 1 to 7, It is characterized in that The reaction temperature in step (2) is 60-120° C. and the reaction time is 10-120 min. Preferably, the post-treatment method in step (2) comprises: adding methanol to the reaction solution for precipitation, washing with water and drying to complete the post-treatment.

9. An ionomer resin, It is characterized in that The ionomer resin is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the ionomer resin prepared by the preparation method according to any one of claims 1 to 8 or the ionomer resin according to claim 9 in the preparation of sports equipment, cosmetic containers, perfume containers, food packaging, glass composite layers, automotive parts or polar exploration equipment.