High-temperature-resistant acidizing corrosion inhibitor, high-temperature-resistant acidizing corrosion inhibitor system, and preparation method and application thereof

By introducing acrylic acid, acrylic esters and diethylene triamine into the acidified corrosion inhibitor, the problem that the existing technology cannot effectively inhibit corrosion under high temperature conditions is solved, and the 160-210 Effective corrosion inhibition performance in deep and ultra-deep reservoirs at ℃ meets the demand for oil and gas well production and transformation.

CN118930732APending Publication Date: 2024-11-12PETROCHINA CO LTD

Patent Information

Application Number
CN202310531678.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing acidified corrosion inhibitors cannot effectively inhibit corrosion in deep and ultra-deep reservoirs with a well temperature above 160℃, and cannot meet the demand for oil and gas well production and transformation under high temperature conditions.

Method used

Initiator is prepared by reacting acrylic acid or acrylate with diethylene triamine, and reacting with alkenyl sulfonate, allyl quaternary ammonium salt, N-vinyl pyrrolidone and acrylamide, and quaternization reactions to obtain high temperature resistance Acidize corrosion inhibitors to form chain polymer corrosion inhibitors, suitable for high temperature conditions of 160-210℃.

Benefits of technology

The corrosion inhibitor shows good corrosion inhibition performance under high temperature conditions of 160-210℃, meeting the transformation needs of deep and ultra-deep reservoirs. The corrosion rate meets the standards of the oil and natural gas industry, and there is no obvious pitting or pit corrosion. Phenomenon.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004224888610000071
    Figure BDA0004224888610000071
  • Figure BDA0004224888610000072
    Figure BDA0004224888610000072
  • Figure BDA0004224888610000081
    Figure BDA0004224888610000081
Patent Text Reader

Abstract

The invention provides a high-temperature-resistant acidizing corrosion inhibitor and system as well as a preparation method and application of the high-temperature-resistant acidizing corrosion inhibitor and system. The preparation method of the high-temperature-resistant acidizing corrosion inhibitor comprises the following steps: (1) reacting acrylic acid and / or acrylate with diethylenetriamine to obtain an initiator; (2) reacting the initiator with alkenyl sulfonate, allyl quaternary ammonium salt, N-vinyl pyrrolidone and acrylamide to prepare a corrosion inhibitor precursor; and (3) carrying out quaternization reaction on the corrosion inhibitor precursor to obtain the high-temperature-resistant acidizing corrosion inhibitor. The obtained high-temperature acidizing-resistant corrosion inhibitor has good corrosion inhibition performance with a system, is suitable for corrosion inhibition at a high temperature of 160-210 DEG C, and can meet the requirements of transformation of deep and ultra-deep reservoirs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil and gas layer production enhancement and transformation, and specifically relates to a composite corrosion inhibitor suitable for high-temperature acidification at 160-210°C or below. Background Art

[0002] Acidizing is an important measure for increasing the production of oil and gas wells. Acid is injected into the formation through the wellbore, and the chemical reaction between the acid and some minerals in the formation is used to dissolve the connected pores or fracture wall rocks in the reservoir, increase the connectivity between pores and the conductivity of fractures, and achieve the purpose of increasing the production of oil and gas wells. During the acidizing process, the acid will corrode the downhole tubing, so it is necessary to add corrosion inhibitors to the acid to inhibit or slow down the corrosion of the acid on the downhole tubing.

[0003] CN106868512A provides an acidification corrosion inhibitor, which is mainly composed of sodium oleyl sarcosinate, mercaptobenzothiazole, and polyethylene polyamine. The acidification corrosion inhibitor can withstand high temperatures of up to 240°C, and the corrosion inhibition rate is only 23g / m 2 ·h, and the effect is achieved under the conditions of 22% HCl and 8% HF. CN103642480A provides an acidified corrosion inhibitor with acetophenone, trioxymethylene and cyclohexylamine as main components, but only explains that it has the advantages of low corrosion inhibition rate and low cost, and does not provide specific corrosion effect evaluation indicators.

[0004] CN112300131A provides an imidazoline corrosion inhibitor with asymmetric terminal groups, a preparation method and an application thereof. The invention uses imidazoline as the main active group, utilizes the intramolecular synergistic adsorption barrier effect, synthesizes the imidazoline ring with organic heterocyclic carboxylic acid and polyamine, and then uses the long-chain carboxylic acid and the terminal amine group of the imidazoline ring side chain to condense and cap, thereby obtaining an imidazoline corrosion inhibitor with asymmetric terminal groups, which has very strong corrosion inhibition performance at high temperatures. The corrosion inhibitor can be resistant to high temperatures because the corrosion inhibitor has a long molecular main chain structure. At the same time, imidazoline, as a macromolecular side chain, has a strong molecular steric effect, thereby improving the temperature resistance of the polymer.

[0005] However, most of the acidizing corrosion inhibitors provided by the current related technologies are used under the condition of well temperature of 160°C. As oil and gas exploration gradually develops towards deep and ultra-deep reservoirs, the well depth exceeds 7,000m, and the bottom hole temperature is generally above 160°C, and the bottom hole temperature in some cases reaches 210°C. The acidizing corrosion inhibitors provided by the existing technology can no longer meet the transformation needs of deep and ultra-deep reservoirs with temperatures reaching 200°C and above. Summary of the invention

[0006] In order to solve the above problems, the purpose of the present invention is to provide a high-temperature acidification resistant corrosion inhibitor and system, and a preparation method and application thereof. The corrosion inhibitor and system are suitable for corrosion inhibition at high temperatures of 160-210°C, and can meet the needs of deep and ultra-deep reservoir transformation.

[0007] In order to achieve the above object, the present invention provides a method for preparing a high temperature acidification corrosion inhibitor, which comprises the following steps:

[0008] (1) reacting acrylic acid and / or acrylic acid ester with diethylenetriamine to obtain an initiator;

[0009] (2) reacting the above initiator with olefin sulfonate, allyl quaternary ammonium salt, N-vinyl pyrrolidone and acrylamide to obtain a corrosion inhibitor precursor;

[0010] (3) The corrosion inhibitor precursor is subjected to a quaternization reaction to obtain the high temperature acidification resistant corrosion inhibitor.

[0011] According to a specific embodiment of the present invention, preferably, in step (1), the reaction temperature is 140-150°C.

[0012] According to a specific embodiment of the present invention, preferably, in step (1), the weight ratio of the acrylic acid and / or acrylic acid ester to diethylenetriamine is 100-150:50, that is, the weight ratio of the acrylic acid or acrylic acid ester to diethylenetriamine is 100-150:50, or the weight ratio of the sum of the mass of the acrylic acid and the acrylic acid ester to diethylenetriamine is 100-150:50.

[0013] According to a specific embodiment of the present invention, preferably, in step (2), the olefin sulfonate comprises one or a combination of two or more of sodium 2-acrylamide-2-methylpropane sulfonate, sodium acrylic acid-2-acrylamide-2-methylpropane sulfonate, sodium allyl sulfonate, and sodium styrene sulfonate.

[0014] According to a specific embodiment of the present invention, preferably, in step (2), the allyl quaternary ammonium salt includes one or a combination of two or more of allyl ammonium chloride, dimethyldiallyl ammonium chloride, trimethylallyl ammonium chloride, and 4-vinylbenzylammonium chloride.

[0015] According to a specific embodiment of the present invention, preferably, in step (2), the reaction temperature is 60-70° C., the reaction time is 10-12 h, and the stirring rate is 600-700 r / min.

[0016] According to a specific embodiment of the present invention, preferably, in step (2), the weight ratio of the initiator, olefin sulfonate, allyl quaternary ammonium salt, N-vinyl pyrrolidone and acrylamide is 5-15:5-10:5-10:1-5:5-15.

[0017] According to a specific embodiment of the present invention, preferably, in step (3), the quaternizing agent used in the quaternization reaction is dimethyl sulfate.

[0018] According to a specific embodiment of the present invention, preferably, in step (3), the mass ratio of the corrosion inhibitor precursor to dimethyl sulfate is 1-5:3-8.

[0019] According to a specific embodiment of the present invention, preferably, in step (3), the temperature of the quaternization reaction is 110-120° C., the reaction time is 10-12 h, and the stirring rate is 800-900 r / min.

[0020] According to a specific embodiment of the present invention, the method for preparing the corrosion inhibitor provided by the present invention may include the following specific steps:

[0021] (1) Under constant temperature conditions, acrylic acid and / or acrylic acid ester and diethylenetriamine are reacted in an organic solvent (such as xylene) to prepare a macromolecular initiator, which is named YS-1;

[0022] (2) Under the action of a macromolecular initiator, olefin sulfonate, allyl quaternary ammonium salt, N-vinyl pyrrolidone and acrylamide react to obtain a high temperature resistant polymer corrosion inhibitor precursor, named HP-1;

[0023] (3) The obtained macromolecular polymer corrosion inhibitor precursor is subjected to a quaternization reaction with dimethyl sulfate to obtain the final high temperature resistant chain polymer acidification corrosion inhibitor KWHS-1.

[0024] The preparation method of the above-mentioned corrosion inhibitor may further include step (4) to obtain the high temperature acidification corrosion inhibition system: compounding the prepared chain polymer acidification corrosion inhibitor with other components to form a corrosion inhibitor system.

[0025] The present invention also provides a high temperature acidification resistant corrosion inhibitor, which is prepared by the above preparation method.

[0026] The present invention also provides a high temperature acidification corrosion resistant system, which comprises the above-mentioned high temperature acidification corrosion resistant inhibitor.

[0027] According to a specific embodiment of the present invention, preferably, the composition of the high temperature acidification corrosion inhibition system includes component A, component B, hydrochloric acid and water; wherein, based on the mass of the high temperature acidification corrosion inhibition system as 100%, the content of component A is 3-5%, the content of component B is 0.1-1%, the content of hydrochloric acid is 15-20% (for example, 20%), and the balance is water, wherein the content of hydrochloric acid is calculated as HCl; wherein, calculated by weight, component A includes 20-35 parts of high temperature acidification corrosion inhibitor (preferably 20-25 parts), 10-29 parts of organic synergist (preferably 10 parts), 17-20 parts of organic acid (preferably 17 parts), 8-9 parts of alcohol solvent (preferably 9 parts), and 10 parts of dispersant; component B includes an inorganic synergist.

[0028] According to a specific embodiment of the present invention, preferably, the preparation method of the high temperature acidification corrosion inhibition system comprises the following steps:

[0029] (1) Compounding, by weight, 20-25 parts of the high temperature acidification corrosion inhibitor, 10 parts of an organic synergist, 17 parts of an organic acid, 9 parts of an alcohol solvent, and 10 parts of a dispersant to obtain component A;

[0030] (2) Component A, component B and hydrochloric acid solution are mixed to obtain the high temperature acidification corrosion inhibition system.

[0031] According to a specific embodiment of the present invention, preferably, the preparation method of the high temperature acidification corrosion inhibition system may include the following specific steps: heating KWHS-1 to 50-60°C, then sequentially adding an organic synergist, an organic acid, an alcohol solvent, and a dispersant under stirring, stirring evenly to obtain component A, and adding it to a hydrochloric acid solution; an inorganic synergist may be added as component B under the condition of 160°C-210°C.

[0032] According to a specific embodiment of the present invention, preferably, the organic synergist includes one or a combination of two or more of formamide, N,N-dimethylformamide, propargyl alcohol propoxy compounds, and propargyl alcohol ethoxy compounds.

[0033] According to a specific embodiment of the present invention, preferably, the organic acid is formic acid and / or acetic acid.

[0034] According to a specific embodiment of the present invention, preferably, the dispersant is alkylphenol polyoxyethylene ether and / or fatty alcohol polyoxyethylene ether.

[0035] According to a specific embodiment of the present invention, preferably, the inorganic synergist includes one or a combination of two or more of cuprous chloride, potassium iodide, potassium pyroantimonate, antimony trioxide, and sodium molybdate.

[0036] The present invention also provides the use of the above-mentioned high temperature acidification corrosion inhibitor or the above-mentioned high temperature acidification corrosion inhibition system in acidification corrosion inhibition of oil and gas wells.

[0037] According to a specific embodiment of the present invention, preferably, the temperature of the oil and gas well is 160-210°C.

[0038] The present invention has the following beneficial effects:

[0039] The present invention synthesizes an initiator from acrylic acid and / or acrylic ester and diethylenetriamine, introduces a C=C active site, and further reacts with olefin sulfonate, allyl quaternary ammonium salt, N-vinyl pyrrolidone and acrylamide to obtain a high-temperature acidification corrosion inhibitor after quaternization. The corrosion inhibitor has good corrosion inhibition performance and high temperature resistance of up to 160-210°C, and can meet the needs of deep and ultra-deep reservoir reconstruction. DETAILED DESCRIPTION

[0040] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.

[0041] Example 1

[0042] This embodiment provides a high temperature resistant chain polymer acidification corrosion inhibitor, and the preparation method thereof comprises the following steps:

[0043] (1) Preparation of macromolecular initiators

[0044] In a 500mL three-necked flask containing 250mL of xylene, 1mol (144.12g) of acrylic acid was added, and then 0.5mol (51.58g) of diethylenetriamine was added dropwise at 0.5mL / min. The temperature was raised to 150°C, stirred at 800r / min for 10h, and then cooled to 100°C. A light yellow solid powder, i.e., the initiator, was obtained by vacuum distillation, and named YS-1.

[0045] (2) Preparation of high temperature resistant polymer (corrosion inhibitor precursor)

[0046] 20 g of macromolecular initiator YS-1 was added to 200 mL of acetone, followed by 0.1 mol (20.72 g) of 2-acrylamido 2-methylpropanesulfonate sodium, 0.15 mol (20.25 g) of allyl ammonium chloride, 0.1 mol (11.11 g) of N-vinyl pyrrolidone and 0.3 mol (21.3 g) of acrylamide. The mixture was heated to 70 ° C and stirred at 600 r / min for 12 h. After the reaction was completed, a high temperature resistant polymer (corrosion inhibitor precursor) was obtained by freeze drying and named HP-1.

[0047] (3) Preparation of corrosion inhibitor for high temperature resistant chain polymer acidification

[0048] 20 g of high temperature resistant polymer and 0.5 mol (63.07 g) of dimethyl sulfate were added to 300 mL of acetone, heated to 120 ° C, stirred at 800 r / min for 12 h, and cooled to 20 ° C after the reaction to obtain a light yellow solid powder, i.e., a high temperature resistant chain polymer acidification corrosion inhibitor (KWHS-1).

[0049] Comparative Example 1

[0050] This comparative example provides a corrosion inhibitor, and its operation steps are consistent with those of Example 1, except that in step (1), acrylic acid is replaced by stearic acid. The obtained product is recorded as KWHS-2.

[0051] Example 2

[0052] This embodiment provides a high temperature acidification corrosion inhibition system component A, and the preparation method thereof is as follows:

[0053] Add 30 parts of KWHS-1 to the reactor and heat to 50-60°C. Then, add 10 parts of propargyl alcohol propoxy compound, 17 parts of formic acid, 19 parts of formamide, 9 parts of ethylene glycol, and 10 parts of fatty alcohol polyoxyethylene ether (O-20) in sequence under stirring. After stirring evenly, component A is obtained, which is recorded as formula 1.

[0054] Comparative Example 2

[0055] This comparative example provides a high temperature acidification corrosion inhibition system component A, and its preparation method is as follows:

[0056] Add 30 parts of KWHS-2 to the reactor and heat to 50-60°C. Then, add 10 parts of propargyl alcohol propoxy compound, 17 parts of formic acid, 19 parts of formamide, 9 parts of ethylene glycol, and 10 parts of fatty alcohol polyoxyethylene ether (O-20) in sequence under stirring. After stirring evenly, component A is obtained, which is recorded as formula 1a.

[0057] Example 3

[0058] This embodiment provides a high temperature acidification corrosion inhibition system, and the preparation method thereof is as follows:

[0059] Add 35 parts of KWHS-1 to the reactor and heat to 40-50°C. Then, add 10 parts of propargyl alcohol propoxy compound, 20 parts of formic acid, 15 parts of formamide, 8 parts of ethylene glycol, and 10 parts of fatty alcohol polyoxyethylene ether (O-20) in sequence under stirring. After stirring evenly, component A is obtained, which is recorded as formula 2.

[0060] Component B in this embodiment is potassium pyroantimonate, and the mass ratio of component A to component B is 3.0:0.25.

[0061] Example 4

[0062] This embodiment provides a high temperature acidification corrosion inhibition system, and the preparation method thereof is as follows:

[0063] Add 35 parts of KWHS-1 to the reactor and heat to 40-50°C. Then, add 10 parts of propargyl alcohol propoxy compound, 20 parts of formic acid, 15 parts of formamide, 8 parts of ethylene glycol, and 10 parts of fatty alcohol polyoxyethylene ether (O-20) in sequence under stirring. After stirring evenly, component A is obtained, which is recorded as formula 2.

[0064] Component B in this embodiment is antimony trioxide, and the mass ratio of component A to component B is 3.0:0.25.

[0065] Comparative Example 3

[0066] This comparative example provides a high temperature acidification corrosion inhibition system, and its preparation method is as follows:

[0067] Add 35 parts of KWHS-2 to the reactor and heat to 40-50°C. Then, add 10 parts of propargyl alcohol propoxy compound, 20 parts of formic acid, 15 parts of formamide, 8 parts of ethylene glycol, and 10 parts of fatty alcohol polyoxyethylene ether (O-20) in sequence under stirring. After stirring evenly, component A is obtained, which is recorded as formula 2a.

[0068] Component B in this comparative example is potassium pyroantimonate, and the mass ratio of component A to component B is 3.0:0.25.

[0069] Comparative Example 4

[0070] This comparative example provides a high temperature acidification corrosion inhibition system, and its preparation method is as follows:

[0071] Add 35 parts of KWHS-2 to the reactor and heat to 40-50°C. Then, add 10 parts of propargyl alcohol propoxy compound, 20 parts of formic acid, 15 parts of formamide, 8 parts of ethylene glycol, and 10 parts of fatty alcohol polyoxyethylene ether (O-20) in sequence under stirring. After stirring evenly, component A is obtained, which is recorded as formula 2a.

[0072] Component B in this comparative example is antimony trioxide, and the mass ratio of component A to component B is 3.0:0.25.

[0073] Test Case

[0074] The composite corrosion inhibitor system prepared in the above examples and comparative examples was tested for corrosion inhibition performance in acid solution. The corrosion inhibition performance test was conducted in accordance with the petroleum and natural gas industry standard of the People's Republic of China "SY / T5405-2019". The specific evaluation method is:

[0075] The acidification corrosion inhibition system components provided in the above embodiments and comparative examples are added to hydrochloric acid with a mass concentration of, for example, 15%, respectively, and the corrosion performance evaluation is carried out using a standard BG110SS test piece.

[0076] 1. 15% hydrochloric acid corrosion evaluation

[0077] 500 mL of an acid solution having a hydrochloric acid concentration of 15 wt %, a component A concentration of 3 wt %, and a component B concentration of 0.25 wt % was prepared indoors.

[0078] Acid solution preparation: Measure 210 mL of 31% industrial hydrochloric acid, add 15.0 g of component A and 1.25 g of component B, stir evenly, dilute to 500 mL with tap water, and stir evenly.

[0079] The hanging pieces are made of N80 steel sheets. They are prepared according to standard requirements and weighing records are kept.

[0080] In the high temperature and high pressure dynamic corrosion test system, the corrosion rate test was carried out at 210°C. The results are shown in Table 1.

[0081] It can be seen from Table 1 that the corrosion rate at 210°C meets the requirements of the oil and gas industry, and there is no pitting or cratering on the test piece after corrosion.

[0082] Table 1 Evaluation results of corrosion performance of corrosion inhibitors under 15% hydrochloric acid acidification

[0083]

[0084] 2. 20% hydrochloric acid corrosion evaluation

[0085] 500 mL of an acid solution having a hydrochloric acid concentration of 20 wt %, a component A concentration of 3 wt %, and a component B concentration of 0.15 wt % was prepared indoors.

[0086] Acid solution preparation: Measure 280 mL of 31% industrial hydrochloric acid, add 15 g of component A and 0.78 g of component B, stir evenly, dilute to 500 mL with tap water, and stir evenly.

[0087] The hanging pieces are made of N80 steel sheets. They are prepared according to standard requirements and weighing records are kept.

[0088] In the high temperature and high pressure dynamic corrosion test system, the corrosion rate test was carried out at 180°C. The results are shown in Table 2.

[0089] Table 2 Evaluation results of corrosion performance of corrosion inhibitors under 20% hydrochloric acid acidification

[0090]

[0091] It can be seen from Table 2 that the corrosion rate of hydrochloric acid at a temperature of 180°C and a concentration of 20% meets the first-level standard requirements of the petroleum and natural gas industry, and there is no pitting or cratering on the test piece after corrosion.

[0092] 3. 20% hydrochloric acid corrosion evaluation

[0093] 500 mL of an acid solution having a hydrochloric acid concentration of 20 wt % and a component A concentration of 3 wt % was prepared indoors.

[0094] Acid solution preparation: Measure 280 mL of 31% industrial hydrochloric acid, add 15 g of component A and stir evenly, dilute to 500 mL with tap water and stir evenly.

[0095] The hanging pieces are made of N80 steel sheets. They are prepared according to standard requirements and weighing records are kept.

[0096] In the high temperature and high pressure dynamic corrosion test system, the corrosion rate test was carried out at 160°C. The results are shown in Table 3.

[0097] Table 3 Evaluation results of corrosion performance of corrosion inhibitors under 20% hydrochloric acid acidification

[0098]

[0099] It can be seen from Table 3 that the corrosion rate of hydrochloric acid at a temperature of 160°C and a concentration of 20% meets the first-level standard requirements of the petroleum and natural gas industry, and there is no pitting or cratering on the test piece after corrosion.

Claims

1. A method for preparing a high temperature acidification corrosion inhibitor, comprising the following steps: (1) reacting acrylic acid and / or acrylic acid ester with diethylenetriamine to obtain an initiator; (2) reacting the above initiator with olefin sulfonate, allyl quaternary ammonium salt, N-vinyl pyrrolidone and acrylamide to obtain a corrosion inhibitor precursor; (3) The corrosion inhibitor precursor is subjected to a quaternization reaction to obtain the high temperature acidification resistant corrosion inhibitor.

2. The preparation method according to claim 1, wherein In step (1), the reaction temperature is 140-150°C.

3. The preparation method according to claim 1, wherein In step (1), the weight ratio of acrylic acid and / or acrylic acid ester to diethylenetriamine is 100-150:

50.

4. The preparation method according to claim 1, wherein In step (2), the olefin sulfonate includes one or a combination of two or more of 2-acrylamide 2-methylpropane sulfonate sodium, acrylic acid-2-acrylamide-2-methylpropane sulfonate sodium, sodium allyl sulfonate, and sodium styrene sulfonate.

5. The preparation method according to claim 1, wherein In step (2), the allyl quaternary ammonium salt includes one or a combination of two or more of allyl ammonium chloride, dimethyl diallyl ammonium chloride, trimethyl allyl ammonium chloride, and 4-vinyl benzyl ammonium chloride.

6. The preparation method according to claim 1, wherein In step (2), the reaction temperature is 60-70°C, the reaction time is 10-12h, and the stirring rate is 600-700r / min.

7. The preparation method according to claim 1, wherein In step (2), the weight ratio of the initiator, olefin sulfonate, allyl quaternary ammonium salt, N-vinyl pyrrolidone and acrylamide is 5-15:5-10:5-10:1-5:5-15.

8. The preparation method according to claim 1, wherein In step (3), the quaternizing agent used in the quaternization reaction is dimethyl sulfate.

9. The preparation method according to claim 8, wherein: In step (3), the mass ratio of the corrosion inhibitor precursor to dimethyl sulfate is 1-5:3-8.

10. The preparation method according to claim 1, wherein: In step (3), the temperature of the quaternization reaction is 110-120° C., the reaction time is 10-12 h, and the stirring rate is 800-900 r / min.

11. A high temperature acidification corrosion inhibitor, which is prepared by the preparation method according to any one of claims 1 to 10.

12. A high temperature acidification corrosion inhibition system, comprising the high temperature acidification corrosion inhibition agent according to claim 11.

13. The high temperature acidification corrosion inhibition system according to claim 12, wherein: The high temperature acidification corrosion inhibition system comprises component A, component B, hydrochloric acid and water; Wherein, based on the mass of the high temperature acidification corrosion inhibition system being 100%, the content of component A is 3%-5%, the content of component B is 0.1-1%, the content of hydrochloric acid is 15-20%, and the balance is water, wherein the content of hydrochloric acid is calculated as HCl; Calculated by weight, component A includes 20-35 parts of high temperature acidification corrosion inhibitor, 10-29 parts of organic synergist, 17-20 parts of organic acid, 8-9 parts of alcohol solvent, and 10 parts of dispersant; Component B comprises an inorganic builder.

14. The high temperature acidification corrosion inhibition system according to claim 13, wherein: The organic synergist includes one or a combination of two or more of formamide, N,N-dimethylformamide, propargyl alcohol propoxy compounds, and propargyl alcohol ethoxy compounds.

15. The high temperature acidification corrosion inhibition system according to claim 13, wherein: The organic acid is formic acid and / or acetic acid.

16. The high temperature acidification corrosion inhibition system according to claim 13, wherein: The dispersant is alkylphenol polyoxyethylene ether and / or fatty alcohol polyoxyethylene ether.

17. The high temperature acidification corrosion inhibition system according to claim 13, wherein: The inorganic synergist includes one or a combination of two or more of cuprous chloride, potassium iodide, potassium pyroantimonate, antimony trioxide, and sodium molybdate.

18. Use of the high temperature acidification corrosion inhibitor according to claim 11 or the high temperature acidification corrosion inhibition system according to any one of claims 12 to 17 in acidification corrosion inhibition of oil and gas wells.

19. The use according to claim 18, wherein: The temperature of the oil and gas well is 160-210°C.

Citation Information

Patent Citations

  • Compounded imidazoline corrosion inhibitor and preparation method thereof

    CN103602328A

  • Polymeric imidazoline corrosion inhibitor and preparation method thereof

    CN104762625A

  • Polymer having corrosion inhibition and viscosity reduction effects and preparing method thereof

    CN106188362A

  • Thickening agent for acid fracturing and preparation method thereof

    CN111253518A

  • High-temperature-resistant saturated-salt-water-resistant filtrate reducer for drilling fluid

    CN112759706A

Cited By

  • Corrosion inhibitor and method for its preparation

    CN122979907A