Weather-resistant water-based acrylic emulsion as well as preparation method and application thereof

By using specific formula composition and step-by-step polymerization technology in aqueous acrylic emulsions, the problems of weather resistance and production efficiency of existing aqueous acrylic resins in building exterior walls and outdoor facilities are solved, achieving high hardness, flexibility and durability The coating properties are suitable for the construction and industrial coatings fields.

CN118930719APending Publication Date: 2024-11-12深圳市深赛尔股份有限公司
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411063076.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the use environment of building exterior walls and outdoor facilities, existing water-based acrylic synthetic resins are difficult to take into account high hardness, flexibility, adhesion and excellent durability. The complexity of formula and process parameters are strictly required to limit the efficiency of large-scale production. and economical.

Method used

Using a weather-resistant aqueous acrylic emulsion, composed and prepared by specific formulations, including acrylate monomers, methyl methacrylate, fluorine-containing acrylate, maleic anhydride, N-vinylpyrrolidone, emulsifier, nanoparticles , light stabilizer and temperature-sensitive monomer to form a pre-emulsion for step-by-step polymerization to ensure uniform dispersion and efficient utilization of the resin, and add nanosilicon dioxide or alumina to improve hardness and density.

Benefits of technology

It significantly improves the weather resistance, physical and mechanical properties and construction properties of the coating, can effectively resist ultraviolet rays, wet temperature changes and acid rain erosion, meets the high standards of building exterior walls and outdoor facilities, and reduces production complexity and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930719A_ABST
    Figure CN118930719A_ABST
Patent Text Reader

Abstract

The invention relates to the field of synthetic resin, in particular to weather-resistant waterborne acrylic emulsion as well as a preparation method and application thereof. The weather-resistant water-based acrylic emulsion is prepared from an acrylate monomer, methyl methacrylate, fluorine-containing acrylate, maleic anhydride, N-vinyl pyrrolidone, an emulsifier, nano particles, an initiator, a light stabilizer and a temperature-sensitive monomer, the preparation method comprises the following steps: pre-emulsifying different acrylic monomers to obtain a pre-emulsion A and a pre-emulsion B, and preparing the water-based acrylic emulsion by using a neutralizing reagent and taking water as a dispersion medium. By designing the raw material formula and the preparation method, the water-based acrylic emulsion is prepared, and through the synergistic effect of all the components, the corresponding coating product can effectively resist ultraviolet rays, humidity and temperature changes and acid rain erosion, meanwhile, good physical and mechanical properties and construction performance are kept, and the service life of the coating is prolonged. Therefore, the high-standard requirements of building exterior wall coatings and outdoor facility protection are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of synthetic resins, and in particular to a weather-resistant water-based acrylic emulsion and a preparation method and application thereof. Background Art

[0002] Waterborne acrylic synthetic resin is an environmentally friendly coating base material that has been rapidly developed and applied in the coating industry in recent years. This type of resin is prepared from acrylic ester monomers through emulsion polymerization or solution polymerization technology. It has the advantages of low VOC content, good environmental performance, excellent weather resistance, chemical resistance, and easy construction and cleaning. It is used in many fields such as building exterior wall coatings, outdoor facility protection, and decoration.

[0003] However, in the use environment of building exterior walls, outdoor facilities, etc., water-based acrylic synthetic resin coatings need to be exposed to ultraviolet radiation, temperature changes and high humidity environments for a long time, resulting in a decrease in weather resistance and physical properties. Existing water-based acrylic resins are difficult to take into account high hardness, flexibility, adhesion and excellent durability. In addition, the complexity of the formula and the strict requirements on process parameters also limit the efficiency and economy of its large-scale production. Therefore, a water-based acrylic synthetic resin with better weather resistance and environmental friendliness is needed to meet the growing demand for high-performance and multifunctional coatings in the field of modern architectural and industrial coatings. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention aims to provide a weather-resistant water-based acrylic emulsion and a preparation method and application thereof.

[0005] A weather-resistant water-based acrylic emulsion, comprising the following components in parts by mass: 50-70 parts of acrylic acid ester monomers, 5-15 parts of methyl methacrylate, 2-8 parts of fluorinated acrylic acid esters, 1-5 parts of maleic anhydride, 1-5 parts of N-vinyl pyrrolidone, 1-5 parts of emulsifiers, 0.1-1 parts of nanoparticles, 0.1-0.8 parts of initiators, 0.1-1 parts of light stabilizers, and 0.1-1 parts of temperature-sensitive monomers; The acrylic acid ester monomers include 15-30 parts of butyl acrylate, 10-25 parts of ethyl acrylate, 5-15 parts of acrylic acid, 2-8 parts of lauryl methacrylate and 2-6 parts of lactic acid acrylate; The light stabilizer is a hindered amine light stabilizer, and the temperature-sensitive monomer is N-isopropyl acrylamide.

[0006] The flexible chain segments of butyl acrylate and ethyl acrylate can enhance the flexibility of the resin, while the carboxyl group of acrylic acid provides polarity to the resin, which helps to improve the adhesion to the substrate. The hydrophobic chain segments of lauryl methacrylate and lactic acid acrylate increase the water resistance and chemical resistance of the resin, so that the final coating product can maintain good performance.

[0007] Maleic anhydride, as a functional monomer, can undergo cross-linking reaction with the active groups in the resin to form a three-dimensional network structure, significantly improving the cohesion and chemical resistance of the resin; N-vinyl pyrrolidone provides temperature sensitivity to the resin, enabling it to exhibit intelligent response at different temperatures, which is beneficial for the coating to remain stable under changing climatic conditions.

[0008] HALS light stabilizers are the key to UV protection. They effectively slow down the aging of resins by capturing free radicals and inhibiting photooxidation processes. N-isopropylacrylamide, as a thermosensitive monomer, has a phase transition temperature close to room temperature, which enables the coating to self-regulate in the face of changes in temperature and humidity, maintaining good physical and mechanical properties and improving the protective effects of building exterior walls and outdoor facilities.

[0009] Furthermore, the emulsifier is 0.5-3 parts by mass of anionic emulsifier and 0.5-3 parts by mass of nonionic emulsifier, the anionic emulsifier is sodium lauryl sulfate, and the nonionic emulsifier is polyoxyethylene octyl phenyl ether.

[0010] Emulsifiers (sodium lauryl sulfate and polyoxyethylene octylphenyl ether) ensure uniform dispersion of the monomers and promote the stability of the emulsion.

[0011] Furthermore, the composition by weight also includes 0.05-0.5 parts of a reducing agent and 0.01-0.5 parts of a chain transfer agent.

[0012] Furthermore, the initiator is a water-soluble ammonium persulfate initiator, the reducing agent is sodium bisulfite, and the chain transfer agent is tert-dodecyl mercaptan.

[0013] Water-soluble ammonium persulfate initiators and tert-dodecyl mercaptan chain transfer agents precisely control the polymerization reaction rate and molecular weight distribution to obtain synthetic resins with balanced properties.

[0014] Furthermore, the nanoparticles are nano-silicon dioxide or nano-aluminum oxide.

[0015] Adding nano-silica or nano-alumina can greatly improve the hardness and wear resistance of the coating. At the same time, by filling the micropores in the resin, the density of the coating is enhanced to form a solid physical barrier, further improving the coating's resistance to acid rain, humidity, heat and other harsh environmental factors.

[0016] A method for preparing a weather-resistant water-based acrylic emulsion comprises the following steps: (1) Pre-emulsify butyl acrylate, ethyl acrylate, methyl methacrylate and 1 / 4 emulsifier with deionized water to obtain pre-emulsion A; (2) pre-emulsifying acrylic acid, lauryl methacrylate, lactic acid acrylate, fluorinated acrylate, maleic anhydride, N-vinyl pyrrolidone, and 1 / 4 emulsifier with deionized water to obtain pre-emulsion B; (3) Add deionized water and the remaining emulsifier into the reactor, raise the temperature to the reaction temperature, add 1 / 2 initiator and 1 / 10 pre-emulsion A, and start the polymerization reaction; (4) During the polymerization reaction, the remaining pre-emulsion A is slowly added to the reactor and reacted for 2.5-4 hours; (5) After the reaction is completed, add a neutralizer to neutralize and adjust the pH to 7.5-8.5; (6) Add the remaining initiator and pre-emulsion B and continue the reaction for 2.5-5 hours until the polymerization is completed; (7) Cooling and filtering. In the post-processing stage, light stabilizer, nanoparticles and thermosensitive monomer are added and mixed evenly to obtain a water-based acrylic emulsion.

[0017] Different functional monomers and emulsifiers are pre-emulsified separately to form pre-emulsion A and pre-emulsion B. The step-by-step pre-emulsification ensures the uniform dispersion of the monomers and the stability of the emulsion, avoiding the phase separation or gelation problems that may occur when all monomers are added at one time. At the same time, the step-by-step pre-emulsification can accurately control the polymerization order and rate of the monomers, promote the efficient utilization of functional monomers, and thus optimize the comprehensive performance of the resin.

[0018] By gradually adding pre-emulsion A to the reacting system instead of adding it all at once, and precisely controlling the reaction temperature, the controllability of the polymerization reaction and the uniformity of the product molecular weight are ensured; the gradual addition strategy combined with temperature control can effectively avoid the explosion phenomenon in the polymerization reaction, reduce the occurrence of side reactions, ensure that the resin emulsion has stable physical and chemical properties, and improve the uniformity and predictability of the product.

[0019] After the polymerization reaction of the raw materials of pre-emulsion A is completed, a neutralizer is added to adjust the pH value to an appropriate range. Fine adjustment of the pH value can improve the water solubility of the resin, enhance the compatibility with additives such as light stabilizers, nanoparticles and thermosensitive monomers, ensure the uniform distribution of these additives in the resin system, and thus improve the overall performance of the resin.

[0020] Adding light stabilizers, nanoparticles and thermosensitive monomers in the post-processing stage rather than during the polymerization reaction helps to maintain the activity of the additives and avoid their decomposition at high temperatures or unnecessary side reactions with the monomers. Optimizing additives in the post-processing stage ensures the best performance of these components in the resin emulsion, improves the weather resistance, hardness and intelligent responsiveness of the resin, and provides the final coating product with better protection and usage experience.

[0021] After the polymerization reaction is completed, the system is cooled to room temperature, and unreacted monomers and possible gel particles are removed by filtration to ensure the final quality of the resin emulsion.

[0022] Furthermore, the neutralizing agent is one or more combinations of ammonia water, N,N-2-methylethanolamine or aminomethyl propanol.

[0023] Furthermore, the reaction temperature is 70-90° C., and the total polymerization reaction time is 5.5-8 h.

[0024] Furthermore, the solid content of the aqueous acrylic emulsion is 55-65%.

[0025] The invention discloses an application of a water-based acrylic emulsion, wherein the water-based acrylic emulsion is used in the production of water-based coatings related to building exterior walls, outdoor facility protection and decoration.

[0026] Building exterior wall paint: The low VOC (volatile organic compound) content of water-based acrylic synthetic resin makes it the preferred paint base material for green buildings, which not only reduces pollution to the environment but also protects the health of residents. Through optimized formula, water-based acrylic synthetic resin can provide excellent weather resistance, effectively resist ultraviolet rays, temperature changes, humidity fluctuations and acid rain erosion, ensuring that the building exterior wall has long-lasting bright colors and stable structure.

[0027] Protection of outdoor facilities: For outdoor facilities such as metal and wood, water-based acrylic synthetic resin coatings can provide effective anti-corrosion and anti-rust protection, extend the service life of the facilities and reduce maintenance costs; outdoor facilities are often subject to physical wear and accidental impacts, and the high hardness and toughness of water-based acrylic synthetic resin coatings can provide good wear resistance and impact resistance, keeping the appearance of the facilities neat and tidy; the smooth surface formed by water-based acrylic synthetic resin coatings is not easy to absorb dust and pollutants, which is convenient for daily cleaning and reduces the difficulty and frequency of maintenance of outdoor facilities.

[0028] Decorative coatings: Water-based acrylic synthetic resin coatings are not limited to protective functions, but can also be used as a medium for creative expression to create unique wall decoration effects through artistic techniques to meet personalized decoration needs; especially in sensitive areas such as children's rooms, hospitals and schools, water-based acrylic synthetic resin coatings have low toxicity, no irritating odor and easy cleaning properties, making them an ideal choice for wall decoration.

[0029] The beneficial effects achieved by the present invention are: 1. The present invention improves the comprehensive performance of waterborne acrylic resin by designing raw material formula and preparation method, optimizing monomer composition, introducing functional monomers and additives, and improving preparation process. Through the synergistic effect of various components, the corresponding coating product can effectively resist ultraviolet rays, humidity and temperature changes and acid rain erosion, improve weather resistance, and maintain good physical and mechanical properties and construction performance, thereby meeting the high standard requirements of building exterior wall coatings and outdoor facility protection.

[0030] 2. The present invention uses fluorinated acrylates and light stabilizers to improve UV resistance. Fluorinated acrylates can effectively resist the degradation of ultraviolet rays and enhance the light stability of the coating. Light stabilizers can absorb ultraviolet rays, prevent or slow down the photo-oxidative decomposition of polymer chains, and extend the service life of the coating.

[0031] 3. The present invention selects N-isopropylacrylamide as a temperature-sensitive monomer, and utilizes its phase transition temperature close to room temperature to make the coating show intelligent response when the temperature changes, which helps the coating maintain good physical and mechanical properties under different temperature and humidity conditions. Maleic anhydride and acrylic acid monomers are copolymerized to introduce additional cross-linking points, thereby enhancing the cohesion of the coating and improving its stability and mechanical strength under hot and humid conditions.

[0032] 4. The present invention uses lactic acid-based acrylate to improve the film-forming properties of the coating, help form a continuous and tough coating, and enhance overall weather resistance. Lauryl methacrylate is used to improve the weather resistance and chemical resistance of the coating, and its long-chain alkyl structure enhances the hydrophobicity of the coating and reduces erosion by water and acid rain.

[0033] 5. The present invention uses acrylic acid and utilizes acidic groups to improve the resistance of the coating to acidic substances. At the same time, the carboxylic acid group of the acrylic acid monomer can neutralize the acidic substances and reduce the erosion of the coating by acid rain. Nano-silicon dioxide is used to enhance the density and hardness of the coating, forming a protective barrier to further reduce the direct erosion of the coating substrate by acid rain. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 A schematic flow chart of a method for preparing a weather-resistant water-based acrylic emulsion used in an embodiment of the present invention; Figure 2 The weather-resistant water-based acrylic emulsion used in the embodiment of the present invention is used to prepare a water-based coating formula; Figure 3 The test results of film appearance, viscosity and drying time of the water-based coating of the weather-resistant water-based acrylic emulsion used in the embodiments of the present invention; Figure 4These are the test results of pencil hardness, acid resistance, artificial aging resistance, and humidity change resistance of the water-based coating of the weather-resistant water-based acrylic emulsion used in the embodiments of the present invention. DETAILED DESCRIPTION

[0035] The present invention is further described in detail below in conjunction with specific embodiments.

[0036] Example 1: A weather-resistant aqueous acrylic emulsion, comprising the following components in parts by mass: 62 parts of acrylic acid ester monomer, 10 parts of methyl methacrylate, 5 parts of fluorinated acrylic acid ester, 3 parts of maleic anhydride, 3 parts of N-vinyl pyrrolidone, 2 parts of emulsifier, 0.5 parts of nano-silicon dioxide, 0.4 parts of initiator, 0.3 parts of light stabilizer, 0.5 parts of temperature-sensitive monomer, 0.2 parts of reducing agent and 0.1 parts of chain transfer agent; The acrylic monomers include 25 parts of butyl acrylate, 20 parts of ethyl acrylate, 8 parts of acrylic acid, 5 parts of lauryl methacrylate and 4 parts of lactic acid acrylate; The light stabilizer is a hindered amine light stabilizer [bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate], and the temperature-sensitive monomer is N-isopropylacrylamide.

[0037] The emulsifier is 1 part by mass of anionic emulsifier and 1 part by mass of nonionic emulsifier, the anionic emulsifier is sodium lauryl sulfate, and the nonionic emulsifier is polyoxyethylene octylphenyl ether.

[0038] The initiator is a water-soluble ammonium persulfate initiator, the reducing agent is sodium bisulfite, and the chain transfer agent is tert-dodecyl mercaptan.

[0039] A method for preparing a weather-resistant water-based acrylic emulsion, such as Figure 1 As shown, the following steps are included: (1) Pre-emulsify butyl acrylate, ethyl acrylate, methyl methacrylate and 1 / 4 emulsifier with deionized water to obtain pre-emulsion A; (2) pre-emulsifying acrylic acid, lauryl methacrylate, lactic acid acrylate, fluorinated acrylate, maleic anhydride, N-vinyl pyrrolidone, and 1 / 4 emulsifier with deionized water to obtain pre-emulsion B; (3) Add deionized water and the remaining emulsifier into the reactor, raise the temperature to 80°C, add 1 / 2 initiator and 1 / 10 pre-emulsion A, and start the polymerization reaction; (4) During the polymerization reaction, the remaining pre-emulsion A was slowly added into the reactor and reacted for 3 hours; (5) After the reaction is completed, add ammonia water as a neutralizer to neutralize and adjust the pH to 7.5; (6) Add the remaining initiator and pre-emulsion B and continue the reaction for 4 hours until the polymerization is completed; (7) Cooling and filtering. In the post-processing stage, light stabilizer, nano-silica and temperature-sensitive monomer are added and mixed evenly to obtain a water-based acrylic emulsion with a solid content of 60%.

[0040] Example 2: A weather-resistant aqueous acrylic emulsion, comprising the following components in parts by mass: 55 parts of acrylic acid ester monomer, 12 parts of methyl methacrylate, 7 parts of fluorinated acrylic acid ester, 4 parts of maleic anhydride, 4 parts of N-vinyl pyrrolidone, 2.5 parts of emulsifier, 0.7 parts of nano-alumina, 0.5 parts of initiator, 0.4 parts of light stabilizer, 0.6 parts of temperature-sensitive monomer, 0.3 parts of reducing agent and 0.2 parts of chain transfer agent; The acrylic monomers include 23 parts of butyl acrylate, 18 parts of ethyl acrylate, 7 parts of acrylic acid, 4 parts of lauryl methacrylate and 3 parts of lactic acid acrylate; The light stabilizer is a hindered amine light stabilizer [bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate], and the temperature-sensitive monomer is N-isopropylacrylamide.

[0041] The emulsifier is 1 part by mass of anionic emulsifier and 1.5 parts by mass of nonionic emulsifier, the anionic emulsifier is sodium lauryl sulfate, and the nonionic emulsifier is polyoxyethylene octylphenyl ether.

[0042] The initiator is a water-soluble ammonium persulfate initiator, the reducing agent is sodium bisulfite, and the chain transfer agent is tert-dodecyl mercaptan.

[0043] A method for preparing a weather-resistant water-based acrylic emulsion, such as Figure 1 As shown, the following steps are included: (1) Pre-emulsify butyl acrylate, ethyl acrylate, methyl methacrylate and 1 / 4 emulsifier with deionized water to obtain pre-emulsion A; (2) pre-emulsifying acrylic acid, lauryl methacrylate, lactic acid acrylate, fluorinated acrylate, maleic anhydride, N-vinyl pyrrolidone, and 1 / 4 emulsifier with deionized water to obtain pre-emulsion B; (3) Add deionized water and the remaining emulsifier into the reactor, raise the temperature to 75°C, add 1 / 2 initiator and 1 / 10 pre-emulsion A, and start the polymerization reaction; (4) During the polymerization reaction, the remaining pre-emulsion A was slowly added into the reactor and reacted for 4 hours; (5) After the reaction is completed, add ammonia water as a neutralizer to neutralize and adjust the pH to 8.0; (6) Add the remaining initiator and pre-emulsion B and continue the reaction for 3.5 hours until the polymerization is complete; (7) Cooling and filtering. In the post-processing stage, light stabilizer, nano-alumina and temperature-sensitive monomer are added and mixed evenly to obtain a water-based acrylic emulsion with a solid content of 55%.

[0044] Example 3: A weather-resistant aqueous acrylic emulsion, comprising the following components in parts by mass: 68 parts of acrylic acid ester monomer, 7 parts of methyl methacrylate, 3 parts of fluorinated acrylic acid ester, 2 parts of maleic anhydride, 5 parts of N-vinyl pyrrolidone, 3 parts of emulsifier, 0.3 parts of nano-silicon dioxide, 0.7 parts of initiator, 0.5 parts of light stabilizer, 0.3 parts of temperature-sensitive monomer, 0.4 parts of reducing agent and 0.3 parts of chain transfer agent; The acrylic monomers include 27 parts of butyl acrylate, 22 parts of ethyl acrylate, 9 parts of acrylic acid, 6 parts of lauryl methacrylate and 4 parts of lactic acid acrylate; The light stabilizer is a hindered amine light stabilizer [bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate], and the temperature-sensitive monomer is N-isopropylacrylamide.

[0045] The emulsifier is 1.5 parts by mass of anionic emulsifier and 1.5 parts by mass of nonionic emulsifier, the anionic emulsifier is sodium lauryl sulfate, and the nonionic emulsifier is polyoxyethylene octylphenyl ether.

[0046] The initiator is a water-soluble ammonium persulfate initiator, the reducing agent is sodium bisulfite, and the chain transfer agent is tert-dodecyl mercaptan.

[0047] A method for preparing a weather-resistant water-based acrylic emulsion, such as Figure 1 As shown, the following steps are included: (1) Pre-emulsify butyl acrylate, ethyl acrylate, methyl methacrylate and 1 / 4 emulsifier with deionized water to obtain pre-emulsion A; (2) pre-emulsifying acrylic acid, lauryl methacrylate, lactic acid acrylate, fluorinated acrylate, maleic anhydride, N-vinyl pyrrolidone, and 1 / 4 emulsifier with deionized water to obtain pre-emulsion B; (3) Add deionized water and the remaining emulsifier into the reactor, raise the temperature to 85°C, add 1 / 2 initiator and 1 / 10 pre-emulsion A, and start the polymerization reaction; (4) During the polymerization reaction, the remaining pre-emulsion A was slowly added to the reactor and reacted for 2.5 hours; (5) After the reaction is completed, add ammonia water as a neutralizer to neutralize and adjust the pH to 7.2; (6) Add the remaining initiator and pre-emulsion B and continue the reaction for 3 hours until the polymerization is completed; (7) Cooling and filtering. In the post-processing stage, light stabilizer, nano-silica and temperature-sensitive monomer are added and mixed evenly to obtain a water-based acrylic emulsion with a solid content of 65%.

[0048] The light stabilizer and the thermosensitive monomer of Examples 1 to 3 are added as follows: the light stabilizer is dispersed in deionized water to form a uniform suspension, and the suspension is slowly added to the resin emulsion cooled to room temperature using a metering pump; the thermosensitive monomer is dissolved in deionized water, added to the completely cooled resin emulsion, gently stirred for 30 minutes and allowed to stand.

[0049] Verification Example: The aqueous acrylic emulsions prepared in Examples 1 to 3 are formulated into aqueous coatings, the formula of which is as follows: Figure 2 As shown; and the performance test of the formulated water-based coating was carried out: 1. Coating appearance: In accordance with the provisions of GB / T 9761-2007 "Appearance inspection method for coating products", the visual effect and surface integrity of the coating are evaluated by combining visual inspection and touch.

[0050] 2. Viscosity test: According to the guidance of GB / T 1723-2018 "Determination of Coating Viscosity", use a rotational viscometer or a Tu-4 cup viscometer to measure the viscosity of the coating at 25°C; the rotational viscometer measures the viscosity by the resistance generated by the rotation of the rotor in the coating, while the Tu-4 cup calculates the viscosity based on the time required for the coating to flow through a standard aperture.

[0051] 3. Drying time: Refer to the requirements of GB / T 1728-2020 "Determination of Actual Drying Time of Paint", apply the paint evenly on the prepared test plate, and record the time from the start of coating to surface drying (non-sticky) and thorough drying (reaching mechanical strength). The surface drying time is measured by the finger touch method, and the thorough drying time is determined by hardness test.

[0052] 4. Pencil hardness: According to the provisions of GB / T 6739-2020 "Determination of pencil hardness of paints and varnishes", use a pencil hardness tester to scratch the surface of the coating with a fixed weight pencil, starting from the softest pencil and gradually increasing the hardness until obvious scratches appear on the coating, and evaluate the pencil hardness level of the coating after the paint dries.

[0053] 5. Acid resistance: Referring to the acid corrosion test method in GB / T 9274-2020 "Chemical resistance test for paints and varnishes", the coating sample was immersed in a 5% by mass sulfuric acid solution, taken out after 48 hours, rinsed with water and dried, and the changes on the coating surface were observed, including discoloration, blistering and peeling.

[0054] 6. Resistance to artificial aging: Follow the guidance of GB / T 1865-2009 "Plastics Artificial Weathering Test Method Xenon Arc Lamp", use xenon arc lamp or UV lamp aging test chamber to simulate natural light and climate change, conduct accelerated aging test on the coating, and evaluate the changes in its color, gloss and physical properties.

[0055] 7. Resistance to humidity changes: According to the requirements of GB / T 1740-2007 "Determination of moisture and heat resistance of coatings", place the coating sample in a constant temperature and humidity chamber, set a specific temperature (40°C) and humidity (95%RH) for 7 days, and observe the expansion, blistering, discoloration or peeling of the coating.

[0056] The results are as follows Figure 3 and Figure 4 As shown, through the above performance tests, it can be seen that the water-based acrylic emulsions provided by Examples 1 to 3 have good acid resistance, artificial aging resistance, physical and mechanical properties and construction performance.

[0057] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A weather-resistant water-based acrylic emulsion, characterized in that: The composition is composed of the following components in percentage by mass: 50-70 parts of acrylate monomers, 5-15 parts of methyl methacrylate, 2-8 parts of fluorinated acrylates, 1-5 parts of maleic anhydride, 1-5 parts of N-vinyl pyrrolidone, 1-5 parts of emulsifiers, 0.1-1 parts of nanoparticles, 0.1-0.8 parts of initiators, 0.1-1 parts of light stabilizers and 0.1-1 parts of temperature-sensitive monomers; The acrylic acid ester monomers include 15-30 parts of butyl acrylate, 10-25 parts of ethyl acrylate, 5-15 parts of acrylic acid, 2-8 parts of lauryl methacrylate and 2-6 parts of lactic acid acrylate; The light stabilizer is a hindered amine light stabilizer, and the temperature-sensitive monomer is N-isopropyl acrylamide.

2. A weather-resistant aqueous acrylic emulsion according to claim 1, characterized in that: The emulsifier comprises 0.5-3 parts by weight of anionic emulsifier and 0.5-3 parts by weight of nonionic emulsifier, the anionic emulsifier is sodium lauryl sulfate, and the nonionic emulsifier is polyoxyethylene octyl phenyl ether.

3. A weather-resistant water-based acrylic emulsion according to claim 1, characterized in that: The composition by weight also includes 0.05-0.5 parts of a reducing agent and 0.01-0.5 parts of a chain transfer agent.

4. A weather-resistant water-based acrylic emulsion according to claim 3, characterized in that: The initiator is a water-soluble ammonium persulfate initiator, the reducing agent is sodium bisulfite, and the chain transfer agent is tert-dodecyl mercaptan.

5. A weather-resistant water-based acrylic emulsion according to claim 1, characterized in that: The nanoparticles are nano silicon dioxide or nano aluminum oxide.

6. A method for preparing a weather-resistant water-based acrylic emulsion, characterized in that: The method comprises the following steps: (1) pre-emulsifying butyl acrylate, ethyl acrylate, methyl methacrylate and 1 / 4 emulsifier with deionized water to obtain pre-emulsion A; (2) pre-emulsifying acrylic acid, lauryl methacrylate, lactic acid acrylate, fluorinated acrylate, maleic anhydride, N-vinyl pyrrolidone, and 1 / 4 emulsifier with deionized water to obtain pre-emulsion B; (3) Add deionized water and the remaining emulsifier into the reactor, raise the temperature to the reaction temperature, add 1 / 2 initiator and 1 / 10 pre-emulsion A, and start the polymerization reaction; (4) During the polymerization reaction, the remaining pre-emulsion A is slowly added to the reactor and reacted for 2.5-4 hours; (5) After the reaction is completed, add a neutralizer to neutralize and adjust the pH to 7.5-8.5; (6) Add the remaining initiator and pre-emulsion B and continue the reaction for 2.5-5 hours until the polymerization is completed; (7) Cooling and filtering. In the post-processing stage, light stabilizer, nanoparticles and thermosensitive monomer are added and mixed evenly to obtain a water-based acrylic emulsion.

7. The method for preparing a weather-resistant water-based acrylic emulsion according to claim 6, characterized in that: The neutralizing agent is one or more combinations of ammonia water, N,N-2-methylethanolamine or aminomethyl propanol.

8. The method for preparing a weather-resistant water-based acrylic emulsion according to claim 6, characterized in that: The reaction temperature is 70-90° C., and the total polymerization reaction time is 5.5-8 hours.

9. The method for preparing a weather-resistant water-based acrylic emulsion according to claim 6, characterized in that: The solid content of the aqueous acrylic emulsion is 55-65%.

10. An application of the weather-resistant water-based acrylic emulsion according to any one of claims 1 to 9, characterized in that: Water-based acrylic emulsions are used in the production of water-based coatings related to building exterior walls, outdoor facility protection and decoration.

Citation Information

Cited By

  • Silicon-based aerogel thermal insulation material

    CN120758109A

  • Silica-based aerogel thermal insulation

    CN120758109B