Polypropylene film, metal layer integrated polypropylene film and film capacitor
By adjusting the molecular structure and manufacturing process of the polypropylene resin, a polypropylene film with excellent dielectric breakdown and heat shrinkage resistance was prepared, which solved the problem of insufficient performance of the polypropylene film in the prior art under high temperature environment, and realized the capacitor High temperature stability and long life.
Patent Information
- Application Number
- CN202180013631.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-12
- Filing Date
- 2021-02-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-02-10
AI Technical Summary
Existing polypropylene films and capacitors are difficult to meet excellent life performance, heat shock resistance, dielectric breakdown strength and heat shrinkage resistance in high temperature environments, especially when high and low temperatures are reused in the engine room. and the problem of reduced electrostatic capacity.
By adjusting the weight fraction w of the weight average molecular weight distribution (Mw/Mn), the Z-average molecular weight (Mz), and the logarithmic molecular weight Log(M) in the molecular weight integral distribution curve of the polypropylene resin in the polypropylene film, a specific molecule is prepared by adjusting the weight fraction w of the logarithmic molecular weight Log(M) in the molecular weight integral distribution curve of the polypropylene resin in the polypropylene film, a weight fraction w with the logarithmic molecular weight Log(M) is prepared. The polypropylene film with a structure is formed by a specific shear speed melting process manufacturing method to form a metal layer integrated polypropylene film to improve its capacitor performance.
It achieves excellent dielectric breakdown strength and heat shrinkage resistance at high temperatures around 120°C, extends the life of the capacitor, suppresses the reduction of the electrostatic capacity and thermal reinforcement, and is suitable for capacitor applications in high-temperature environments.
Smart Images

Figure BDA0003788626220000241 
Figure BDA0003788626220000281 
Figure BDA0003788626220000291
Abstract
Description
Technical Field
[0001] The invention relates to a polypropylene film, a metal layer integrated polypropylene film and a film capacitor. Background Art
[0002] Polypropylene film can be used for inductors of capacitors. For example, it can be used for inductors of capacitors in inverters constituting power control units of hybrid vehicles and electric vehicles.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: International Publication No. 2018 / 056404 Summary of the invention
[0006] Problem that the invention aims to solve
[0007] From the viewpoint of the above-mentioned use environment (for example, the environment in which the temperature rises in the engine room, the self-heating of the capacitor, etc.), it is desired that the capacitor using the polypropylene film as the capacitor inductor is small / lightweight / high-capacity and has excellent heat resistance at a high temperature of about 120°C (100°C to 120°C). Specifically, it is required that the decrease in the electrostatic capacitance of the capacitor can be suppressed even when used for a long time at the above-mentioned high temperature (excellent life performance), and that the thermal hardening (deformation) of the capacitor is suppressed when repeatedly used between the above-mentioned high and low temperatures in the engine room (excellent heat shock resistance), etc.
[0008] In addition, the polypropylene film used to make the above-mentioned capacitor is required to have excellent dielectric breakdown strength (dielectric breakdown strength) when a DC voltage is applied at the above-mentioned high temperature and excellent dielectric breakdown strength when an AC voltage is applied, when the thickness of the film is as thin as less than 20 μm, and to suppress thermal shrinkage in the machine direction (MD) at a temperature of about 150°C exceeding the above-mentioned high temperature (excellent heat shrinkage resistance), etc.
[0009] However, the polypropylene film and the capacitor using the same described in Patent Document 1 do not simultaneously satisfy the above-mentioned excellent life performance and excellent heat shock resistance as capacitor performance, and the above-mentioned excellent dielectric breakdown strength and excellent heat shrinkage resistance as film performance, and there is room for further improvement.
[0010] The present invention is made in view of the above-mentioned problems, and its purpose is to provide: a polypropylene film having excellent dielectric breakdown strength and heat shrinkage resistance at high temperatures, a film capacitor using the above-mentioned polypropylene film and having excellent life performance at high temperatures and excellent heat shock resistance, and their manufacturing methods.
[0011] Another object of the present invention is to provide a metal layer integrated polypropylene film having the above-mentioned polypropylene film, a film capacitor having the metal layer integrated polypropylene film, and methods for producing the same.
[0012] Solutions for solving problems
[0013] The present inventors have conducted in-depth research on polypropylene films. As a result, they found that: with respect to the polypropylene resin constituting the polypropylene film, a polypropylene film having a molecular weight distribution (Mw / Mn) of weight average molecular weight Mw and number average molecular weight Mn, a Z average molecular weight Mz, and a weight fraction w when the logarithmic molecular weight Log(M)=4.0 in the molecular weight integral distribution curve, respectively, within specific ranges has the aforementioned film properties, and a capacitor using the aforementioned polypropylene film has the aforementioned capacitor properties, thus completing the polypropylene film and film capacitor of the present invention. In addition, they found that: the aforementioned polypropylene film can be suitably manufactured according to a manufacturing method including a step of melting a polypropylene resin composition at a specific shear rate.
[0014] That is, the present invention relates to the following polypropylene film, metal layer integrated polypropylene film and film capacitor, and methods for producing the same.
[0015] 1. A polypropylene film, characterized in that the polypropylene resin constituting the polypropylene film is as follows:
[0016] The molecular weight distribution (Mw / Mn) of the weight average molecular weight Mw and the number average molecular weight Mn is 5.0 or more and 6.9 or less,
[0017] · Z average molecular weight Mz is 650,000 or more and 945,000 or less,
[0018] The weight fraction w when the logarithmic molecular weight Log(M)=4.0 in the molecular weight integrated distribution curve is 2.6% or more and 4.2% or less.
[0019] 2. The polypropylene film according to item 1 above, which is used for capacitors.
[0020] 3. The polypropylene film according to item 1 or 2 above, which is a biaxially stretched film.
[0021] 4. The polypropylene film according to any one of items 1 to 3 above, wherein the polypropylene film has a strength of 2.17 N / mm 2 Under a load, the temperature is increased from 25°C to 155°C at a rate of 10°C / min, and the horizontal axis is taken as the temperature and the vertical axis is taken as the dimensional change rate in the mechanical direction (MD) of the film. When a heating dimensional change curve is plotted, the dimensional change rate in the above-mentioned heating process from 25°C to 155°C is greater than 0%.
[0022] 5. The polypropylene film according to any one of items 1 to 4, wherein the dielectric breakdown strength (V DC120℃ ) and the dielectric breakdown strength under AC voltage at 120°C (V AC120℃ ) difference (V DC120℃ -V AC120℃ ) is greater than or equal to 280 V / μm and less than or equal to 300 V / μm.
[0023] 6. The polypropylene film according to any one of items 1 to 5 above, wherein the Mz exceeds 700,000.
[0024] 7. The polypropylene film according to any one of items 1 to 6 above, wherein
[0025] The molecular weight distribution (Mw / Mn) is 5.0 or more and 6.6 or less,
[0026] · The aforementioned Mz is 720,000 or more and 790,000 or less,
[0027] The weight fraction w is 3.5% or more and 3.7% or less.
[0028] 8. The polypropylene film according to any one of items 1 to 7 above, wherein the polypropylene resin comprises a polypropylene resin A and a polypropylene resin B, and the content of the polypropylene resin A in the polypropylene resin is greater than the content of the polypropylene resin B in the polypropylene resin.
[0029] The Mw of the polypropylene resin A is 275,000 or more and less than 350,000,
[0030] The molecular weight distribution (Mw / Mn) of the polypropylene resin A is 5.8 or more and 10.0 or less,
[0031] The melt flow rate (MFR) of the polypropylene resin A is A ) is 4.8 g / 10 minutes or more and 5.5 g / 10 minutes or less.
[0032] 9. The polypropylene film according to any one of items 1 to 8 above, wherein the polypropylene resin comprises a polypropylene resin A and a polypropylene resin B, and the content of the polypropylene resin A in the polypropylene resin is greater than the content of the polypropylene resin B in the polypropylene resin.
[0033] The Mw of the polypropylene resin B is 385,000 or more and 550,000 or less,
[0034] The molecular weight distribution (Mw / Mn) of the polypropylene resin B is 8.4 or more and 11.0 or less,
[0035] The melt flow rate (MFR) of the polypropylene resin B is B ) is 0.1 g / 10 minutes or more and 2.2 g / 10 minutes or less.
[0036] 10. The polypropylene film according to item 8 or 9, wherein the ratio of the mass of the polypropylene resin A to the total mass of the polypropylene resin A and the polypropylene resin B is 65 to 75% by mass.
[0037] 11. The polypropylene film according to any one of items 1 to 10, wherein the polypropylene film has a thickness of 1.0 μm to 6.0 μm.
[0038] 12. A metal layer integrated polypropylene film, comprising:
[0039] The polypropylene film according to any one of items 1 to 11 above; and
[0040] A metal layer laminated on one or both sides of the polypropylene film.
[0041] 13. A film capacitor comprising the metal layer integrated polypropylene film according to item 12 above in a wound state, or a structure in which a plurality of metal layer integrated polypropylene films according to item 12 above are stacked.
[0042] 14. A method for producing a polypropylene film, characterized in that it is the method for producing a polypropylene film according to any one of items 1 to 11 above, and the method comprises the following steps:
[0043] A polypropylene resin composition containing at least a polypropylene resin A and a polypropylene resin B is heated at a temperature of 225° C. to 270° C. and a shear rate of 2000 s. -1 Above and 15000s -1 The following melting is performed,
[0044] MFR of the above-mentioned polypropylene resin A A Compared with the MFR of the above-mentioned polypropylene resin B B The difference in MFR A -MFR B 1.5g / 10 minutes or more,
[0045] The content of the polypropylene resin A in the polypropylene resin composition is greater than the content of the polypropylene resin B in the polypropylene resin composition.
[0046] 15. The method for producing a polypropylene film according to item 14 above, wherein the polypropylene film is used for capacitors.
[0047] 16. The method for producing a polypropylene film according to item 14 or 15 above, wherein the polypropylene film is a biaxially stretched film.
[0048] 17. The method for producing a polypropylene film according to any one of items 14 to 16, wherein the ratio of the mass of the polypropylene resin A to the total mass of the polypropylene resin A and the polypropylene resin B is 65 to 75% by mass.
[0049] 18. The method for producing a polypropylene film according to any one of items 14 to 17, wherein the polypropylene film has a thickness of 1.0 μm to 2.4 μm.
[0050] 19. A method for producing a metal layer integrated polypropylene film, comprising the method according to any one of items 14 to 18, further comprising the step of forming a metal layer on at least one surface of the polypropylene film.
[0051] 20. A method for manufacturing a film capacitor, comprising the method according to item 19, further comprising the step of winding the metal layer integrated polypropylene film.
[0052] Effects of the Invention
[0053] The polypropylene film of the present invention has excellent dielectric breakdown strength (dielectric breakdown strength) when a direct current voltage is applied and dielectric breakdown strength when an alternating current voltage is applied at a high temperature of about 120° C. (100° C. to 120° C.) by making the molecular weight distribution (Mw / Mn) of the weight average molecular weight Mw and the number average molecular weight Mn of the polypropylene resin constituting the film, the Z average molecular weight Mz, and the weight fraction w when the logarithmic molecular weight Log(M)=4.0 in the molecular weight integral distribution curve all fall within specific ranges. In this way, even when the film is as thin as 6.0 μm or less in thickness, the film has excellent heat shrinkage resistance in terms of suppressing heat shrinkage in the machine direction (MD) at a temperature exceeding the above high temperature up to about 150° C. In addition, the film capacitor of the present invention using the above-mentioned polypropylene film as a capacitor inductor has excellent heat resistance at a high temperature of about 120°C (100°C to 120°C), and specifically, has excellent life performance in that the reduction of the electrostatic capacitance of the capacitor is suppressed even when used for a long time at the above high temperature, and has excellent heat shock resistance in that the thermal hardening (deformation) of the capacitor is suppressed when repeatedly used between the above high and low temperatures in the engine room. Therefore, the polypropylene film of the present invention is suitable for use as a film capacitor. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1This is a graph showing the results of thermomechanical analysis (TMA) of the polypropylene films produced in Example 1, Comparative Example 5 and Comparative Example 14, in which the heating dimensional change curve is plotted with the horizontal axis as temperature and the vertical axis as the dimensional change rate in the machine direction (MD) of the film.
[0055] Figure 2 Schematic diagram showing the appearance of a jumbo roll except for the two ends of about 100 mm after aging. (A) is a schematic diagram showing the case where there is no circumferential mold (longitudinal mold) with a depth of 0.5 mm or more, and (B) is a schematic diagram showing the case where there are two circumferential molds (longitudinal molds) with a depth of 0.5 mm or more. DETAILED DESCRIPTION
[0056] Hereinafter, the polypropylene film, the metal layer integrated polypropylene film, and the film capacitor of the present invention and the method for producing the same will be described in detail.
[0057] In this specification, polypropylene may be simply referred to as PP, and polypropylene resin may be simply referred to as PP resin.
[0058] In the present specification, the expressions “comprise” and “include” include the concepts of “comprises”, “comprising”, “consisting essentially of” and “consisting only of”.
[0059] In this specification, the expression "capacitor" includes the concepts of "capacitor", "capacitor element" and "film capacitor".
[0060] In this specification, the directions of the polypropylene film are as follows. First, the machine direction of the film is the same direction as the Machine Direction (hereinafter referred to as the "MD direction"). The MD direction is sometimes referred to as the length direction or the flow direction. Next, the transverse direction of the film is the same direction as the Transverse Direction (hereinafter referred to as the "TD direction"). The TD direction is sometimes referred to as the width direction.
[0061] Polypropylene film
[0062] The polypropylene film of the present invention is characterized in that the polypropylene resin constituting the polypropylene film is as follows:
[0063] The molecular weight distribution (Mw / Mn) of the weight average molecular weight Mw and the number average molecular weight Mn is 5.0 or more and 6.9 or less,
[0064] · Z average molecular weight Mz is 650,000 or more and 945,000 or less,
[0065] The weight fraction w when the logarithmic molecular weight Log(M)=4.0 in the molecular weight integrated distribution curve is 2.6% or more and 4.2% or less.
[0066] Hereinafter, it will be abbreviated as “Mw”, “Mn”, “molecular weight distribution (Mw / Mn)”, “Mz”, “weight fraction w” and the like.
[0067] The polypropylene film of the present invention having the above-mentioned characteristics is characterized in that the molecular weight distribution (Mw / Mn) of the weight average molecular weight Mw and the number average molecular weight Mn of the polypropylene resin constituting the film, the Z average molecular weight Mz, and the weight fraction w when the logarithmic molecular weight Log(M)=4.0 in the molecular weight integral distribution curve are all within specific ranges. Thus, even when the film is as thin as 6.0 μm or less in thickness, the film has excellent dielectric breakdown strength (dielectric breakdown strength) when a direct current voltage is applied and dielectric breakdown strength when an alternating current voltage is applied at a high temperature of about 120° C. (100° C. to 120° C.), and has excellent heat shrinkage resistance in that heat shrinkage in the machine direction (MD) is suppressed at a temperature of about 150° C. exceeding the above-mentioned high temperature. In addition, the film capacitor of the present invention using the aforementioned polypropylene film as a capacitor inductor has excellent heat resistance at a high temperature of about 120°C (100°C to 120°C). Specifically, it has excellent life performance in that the reduction of the electrostatic capacitance of the capacitor is also suppressed when used for a long time at the above high temperature, and it also has excellent heat shock resistance in that the thermal reinforcement (deformation) of the capacitor is suppressed when it is repeatedly used between the above high and low temperatures in the engine room. Therefore, the polypropylene film of the present invention is suitable for use as a film capacitor. In addition, the polypropylene film of the present invention is not limited to the presence or absence of stretching, but is preferably a biaxially stretched film considering the above-mentioned use.
[0068] The two sides of the polypropylene film in the present invention can be defined as the first side and the second side. The first side can be a rough surface. If the first side is a rough surface, it is not easy to generate wrinkles when the element is wound in the capacitor manufacturing. The second side can also be a rough surface.
[0069] From the viewpoint of ensuring the miniaturization and high capacity of the capacitor when used in the capacitor, the thickness of the polypropylene film is preferably 0.8 μm or more and 6.0 μm or less. Specifically, it is preferably 5.5 μm or less, more preferably 3.5 μm or less, further preferably 3.0 μm or less, and particularly preferably 2.4 μm or less. In addition, from the viewpoint of manufacturing, the thickness of the polypropylene film is preferably 1.0 μm or more, more preferably 1.8 μm or more, and further preferably 2.2 μm or more. The method for measuring the thickness of the polypropylene film in this specification is based on the method described in the examples.
[0070] The density of the polypropylene film is not limited, but is preferably set to 919 g / cm 3 Above and 925g / cm 3 The following is the method for measuring the density of the polypropylene film in this specification based on the method described in Examples.
[0071] The polypropylene film of the present invention has a molecular weight distribution (Mw / Mn) of 5.0 to 6.9 for the polypropylene resin constituting the polypropylene film (when the polypropylene resin is composed of a mixture of a plurality of resins, after the mixture).
[0072] The molecular weight distribution (Mw / Mn) can be 5.0 or more and 6.9 or less, and the lower limit is preferably 5.2 or more, more preferably 5.6 or more, further preferably 5.8 or more, further preferably 6.0 or more, further preferably 6.2 or more, and further preferably 6.3 or more. In addition, the upper limit is preferably 6.8 or less, more preferably 6.7 or less, and further preferably 6.6 or less. By making the molecular weight distribution (Mw / Mn) within the above range, as an effect of a combination with other features, a polypropylene film having excellent dielectric breakdown strength at high temperature and suppressed heat shrinkage in the machine direction (MD) is obtained.
[0073] In the polypropylene film of the present invention, the Mz of the polypropylene resin constituting the polypropylene film (when the polypropylene resin is composed of a mixture of a plurality of resins, after the mixture) is 650,000 or more and 945,000 or less.
[0074] Mz only needs to be 650,000 or more and 945,000 or less, and the lower limit is preferably more than 700,000, more preferably more than 710,000, and further preferably more than 720,000. In addition, the upper limit is preferably less than 920,000, more preferably less than 850,000, and further preferably less than 790,000. By making Mz within the above range, as an effect of a combination with other features, a polypropylene film having excellent dielectric breakdown strength at high temperature and particularly suppressed heat shrinkage in the machine direction (MD) is obtained. When Mz exceeds 945,000, which is not within the scope of the present invention, the heat shrinkage of the polypropylene film at high temperature tends to increase.
[0075] The polypropylene film of the present invention has a weight fraction w of 2.6% to 4.2% when the logarithmic molecular weight Log(M)=4.0 in the molecular weight integral distribution curve of the polypropylene resin (when the polypropylene resin is composed of a mixture of multiple resins, it is mixed) constituting the aforementioned polypropylene film.
[0076] The weight fraction w only needs to be 2.6% or more and 4.2% or less, and the lower limit is preferably 2.8% or more, more preferably 3.0% or more, further preferably 3.2% or more, and further preferably 3.4% or more. In addition, the upper limit is preferably 4.1% or less, more preferably 4.0% or less, further preferably 3.7% or less, and further preferably 3.6% or less. By making the weight fraction w within the above range, as a combination effect with other features, a polypropylene film having excellent dielectric breakdown strength at high temperatures and suppressed thermal shrinkage in the machine direction (MD) is obtained. In addition, by making the weight fraction w within the above range, the film capacitor of the present invention using the aforementioned polypropylene film as a capacitor inductor has excellent heat shock resistance in that thermal reinforcement (deformation) of the capacitor is suppressed during repeated use between high and low temperatures.
[0077] As a suitable embodiment of the polypropylene film of the present invention, the polypropylene resin constituting the polypropylene film (when the polypropylene resin is composed of a mixture of multiple resins, it is mixed) can be in the following manner:
[0078] The molecular weight distribution (Mw / Mn) is 5.0 or more and 6.6 or less,
[0079] · The aforementioned Mz is not less than 720,000 and not more than 850,000,
[0080] The weight fraction w is 3.3% or more and 3.7% or less.
[0081] By using a polypropylene resin having such physical properties, it becomes easy to obtain a polypropylene film which is excellent in dielectric breakdown strength at high temperatures and in which heat shrinkage in the machine direction (MD) is suppressed.
[0082] As a more suitable embodiment of the polypropylene film of the present invention, the polypropylene resin constituting the polypropylene film (when the polypropylene resin is composed of a mixture of multiple resins, it is mixed) can be formed in the following manner:
[0083] The molecular weight distribution (Mw / Mn) is 5.0 or more and 6.6 or less,
[0084] · The aforementioned Mz is 720,000 or more and 790,000 or less,
[0085] The weight fraction w is 3.5% or more and 3.7% or less.
[0086] By using a polypropylene resin having such physical properties, it becomes easy to obtain a polypropylene film which is excellent in dielectric breakdown strength at high temperatures and in which heat shrinkage in the machine direction (MD) is suppressed.
[0087] The Mw, Mn, Mz, molecular weight distribution (Mw / Mn), and weight fraction w of the polypropylene resin constituting the polypropylene film in this specification, and the Mw, Mn, Mz, molecular weight distribution (Mw / Mn), molecular weight distribution (Mz / Mn), differential distribution value when the logarithmic molecular weight Log(M)=4.5, differential distribution value when the logarithmic molecular weight Log(M)=6.0, and molecular weight differential distribution value difference (D M ), and the weight fraction w are determined based on the methods described in the Examples.
[0088] The polypropylene film of the present invention contains a polypropylene resin. The content of the polypropylene resin is preferably 90% by weight or more, more preferably 95% by weight or more, relative to the entire polypropylene film (when the entire polypropylene film is set to 100% by weight). The upper limit of the content of the polypropylene resin is, for example, 100% by weight, 98% by weight, etc. relative to the entire polypropylene film.
[0089] The less total ash content of the polypropylene resin is, the more preferred it is for electrical properties. Taking the polypropylene resin as a reference, the total ash content is preferably 50 ppm or less, more preferably 40 ppm or less, and further preferably 30 ppm or less. The lower limit of the total ash content is, for example, 2 ppm, 5 ppm, etc. The less the total ash content is, the less impurities such as polymerization catalyst residues are.
[0090] The polypropylene resin may include one type of polypropylene resin alone, or may include two or more types of polypropylene resins.
[0091] When the polypropylene film of the present invention contains two or more polypropylene resins, the polypropylene resin with the largest content is placed as the main component in this specification, and is referred to as the "main component polypropylene resin" or "base resin" in this specification. In addition, when the polypropylene film contains only one type of polypropylene resin, the polypropylene resin is also set as the main component in this specification, and is referred to as the "main component polypropylene resin" in this specification.
[0092] In the case where the polypropylene film of the present invention contains two or more (particularly two) polypropylene resins, for example, the following polypropylene resin A (base resin as a main component) and the following polypropylene resin B (blended resin) may be simultaneously contained. Hereinafter, the case where the polypropylene resin A (base resin) and the polypropylene resin B (blended resin) are used will be exemplified.
[0093] The content of the polypropylene resin A is more than 50% by weight, preferably 55% by weight or more, more preferably 60% by weight or more, and further preferably 65% by weight or more, relative to 100% by weight of the polypropylene resin. The upper limit of the content of the polypropylene resin A is less than 100% by weight, preferably 95% by weight or less, more preferably 90% by weight or less, further preferably 80% by weight or less, and further preferably 75% by weight or less, relative to 100% by weight of the polypropylene resin. Examples of the polypropylene resin A include isotactic polypropylene.
[0094] The weight average molecular weight Mw of the polypropylene resin A is preferably 250,000 or more and less than 350,000, more preferably 280,000 or more and less than 350,000, and further preferably 280,000 or more and less than 340,000. When Mw is 250,000 or more and less than 350,000, the thickness of the cast blank sheet can be easily controlled in the manufacturing process of the polypropylene film, and thickness unevenness is less likely to occur.
[0095] The number average molecular weight Mn of the polypropylene resin A is preferably 30,000 to 54,000, more preferably 33,000 to 52,000, and further preferably 33,000 to 47,000. When Mn is 30,000 to 54,000, thermal shrinkage is small, and a capacitor element having good heat shock resistance is easily obtained.
[0096] The z average molecular weight Mz of the polypropylene resin A is preferably 700,000 to 1,550,000, more preferably 750,000 to 1,500,000. When Mz is 700,000 to 1,550,000, a film having high dielectric breakdown strength at high temperatures is easily obtained.
[0097] The molecular weight distribution (Mw / Mn) of the polypropylene resin A is preferably 5.0 or more, more preferably 5.5 or more, and further preferably 6.0 or more. The Mw / Mn of the polypropylene resin A is preferably 10.0 or less, and more preferably 9.5 or less. When Mw / Mn is 5.0 or more and 10.0 or less, stretchability is improved and a thin film can be easily obtained.
[0098] The molecular weight distribution (Mz / Mn) of the polypropylene resin A is preferably 10 to 70, more preferably 15 to 60, further preferably 15 to 50. When Mz / Mn is 10 to 70, stretchability improves and a thin film can be easily obtained.
[0099] In the molecular weight distribution curve of polypropylene resin A, the differential distribution value when the logarithmic molecular weight Log(M)=4.5 is preferably 28.0 or more. The upper limit is preferably 32.0 or less. In addition, the differential distribution value when the logarithmic molecular weight Log(M)=6.0 is preferably 17.0 or more, more preferably 20.0 or more. The upper limit is preferably 24.0 or less, more preferably 22.0 or less. Furthermore, the difference (molecular weight differential distribution value difference (D)) obtained by subtracting the differential distribution value when the logarithmic molecular weight Log(M)=6.0 from the differential distribution value when the logarithmic molecular weight Log(M)=4.5 is M )) is preferably 8.0 or more and 18.0 or less, more preferably 8.0 or more and 11.0 or less, further preferably 8.2 or more and 10.0 or less, and further preferably 8.4 or more and 8.8 or less.
[0100] As a representative distribution value of a component having a molecular weight of 10,000 to 100,000 (hereinafter also referred to as a "low molecular weight component") on the lower molecular weight side than the Mw value (250,000 or more and less than 350,000) of the polypropylene resin A, and as a representative distribution value of a component having a molecular weight of around 1,000,000 (hereinafter also referred to as a "high molecular weight component") on the higher molecular weight side, a component having a logarithmic molecular weight Log(M)=4.5, it is understood that the low molecular weight component accounts for a larger proportion of 8.0% or more and 18.0% or less than the component having a Log(M)=6.0 or more.
[0101] That is, the molecular weight distribution Mw / Mn of 5.0 to 10.0 simply indicates that the molecular weight distribution is wide, and the quantitative relationship between the high molecular weight component and the low molecular weight component cannot be known. Therefore, the polypropylene resin A of the present invention preferably has a wide molecular weight distribution and contains more components with a molecular weight of 10,000 to 100,000 at a ratio of 8.0% or more and 18.0% or less compared to the components with a molecular weight of 1,000,000. This makes it easier to obtain a roughened surface of the polypropylene film because the crystallite size is small, which is preferred.
[0102] The lower limit of the weight fraction w of the polypropylene resin A is preferably 3.8% or more, more preferably 4.0% or more. In addition, the upper limit is preferably 4.4% or less, more preferably 4.2% or less. When the weight fraction w of the polypropylene resin A is within the above range and the weight fraction w of the polypropylene resin B described later is combined with the weight fraction w of the polypropylene resin A and the polypropylene resin B, the weight fraction w after mixing is 2.6% or more and 4.2% or less, thereby making it easy to obtain a polypropylene film having excellent dielectric breakdown strength at high temperatures and suppressed heat shrinkage in the machine direction (MD).
[0103] The melt flow rate (MFR) of polypropylene resin A at 230°C A) is preferably 4.8 g / 10 minutes or more, more preferably 5.0 g / 10 minutes or more, and further preferably 5.5 g / 10 minutes or more. A The upper limit of MFR is preferably 10.0 g / 10 minutes or less, more preferably 8.0 g / 10 minutes or less, and further preferably 6.0 g / 10 minutes or less. A It can also be set to 4.8 g / 10 minutes or more and 5.5 g / 10 minutes or less. The melt flow rate (MFR) in this specification is measured based on the method described in the Examples. In addition, the unit of the melt flow rate g / 10 minutes is also referred to as dg / min.
[0104] As a suitable embodiment of the polypropylene film of the present invention, the following method can be adopted for the polypropylene resin A:
[0105] The Mw of the polypropylene resin A is 275,000 or more and less than 350,000.
[0106] The molecular weight distribution (Mw / Mn) of the polypropylene resin A is 5.8 or more and 10.0 or less.
[0107] The melt flow rate (MFR) of the polypropylene resin A is A ) is 4.8 g / 10 minutes or more and 5.5 g / 10 minutes or less.
[0108] By using the polypropylene resin A having such physical properties, it becomes easy to mold a cast sheet (stretched precursor) using an extruder.
[0109] In addition, the polypropylene film of the present invention, as a more suitable embodiment, can adopt the following mode for the polypropylene resin A:
[0110] The Mw of the polypropylene resin A is 280,000 or more and 300,000 or less,
[0111] The molecular weight distribution (Mw / Mn) of the polypropylene resin A is 6.0 or more and 6.5 or less,
[0112] The melt flow rate (MFR) of the polypropylene resin A is A ) is 5.0 g / 10 minutes or more and 5.5 g / 10 minutes or less.
[0113] The heptane-insoluble matter of the polypropylene resin A is preferably 97.0% or more. The heptane-insoluble matter is preferably 98.5% or less. The more heptane-insoluble matter there is, the higher the stereoregularity of the resin. If the aforementioned heptane-insoluble matter (HI) is 97.0% or more and 98.5% or less, the crystallinity of the polypropylene resin in the polypropylene film is moderately improved due to the moderately high stereoregularity, and the dielectric breakdown strength at high temperature is improved. Furthermore, in the manufacturing process of the polypropylene film, the solidification (crystallization) speed during the molding of the cast blank sheet becomes moderate, and it has moderate stretchability. The method for measuring the heptane-insoluble matter (HI) in this specification is based on the method described in the examples.
[0114] The less total ash content of the polypropylene resin A is, the better for electrical properties. The total ash content is preferably 50 ppm or less, more preferably 40 ppm or less, and further preferably 30 ppm or less, based on the polypropylene resin A. The lower limit of the total ash content is, for example, 2 ppm, 5 ppm, etc.
[0115] The content of the polypropylene resin B is less than 50% by weight, preferably less than 49% by weight, more preferably less than 40% by weight, and particularly preferably less than 35% by weight, relative to 100% by weight of the polypropylene resin. In addition, the lower limit of the content of the polypropylene resin B is, for example, preferably more than 10% by weight, more preferably more than 15% by weight, and further preferably more than 25% by weight, relative to 100% by weight of the polypropylene resin. As the polypropylene resin B, for example, isotactic polypropylene can be cited. It should be noted that in the present invention, the following embodiment is particularly preferred: the ratio of the mass of the polypropylene resin A to the total mass of the polypropylene resin A and the polypropylene resin B is 65% by weight or more and 75% by weight or less.
[0116] The Mw of the polypropylene resin B is preferably 350,000 or more, more preferably 390,000 or more. The Mw of the polypropylene resin B is preferably 550,000 or less, more preferably 450,000 or less, and further preferably 400,000 or less. When the Mw is 350,000 or more and 550,000 or less, the thickness of the cast blank sheet can be easily controlled in the manufacturing process of the polypropylene film, and uneven thickness is less likely to occur.
[0117] The Mn of the polypropylene resin B is preferably 40,000 to 54,000, more preferably 42,000 to 50,000, and further preferably 44,000 to 48,000. When Mn is 40,000 to 54,000, thermal shrinkage is small, and a capacitor element having good thermal shock resistance is easily obtained.
[0118] The Mz of the polypropylene resin B is preferably greater than 1,550,000 and less than 2,000,000, and more preferably greater than 1,580,000 and less than 1,700,000. When the Mz is greater than 1,550,000 and less than 2,000,000, a film having high dielectric breakdown strength at high temperatures is easily obtained.
[0119] The molecular weight distribution (Mw / Mn) of the polypropylene resin B is preferably 5.0 or more, more preferably 5.5 or more, further preferably 7.0 or more, and further preferably 7.5 or more. The upper limit of Mw / Mn in the polypropylene resin B is, for example, 11.0 or less, preferably 10.0 or less, and more preferably 8.5 or less. When Mw / Mn is 5.0 or more and 11.0 or less, stretchability is improved and a thin film is easily obtained.
[0120] The molecular weight distribution (Mz / Mn) of the polypropylene resin B is preferably 30 to 40, more preferably 33 to 36. When Mz / Mn is 30 to 40, stretchability improves and a thin film is easily obtained.
[0121] In the molecular weight distribution curve of polypropylene resin B, the differential distribution value when the logarithmic molecular weight Log(M)=4.5 is preferably 24.0 or more, more preferably 27.0 or more. The upper limit is preferably 35.0 or less, more preferably 32.0 or less. In addition, the differential distribution value when the logarithmic molecular weight Log(M)=6.0 is preferably 28.0 or more, more preferably 30.0 or more. The upper limit is preferably 35.0 or less, more preferably 33.0 or less. Furthermore, the difference (molecular weight differential distribution value difference (D)) obtained by subtracting the differential distribution value when the logarithmic molecular weight Log(M)=6.0 from the differential distribution value when the logarithmic molecular weight Log(M)=4.5 is M )) is preferably from -11.0 to 7.0, more preferably from -6.0 to 0.0, further preferably from -4.0 to -2.0.
[0122] When the polypropylene resin includes the above-mentioned polypropylene resins A and B, the difference in Mw, Mw / Mn, and differential distribution value between the polypropylene resins A and B is different, that is, there is a difference in the composition of the molecular weight distribution, so that the quantitative relationship between the high molecular weight component and the low molecular weight component of the polypropylene film obtained by mixing and molding is slightly different. Therefore, it is believed that: a certain fine mixing (phase separation) state is adopted, and the crystal size is easy to be fine, which is preferred. It is further believed that: even at the same stretching ratio, there is a tendency to be easily highly oriented, and it is easy to obtain fine surface roughening, which is preferred. When the polypropylene resin includes the polypropylene resins A and B, it is believed that: due to the above reasons, the present invention exerts excellent effects, but the present invention is not limited by such reasons.
[0123] The lower limit of the weight fraction w of the polypropylene resin B is preferably 2.0% or more, more preferably 3.0% or more. In addition, the upper limit is preferably 5.0% or less, more preferably 4.2% or less. When the weight fraction w of the polypropylene resin B is within the above range and the weight fraction w of the polypropylene resin A is combined with the weight fraction w of the polypropylene resin A, the weight fraction w after the polypropylene resin A and the polypropylene resin B are mixed is 2.6% or more and 4.2% or less, thereby making it easy to obtain a polypropylene film having excellent dielectric breakdown strength at high temperatures and suppressed heat shrinkage in the machine direction (MD).
[0124] The melt flow rate (MFR) of polypropylene resin B at 230°C B ) is preferably 4.5 g / 10 minutes or less, more preferably 4.0 g / 10 minutes or less, further preferably 3.0 g / 10 minutes or less, and further preferably 2.1 g / 10 minutes or less. In addition, MFR B The lower limit of is preferably 0.1 g / 10 minutes or more, more preferably 0.5 g / 10 minutes or more, and further preferably 1.5 g / 10 minutes or more.
[0125] It should be noted that the MFR of the polypropylene resin A as the main component base resin is A MFR of polypropylene resin B as blending resin B The difference in MFR A -MFR B It is preferably set to 1.5 g / 10 minutes or more. A Greater than MFR B The above difference MFR A -MFR B It is preferably 1.6 g / 10 minutes or more, more preferably 2.0 g / 10 minutes or more, and even more preferably 3.0 g / 10 minutes or more. A -MFR B When the MFR is less than 1.5 g / 10 minutes (including negative values), the sea-island phase separation structure at the time of forming the cast blank sheet is not formed in the production process of the polypropylene film, or even if the islands are formed, the size of the islands is very small, so it may be difficult to finally obtain a polypropylene film having excellent dielectric breakdown strength at high temperatures. In particular, MFR A With MFR B Even if the difference is large, MFR B When the difference is greater (the above MFR A -MFR B becomes a negative value), the size of the islands in the sea-island phase separation structure also becomes very small.
[0126] As for the polypropylene film of the present invention, as a suitable embodiment, the polypropylene resin B can be used in the following manner:
[0127] The Mw of the polypropylene resin B is 385,000 or more and 550,000 or less.
[0128] The molecular weight distribution (Mw / Mn) of the polypropylene resin B is 8.4 or more and 11.0 or less.
[0129] The melt flow rate (MFR) of the polypropylene resin B is B ) is 0.1 g / 10 minutes or more and 2.2 g / 10 minutes or less.
[0130] By using the polypropylene resin B having such physical properties, it becomes easy to mold a cast sheet (stretched precursor) using an extruder.
[0131] As a more suitable embodiment, for the polypropylene film of the present invention, the following method can be adopted for the polypropylene resin B:
[0132] The Mw of the polypropylene resin B is 390,000 or more and 550,000 or less,
[0133] The molecular weight distribution (Mw / Mn) of the polypropylene resin B is 8.5 or more and 11.0 or less,
[0134] The melt flow rate (MFR) of the polypropylene resin B is B ) is 1.0 g / 10 minutes or more and 2.1 g / 10 minutes or less.
[0135] The heptane-insoluble matter content of the polypropylene resin B is preferably 97.5% or more, more preferably 98.0% or more, further preferably more than 98.5%, particularly preferably 98.6% or more. The heptane-insoluble matter content is preferably 99.5% or less, more preferably 99.0% or less.
[0136] The less total ash content of the polypropylene resin B is, the better for electrical properties. The total ash content is preferably 50 ppm or less, more preferably 40 ppm or less, and further preferably 30 ppm or less, based on the polypropylene resin B. The lower limit of the total ash content is, for example, 2 ppm, 5 ppm, etc.
[0137] In the above, the case of using two types of polypropylene resin A (base resin) and polypropylene resin B (blended resin) is exemplified, but in the present invention, the polypropylene film may contain a resin other than the polypropylene resin. In this case, when the entire resin is taken as 100% by weight, the total amount of the polypropylene resin A and the polypropylene resin B may be, for example, 90% by weight or more, 95% by weight or more, or 100% by weight.
[0138] The polypropylene film of the present invention may further contain additives. Examples of the additives include antioxidants, chlorine absorbers, ultraviolet absorbers, lubricants, plasticizers, flame retardants, antistatic agents, colorants, etc.
[0139] The polypropylene film of the present invention may be a biaxially stretched film, a uniaxially stretched film, or an unstretched film, but is preferably a biaxially stretched film.
[0140] The polypropylene film of the present invention is preferably used for capacitors, and specifically, can be suitable for use as a dielectric of capacitors. As described later, the polypropylene film of the present invention can be formed into a metal layer integrated polypropylene film having a metal layer stacked on one or both sides, and the metal layer integrated polypropylene film can be wound or Make it The invention comprises a structure of laminating a plurality of metal layer integrated polypropylene films, thereby making it possible to manufacture a film capacitor.
[0141] In view of the above-mentioned use for capacitors, the polypropylene film of the present invention is expected to have the following properties of dielectric breakdown strength and heat shrinkage resistance.
[0142] The dielectric breakdown strength (V AC100℃ ) is preferably 240 V / μm or more, more preferably 245 V / μm or more, and further preferably 250 V / μm or more. The upper limit of the dielectric breakdown strength under AC voltage at 100°C is preferably higher, for example, 270 V / μm, 265 V / μm, etc.
[0143] The dielectric breakdown strength (V AC110℃ ) is preferably 240 V / μm or more, more preferably 242 V / μm or more, and further preferably 244 V / μm or more. The upper limit of the dielectric breakdown strength under AC voltage at 110°C is preferably higher, for example, 260 V / μm, 255 V / μm, etc.
[0144] The dielectric breakdown strength (V AC120℃ ) is preferably 230 V / μm or more, more preferably 235 V / μm or more, and further preferably 238 V / μm or more. The upper limit of the dielectric breakdown strength under AC voltage at 120°C is preferably higher, for example, 250 V / μm, 245 V / μm, etc.
[0145] The dielectric breakdown strength (V DC120℃) is preferably 520 V / μm or more, more preferably 527 V / μm or more, and further preferably 532 V / μm or more. The upper limit of the dielectric breakdown strength at a DC voltage at 120°C is preferably higher, for example, 550 V / μm, 540 V / μm, etc.
[0146] The aforementioned V of the polypropylene film of the present invention AC120℃ With the aforementioned V DC120℃ The total value (V AC120℃ +V DC120℃ ) is preferably 750V / μm or more, more preferably 760V / μm or more, and further preferably 770V / μm or more. The upper limit of the total value of the aforementioned VAC120°C and the aforementioned VDC120°C is preferably as high as possible, for example, 1000V / μm, 900V / μm, 850V / μm, etc.
[0147] The aforementioned V of the polypropylene film of the present invention DC120℃ With the aforementioned V AC120℃ The difference (V DC120℃ -V AC120℃ Preferably, it is 300V / μm or less. Such a small difference has the advantage that dielectric breakdown is not easy even for superimposed current (current overlapping DC and AC). It should be noted that the lower limit of the above difference is preferably set to 280V / μm or more, for example, it can be set to 280V / μm or more and 300V / μm or less.
[0148] The polypropylene film of the present invention has excellent heat shrinkage resistance. Specifically, in the thermomechanical analysis (TMA) of the polypropylene film, the heat shrinkage resistance of the polypropylene film is 2.17 N / mm 2 Under a load, the temperature is raised from 25°C to 155°C at a rate of 10°C / min, the horizontal axis is the temperature, and the vertical axis is the dimensional change rate in the mechanical direction (MD) of the film. When a heating dimensional change curve is drawn, the dimensional change rate in the aforementioned heating process from 25°C to 155°C is expected to be 0% or more. Here, the dimensional change rate is 0% or more (that is, not less than 0%) when no thermal shrinkage is observed. For the method of thermomechanical analysis (TMA), the method described in the embodiment is based on the method.
[0149] Figure 1 This is a graph showing the results of the above-mentioned thermomechanical analysis of the polypropylene films produced in Example 1, Comparative Example 5 and Comparative Example 14, which is the result obtained by plotting the heating dimensional change curve with the horizontal axis being the temperature and the vertical axis being the dimensional change rate in the machine direction (MD) of the film. Figure 1It can be seen that the dimensional change rate of the polypropylene film produced in Example 1 in the machine direction of the film is 0% or more in the entire temperature increase process from 25°C to 155°C. On the other hand, the polypropylene films produced in Comparative Examples 5 and 14 have a temperature region in which the dimensional change rate of the film in the machine direction becomes lower than 0% in the temperature increase process from 25°C to 155°C.
[0150] Method for producing polypropylene film
[0151] The method for producing the polypropylene film of the present invention is not limited, and the polypropylene film of the present invention can be preferably produced by, for example, adopting the following production method (hereinafter referred to as "the production method of the polypropylene film of the present invention").
[0152] The method for producing a polypropylene film of the present invention is characterized in that it is a method for producing the polypropylene film of the present invention.
[0153] The production method comprises the following steps: subjecting a polypropylene resin composition containing at least a polypropylene resin A and a polypropylene resin B to a temperature of 225° C. to 270° C. and a shear rate of 2000 s -1 Above and 15000s -1 The following melting is performed,
[0154] The melt flow rate (MFR) of the polypropylene resin A is A ) and the (MFR B ) A -MFR B 1.5g / 10 minutes or more,
[0155] The content of the polypropylene resin A in the polypropylene resin composition is greater than the content of the polypropylene resin B in the polypropylene resin composition.
[0156] According to this production method, a polypropylene film having good dielectric breakdown strength at high temperatures can be provided. The reason for this is believed to be due to the sea-island phase separation structure (particularly appropriate island size) of the cast green sheet produced by using two specific different polypropylene resins.
[0157] In the method for producing a polypropylene film of the present invention, a polypropylene resin composition containing at least a polypropylene resin A and a polypropylene resin B is used. Here, the content of the polypropylene resin A in the polypropylene resin composition is greater than the content of the polypropylene resin B in the polypropylene resin composition, which means that in the relationship between the polypropylene resin A and the polypropylene resin B, the polypropylene resin A is a base resin with the main component, and the polypropylene resin B is a blended resin for the base resin. It should be noted that the terms "polypropylene resin A" and "polypropylene resin B" in the method for producing a polypropylene film of the present invention correspond to the terms "polypropylene resin A" and "polypropylene resin B" in the items of the aforementioned polypropylene film, and the Mw, Mn, Mz, molecular weight distribution (Mw / Mn), molecular weight distribution (Mz / Mn), differential distribution value when the logarithmic molecular weight Log(M)=4.5, differential distribution value when the logarithmic molecular weight Log(M)=6.0, and molecular weight differential distribution value difference (D M ), weight fraction w, and MFR are as described above, but in the method for producing the polypropylene resin of the present invention, MFR is particularly used. A With MFR B The difference in MFR A -MFR B 1.5g / 10 minutes or more.
[0158] There are no particular restrictions on the method for mixing the resins used in the manufacturing method of the present invention, and the following methods can be cited: a method of dry mixing the polymer powder or pellets of the base resin and the blended resin using a mixer or the like; a method of supplying the polymer powder or pellets of the base resin and the blended resin to a mixer and melt-kneading to obtain a mixed product.
[0159] The mixer and the kneading machine are not particularly limited. The kneading machine may be a single screw type, a twin screw type, or a multi-screw type. In the case of a twin screw or multi-screw type, the kneading machine may be a kneading machine that rotates in the same direction or in opposite directions.
[0160] When mixing by melt mixing, there is no particular restriction on the mixing temperature as long as a good mixed material is obtained. It is usually in the range of 200°C to 300°C, and preferably 230°C to 270°C from the viewpoint of suppressing the degradation of the resin. In addition, in order to suppress the degradation of the resin during mixing, an inert gas such as nitrogen can be purged into the mixer. The resin after melt mixing can usually be granulated into a suitable size using a known granulator. Thus, a mixed polypropylene raw resin pellet can be obtained.
[0161] In order to improve electrical properties, the total ash content generated by polymerization catalyst residues contained in the polypropylene raw material resin is preferably as small as possible. The total ash content is preferably 50 ppm or less, more preferably 40 ppm or less, and particularly preferably 30 ppm or less based on the polypropylene resin (100 parts by weight).
[0162] The polypropylene resin may contain additives. "Additives" generally refer to additives used in polypropylene resins, and there are no particular restrictions as long as a polypropylene film can be obtained. Examples of the additives include antioxidants, chlorine absorbers, ultraviolet absorbers, lubricants, plasticizers, flame retardants, antistatic agents, and the like. The polypropylene resin may contain the additives in an amount that does not adversely affect the polypropylene film.
[0163] In the method for producing a polypropylene film of the present invention, first, polypropylene resin pellets, dry-blended polypropylene resin pellets, or mixed polypropylene resin pellets prepared by melt-kneading in advance are supplied to an extruder and heated and melted.
[0164] The polypropylene resin composition is melted at 225° C. to 270° C. Specifically, the extruder setting temperature during the heating and melting of the polypropylene resin composition is set to 225° C. to 270° C. Thus, under the premise of using the above-mentioned specific polypropylene resin composition, a sea-island phase separation structure is formed at the time of casting blank sheet molding described later, and finally a polypropylene film having excellent dielectric breakdown strength at high temperature is obtained.
[0165] The polypropylene resin composition is heated at a temperature of 225°C to 270°C at a shear rate of 2000 s. -1 Above and 15000s -1 The following is melted. Thus, under the premise of using the above-mentioned specific polypropylene resin composition, a sea-island phase separation structure is formed at the time of casting blank sheet molding described later, and finally a polypropylene film with excellent dielectric breakdown strength at high temperature is obtained. If the shear rate is less than 2000s -1 , the extrusion amount is not constant, the shape and size of the blank sheet become irregular or change regularly, and it becomes easy for the blank sheet to break during transportation or stretching.
[0166] In addition, if the shear speed is higher than 15000s -1 , the unmelted material is extruded due to a phenomenon called disintegration in the extruder, and a uniform blank sheet cannot be obtained, which easily causes breakage during stretching, or excessive heat generation during passing through the gap between small sheets, and the degradation of the polypropylene resin composition becomes significant. Therefore, even if a uniform blank sheet is obtained, the dielectric breakdown strength of the film obtained by stretching will be reduced. The shear rate can be adjusted by the barrel diameter of the extruder, the screw speed, and the groove depth of the screw.
[0167] The above shear speed is only 2000s -1 Above and 15000s -1 Below, preferably 2000s -1 More than 10000s -1 Below, more preferably 2000s -1 Above and 2300s -1 By setting the shear rate within the above range, it becomes easy to obtain a polypropylene film having a weight fraction w of 2.6% or more and 4.2% or less, and by combining with other features, a film capacitor using the polypropylene film as a capacitor inductor can obtain excellent heat shock resistance in that thermal strengthening (deformation) of the capacitor is suppressed during repeated use between high and low temperatures.
[0168] Next, the resin composition melted by a T-die is extruded into a sheet, cooled and solidified by at least one metal drum, thereby forming an unstretched cast blank sheet. In addition, the surface temperature of the metal drum (the temperature of the metal drum that is first contacted after extrusion) is preferably above 50°C and below 105°C, more preferably above 60°C and below 100°C. The surface temperature of the metal drum can be determined based on the physical properties of the polypropylene resin used. If the surface temperature of the metal drum is significantly lower than 50°C, it is difficult to obtain good sheet formability of the blank sheet, and therefore, it becomes difficult to obtain a good polypropylene film without uneven stretching or breakage during stretching film formation.
[0169] The thickness of the cast green sheet is not particularly limited as long as the polypropylene film can be obtained, but is usually preferably 0.05 mm to 2 mm, more preferably 0.1 mm to 1 mm.
[0170] The aforementioned polypropylene film can be manufactured by stretching the aforementioned polypropylene cast blank sheet. The stretching is preferably biaxial stretching in which the biaxial orientation is performed longitudinally and transversely. As a stretching method, a sequential biaxial stretching method is preferred. As a sequential biaxial stretching method, for example, first, the cast blank sheet is maintained at a temperature of 110°C or more and 170°C or less (preferably 135°C or more and 170°C or less), and is stretched along the flow direction between rollers with a speed difference. The stretching ratio in the flow direction is preferably 3.5 times or more and 5.5 times or less, more preferably 4.2 times or more and 5.4 times or less. Then, the sheet is introduced into a tenter and stretched in the transverse direction. The temperature during transverse stretching is preferably 150°C or more and 165°C or less, and the transverse stretching ratio is preferably 9 times or more and 11 times or less. Afterwards, relaxation and heat setting are performed at 2 times or more and 10 times or less. From the above, a biaxially stretched polypropylene film is obtained.
[0171] From the viewpoint of ensuring the miniaturization and high capacity of the capacitor when used in the capacitor, the thickness of the polypropylene film is preferably 0.8 μm or more and 6.0 μm or less as described above. Specifically, it is preferably 5.5 μm or less, more preferably 3.5 μm or less, further preferably 3.0 μm or less, and particularly preferably 2.4 μm or less. In addition, from the viewpoint of manufacturing, the thickness of the polypropylene film is preferably 1.0 μm or more, more preferably 1.8 μm or more, and further preferably 2.2 μm or more.
[0172] For the polypropylene film, for the purpose of improving the adhesive properties in the post-process of metal deposition processing, after the stretching and heat setting process, the corona discharge treatment can be carried out online or offline. The corona discharge treatment can be carried out by a known method. As the atmosphere gas, it is preferably carried out using air, carbon dioxide, nitrogen, or a mixed gas thereof.
[0173] The polypropylene film of the present invention thus obtained has excellent dielectric breakdown strength (dielectric breakdown strength) when a DC voltage is applied at a high temperature of about 120°C (100°C to 120°C) and dielectric breakdown strength when an AC voltage is applied, even when the film thickness is as thin as 6.0 μm or less, and has excellent heat shrinkage resistance in terms of suppressing heat shrinkage in the machine direction (MD) at a temperature of about 150°C exceeding the above high temperature. In addition, the film capacitor of the present invention using the above polypropylene film as a capacitor inductor has excellent heat resistance at a high temperature of about 120°C (100°C to 120°C), specifically, has excellent life performance in terms of suppressing the reduction of the electrostatic capacitance of the capacitor when used for a long time at the above high temperature, and has excellent heat shock resistance in terms of suppressing the thermal hardening (deformation) of the capacitor when repeatedly used between the above high and low temperatures in the engine room. Therefore, the polypropylene film of the present invention is suitable for use as a film capacitor, and can be preferably used as an inductor of a capacitor constituting an inverter in a hybrid vehicle / electric vehicle.
[0174] Metal layer integrated polypropylene film capacitor and its manufacturing method
[0175] The polypropylene film of the present invention may be formed into a metal layer integrated polypropylene film having a polypropylene film and a metal layer laminated on one or both sides of the polypropylene film in consideration of processing for capacitors.
[0176] The metal layer functions as an electrode. As the metal used for the metal layer, for example, single metals such as zinc, lead, silver, chromium, aluminum, copper, and nickel, mixtures thereof, and alloys thereof can be used, but zinc and aluminum are preferred in consideration of the environment, economy, and capacitor performance.
[0177] As a method for laminating a metal layer on one or both sides of a polypropylene film, for example, a vacuum evaporation method and a sputtering method can be exemplified. From the viewpoints of productivity and economy, the vacuum evaporation method is preferred. As a vacuum evaporation method, a crucible method, a wire method, etc. can generally be exemplified, but there is no particular limitation, and the best one can be appropriately selected.
[0178] The edge pattern when the metal layer is laminated by vapor deposition is not particularly limited. From the perspective of improving the safety of the capacitor, it is preferred to apply a fishnet pattern or a T-shaped edge pattern on one side of the polypropylene film, including a so-called special edge. This is also effective from the perspective of improving safety and preventing damage and short circuit of the capacitor.
[0179] The method for forming the edge can be used without limitation, and generally known methods such as a tape method and an oil method can be used.
[0180] Furthermore, the metal layer integrated polypropylene film of the present invention can be laminated or wound by a conventionally known method to form a film capacitor.
[0181] That is, the film capacitor may have a structure of stacking a plurality of metal layer integrated polypropylene films, or may have a wound metal layer integrated polypropylene film. Such a film capacitor may be suitable for use as an inverter power supply machine capacitor for controlling a drive motor of an electric vehicle, a hybrid vehicle, etc. In addition, it may also be suitable for use in railway vehicles, wind power generation, solar power generation, general household appliances, etc.
[0182] Example
[0183] Hereinafter, the present invention will be described in detail with reference to Examples and Comparative Examples, but the present invention is not limited to the Examples.
[0184] Resin
[0185] Details of the resins (PP resins A1 to A6 and PP resins B1 to B8) used in Examples and Comparative Examples are summarized in the following Table 1, and methods for measuring the properties thereof are described.
[0186] [Table 1]
[0187]
[0188] PP resin A1~A6: Made by Prime Polymer Co., Ltd.
[0189] PP resin B1: manufactured by Korea Petrochemical Corporation, S802M type A
[0190] PP resin B2: HC300BF manufactured by Borealis Co., Ltd.
[0191] PP resin B3: S800 manufactured by Korea Petrochemical Corporation
[0192] PP resin B4: manufactured by Samsung Total Co., Ltd., HU300
[0193] PP resin B5: manufactured by Korea Petrochemical Corporation, HPT-1 type A
[0194] PP resin B6: manufactured by Korea Petrochemical Corporation, HPT-1 type B
[0195] PP resin B7: manufactured by Korea Petrochemical Corporation, S802M type B
[0196] PP resin B8: manufactured by Korea Petrochemical Corporation, S802M type C.
[0197] 《Determination of number average molecular weight (Mn), weight average molecular weight (Mw), z average molecular weight (Mz), molecular weight distribution (Mw / Mn), molecular weight distribution (Mz / Mn), and weight fraction w of polypropylene resin》
[0198] First, the average molecular weight and molecular weight distribution of each polypropylene resin were measured using SEC (size exclusion chromatography) under the following conditions.
[0199] Apparatus: HLC-8321GPC / HT (detector: differential refractometer (RI)) (manufactured by Tosoh Corporation)
[0200] Column: TSKgel guardcolumnHHR (30)HT (7.5mmI.D.×7.5cm) × 1 column + TSKgel GMHHR-H (20)HT (7.8mmI.D.
[0201] Eluent: 1,2,4-trichlorobenzene (for GPC manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) + BHT (0.05%)
[0202] Flow rate: 1.0mL / min
[0203] Detection conditions: Polarity -(-)
[0204] Injection volume: 0.3mL
[0205] Column temperature: 140°C
[0206] System temperature: 40℃
[0207] Sample concentration: 1mg / mL
[0208] Sample pretreatment: The sample was weighed, added with a solvent (1,2,4-trichlorobenzene to which 0.1% BHT was added), and dissolved by shaking at 140° C. for 1 hour. Thereafter, the sample was heated and filtered using a 0.5 μm sintered filter.
[0209] Calibration curve: A calibration curve was prepared using a fifth-order approximation curve of standard polystyrene manufactured by Tosoh Corporation. The molecular weight was converted to the molecular weight of polypropylene using the Q-factor.
[0210] Based on the obtained standard curve and SEC chromatogram, the molecular weight (logarithmic value) is plotted on the horizontal axis and the integral value of the concentration fraction is plotted on the vertical axis using the analytical software for the measuring device to obtain a molecular weight integral distribution curve. The differential value of the molecular weight integral distribution curve in each molecular weight (the slope of the molecular weight integral distribution curve) is calculated, and the molecular weight (logarithmic value) is plotted on the horizontal axis and the differential value is plotted on the vertical axis to obtain a differential molecular weight distribution curve.
[0211] From these curves, the number average molecular weight Mn, the weight average molecular weight Mw, and the Z average molecular weight Mz are obtained. Using the values of Mw and Mn, the molecular weight distribution (Mw / Mn) is obtained. In addition, the value when the logarithmic molecular weight Log(M)=4.0 in the molecular weight integral distribution curve is taken as the weight fraction w. The weight fraction w represents the weight fraction of molecules with a logarithmic molecular weight Log(M)=4.0, that is, a molecular weight of 10,000 or less.
[0212] The differential distribution value when the logarithmic molecular weight Log(M) = 4.5, the differential distribution value when the logarithmic molecular weight Log(M) = 6.0, and the molecular weight differential distribution value difference (D M ) determination
[0213] In addition, for each polypropylene resin, the differential distribution value when the logarithmic molecular weight Log(M) = 4.5 and the differential distribution value when the logarithmic molecular weight Log(M) = 6.0 are obtained by the following method. First, using the standard curve prepared using the above-mentioned standard polystyrene, the time curve (dissolution curve) of the intensity distribution detected using the RI detector is converted into a distribution curve relative to the molecular weight M (Log(M)) of the standard polystyrene. Next, after obtaining the integral distribution curve relative to Log(M) when the total area of the distribution curve is taken as 100%, the integral distribution curve is differentiated by Log(M) to obtain the differential distribution curve relative to Log(M). From the differential distribution curve, the differential distribution values when Log(M) = 4.5 and Log(M) = 6.0 are read. In addition, the difference between the differential distribution value when Log(M) = 4.5 and the differential distribution value when Log(M) = 6.0 is taken as the molecular weight differential distribution value difference (D M). It should be noted that a series of operations until the differential distribution curve is obtained are performed using analysis software built into the GPC measurement device used.
[0214] 《Determination of Heptane-Insoluble Matter (HI)》
[0215] Each polypropylene resin was press-molded into a size of 10 mm×35 mm×0.3 mm to prepare a sample for measurement of about 3 g. Then, about 150 mL of heptane was added to perform Soxhlet extraction for 8 hours. The heptane-insoluble matter was calculated from the sample mass before and after the extraction.
[0216] 《Determination of melt flow rate (MFR)》
[0217] The melt index of Toyo Seiki Co., Ltd. was used to measure the melt flow rate (MFR) of the raw resin pellets used in the examples and comparative examples according to the condition M of JIS K 7210. Specifically, first, a 4-g sample was inserted into a barrel at a test temperature of 230°C and preheated for 3.5 minutes under a load of 2.16 kg. Thereafter, the weight of the sample extruded from the bottom hole within 30 seconds was measured to determine the MFR (unit: g / 10 minutes or g / 10min). The above measurement was repeated 3 times, and the average value was taken as the measured value of the MFR.
[0218] Examples 1 to 14 and Comparative Examples 1 to 18
[0219] [Manufacturing of biaxially stretched polypropylene film and evaluation of its properties]
[0220] According to Table 2, polypropylene resins A and B are measured and mixed in the weight ratio described in Table 2 to obtain a dry mixed resin composition. Next, the aforementioned dry mixed resin composition is supplied to an extruder and melted at the melting temperature and shear rate of Table 2. The molten resin is extruded with a T die, wound on a metal drum maintaining a surface temperature of 95°C and solidified to prepare a cast blank sheet. The unstretched cast blank sheet is maintained at a temperature of 140°C, stretched to 4.5 times in the flow direction through a roller with a speed difference, and immediately cooled to room temperature. Then, the stretched film obtained by stretching in the flow direction is introduced into a tenter, stretched to 10 times in the width direction at a transverse stretching temperature of 158°C, and then relaxed and heat-set at a relaxation rate of 12%. The biaxially stretched polypropylene film with a width of about 5m and a thickness of 2.3μm is wound around an iron core of about 400mm in diameter under the atmosphere of Table 2, and wound as a large roll. The biaxially stretched polypropylene film after winding was treated in an atmosphere at 35° C. for 24 hours as an aging treatment.
[0221] [Table 2-1]
[0222]
[0223] [Table 2-2]
[0224]
[0225] The following are the methods for measuring the thickness, density and dielectric breakdown strength of the biaxially stretched polypropylene films obtained in each example and comparative example, the method for implementing thermomechanical analysis (TMA), and the method for evaluating the winding quality (wrinkles) during the aging of the large roll. In addition, the results of each measurement and evaluation are shown in Table 2.
[0226] 《Determination of thickness of polypropylene film》
[0227] The paper thickness was measured using a paper thickness measuring instrument MEI-11 manufactured by Citizen Fine Device Co., Ltd. (measuring pressure 100 kPa, descending speed 3 mm / sec, measuring terminal The measuring force is 20.1N). The sample is cut out by the roller without changing when 10 sheets are overlapped. When cutting, the film is handled in a way that wrinkles and air are not introduced into the film. For the sample with 10 sheets overlapped, 5 measurements are carried out, and the average value of the 5 times is divided by 10 to calculate the thickness.
[0228] 《Determination of density of polypropylene film》
[0229] The density of the polypropylene film was measured according to JIS K7112 (1999) D method.
[0230] Measuring device: Density gradient tube specific gravity measuring device type A manufactured by Shibayama Scientific Instruments Co., Ltd.
[0231] Gradient solution: ethanol-water solution
[0232] Measurement temperature: 23±0.5℃
[0233] Number of measurements: n = 3
[0234] 《Determination of dielectric breakdown strength of polypropylene films: direct current (DC)》
[0235] The dielectric breakdown voltage (BDV) of the polypropylene film of the embodiment and the comparative example was measured 16 times under the following test conditions using the electrode configuration described in JIS C2151 (2006) 17.2.2 (flat electrode method). It should be noted that the applied voltage at the moment when the leakage current of the following upper limit reference value is detected during the voltage increase process is taken as BDV. The BDV is divided by the thickness (μm) of the film, and the average value of 12 points after removing the two highest points and the two lowest points from the 16 measurement results is taken as the dielectric breakdown strength ES (VDC / μm).
[0236] Test piece: about 150mm×150mm
[0237] Conditioning of test piece: 30 minutes under atmospheric conditions
[0238] Power supply: DC
[0239] Atmosphere: Air, 120℃
[0240] Testing machine: DC withstand voltage / insulation resistance testing machine TOS9213AS manufactured by Kikusui Electronics Co., Ltd.
[0241] Voltage rise speed: 100V / s
[0242] Current detection response speed: MID
[0243] Upper limit reference value: 5mA
[0244] 《Determination of dielectric breakdown strength of polypropylene films: alternating current (AC)》
[0245] The dielectric breakdown voltage (BDV) of the films of the examples and comparative examples was measured 12 times under the following test conditions using the electrode configuration described in JIS C2151 (2006) 17.2.2 (flat electrode method). It should be noted that the applied voltage at the moment when the leakage current of the following upper limit reference value is detected during voltage boost is taken as BDV. The BDV is divided by the thickness (μm) of the film, and the average value of the 8 points after removing the 2 highest points and the 2 lowest points from the 12 measurement results is taken as the dielectric breakdown strength ES (VAC / μm). Test piece: approximately 150 mm × 150 mm
[0246] Conditioning of test piece: 30 minutes under atmospheric conditions
[0247] Power supply: AC
[0248] Atmosphere: Air, 100℃, 110℃, 120℃
[0249] Tester: Withstand voltage tester TOS5051A manufactured by Kikusui Electronics Co., Ltd.
[0250] Voltage rise speed: 100V / s
[0251] Upper limit reference value: 5mA
[0252] 《Thermomechanical Analysis (TMA)》
[0253] Thermomechanical analysis was performed as follows.
[0254] Device: EXSTAR6000 and TMA / SS6000 manufactured by Seiko Instruments Inc.
[0255] Film width: 4mm
[0256] Chuck spacing: 15mm
[0257] Load: 2.17N / mm 2
[0258] Measuring temperature range: 25℃~155℃
[0259] Heating rate: 10℃ / min
[0260] When drawing a heating dimensional change curve with the horizontal axis as temperature and the vertical axis as the dimensional change rate in the mechanical direction (MD) of the film, a dimensional change rate of 0% or more during the heating process from 25°C to 155°C is recorded as qualified "A", and a dimensional change rate of less than 0% is recorded as unqualified "C".
[0261] 《Coiling quality (wrinkles) after aging of large rolls》
[0262] The appearance of the large coil after aging with about 100 mm of both ends removed was evaluated from the viewpoint of coiling quality (wrinkles). It should be noted that the following die (longitudinal die) refers to a defect in the coiling shape such as a ribbed metal can that occurs parallel to the circumferential direction and is generally called MD line or can shape.
[0263] If there is no circumferential mold (longitudinal mold) with a depth of 0.5 mm or more, it is recorded as "AA".
[0264] If there is only one die (vertical die) with a depth of 0.5 mm or more, it is rated as good "A".
[0265] If there are 2 or 3 circumferential molds (vertical molds) with a depth of 0.5 mm or more, it is recorded as "B"
[0266] The presence of four or more circumferential molds (longitudinal molds) with a depth of 0.5 mm or more is recorded as a defective "C". In the case of the above-mentioned excellent "AA", even if there are circumferential molds (longitudinal molds), it can be said that the depth is less than 0.5 mm and the width direction is basically uniform. Here, excellent "AA" and good "A" are qualified (allowable range), and "B" and defective "C" are unqualified.
[0267] [Manufacturing of film capacitors and evaluation of their characteristics]
[0268] Using the biaxially stretched polypropylene films obtained in the respective Examples and Comparative Examples, film capacitors were produced according to the following procedures.
[0269] A special vapor deposition pattern edge and an insulating edge for providing security to the film capacitor are formed on the biaxially stretched polypropylene film, and aluminum vapor deposition is performed in such a way that the surface resistivity of the metal film becomes 20Ω / □, thereby obtaining a metal layer integrated polypropylene film. Next, after the metal layer integrated polypropylene film is cut into any width, two metal layer integrated polypropylene films are combined and wound using an automatic winder 3KAW-N2 manufactured by Kaito Seisakusho, with a winding speed of 4m / sec, a winding tension of 180g, and a contact roller contact pressure of 260g, and the number of turns is set so that the electrostatic capacitance of the element becomes 50μF.
[0270] The wound element was flattened by pressurization, and then zinc metal was sprayed on the end surface of the element under pressure to form an electrode lead-out portion, and then heated at 120°C for 15 hours to thermally cure it.
[0271] After thermal curing, the lead wires were soldered to the end faces of the element and sealed with epoxy resin to obtain a flat film capacitor. The electrostatic capacitance of the obtained film capacitors was 50 μF (±3 μF).
[0272] The following is a method for evaluating the vapor deposition processability, element winding processability, life (life) characteristics, and thermal shock resistance of the film capacitors obtained in each example and comparative example.
[0273] 《Evaporation Processability》
[0274] The case where the occurrence rate of wrinkles due to thermal deformation in the film after vapor deposition was less than 5% was marked as "A", and the case where it was 5% or more was marked as "C".
[0275] 《Evaluation of component winding processability》
[0276] Using the winding reel at the left edge and the winding reel at the right edge of the small coil obtained by vapor deposition / cutting, overlap two sheets and wind them in a way that the vapor deposition part overflows from the edge part in the width direction (component winding process). The winding is performed using an automatic winder 3KAW-N2 model manufactured by Kaito Seisakusho Co., Ltd., and 1360 strands are performed at a winding tension of 200g. At this time, visual observation is made from the beginning to the end of the coil, and wrinkles and misalignments are recorded as unqualified, and the ratio of the number of unqualified but percentage-expressed numbers to the total number of manufactured products is used as an indicator of processability (hereinafter referred to as component winding yield). The higher the component winding yield, the better. 95% or more is evaluated as good "A", and less than 95% is evaluated as poor "C".
[0277] 《Lifespan characteristics (capacitance change rate)》
[0278] The initial electrostatic capacitance of the capacitor before the test was measured using LCR High tester 3522-50 manufactured by Hioki Electric Co., Ltd. Then, the capacitor was continuously loaded with a DC voltage of 800V (348V / μm) for 500 hours in a high-temperature tank at 115°C. Similarly, the electrostatic capacitance of the capacitor after 500 hours was measured, and the capacitance change rate before and after the voltage load was calculated according to the following formula. The test was performed on 2 samples, and the evaluation was performed based on the average value.
[0279] (Change rate of electrostatic capacitance) = [(Electrostatic capacitance after voltage load) - (Initial electrostatic capacitance)] / (Initial electrostatic capacitance) × 100 (%)
[0280] The capacity change rate after 500 hours was rated as good "A" if it was within -4%, "B" if it was more than -4% and less than -6%, and "C" if it was more than -6%.
[0281] 《Heat shock resistance (change rate of tanδ)》
[0282] The obtained capacitor was placed in a thermal shock test device (Espec TSA-101S-W), and the temperature was rapidly increased and decreased 500 times between the lower limit temperature of -40°C and the upper limit temperature of 105°C. Specifically, 50 minutes at -40°C and 50 minutes at 105°C were repeated 500 times as a group. It should be noted that the temperature switching is as follows: air at the set temperature is delivered and forced to be replaced. In addition, the temperature switching time is also included in the 50-minute holding time.
[0283] Tan δ before and after the heat shock test was measured using LCR High Tester 3522-50 manufactured by Hioki Electric Co., Ltd. The increase rate of tan δ was calculated according to the following formula.
[0284] (increase rate of tan δ) = [(tan δ after thermal shock test) - (tan δ before thermal shock test)] / (tan δ before thermal shock test) × 100 (%)
[0285] The test was performed on three samples, and evaluation was performed based on the average value.
[0286] An increase rate of 100% or less was rated as good "A", an increase rate of more than 100% and 105% or less was rated as "B", and an increase rate of more than 105% was rated as bad "C".
[0287] Investigation
[0288] The polypropylene films of the present invention produced in Examples 1 to 14 have molecular weight distribution (Mw / Mn) of weight average molecular weight Mw and number average molecular weight Mn of the polypropylene resin constituting the films, Z average molecular weight Mz, and weight fraction w when logarithmic molecular weight Log(M)=4.0 in the molecular weight integral distribution curve within the prescribed ranges. Thus, when the film is as thin as 6.0 μm or less in thickness, the films have excellent dielectric breakdown strength (dielectric breakdown strength) when a direct current voltage is applied at a high temperature of about 120° C. (100° C. to 120° C.) and dielectric breakdown strength when an alternating current voltage is applied, and have excellent heat shrinkage resistance in that heat shrinkage in the machine direction (MD) is suppressed at temperatures exceeding the above high temperature up to about 150° C. In addition, the film capacitors produced in the examples have excellent heat resistance at high temperatures of about 120°C (100°C to 120°C), and specifically, have excellent life performance in that the reduction in the electrostatic capacitance of the capacitor is suppressed when used for a long time at the above high temperature, and have excellent heat shock resistance in that the thermal reinforcement (deformation) of the capacitor is suppressed when used repeatedly between the above high and low temperatures in the engine room. In addition, the polypropylene film according to the present invention has also obtained good evaluation results in terms of appearance (winding quality (wrinkles)) after large roll aging, vapor deposition processability during capacitor production, and element winding processability.
Claims
1. A polypropylene film, characterized in that The polypropylene resin constituting the polypropylene film is as follows: The molecular weight distribution (Mw / Mn) of the weight average molecular weight Mw and the number average molecular weight Mn is 5.0 or more and 6.9 or less, · Z average molecular weight Mz is 650,000 or more and 945,000 or less, The weight fraction w when the logarithmic molecular weight Log(M)=4.0 in the molecular weight integrated distribution curve is 2.6% or more and 4.2% or less, The polypropylene film is as follows: ·It is a biaxially stretched film. · The thickness is 0.8 μm or more and 6.0 μm or less, Density: 919g / cm 3 Above and 925g / cm 3 the following.
2. The polypropylene film according to claim 1, which is used for capacitors.
3. The polypropylene film according to claim 1 or 2, wherein In the thermomechanical analysis, the 2 Under a load, the temperature is increased from 25°C to 155°C at a rate of 10°C / min, and the horizontal axis is taken as the temperature and the vertical axis is taken as the dimensional change rate in the mechanical direction (MD) of the film. When a heating dimensional change curve is drawn, the dimensional change rate in the heating process from 25°C to 155°C is greater than 0%.
4. The polypropylene film according to claim 1 or 2, wherein Dielectric breakdown strength under DC voltage at 120°C (V DC120℃ ) and the dielectric breakdown strength under AC voltage at 120°C (V AC120℃ ) difference (V DC120℃ -V AC120℃ ) is greater than or equal to 280 V / μm and less than or equal to 300 V / μm.
5. The polypropylene film according to claim 1 or 2, wherein Said Mz exceeds 700,000.
6. The polypropylene film according to claim 1 or 2, wherein The molecular weight distribution (Mw / Mn) is 5.0 or more and 6.6 or less, The Mz is greater than or equal to 720,000 and less than or equal to 790,000, The weight fraction w is 3.5% or more and 3.7% or less.
7. The polypropylene film according to claim 1 or 2, wherein The polypropylene resin contains polypropylene resin A and polypropylene resin B, the content of the polypropylene resin A in the polypropylene resin is greater than the content of the polypropylene resin B in the polypropylene resin, The Mw of the polypropylene resin A is 275,000 or more and less than 350,000, The molecular weight distribution (Mw / Mn) of the polypropylene resin A is 5.8 or more and 10.0 or less, The melt flow rate (MFR) of the polypropylene resin A A ) is 4.8 g / 10 minutes or more and 5.5 g / 10 minutes or less, The Mw of the polypropylene resin B is 350,000 or more and 550,000 or less, The molecular weight distribution (Mw / Mn) of the polypropylene resin B is 5.0 or more and 11.0 or less, The melt flow rate (MFR) of the polypropylene resin B B ) is 0.1 g / 10 minutes or more and 4.5 g / 10 minutes or less.
8. The polypropylene film according to claim 1 or 2, wherein The polypropylene resin contains polypropylene resin A and polypropylene resin B, the content of the polypropylene resin A in the polypropylene resin is greater than the content of the polypropylene resin B in the polypropylene resin, The Mw of the polypropylene resin B is 385,000 or more and 550,000 or less, The molecular weight distribution (Mw / Mn) of the polypropylene resin B is 8.4 or more and 11.0 or less, The melt flow rate (MFR) of the polypropylene resin B B ) is 0.1 g / 10 minutes or more and 2.2 g / 10 minutes or less, The Mw of the polypropylene resin A is 250,000 or more and less than 350,000, The molecular weight distribution (Mw / Mn) of the polypropylene resin A is 5.0 or more and 10.0 or less, The melt flow rate (MFR) of the polypropylene resin A A ) is 4.8 g / 10 minutes or more and 10.0 g / 10 minutes or less.
9. The polypropylene film according to claim 7, wherein The ratio of the mass of the polypropylene resin A to the total mass of the polypropylene resin A and the polypropylene resin B is 65 to 75 mass %.
10. The polypropylene film according to claim 1 or 2, wherein: The polypropylene film has a thickness of 1.0 μm or more and 6.0 μm or less.
11. A metal layer integrated polypropylene film, comprising: The polypropylene film according to any one of claims 1 to 10; and A metal layer is laminated on one or both sides of the polypropylene film. 12 . A film capacitor comprising the metal layer integrated polypropylene film according to claim 11 which is wound, or a structure in which a plurality of metal layer integrated polypropylene films according to claim 11 are stacked.