Aqueous resin composition for heat-resistant layer of lithium ion secondary battery separator

By using an aqueous resin composition of specific acrylic polymers and aqueous media, the heat shrinkage problem of lithium-ion secondary battery spacers in high temperature environments is solved, the performance of the heat-resistant layer is significantly improved, and the safety of the battery is enhanced. stability.

CN118930716APending Publication Date: 2024-11-12DIC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410430671.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-11
Filing Date
2024-04-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing lithium-ion secondary battery spacers are prone to heat shrinkage in high temperature environments, resulting in film rupture and pole short circuits. The existing heat-resistant layer technology has poor effect on suppressing heat shrinkage in high temperature environments, making it difficult to effectively prevent abnormal heating. Safety hazards.

Method used

The aqueous resin composition containing a specific acrylic polymer and an aqueous medium is used as the heat-resistant layer of the spacer, and is prepared by the emulsion polymerization method to optimize the ratio of the polymerization initiator and monomer, and improve heat shrinkage resistance.

Benefits of technology

It significantly improves the heat shrinkage resistance of the lithium-ion secondary battery spacer, reduces the possibility of heat shrinkage and film rupture in high-temperature environments, and enhances the safety and reliability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004785467580000111
    Figure BDA0004785467580000111
Patent Text Reader

Abstract

Provided is a water-based resin composition for a heat-resistant layer of a lithium ion secondary battery separator, said water-based resin composition being capable of obtaining a separator having excellent heat shrinkage resistance. The present invention uses a water-based resin composition for a heat-resistant layer of a separator for a lithium ion secondary battery, the present invention is characterized by containing: an acrylic polymer (A) having, as essential raw materials, an alkyl (meth) acrylate (a1) having an alkyl group having 4 or more carbon atoms and one or more monomers (a2) selected from the group consisting of N-hydroxymethyl (meth) acrylamide and unsaturated monomers having a carboxyl group; and an aqueous medium (B). The content of the alkyl (meth) acrylate (a1) is 50-95% by mass and the content of the monomer (a2) is 1-5% by mass in the monomer raw material of the acrylic polymer (A), and the content of the polymerization initiator in the main reaction of the acrylic polymer (A) is 0.05-0.25 parts by mass per 100 parts by mass of the monomer raw material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a water-based resin composition for a heat-resistant layer of a lithium ion secondary battery separator. Background Art

[0002] Polyolefin porous membranes are widely used as separators for batteries, capacitors, etc. due to their excellent electrical insulation and ion permeability. In recent years, as portable devices have become more multifunctional and lightweight, lithium-ion secondary batteries with high output power density and high capacity density are used as their power sources, and polyolefin porous membranes are also mainly used as separators for such batteries.

[0003] Lithium-ion secondary batteries have high output power density and capacity density. However, on the other hand, since organic solvents are used in the electrolyte, the electrolyte decomposes due to heat generated by abnormal situations such as short circuits and overcharging, which may cause fire in the worst case. In order to prevent such situations, several safety functions are embedded in lithium-ion secondary batteries, one of which is the shutdown function of the spacer. The so-called shutdown function is a function that inhibits ion conduction in the electrolyte and prevents the advancement of electrochemical reactions by blocking the micropores of the spacer due to heat melting when the battery generates abnormal heat. It is generally believed that the lower the shutdown temperature, the higher the safety. One of the reasons why polyethylene is used as a component of the spacer is that it has a moderate shutdown temperature.

[0004] However, in a high-energy battery, even if the electrochemical reaction is stopped by shutdown, the temperature inside the battery continues to rise, resulting in thermal contraction of the separator and film rupture, which may cause a short circuit between the two electrodes.

[0005] For the purpose of manufacturing a battery with high safety, a technique has been proposed in which a separator is formed by laminating a heat-resistant layer on a first porous layer mainly composed of a thermoplastic resin (see, for example, Patent Document 1).

[0006] However, the high-capacity battery that has promoted the high capacity of the battery has a large heat generation during abnormal heating, which is more likely to become a high-temperature environment. Although the separator described in the bulletin is considered to be safer than the usual separator without a heat-resistant layer, there is room for further improvement from the perspective of suppressing the thermal shrinkage of the separator in a high-temperature environment and reducing the possibility of short circuiting the two electrodes due to the rupture of the separator.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent No. 3756815 Summary of the invention

[0010] Problems to be solved by the invention

[0011] The problem to be solved by the present invention is to provide an aqueous resin composition for a heat-resistant layer of a lithium ion secondary battery separator, which can provide a separator having excellent heat shrinkage resistance.

[0012] Means for solving problems

[0013] The present inventors have conducted intensive studies to solve the above problems and have found that the above problems can be solved by using an aqueous resin composition containing a specific acrylic polymer and an aqueous medium, thereby completing the present invention.

[0014] That is, the present invention relates to a water-based resin composition for a heat-resistant layer of a lithium ion secondary battery separator, characterized in that it contains an acrylic polymer (A) having an alkyl (meth)acrylate (a1) having an alkyl group with more than 4 carbon atoms and one or more monomers (a2) selected from N-hydroxymethyl (meth)acrylamide and an unsaturated monomer having a carboxyl group as essential raw materials, and an aqueous medium (B), wherein the alkyl (meth)acrylate (a1) in the monomer raw material of the acrylic polymer (A) is 50 to 95% by mass, the monomer (a2) is 1 to 5% by mass, and the polymerization initiator in the main reaction of the acrylic polymer (A) is 0.05 to 0.25 parts by mass relative to 100 parts by mass of the monomer raw material.

[0015] Effects of the Invention

[0016] The aqueous resin composition for a heat-resistant layer of a lithium ion secondary battery separator of the present invention can be preferably used as a binder for a heat-resistant layer of a lithium ion secondary battery separator because a separator having excellent heat shrinkage resistance can be obtained. DETAILED DESCRIPTION

[0017] The water-based resin composition for the heat-resistant layer of the lithium ion secondary battery separator of the present invention contains an acrylic polymer (A) having an alkyl (meth)acrylate (a1) having an alkyl group with more than 4 carbon atoms and one or more monomers (a2) selected from N-hydroxymethyl (meth)acrylamide and an unsaturated monomer having a carboxyl group as essential raw materials, and an aqueous medium (B), wherein the alkyl (meth)acrylate (a1) in the monomer raw material of the acrylic polymer (A) is 50 to 95% by mass, the monomer (a2) is 1 to 5% by mass, and the polymerization initiator in the main reaction of the acrylic polymer (A) is 0.05 to 0.25 parts by mass relative to 100 parts by mass of the monomer raw material.

[0018] It should be noted that, in the present invention, the so-called "(meth)acrylamide" refers to one or both of acrylamide and methacrylamide, the so-called "(meth)acrylate" refers to one or both of acrylate and methacrylate, the so-called "(meth)acrylic acid" refers to one or both of acrylic acid and methacrylic acid, and the so-called "(meth)acryloyl" refers to one or both of acryloyl and methacryloyl.

[0019] The radical polymer (A) contains as essential raw materials an alkyl (meth)acrylate (a1) having an alkyl group having 4 or more carbon atoms and at least one monomer (a2) selected from N-methylol (meth)acrylamide and an unsaturated monomer having a carboxyl group.

[0020] The above-mentioned (meth) alkyl ester (a1) is a monomer having an alkyl group with 4 or more carbon atoms, for example, n-butyl (meth) acrylate, isobutyl (meth) acrylate, tert-butyl (meth) acrylate, n-hexyl (meth) acrylate, cyclohexyl (meth) acrylate, 2-ethylhexyl (meth) acrylate, n-octyl (meth) acrylate, lauryl (meth) acrylate, stearyl (meth) acrylate, etc. Among them, from the viewpoint of the heat shrinkage resistance of the obtained spacer, a monomer having an alkyl group with 4 to 8 carbon atoms is preferred. It should be noted that these acrylic monomers (a1) can be used alone or in combination of two or more.

[0021] The content of the alkyl (meth)acrylate (a1) in the monomer raw material of the acrylic polymer (A) is 50 to 95% by mass, and preferably 55 to 95% by mass in terms of further improving the heat shrinkage resistance.

[0022] Examples of the monomer (a2) include N-methylol (meth)acrylamide and unsaturated monomers having a carboxyl group. These monomers (a2) may be used alone or in combination of two or more.

[0023] Examples of the unsaturated monomer having a carboxyl group include unsaturated monocarboxylic acids such as (meth) acrylic acid and crotonic acid; and unsaturated dicarboxylic acids such as itaconic acid (anhydride), maleic acid (anhydride), and fumaric acid. Among them, unsaturated monocarboxylic acids are preferred. The monomer (a2) in the monomer raw material of the acrylic polymer (A) is 1 to 5% by mass, but is preferably 1 to 3% by mass in terms of further improving heat shrinkage resistance.

[0024] The acrylic polymer (A) contains the (meth)acrylic acid alkyl ester (a1) and the monomer (a2) as essential raw materials, but other monomers may be used as monomer raw materials.

[0025] Examples of the other monomers include (meth)acrylic acid alkyl esters having an alkyl group having 1 to 3 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, and propyl (meth)acrylate; 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxy-n-butyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-n-butyl (meth)acrylate, 3-hydroxy-n-butyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, N-(2-hydroxyethyl) (meth)acrylamide, glycerol mono(meth)acrylate, and 1,4-dimethylaminopropane. Monomers having hydroxyl groups, such as (meth)acrylates, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, 2-hydroxy-3-phenoxypropyl(meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethylphthalate, and lactone-modified (meth)acrylates having hydroxyl groups at the terminals; (meth)acrylates having amino groups, such as N,N-dimethylaminoethyl(meth)acrylate, N,N-diethylaminoethyl(meth)acrylate, N,N-dimethylaminopropyl(meth)acrylate, and N,N-diethylaminopropyl(meth)acrylate. Ester; monomers having an N-hydroxymethylamide group such as N-hydroxymethyl (meth) acrylamide; monomers having an N-alkoxymethylamide group such as N-butoxymethyl acrylamide; (meth)acrylates having a glycidyl group such as (meth) acrylate; monomers having an alkoxysilyl group such as vinyl trimethoxysilane, vinyl triethoxysilane, vinyl methyl dimethoxysilane, 3-(meth) acryloxypropyl trimethoxysilane, 3-(meth) acryloxypropyl triethoxysilane, 3-(meth) acryloxypropyl methyl dimethoxysilane; polyethylene glycol Polyalkylene glycol (meth)acrylates such as (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, polybutylene glycol (meth)acrylate, and methoxypolybutylene glycol (meth)acrylate; vinyl monomers such as styrene, α-methylstyrene, p-methylstyrene, chloromethylstyrene, vinyl acetate, and (meth)acrylonitrile; tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate; di(meth)acrylates such as ethylene glycol di(meth)acrylate and propylene glycol di(meth)acrylate, etc. It should be noted that these monomers can be used alone or in combination of two or more.

[0026] As a method for producing the acrylic polymer (A), various methods can be mentioned, but from the viewpoint of obtaining the acrylic polymer (A) in a simple manner, an emulsion polymerization method is preferred.

[0027] Examples of a method for obtaining the acrylic polymer (A) by emulsion polymerization include a method in which monomers serving as raw materials of the acrylic polymer (A) are radically polymerized in an aqueous medium at a temperature of 50 to 100° C. in the presence of an emulsifier and a polymerization initiator.

[0028] As the above-mentioned emulsifier, for example, anionic emulsifiers such as sulfuric acid esters and salts thereof of higher alcohols, alkylbenzene sulfonates, polyoxyethylene alkylphenyl sulfonates, polyoxyethylene alkyldiphenyl ether sulfonates, sulfuric acid half-ester salts of polyoxyethylene alkyl ethers, alkyldiphenyl ether disulfonates, and dialkyl succinate ester sulfonates can be cited; nonionic emulsifiers such as polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene diphenyl ethers, polyoxyethylene-polyoxypropylene block copolymers, and acetylene glycol systems; cationic emulsifiers such as alkylammonium salts; zwitterionic emulsifiers such as alkyl (amide) betaines and alkyl dimethylamine oxides, etc. It should be noted that these emulsifiers can be used alone or in combination of two or more. In addition, these emulsifiers are preferably used in a range of 0.5 to 5.0 mass % relative to the total amount of the monomers that become the raw materials of the polymer.

[0029] As the above-mentioned polymerization initiator, for example, azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), and azobiscyanovaleric acid; organic peroxides such as tert-butyl peroxypivalate, tert-butyl peroxybenzoate, tert-butyl peroxy-2-ethylhexanoate, di-tert-butyl peroxide, cumene hydroperoxide, benzoyl peroxide, and tert-butyl hydroperoxide; inorganic peroxides such as hydrogen peroxide, ammonium persulfate, potassium persulfate, and sodium persulfate, etc. It should be noted that these polymerization initiators can be used alone or in combination of two or more.

[0030] From the perspective of improving heat shrinkage resistance, the polymerization initiator in the main reaction of the acrylic polymer (A) is 0.05 to 0.25 parts by mass relative to 100 parts by mass of the monomer raw material. It should be noted that the main reaction of the acrylic polymer (A) in the present invention refers to a process of adding the monomer raw material and the polymerization initiator to the reaction system by dropwise addition to react. It is also possible to add an additional polymerization initiator after the addition of the monomer raw material to the reaction system is completed, but the additional polymerization initiator is not included in the polymerization initiator in the main reaction of the acrylic polymer (A).

[0031] As the above-mentioned aqueous medium (B), water, organic solvents miscible with water and mixtures thereof can be cited. As organic solvents miscible with water, for example, alcohols such as methanol, ethanol, n-propanol and isopropanol; ketones such as acetone and methyl ethyl ketone; polyalkylene glycols such as ethylene glycol, diethylene glycol and propylene glycol; alkyl ethers of polyalkylene glycols; lactams such as N-methyl-2-pyrrolidone, etc. can be cited. In the present invention, only water can be used, and a mixture of water and an organic solvent miscible with water can also be used, or only an organic solvent miscible with water can also be used. From the aspects of safety and environmental burden, it is preferred to use only water, or a mixture of water and an organic solvent miscible with water, and it is particularly preferred to use only water.

[0032] As the aqueous medium (B), it is convenient and preferred to use the aqueous medium used when producing the acrylic polymer (A) by emulsion polymerization or the like as it is.

[0033] Furthermore, by subjecting the resin composition to a desolvation step as necessary, the amount of the organic solvent in the resin composition of the present invention can be reduced.

[0034] The aqueous resin composition of the present invention obtained by the above method preferably contains 5 to 60% by mass of the acrylic polymer (A) based on the total amount of the aqueous resin composition, and more preferably 30 to 55% by mass, from the viewpoint of further improving coating workability.

[0035] In order to further improve coating workability, the aqueous resin composition of the present invention preferably contains 40 to 95% by mass of the aqueous medium (B), more preferably 45 to 70% by mass, based on the total amount of the aqueous resin composition.

[0036] The aqueous resin composition of the present invention may be used in combination with additives such as a curing agent, a curing catalyst, a lubricant, a filler, a thixotropy-imparting agent, a tackifier, a wax, a heat stabilizer, a light-resistant stabilizer, a fluorescent whitening agent, a foaming agent, a pH adjuster, a leveling agent, an anti-gelling agent, a dispersion stabilizer, an antioxidant, a free radical scavenger, a heat resistance-imparting agent, an inorganic filler, an organic filler, a plasticizer, a reinforcing agent, a catalyst, an antibacterial agent, an antifungal agent, an antirust agent, a thermoplastic resin, a thermosetting resin, a pigment, a dye, an electrical conductivity-imparting agent, an antistatic agent, a moisture permeability-improving agent, a water repellent, an oil repellent, a hollow foam, a compound containing crystal water, a flame retardant, a water absorbent, a moisture absorbent, a deodorant, a foam stabilizer, a defoamer, an antifungal agent, a preservative, an antialgae agent, a pigment dispersant, an antiblocking agent, an antihydrolysis agent, and a pigment, as needed.

[0037] The aqueous resin composition of the present invention can be suitably used as a binder for a heat-resistant layer of a lithium ion secondary battery from the viewpoint of obtaining a separator having excellent heat shrinkage resistance.

[0038] The slurry for a heat-resistant layer of a lithium ion secondary battery separator of the present invention contains the aqueous resin composition of the present invention, and preferably further contains non-conductive particles and a water-soluble polymer.

[0039] The heat-resistant layer slurry preferably contains 0.1 to 100 parts by mass of the acrylic polymer (A) and 0.1 to 100 parts by mass of the water-soluble polymer, based on 100 parts by mass of the non-conductive particles.

[0040] As the non-conductive particles, for example, inorganic particles and organic particles can be used, and inorganic particles are preferred.

[0041] As the above-mentioned inorganic particles, for example, oxide particles such as aluminum oxide (alumina), silicon oxide, magnesium oxide, titanium oxide, BaTiO2, ZrO, aluminum oxide-silicon dioxide composite oxide, nitride particles such as aluminum nitride, boron nitride, covalent bond crystalline particles such as silicon, diamond, insoluble ionic crystalline particles such as barium sulfate, calcium fluoride, barium fluoride, talc, clay particles such as montmorillonite, etc. can be cited, among which aluminum oxide (alumina) is preferred. It should be noted that these inorganic particles can be used alone or in combination of two or more.

[0042] In addition, as the above-mentioned organic particles, for example, polyethylene, polystyrene, polydivinylbenzene, styrene-divinylbenzene copolymer crosslinked products, and various crosslinked polymer particles such as polyimide, polyamide, polyamide-imide, melamine resin, phenolic resin, benzoguanamine-formaldehyde condensate, polysulfone, polyacrylonitrile, polyaramide, polyacetal, thermoplastic polyimide, etc. can be cited. It should be noted that these organic particles can be used alone or in combination of two or more.

[0043] As the water-soluble polymer, for example, cellulose polymers such as carboxymethyl cellulose, methyl cellulose, hydroxypropyl cellulose, and their ammonium salts and alkali metal salts; poly(meth)acrylic acid and their ammonium salts and alkali metal salts; polyvinyl alcohol compounds such as polyvinyl alcohol, copolymers of acrylic acid or acrylic acid salt and vinyl alcohol, maleic anhydride or copolymers of maleic acid or fumaric acid and vinyl alcohol; polyethylene glycol, polyethylene oxide, polyvinyl pyrrolidone, modified polyacrylic acid, oxidized starch, starch phosphate, casein, various modified starches, etc. It should be noted that these water-soluble polymers can be used alone or in combination of two or more.

[0044] Examples of the particulate polymer include cross-linked poly(meth)acrylic acid particles, cross-linked poly(meth)acrylate particles, cross-linked polystyrene particles, cross-linked resin particles of (meth)acrylate and styrene, melamine resin particles, nylon particles, polyimide particles, polyamide-imide particles, phenolic resin particles, polytetrafluoroethylene particles, fluorine resin particles, silicone resin particles, etc. It should be noted that these particulate polymers may be used alone or in combination of two or more.

[0045] The heat-resistant layer of the present invention can be formed by coating the heat-resistant layer slurry on the spacer. As a method for coating the heat-resistant layer slurry on the substrate, for example, a scraper method, a dipping method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, a brush coating method, etc. can be used. At this time, the heat-resistant layer slurry can be coated only on one side of the substrate, or on both sides.

[0046] As a method for drying the slurry composition for the heat-resistant layer on the substrate, for example, there can be mentioned a drying method using warm air, hot air, low-humidity air, a vacuum drying method, and a drying method using irradiation with infrared rays, electron beams, etc. By drying the slurry composition for the heat-resistant layer on the substrate in this way, the spacer of the present invention having a heat-resistant layer formed on the substrate can be obtained.

[0047] Example

[0048] The present invention will be further described in detail with reference to specific examples below.

[0049] (Example 1: Production and evaluation of aqueous resin composition (1))

[0050] After adding 50.0 parts by mass of ion exchange water to a 1.0L reaction container equipped with a stirrer, a thermometer, a condenser and nitrogen blowing and heating to 80°C, a monomer premix (a mixture of 1.0 parts by mass of acrylic acid, 1.5 parts by mass of N-hydroxymethyl acrylamide, 90.0 parts by mass of n-butyl acrylate and 7.5 parts by mass of acrylonitrile emulsified with an aqueous solution of an anionic emulsifier ("Hitenol LA-12" manufactured by Daiichi Industrial Pharmaceutical) dissolved in 35.5 parts by mass of ion exchange water) and 10 parts by mass of a 2% by mass sodium persulfate aqueous solution were added dropwise over 3 hours to react. After the reaction was completed, the temperature was maintained for 2 hours, and then cooled, and the non-volatile content was adjusted to 45.3% by mass and the pH was 8.1 using ion exchange water and 12.5% ​​ammonia aqueous solution to obtain an aqueous resin composition (1). The viscosity of the aqueous resin composition at 25°C was 18 mPa·s.

[0051] (Example 2: Production and evaluation of aqueous resin composition (2))

[0052] After adding 50.0 parts by mass of ion exchange water to a 1.0L reaction vessel equipped with a stirrer, a thermometer, a condenser and nitrogen blowing and heating to 80°C, a monomer premix (a mixture of 1.0 parts by mass of acrylic acid, 1.5 parts by mass of N-hydroxymethyl acrylamide, 60.0 parts by mass of n-butyl acrylate and 37.5 parts by mass of acrylonitrile emulsified with an aqueous solution of an anionic emulsifier ("Hitenol N-08" manufactured by Daiichi Industrial Pharmaceutical) dissolved in 35.5 parts by mass of ion exchange water) and 10 parts by mass of a 2% by mass sodium persulfate aqueous solution were added dropwise over 3 hours to react. After the reaction was completed, the temperature was maintained for 2 hours, and then cooled, and the non-volatile content was adjusted to 45.1% by mass and the pH was 8.2 using ion exchange water and 12.5% ​​ammonia aqueous solution to obtain an aqueous resin composition (2). The viscosity of the aqueous resin composition at 25°C was 15 mPa·s.

[0053] (Example 3: Production and evaluation of aqueous resin composition (3))

[0054] After adding 50.0 parts by mass of ion exchange water to a 1.0L reaction vessel equipped with a stirrer, a thermometer, a condenser and nitrogen blowing and heating to 80°C, a monomer premix (a mixture of 2.0 parts by mass of acrylic acid, 2.5 parts by mass of N-hydroxymethyl acrylamide, 89.0 parts by mass of n-butyl acrylate and 6.5 parts by mass of acrylonitrile emulsified with an aqueous solution of an anionic emulsifier ("Hitenol N-08" manufactured by Daiichi Industrial Pharmaceutical) dissolved in 35.5 parts by mass of ion exchange water) and 10 parts by mass of a 1% sodium persulfate aqueous solution were added dropwise over 3 hours to react. After the reaction was completed, the temperature was maintained for 2 hours, and then cooled, and the non-volatile component was adjusted to 45.4% by mass and pH 8.0 using ion exchange water and 12.5% ​​ammonia aqueous solution to obtain an aqueous resin composition (3). The viscosity of the aqueous resin composition at 25°C was 32 mPa·s.

[0055] (Example 4: Production and evaluation of aqueous resin composition (4))

[0056] After adding 50.0 parts by mass of ion exchange water to a 1.0L reaction container equipped with a stirrer, a thermometer, a condenser and nitrogen blowing and heating to 80°C, a monomer premix (a mixture of 1.0 parts by mass of acrylic acid, 1.5 parts by mass of N-hydroxymethyl acrylamide, 90.0 parts by mass of 2-ethylhexyl acrylate and 7.5 parts by mass of acrylonitrile emulsified with an aqueous solution of an anionic emulsifier ("Hitenol LA-12" manufactured by Daiichi Kogyo Seiyaku) dissolved in 35.5 parts by mass of ion exchange water) and 10 parts by mass of a 1% by mass sodium persulfate aqueous solution were added dropwise over 3 hours to react. After the reaction was completed, the temperature was maintained for 2 hours, and then cooled, and the non-volatile content was adjusted to 45.2% by mass and the pH was 8.2 using ion exchange water and 12.5% ​​ammonia aqueous solution to obtain an aqueous resin composition (1). The viscosity of the aqueous resin composition at 25°C was 26 mPa·s.

[0057] (Example 5: Production and evaluation of aqueous resin composition (5))

[0058] After 50.0 parts by mass of ion exchange water was added to a 1.0 L reaction container equipped with a stirrer, a thermometer, a condenser and nitrogen blowing, and heated to 80° C., a monomer premix (a mixture of 1.0 parts by mass of methacrylic acid, 1.5 parts by mass of N-methylol acrylamide, 81.5 parts by mass of n-butyl acrylate, 5.0 parts by mass of acrylonitrile, 8.0 parts by mass of methyl methacrylate, 1.5 parts by mass of n-butyl methacrylate, and 1.5 parts by mass of 2-ethylhexyl acrylate, emulsified with an aqueous emulsifier solution in which 1.5 parts by mass of an anionic emulsifier (“Hitenol N-08” manufactured by Daiichi Kogyo Seiyaku) was dissolved in 35.5 parts by mass of ion exchange water) and 10 parts by mass of a 2% by mass sodium persulfate aqueous solution were added dropwise over 3 hours to react. After the reaction was completed, the temperature was maintained for 2 hours, and then cooled, and the nonvolatile content was adjusted to 45.5% by mass and the pH was adjusted to 8.3 using ion exchange water and a 12.5% ​​ammonia aqueous solution to obtain an aqueous resin composition (5). The viscosity of the aqueous resin composition at 25° C. was 18 mPa·s.

[0059] (Comparative Example 1: Production and Evaluation of Aqueous Resin Composition (R1))

[0060] 100.0 parts by mass of the monomer composition, 0.3 parts by mass of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts by mass of ion exchange water and 0.3 parts by mass of potassium persulfate as a polymerization initiator were added to a 5MPa pressure-resistant container with a stirrer, and after sufficient stirring, the mixture was heated to 50°C to initiate polymerization. The monomer composition was set to a composition containing 92.8 parts by mass of n-butyl acrylate, 2.0 parts by mass of acrylonitrile, 2.0 parts by mass of methacrylic acid, 1.6 parts by mass of N-hydroxymethyl acrylamide and 1.6 parts by mass of acrylamide. The reaction was stopped by cooling at a polymerization conversion rate of 96% to obtain a mixture containing a particulate polymer. A 5% aqueous sodium hydroxide solution was added to the mixture containing the above-mentioned particulate polymer, and after adjusting the pH to 6, the unreacted monomers were removed by heating and reduced pressure distillation, and then cooled to below 30°C to obtain an aqueous resin composition (R1) in the form of an aqueous dispersion containing a particulate (meth) acrylic polymer.

[0061] (Comparative Example 2: Production and Evaluation of Aqueous Resin Composition (R2))

[0062] After adding 50.0 parts by mass of ion exchange water to a 1.0L reaction vessel equipped with a stirrer, a thermometer, a condenser and nitrogen blowing and heating to 80°C, a monomer premix (a mixture of 1.0 parts by mass of acrylic acid, 1.5 parts by mass of N-hydroxymethyl acrylamide, 90.0 parts by mass of lauryl methacrylate and 7.5 parts by mass of acrylonitrile, emulsified with an aqueous solution of an anionic emulsifier ("Hitenol LA-12" manufactured by Daiichi Industrial Pharmaceutical) dissolved in 35.5 parts by mass of ion exchange water) and 10 parts by mass of a 3% sodium persulfate aqueous solution were added dropwise over 3 hours and reacted. After the reaction was completed, the same temperature was maintained for 2 hours, and then cooled, and the non-volatile component was adjusted to 45.3% by mass and pH 8.1 using ion exchange water and 12.5% ​​ammonia aqueous solution to obtain an aqueous resin composition (R2). The viscosity of the aqueous resin composition at 25°C was 18mPa·s.

[0063] [Preparation of heat-resistant layer slurry]

[0064] While stirring at 5000 rpm with a homodispersor, 100 parts by mass of alumina (AKP3000 manufactured by Sumitomo Chemical Co., Ltd.) was slowly added to 100 parts by mass of 1% carboxymethyl cellulose (DN-800H manufactured by Daicel Chemical Co., Ltd.) to disperse the mixture. After the mixture was uniformly mixed, 12.5 parts by mass of the aqueous resin composition obtained above and 52.4 parts by mass of ion exchange water were added and uniformly mixed to prepare a heat-resistant layer slurry.

[0065] [Production of a spacer having a heat-resistant layer]

[0066] The heat-resistant layer slurry obtained above was applied to both surfaces of a polyethylene separator substrate having a thickness of 12 μm using a bar coater so that the film thickness after drying was 4 μm, thereby obtaining a separator having a heat-resistant layer. The drying temperature was set to 80° C. and the drying time was set to 5 minutes.

[0067] [Evaluation of Heat Shrinkage Resistance]

[0068] The heat-resistant spacer prepared above was cut into 5 cm squares, and placed in a 180°C warm air dryer for 1 hour while sandwiched between thick paper, and a heat resistance test was performed. The longitudinal and transverse lengths of the spacer after the test were measured, and the shrinkage rate in the longitudinal direction (MD shrinkage rate (%)) and the shrinkage rate in the transverse direction (TD shrinkage rate (%)) were calculated to evaluate the heat shrinkage resistance.

[0069] Shrinkage rate (%) = length of spacer after test / length of spacer before test × 100 (%)

[0070] Table 1 shows the evaluation results of Examples 1 to 4 and Comparative Example 1 described above.

[0071] [Table 1]

[0072]

[0073] It was confirmed that the heat-resistant layers obtained from the compositions of Examples 1 to 5, which are the aqueous resin compositions of the present invention, have excellent heat shrinkage resistance.

[0074] On the other hand, Comparative Examples 1 and 2 are examples in which the amount of the polymerization initiator used relative to the monomer raw material of the acrylic polymer (a1) was greater than the upper limit of the present invention, and it was confirmed that the heat shrinkage resistance was insufficient.

Claims

1. A water-based resin composition for a heat-resistant layer of a lithium-ion secondary battery separator, characterized in that: contain: An acrylic polymer A comprising as essential raw materials an alkyl (meth)acrylate a1 having an alkyl group with 4 or more carbon atoms and at least one monomer a2 selected from N-methylol (meth)acrylamide and an unsaturated monomer having a carboxyl group, and Aqueous medium B, The (meth)acrylic acid alkyl ester a1 in the monomer raw material of the acrylic polymer A is 50 mass % to 95 mass %, the monomer a2 is 1 mass % to 5 mass %, and the polymerization initiator in the main reaction of the acrylic polymer A is 0.05 mass part to 0.25 mass part relative to 100 mass parts of the monomer raw material. 2 . A slurry for a heat-resistant layer of a lithium ion secondary battery separator, comprising the aqueous resin composition for a heat-resistant layer of a lithium ion secondary battery separator according to claim 1 . 3 . A separator for a lithium ion secondary battery, comprising a heat-resistant layer obtained by using the slurry for a heat-resistant layer of a lithium ion secondary battery separator according to claim 2 .