Poly (N-isopropylacrylamide) microgel and preparation method thereof, and poly (N-isopropylacrylamide) / polyvinyl alcohol hydrogel and preparation method and application thereof

Poly(N-isopropylacrylamide) microgels and poly(N-isopropylacrylamide)/polyvinyl alcohol hydrogels prepared by emulsion polymerization and freeze-thaw cycle technology solve the temperature sensitivity of PNIPAM hydrogels The problem of insufficient characteristics has achieved significant temperature-sensitive characteristics and application potential, and is particularly suitable for acoustic metamaterials and craniocerebral ultrasound imaging.

CN118930731APending Publication Date: 2024-11-12ZHEJIANG UNIV

Patent Information

Application Number
CN202411253850.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The insufficient temperature-sensitive properties of PNIPAM hydrogels limit their applications in fields such as information encryption, biological dressings and moisture collection.

Method used

Poly(N-isopropylacrylamide) microgels and poly(N-isopropylacrylamide)/polyvinyl alcohol hydrogels were prepared by emulsion polymerization, using surfactant, acrylic acid, crosslinking agent, and pH value. The buffer and initiator undergo emulsion polymerization, combining freeze-drying and freeze-thaw cycle technology, to regulate the size and temperature-sensitive properties of the microgel.

Benefits of technology

It significantly improved the temperature sensitive characteristics of poly(N-isopropylacrylamide) microgels and poly(N-isopropylacrylamide)/polyvinyl alcohol hydrogels, making them significantly change in volume under near body temperature heat stimulation. , suitable for acoustic metamaterials, especially in craniocerebral ultrasound imaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930731A_ABST
    Figure CN118930731A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of functional materials, and particularly relates to poly (N-isopropylacrylamide) microgel and a preparation method thereof, and poly (N-isopropylacrylamide) / polyvinyl alcohol hydrogel and a preparation method and application thereof. The poly (N-isopropylacrylamide) microgel provided by the invention has a stimulation response function, the volume of the poly (N-isopropylacrylamide) microgel can be obviously changed under thermal stimulation close to body temperature, and the elastic modulus of the microspheres is correspondingly changed. The poly (N-isopropylacrylamide) / polyvinyl alcohol hydrogel provided by the invention also has a remarkable temperature-sensitive characteristic. Under the action of external thermal stimulation, the internal microsphere poly (N-isopropylacrylamide) has an obvious shrinkage and water loss phenomenon, and the whole material can be used as an acoustic metamaterial, and is particularly suitable for craniocerebral ultrasonic imaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional materials, and specifically relates to a poly(N-isopropylacrylamide) microgel and a preparation method thereof, and a poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel and a preparation method and application thereof. Background Art

[0002] Polyisopropylacrylamide (PNIPAM) hydrogel is a temperature-sensitive material with a low critical solution temperature. As the temperature rises, when it reaches above the critical solution temperature, the volume will shrink suddenly and the gel transparency will change. Therefore, it is widely used in information encryption, biological dressings, and moisture collection.

[0003] However, the thermosensitive properties of PNIPAM hydrogels are not ideal enough, which limits their applications. Summary of the invention

[0004] The purpose of the present invention is to provide a poly (N-isopropylacrylamide) microgel and a preparation method thereof, and a poly (N-isopropylacrylamide) / polyvinyl alcohol hydrogel and a preparation method and application thereof. The poly (N-isopropylacrylamide) / polyvinyl alcohol hydrogel provided by the present invention has significant temperature-sensitive properties.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The present invention provides a poly(N-isopropylacrylamide) microgel, the structural formula of which is shown in Formula I:

[0007]

[0008] In formula I, x is 180 to 200, y is 35 to 80, and n is 1.5 to 2.0.

[0009] The present invention also provides a method for preparing the poly(N-isopropylacrylamide) microgel of the above scheme, comprising the following steps:

[0010] (1) mixing a surfactant and water to obtain a micellar solution;

[0011] (2) The micelle solution is mixed with N-isopropylacrylamide, acrylic acid, a crosslinking agent, a pH buffer and an initiator in a protective atmosphere to carry out an emulsion polymerization reaction, followed by cooling and freeze-drying in sequence to obtain the poly(N-isopropylacrylamide) microgel.

[0012] Preferably, the mass ratio of the surfactant to water is 0.1-0.3:200; the mass ratio of the N-isopropylacrylamide to the surfactant is 2.24-2.80:0.10-0.30; the volume ratio of the acrylic acid to water is not more than 533:200000; the mass ratio of the N-isopropylacrylamide to the cross-linking agent is 224-280:8.8; the mass ratio of the pH buffer to the cross-linking agent is not more than 240:8.8; the mass ratio of the N-isopropylacrylamide to the initiator is 224-280:15.

[0013] Preferably, the temperature of the emulsion polymerization reaction is 70° C., and the insulation time is 2 hours; the emulsion polymerization reaction is carried out under stirring conditions; and the rotation speed of the stirring conditions is 400-500 rpm.

[0014] Preferably, the freeze-drying temperature is -60°C and the insulation time is 4 to 8 days.

[0015] The present invention also provides a poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel, comprising a polyvinyl alcohol hydrogel and a poly(N-isopropylacrylamide) microgel attached to the polyvinyl alcohol molecular chain; the poly(N-isopropylacrylamide) microgel is the poly(N-isopropylacrylamide) microgel described in the above scheme or the poly(N-isopropylacrylamide) microgel obtained by the preparation method described in the above scheme.

[0016] Preferably, the mass ratio of the polyvinyl alcohol hydrogel to the poly(N-isopropylacrylamide) microgel is 960-995:5-40; the mass ratio of polyvinyl alcohol to water in the polyvinyl alcohol hydrogel is 2-3:17-18.

[0017] The present invention also provides a method for preparing the poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel described in the above scheme, comprising the following steps:

[0018] After polyvinyl alcohol, poly(N-isopropylacrylamide) microgel and water are mixed, defoaming and freeze-thaw cycles are performed in sequence, and the number of freeze-thaw cycles is more than 5 times to obtain poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel.

[0019] Preferably, the number of freeze-thaw cycles is 5 to 6 times; the freezing temperature of the freeze-thaw cycle is 0 to -30°C, and the freezing time is based on the freezing of all the water in the mixed solution; the thawing temperature of the freeze-thaw cycle is room temperature, and the thawing time is based on the melting of all the water in the mixed solution.

[0020] The present invention also provides the use of the poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel described in the above scheme or the poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel obtained by the preparation method described in the above scheme as an acoustic metamaterial.

[0021] The present invention provides a poly(N-isopropylacrylamide) microgel. The poly(N-isopropylacrylamide) microgel (PNIPAm microgel) provided by the present invention has a stimulus response function, and its volume changes significantly under thermal stimulation close to body temperature, and the elastic modulus of the microspheres also changes accordingly.

[0022] The present invention also provides a method for preparing the poly(N-isopropylacrylamide) microgel described in the above scheme. The present invention prepares monodisperse poly(N-isopropylacrylamide) microgel by emulsion polymerization.

[0023] The present invention also provides a poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel. The poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel (PNIPAM / PVA hydrogel) provided by the present invention also has significant temperature-sensitive properties. Under external thermal stimulation, the internal microsphere poly(N-isopropylacrylamide) will show obvious shrinkage and water loss.

[0024] The present invention also provides a method for preparing the poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel described in the above scheme. The preparation method provided by the present invention has simple steps, convenient operation and good feasibility.

[0025] The present invention also provides the use of the poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel described in the above scheme or the poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel obtained by the preparation method described in the above scheme as an acoustic metamaterial. The poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel provided by the present invention also has significant temperature-sensitive properties. Under the action of external thermal stimulation (about human body temperature), the internal microsphere poly(N-isopropylacrylamide) will show obvious shrinkage and water loss phenomenon. The whole material can be used as an acoustic metamaterial, especially suitable for cranial ultrasound imaging. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 The synthetic route of PNIPAM microgel (A) and the experimental preparation diagram (B);

[0028] Figure 2The relationship diagram of the particle size distribution of PNIPAM microgel when the amount of SDS added is 0.1g (A), 0.2g (B), and 0.3g (C);

[0029] Figure 3 The relationship diagram of the particle size distribution of PNIPAM microgel when the amount of AAc added is 0 μL (A), 266 μL (B), and 533 μL (C);

[0030] Figure 4 The SEM images of PNIPAM microgels when the amount of SDS added was 0.1 g (A), 0.2 g (B), and 0.3 g (C);

[0031] Figure 5 is the infrared spectrum of PNIPAm microgel;

[0032] Figure 6 Schematic diagram of the shrinkage upon heating and expansion upon cooling of PNIPAM microgel;

[0033] Figure 7 The particle size changes of PNIPAM microgels of different sizes at room temperature and 37°C are shown when the amount of SDS added is 0.1g (A), 0.2g (B), and 0.5g (C).

[0034] Figure 8 SEM images of PVA hydrogel and PNIPAM / PVA hydrogel;

[0035] Fig. 9 SEM image of microgel distribution on PNIPAM / PVA hydrogel;

[0036] Fig.10 The infrared spectra of PVA hydrogel and PNIPAM / PVA hydrogel;

[0037] Reference symbols: MG is PNIPAM microgel. DETAILED DESCRIPTION

[0038] The present invention provides a poly(N-isopropylacrylamide) microgel, the structural formula of which is shown in Formula I:

[0039]

[0040] In formula I, x is 180 to 200, y is 35 to 80, and n is 1.5 to 2.0.

[0041] The present invention also provides a method for preparing the poly(N-isopropylacrylamide) microgel of the above scheme, comprising the following steps:

[0042] (1) mixing a surfactant and water to obtain a micellar solution;

[0043] (2) The micelle solution is mixed with N-isopropylacrylamide, acrylic acid, a crosslinking agent, a pH buffer and an initiator in a protective atmosphere to carry out an emulsion polymerization reaction, followed by cooling and freeze-drying in sequence to obtain the poly(N-isopropylacrylamide) microgel.

[0044] The present invention mixes a surfactant and water (referred to as the first mixing) to obtain a micellar solution. In the present invention, the surfactant is preferably sodium dodecyl sulfate (SDS).

[0045] In the present invention, the water is preferably deionized water.

[0046] In the present invention, the mass ratio of the surfactant to water is preferably 0.1 to 0.3:200, more preferably 0.15 to 0.30:200, and further preferably 0.2 to 0.3:200.

[0047] In the present invention, the temperature of the first mixing is preferably room temperature; the first mixing is preferably stirring mixing.

[0048] In the present invention, after the first mixing, the micellar solution is preferably deoxygenated; the deoxygenation is preferably carried out while stirring while passing nitrogen; the speed of stirring while passing nitrogen is preferably 500 rpm, and the stirring time is preferably more than 20 minutes, more preferably 20 to 60 minutes, and further preferably 20 to 40 minutes. The present invention stabilizes the micellar system by removing dissolved oxygen.

[0049] After obtaining the micellar solution, the present invention mixes the micellar solution with N-isopropylacrylamide (NIPAM), acrylic acid (AAc), a crosslinking agent, a pH buffer and an initiator (referred to as the second mixing), performs emulsion polymerization in a protective atmosphere, and then sequentially cools and freeze-dries to obtain the poly (N-isopropylacrylamide) microgel. In the present invention, the mass ratio of the N-isopropylacrylamide to the surfactant is preferably 2.24-2.80:0.10-0.30, more preferably 2.3-2.7:0.15-0.30, and further preferably 2.4-2.6:0.2-0.3.

[0050] In the present invention, the volume ratio of acrylic acid to water is preferably no more than 533:200000, more preferably 266-533:200000, and further preferably 350-450:200000. The present invention can achieve size control of microgels by regulating the amount of surfactant or acrylic acid added: as the surfactant increases, the size of the microgels gradually decreases; as the acrylic acid continues to decrease, the particle size of the microgels gradually increases.

[0051] In the present invention, the crosslinking agent is preferably N,N'-methylenebisacrylamide. The present invention forms a three-dimensional network through the crosslinking agent.

[0052] In the present invention, the mass ratio of the N-isopropylacrylamide to the cross-linking agent is preferably 224-280:8.8, more preferably 235-265:8.8, and further preferably 245-255:8.8.

[0053] In the present invention, the pH buffer is preferably KH2PO4. The present invention stabilizes micelles by adjusting the pH value.

[0054] In the present invention, the mass ratio of the pH buffer to the cross-linking agent is preferably not greater than 240:8.8, more preferably 10 to 240:8.8, and further preferably 120 to 160:8.8.

[0055] In the present invention, the initiator preferably includes one or more of azobisisobutyramidine hydrochloride (AAPH) and persulfate; the persulfate preferably includes one or both of ammonium persulfate and potassium persulfate.

[0056] In the present invention, the mass ratio of the N-isopropylacrylamide to the initiator is preferably 224 to 280:15, more preferably 235 to 270:15, and further preferably 245 to 260:15.

[0057] In the present invention, the temperature of the second mixing is preferably 70° C., the mixing time is preferably more than 1 hour, more preferably 1 to 5 hours; the second mixing is preferably stirring mixing.

[0058] In a specific embodiment of the present invention, the second mixing is preferably: mixing water and a surfactant until the resulting solution is clear, then mixing the solution with N-isopropylacrylamide, acrylic acid, a crosslinking agent and a pH buffer in a protective atmosphere to obtain a mixture, and then mixing the mixture with an initiator in an inert atmosphere; the protective atmosphere is preferably nitrogen; the inert atmosphere is preferably nitrogen.

[0059] In the present invention, the protective atmosphere is preferably nitrogen; the temperature of the emulsion polymerization reaction is preferably 70°C, and the insulation time is preferably 2h; the emulsion polymerization reaction is preferably carried out under stirring conditions; the rotation speed of the stirring conditions is preferably 400-500rpm, more preferably 420-480rpm, and further preferably 450-460rpm.

[0060] In the present invention, the cooling is preferably: placing the obtained reaction system into an ice water bath for rapid cooling.

[0061] In the present invention, the cooling preferably further comprises dialyzing the obtained reaction system; the cut-off weight average molecular weight of the dialysis is preferably 5000. The present invention removes unreacted monomers and impurities through dialysis.

[0062] In the present invention, the freeze-drying temperature is preferably -60°C, and the insulation time is preferably 4 to 8 days, more preferably 5 to 7 days.

[0063] The present invention also provides a poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel, comprising a polyvinyl alcohol hydrogel and a poly(N-isopropylacrylamide) microgel attached to the molecular chain of the polyvinyl alcohol hydrogel; the poly(N-isopropylacrylamide) microgel is the poly(N-isopropylacrylamide) microgel described in the above scheme or the poly(N-isopropylacrylamide) microgel obtained by the preparation method described in the above scheme.

[0064] In the present invention, the mass ratio of the polyvinyl alcohol hydrogel to the poly(N-isopropylacrylamide) microgel is preferably 960-995:5-40, more preferably 970-995:5-30, and further preferably 970-990:10-30; the mass ratio of polyvinyl alcohol to water in the polyvinyl alcohol hydrogel is preferably 2-3:17-18, more preferably 1:9.

[0065] The present invention also provides a method for preparing the poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel described in the above scheme, comprising the following steps:

[0066] After polyvinyl alcohol, poly(N-isopropylacrylamide) microgel and water are mixed, defoaming and freeze-thaw cycles are performed in sequence, and the number of freeze-thaw cycles is more than 5 times to obtain poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel.

[0067] In the present invention, polyvinyl alcohol, poly(N-isopropylacrylamide) microgel and water are mixed (referred to as the third mixing). In the present invention, the polyvinyl alcohol is preferably 1799 type polyvinyl alcohol; and the water is preferably deionized water.

[0068] In the present invention, the mass ratio of the polyvinyl alcohol to water is preferably 2-3:17-18, more preferably 1:9; the mass ratio of the total mass of the polyvinyl alcohol and water to the poly(N-isopropylacrylamide) microgel is preferably 960-995:5-40, more preferably 970-995:5-30, further preferably 970-990:10-30.

[0069] In the present invention, the third mixing is preferably: mixing polyvinyl alcohol and water, heating, condensing and refluxing to obtain a transparent solution, and then stirring and mixing the transparent solution and poly(N-isopropylacrylamide) microgel.

[0070] In the present invention, the temperature of the heating condensation reflux is preferably 90°C, and the reflux time is preferably based on the clarity of the solution, more preferably 2 to 3 hours. The present invention obtains a transparent and viscous PVA aqueous solution by heating condensation reflux, and stores it in a refrigerator at 2 to 6°C.

[0071] In the present invention, the stirring and mixing is preferably continued until no poly(N-isopropylacrylamide) microgel agglomerates in the obtained mixed solution.

[0072] After mixing, the present invention sequentially performs defoaming and freeze-thaw cycles, the number of freeze-thaw cycles being more than 5 times, to obtain poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel. In the present invention, the defoaming is preferably performed by standing; the defoaming is preferably performed in a sandwich glass mold.

[0073] In the present invention, the number of freeze-thaw cycles is preferably 5 to 6 times; the freezing temperature of the freeze-thaw cycle is preferably 0 to -30°C, more preferably -20 to -30°C, and the freezing time is preferably based on the freezing of all the water in the mixed solution, more preferably more than 2 hours, and further preferably 2 to 3 hours; the thawing temperature of the freeze-thaw cycle is preferably room temperature, and the thawing time is based on the melting of all the water in the mixed solution.

[0074] The present invention also provides the use of the poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel described in the above scheme or the poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel obtained by the preparation method described in the above scheme as an acoustic metamaterial.

[0075] The poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel provided by the present invention also has significant temperature-sensitive properties. Under the action of external thermal stimulation (about human body temperature), the internal microsphere poly(N-isopropylacrylamide) will show obvious shrinkage and water loss. The entire material can be used as an acoustic metamaterial, and is particularly suitable for cranial ultrasound imaging.

[0076] In order to further illustrate the present invention, the scheme of the present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be understood as limiting the protection scope of the present invention.

[0077] In the specific embodiment of the present invention, the models and manufacturers of the instruments used are shown in Table 1.

[0078] Table 1 Models and manufacturers of instruments used in the examples

[0079] Instrument Name model factory Freeze Dryer LGJ-10C Beijing Sihuan Scientific Instrument Factory Co., Ltd. refrigerator Low temperature freezer Haier Group Corporation Wall breaking machine P132 Joyoung Co., Ltd. Field Emission Scanning Electron Microscope S-4800 Hitachi Corporation Fourier Transform Infrared Spectrometer NICOLET6700 Thermo Dynamic Light Scattering ZetasizerNanoZS Malvern, UK

[0080] Example

[0081] This embodiment uses an emulsion polymerization method to prepare PNIPAM / PVA hydrogel, including the following steps:

[0082] (1) Preparation of PNIPAm microgels, the preparation route is as follows Figure 1 As shown:

[0083] First, the surfactant SDS was added to a three-necked flask containing 200 mL of deionized water and stirred at room temperature until it was completely dissolved to obtain a micellar solution;

[0084] Subsequently, nitrogen was introduced into the three-necked round-bottom flask, and the mixture was stirred at 500 rpm for 20 min to remove dissolved oxygen; N-isopropylacrylamide (NIPAM), acrylic acid (AAc) and N,N'-methylenebisacrylamide (Bis) were added to the micelle solution, and KH2PO4 was added to stabilize the micelles to obtain a mixture;

[0085] The mixture was stirred at 70° C. for 1 h, the flask was sealed, and nitrogen was introduced below the liquid surface; then, azobisisobutyramidine hydrochloride (AAPH) was added to the mixture, the reaction temperature was 70° C., the stirring speed was 450 rpm, and the reaction lasted for 2 h;

[0086] After the reaction was completed, the flask was placed in an ice-water bath and rapidly cooled to obtain a microgel polymer solution; the microgel polymer solution was poured into a dialysis bag with a molecular chain cutoff of 5000 for dialyzing to remove unreacted monomers and impurities, and freeze-dried at -60°C for 4 days to obtain a monodisperse PNIPAm microgel.

[0087] On this basis, the size of PNIPAm microgel was regulated by adjusting the amount of surfactant SDS or acrylic acid AAc added (as shown in Table 2): as the amount of SDS added increased, the size of PNIPAm microgel decreased; as the amount of acrylic acid added decreased, the size of PNIPAm microgel increased.

[0088] (2) Preparation of PNIPAM / PVA hydrogel:

[0089] 30 g of polyvinyl alcohol solid powder (CAS: 9002-89-5; 1799 type) and 270 mL of deionized water were added to a round-bottom flask, and condensed and refluxed at 90° C. until the solution became transparent and clear to obtain a transparent and viscous PVA aqueous solution, which was then stored in a refrigerator at 2 to 6° C.

[0090] The PNIPAm microgel was added to 10 g of the PVA aqueous solution and stirred until there was no microgel agglomeration in the mixed solution, and then poured into a sandwich glass mold and allowed to stand until the bubbles disappeared; then freeze-thaw cycles were performed 6 times (freezing in a -20°C refrigerator for 3 h, then taking out and thawing at room temperature) to obtain PNIPAM / PVA hydrogel.

[0091] Table 2 Formulations of PNIPAM / PVA hydrogels of Examples 1 to 5

[0092] Example SDS / g NIPAM / g AAc / μL Bis / g <![CDATA[KH2PO4 / g]]> AAPH / g <![CDATA[H2O / mL]]> Example 1 0.3 2.24 533 0.088 2.4 0.15 200 Example 2 0.2 2.24 533 0.088 2.4 0.15 200 Example 3 0.1 2.24 533 0.088 2.4 0.15 200 Example 4 0.3 2.52 266 0.088 1.2 0.15 200 Example 5 0.3 2.80 0 0.088 0 0.15 200 Example 6 0.3 2.26 305 0.088 2.4 0.15 200 Example 7 0.5 2.24 533 0.088 2.4 0.15 200

[0093] The size distribution of the PNIPAM microgels prepared in Examples 1 to 3 was tested using dynamic light scattering (DLS). Figure 2 As shown. Figure 2 It can be seen that with the increase of SDS addition, the size of PNIPAM microgels gradually decreased.

[0094] The size distribution of the PNIPAM microgels prepared in Examples 1 and 4 to 5 was tested by dynamic light scattering (DLS). Figure 3 As shown. Figure 3 It can be seen that when the amount of SDS added is fixed, as the amount of acrylic acid added continues to decrease, the size of PNIPAM microgel increases.

[0095] The morphology of the PNIPAM microgels prepared in Examples 1 to 3 was observed using a scanning electron microscope (SEM) to verify their size. Figure 4 As shown. Figure 4 It can be seen that with the continuous increase in the amount of surfactant SDS added, the size of the prepared microspheres decreases significantly.

[0096] The PNIPAM microgel prepared in Example 1 was characterized by infrared spectroscopy. Figure 5 As shown. Figure 5 It can be seen that the present invention successfully prepared PNIPAm microgel.

[0097] The temperature shrinkage and temperature expansion characteristics of PNIPAM microgels were tested by dynamic light scattering tests at room temperature and 37°C to observe the changes in particle size. The results are as follows: Figure 6 As shown. Figure 6 It can be seen that the PNIPAm microgel prepared in the present invention has significant temperature-sensitive properties. The PNIPAm hydrogel containing a large amount of water will show obvious shrinkage and water loss under the action of external thermal stimulation (about human body temperature).

[0098] Dynamic light scattering (DLS) was used to perform temperature sensitivity tests on the PNIPAM microgels of different sizes prepared in Examples 2 to 3 and Example 7 to test the changes in particle size at room temperature and 37°C. The results are shown in Figure 7. Figure 7 It can be seen that the dynamic light scattering data intuitively shows the particle size distribution of PNIPAm microgel at room temperature and 37°C. When the temperature rises to 37°C, the size of PNIPAm microgel decreases significantly.

[0099] The PNIPAM / PVA hydrogel prepared in Example 1 and the PVA hydrogel (control) were subjected to SEM testing, and the results were as follows: Figure 8 and Fig. 9 As shown. Figure 8 It can be seen that there are certain differences in the microscopic morphology between PNIPAM / PVA hydrogel and pure PVA hydrogel, and the internal pores of PVA-MG hydrogel are looser than those of PVA hydrogel. Fig. 9 It can be seen that PNIPAM microgel is attached to the molecular chain of PVA.

[0100] The infrared spectra of the PNIPAM / PVA hydrogel and the PVA hydrogel (control) prepared in Example 1 were analyzed. Fig.10 As shown. Fig.10 It can be seen that in PVA polymer, the absorption peak of -OH appears at 3266.83 cm -1 ; However, in the PVA-MG system, the -OH peak undergoes a red shift; this is mainly because the -OH on the PVA polymer chain combines with the microgel, resulting in an increase in the steric hindrance between the polymer chains, thereby weakening the hydrogen bonding effect between the hydroxyl groups and reducing the association effect of the hydroxyl groups, thus resulting in a red shift in the peak position.

[0101] It can be seen from the above examples that the poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel provided by the present invention has significant temperature-sensitive properties.

[0102] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A poly(N-isopropylacrylamide) microgel, characterized in that: The structural formula is shown in Formula I: In formula I, x is 180 to 200, y is 35 to 80, and n is 1.5 to 2.

0.

2. The method for preparing the poly(N-isopropylacrylamide) microgel according to claim 1, characterized in that: The following steps are involved: (1) mixing a surfactant and water to obtain a micellar solution; (2) The micelle solution is mixed with N-isopropylacrylamide, acrylic acid, a crosslinking agent, a pH buffer and an initiator in a protective atmosphere to carry out an emulsion polymerization reaction, followed by cooling and freeze-drying in sequence to obtain the poly(N-isopropylacrylamide) microgel.

3. The preparation method according to claim 2, characterized in that: The mass ratio of the surfactant to water is 0.1-0.3:200; the mass ratio of the N-isopropylacrylamide to the surfactant is 2.24-2.80:0.10-0.30; the volume ratio of the acrylic acid to water is not greater than 533:200000; the mass ratio of the N-isopropylacrylamide to the cross-linking agent is 224-280:8.8; the mass ratio of the pH buffer to the cross-linking agent is not greater than 240:8.8; the mass ratio of the N-isopropylacrylamide to the initiator is 224-280:

15.

4. The preparation method according to claim 2 or 3, characterized in that: The temperature of the emulsion polymerization reaction is 70° C., and the heat preservation time is 2 hours; the emulsion polymerization reaction is carried out under stirring conditions; and the rotation speed of the stirring conditions is 400-500 rpm.

5. The preparation method according to claim 2, characterized in that: The freeze-drying temperature is -60°C and the insulation time is 4 to 8 days.

6. A poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel, characterized in that: It includes a polyvinyl alcohol hydrogel and a poly(N-isopropylacrylamide) microgel attached to the molecular chain of the polyvinyl alcohol hydrogel; The poly(N-isopropylacrylamide) microgel is the poly(N-isopropylacrylamide) microgel according to claim 1 or the poly(N-isopropylacrylamide) microgel obtained by the preparation method according to any one of claims 2 to 5.

7. The poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel according to claim 6, characterized in that The mass ratio of the polyvinyl alcohol hydrogel to the poly(N-isopropylacrylamide) microgel is 960-995:5-40; the mass ratio of polyvinyl alcohol to water in the polyvinyl alcohol hydrogel is 2-3:17-18.

8. The method for preparing the poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel according to any one of claims 6 to 7, characterized in that: The following steps are involved: After polyvinyl alcohol, poly(N-isopropylacrylamide) microgel and water are mixed, defoaming and freeze-thaw cycles are performed in sequence, and the number of freeze-thaw cycles is more than 5 times to obtain poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel.

9. The preparation method according to claim 8, characterized in that: The number of freeze-thaw cycles is 5 to 6 times; The freezing temperature of the freeze-thaw cycle is 0 to -30°C, and the freezing time is based on the complete freezing of the water in the mixed solution; The thawing temperature of the freeze-thaw cycle is room temperature, and the thawing time is based on when all the water in the mixed solution is melted.

10. Use of the poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel according to any one of claims 6 to 7 or the poly(N-isopropylacrylamide) / polyvinyl alcohol hydrogel obtained by the preparation method according to any one of claims 8 to 9 as an acoustic metamaterial.

Citation Information

Patent Citations

  • PVA (polyvinyl alcohol) matrix poly-N-isopropyl acrylamide microgel and preparation method thereof

    CN101735544A

  • Method for preparing high-strength hydrogel with macromolecular microgel composite structure

    CN102675549A

  • Preparation method of rapid-response high-strength poly(N-isopropylacrylamide) hydrogel

    CN107840926A

  • Hydrogel driver containing nanometer microspheres, and preparation method and application of hydrogel driver

    CN111909304A

  • Double-layer hydrogel material and preparation method and application thereof

    CN113683820A