Preparation method of large-size monodisperse polystyrene microspheres
By using a combination method of stabilizing agent, ionic liquid and low boiling point organic matter in the preparation of polystyrene microspheres, the problem of difficulty in removing swelling agents and low production efficiency in the preparation of large-size monodisperse microspheres is solved, and high efficiency is achieved. The preparation of low-cost large-size monodispersed polystyrene microspheres improves the dispersion and particle size uniformity of the microspheres.
Patent Information
- Application Number
- CN202411054785.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-12
AI Technical Summary
It is difficult to effectively prepare large-size monodisperse polystyrene microspheres in the prior art, and common methods have problems such as difficulty in removing swelling agents, low production efficiency and high cost.
Monodispersed polystyrene microspheres, stabilizers, ionic liquids, low boiling organic matter and water stir and swell, then add oil-soluble initiator and vinyl monomer for ultrasonic dispersion, and obtain large amounts through temperature control reaction and nitrogen bubbles. Size monodisperse polystyrene microspheres, optimized swelling agent removal and polymerization process.
The efficient preparation of large-size monodispersed polystyrene microspheres is achieved, which improves production efficiency, reduces production costs, and improves the dispersion and particle size uniformity of the microspheres.
Smart Images

Figure CN118930743A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer functional materials, and more specifically to a method for preparing large-size monodisperse polystyrene microspheres. Background Art
[0002] Monodisperse polymer microspheres have a wide range of applications in the biomedicine, inspection and testing, electronics and other industries. For example, they can be used as chromatographic fillers, conductive film fillers, liquid crystal display intervals, adsorbents, particle exchange resins and other fields. In the application fields of conductive glue fillers, liquid crystal display intervals, chromatographic fillers, etc., the polymer microsphere size is required to have excellent monodispersity. At present, small-sized monodisperse polymer microspheres can be obtained by emulsion polymerization, but due to the limitation of its polymerization method, large-sized polymer microspheres cannot be effectively prepared. For polymer microspheres of 1 to 10 μm, they can be obtained by dispersion polymerization. Dispersion polymerization can obtain polymer microspheres with good dispersion, but usually when preparing polymer microspheres above 5 μm, polymer microspheres with good monodispersity cannot be obtained. Usually, suspension polymerization can prepare large-sized polymer microspheres above 50 μm, but it is very difficult to obtain polymer microspheres with good monodispersity through suspension polymerization. How to prepare large-sized monodisperse polymer microspheres conveniently and quickly has always been a difficulty and pain point in industry research.
[0003] After years of development, the preparation technology of large-sized monodisperse microspheres has made significant progress. The commonly used methods are the swelling agent swelling method and the dynamic swelling method. Both methods have obvious disadvantages. For example, the swelling agent swelling method uses a water-insoluble swelling agent, which cannot be effectively removed in conventional technical solutions; and the volume growth of one swelling is limited. For large-sized microspheres, multiple swellings are required to reach the target size, resulting in a large amount of wastewater in the production process, which not only wastes water resources, but also does not conform to the green and environmentally friendly industry development direction. The dynamic swelling method can increase the volume of one swelling by more than 500 times. For large-sized microspheres, multiple swellings are not required, and it has more advantages in the preparation of large-sized polymer microspheres. However, the preparation process involves extremely low-concentration seed solutions, which leads to the generation of a large amount of wastewater. At the same time, its technical solution has very strict requirements on the control of the water droplet addition speed, requiring the water droplet addition speed to be as slow as possible, and the droplets added should be as small as possible, otherwise, polymer microspheres with good dispersion cannot be obtained. If used for mass production, it will inevitably cause the water droplet addition time to be too long, and the production efficiency will be reduced.
[0004] Currently, CN 115785349 A discloses a method for preparing micron-sized monodisperse cross-linked polystyrene microspheres, which is characterized by comprising the following steps: S1: mixing polyvinyl pyrrolidone, ethanol and water to obtain a mixed solution A; mixing styrene monomer and azobisisobutyronitrile to obtain a mixed solution B; adding the mixed solution B to the mixed solution A under stirring and heating to react, and obtaining seed microspheres after the reaction; S2: mixing the seed microspheres, an aqueous solution containing a surfactant and a swelling agent, and performing a swelling treatment to obtain a mixed solution after the swelling treatment; S3: adding styrene monomer, benzoyl peroxide, divinylbenzene and ethanol to the mixed solution after the swelling treatment, performing a swelling treatment again, and then adding a polyvinyl alcohol solution to perform a heating polymerization treatment to obtain a micron-sized monodisperse cross-linked polystyrene microsphere; and the swelling agent is one of dibutyl phthalate, ethyl acetate, and NN dimethylformamide; in the preparation method, the post-treatment of the swelling agent is relatively difficult, and the dispersion performance of the obtained polystyrene microsphere particle size is still poor and the particle size is small, which cannot meet the high requirements of the biomedicine, inspection and testing, electronics and other industries.
[0005] CN1038756C discloses a method for producing particles whose particle size can be uniformly controlled within the range of 1 to 50 microns, which mainly comprises mixing a monomer or a monomer mixture with a polymer seed particle dispersion under certain conditions, and then maintaining the temperature at the activation temperature of the initiator to react until the particles increase to a selected size and until all the monomers are polymerized, and repeating the above steps until the particle size reaches the target size. This technical solution adopts difficult-to-control technical solutions such as adjusting the feeding rate according to the reaction kinetics, repeated heating and cooling, and screen filtering, resulting in the technical solution having problems such as poor product batch stability, difficulty in controlling the size of each batch of products, low production efficiency, and the need to handle swelling agents in actual applications.
[0006] CN101186661 B discloses a method for preparing polymer particles, and its technical solution mainly includes adding a polymerizable monomer and an initiator to a seed dispersion liquid, heating the liquid for a first-stage reaction, adjusting the temperature, adding a polymerizable monomer, an initiator and a cross-linking agent, and then heating the liquid for a certain period of time for swelling reaction, and then heating the liquid for polymerization to obtain a polymer microsphere of a target size. The technical solution adopts a technical solution of swelling and polymerization, and can obtain a microsphere product with good monodispersity. However, the technical solution still adopts a technical solution of gradually increasing the dripping speed to drip the monomer mixture, and once the dripping speed is not well controlled, the monodispersity will be significantly deteriorated or even polydisperse, which will also cause problems such as poor stability of batch products in actual production applications. In addition, the technical solution is implemented by a two-stage reaction, and the first-stage reaction generally controls the reaction degree to about 80%, which is also a difficulty that is difficult to operate in actual production. In general, the technical solution has many problems in actual production, and it is difficult to effectively reduce production costs. Summary of the invention
[0007] In order to overcome the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing large-sized monodisperse polystyrene microspheres to improve production efficiency, reduce production costs, avoid post-treatment of swelling agents, and at the same time obtain polystyrene microspheres with larger size and better dispersion.
[0008] The present invention provides a method for preparing large-sized monodisperse polystyrene microspheres, comprising the following steps:
[0009] S1. Add monodisperse polystyrene microspheres, stabilizer, ionic liquid and low-boiling point organic matter into water, mix well, and stir to swell at 5-20° C. for 6-8 hours to obtain a seed swelling solution;
[0010] S2, adding the oil-soluble initiator to the vinyl monomer, dispersing under ultrasound for 5-10 minutes, to obtain a monomer mixture;
[0011] S3, adding the monomer mixture to the seed swelling solution, stirring and swelling at 5-20° C. for 6-10 hours to obtain a seed reaction solution;
[0012] S4. Bubble nitrogen into the seed reaction solution and control the temperature to obtain a suspension. After centrifugation, washing and drying, large-sized monodisperse polystyrene microspheres are obtained.
[0013] Preferably, the mass ratio of the monodisperse polystyrene microspheres, stabilizer, ionic liquid, low boiling point organic matter, water, oil-soluble initiator and vinyl monomer is (3-4):1:(0.1-0.5):(10-12):200:(0.8-1.2):(40-50).
[0014] Preferably, the particle size of the monodisperse polystyrene microspheres is 2-5 μm.
[0015] Preferably, the stabilizer is at least one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sorbitan oleate, sorbitan monostearate, and polyoxyethylene sorbitan ester.
[0016] Preferably, the low boiling point organic matter is at least one of dichloromethane, n-pentane and cyclopentane.
[0017] Preferably, the low boiling point organic matter is obtained by mixing dichloromethane, n-pentane and cyclopentane in a mass ratio of 1:2:4.
[0018] Preferably, the ionic liquid is obtained by mixing N-butyl-N-methylpiperidinium bromide and 1,3-dimethylimidazole bis(trifluoromethanesulfonyl)imide in a mass ratio of (1-5):3.
[0019] Preferably, the oil-soluble initiator is benzoyl peroxide.
[0020] Preferably, the vinyl monomer is obtained by mixing styrene and divinylbenzene in a mass ratio of 5:1.
[0021] Preferably, the specific operation of the temperature control reaction in S4 is:
[0022] The seed reaction liquid is first heated to 60-70°C, reacted for 8-10 hours, and then cooled to 40-50°C, reacted for 1-2 hours to obtain a large-sized monodisperse polymer microsphere suspension.
[0023] In summary, the present invention has the following beneficial effects:
[0024] 1. In the swelling stage of the monodisperse polystyrene microspheres in step S1, the present invention adds low-boiling-point organic matter to swell the seed microspheres, thereby solving the problem of subsequent swelling agent removal. In the swelling stage, the low-boiling-point organic matter can swell the seed microspheres well. In step S4, since the temperature has exceeded its boiling point, the low-boiling-point organic matter will volatilize faster. At the same time, the volatilization of the low-boiling-point swelling agent can also be accelerated by passing nitrogen to remove the inhibitory dissolved oxygen in the system, thereby better achieving the expected effect of no residual swelling agent, thereby solving the problem of subsequent swelling agent removal. At the same time, the present invention further preferably uses a mixture of methylene chloride, n-pentane and cyclopentane in a specific mass ratio as the low-boiling-point organic matter, further improving the swelling effect of the monodisperse polystyrene microspheres, facilitating the polymerization of vinyl monomers on the surface of the microspheres, and obtaining large-sized, highly dispersible polystyrene microspheres.
[0025] 2. In the swelling stage of the monodisperse polystyrene microspheres in step S1 of the present invention, an ionic liquid is added, and preferably a mixture of N-butyl-N-methylpiperidinium bromide and 1,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide in a specific mass ratio is used as the ionic liquid. The two synergize with low-boiling organic matter to swell the seed microspheres and activate the seed microspheres. In addition, in the temperature control reaction stage of step S4, the ionic liquid can play an initiating role, promote the polymerization of vinyl monomers on the surface of the microspheres, and help prepare large-sized polystyrene microspheres.
[0026] 3. The present invention performs a temperature-controlled reaction in step S4. In the high-temperature stage, the polymerization reaction is accelerated, and in the low-temperature stage, the remaining vinyl monomer is slowly and evenly polymerized on the surface of the microspheres, thereby increasing the particle size of the polystyrene microspheres, reducing adhesion between the polystyrene microspheres, and improving the dispersibility between the polystyrene microspheres, thereby obtaining polystyrene microspheres with better performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a scanning electron microscope image of the polystyrene microspheres prepared in Example 1;
[0028] Figure 2 This is a scanning electron microscope image of the polystyrene microspheres prepared in Example 2;
[0029] Figure 3 This is a scanning electron microscope image of the polystyrene microspheres prepared in Example 3;
[0030] Figure 4 This is a scanning electron microscope image of the polystyrene microspheres prepared in Example 4;
[0031] Figure 5 This is a scanning electron microscope image of the polystyrene microspheres prepared in Example 5;
[0032] Figure 6 This is a scanning electron microscope image of the polystyrene microspheres prepared in Example 6;
[0033] Figure 7 This is a scanning electron microscope image of the polystyrene microspheres prepared in Example 7;
[0034] Figure 8 This is a scanning electron microscope image of the polystyrene microspheres prepared in Comparative Example 1;
[0035] Fig. 9 This is a scanning electron microscope image of the polystyrene microspheres prepared in Comparative Example 2;
[0036] Fig.10 This is a scanning electron microscope image of the polystyrene microspheres prepared in Comparative Example 3;
[0037] Fig.11 This is a scanning electron microscope image of the polystyrene microspheres prepared in Comparative Example 4;
[0038] Fig.12 This is a scanning electron microscope image of the polystyrene microspheres prepared in Comparative Example 5. DETAILED DESCRIPTION
[0039] The present invention is further described in detail below with reference to the embodiments.
[0040] The specific sources of each raw material and reagent are as follows: monodisperse polystyrene microspheres were purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd. with a particle size of 2-5 μm; 1,3-dimethylimidazole bis(trifluoromethanesulfonyl)imide salt was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No.: 174899-81-1; N-butyl-N-methylpiperidinium bromide was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No.: 94280-72-5; the remaining raw materials, reagents or processing techniques, unless otherwise specified, are all conventional commercially available raw materials or conventional processing techniques in the field.
[0041] Examples 1-7 provide a method for preparing large-sized monodisperse polystyrene microspheres.
[0042] Example 1
[0043] A method for preparing large-sized monodisperse polystyrene microspheres comprises the following steps:
[0044] S1. At room temperature, add 3 g of monodisperse polystyrene microspheres with a particle size of 2 μm, 1 g of sodium dodecyl sulfate, 0.1 g of ionic liquid, and 10 g of dichloromethane to 200 g of water, mix well, and stir and swell at 5° C. for 8 h to obtain a seed swelling solution;
[0045] The ionic liquid is obtained by mixing N-butyl-N-methylpiperidinium bromide and 1,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide in a mass ratio of 1:3;
[0046] S2, adding 0.8 g of benzoyl peroxide to 40 g of vinyl monomer, dispersing under ultrasound for 5 min to obtain a monomer mixture;
[0047] The vinyl monomer is obtained by mixing styrene and divinylbenzene in a mass ratio of 5:1;
[0048] S3, adding the monomer mixture to the seed swelling solution, stirring and swelling at 5° C. for 10 h to obtain a seed reaction solution;
[0049] S4. Bubble nitrogen into the seed reaction solution, first heat it to 60°C, react for 8 hours, then cool it to 40°C, react for 1 hour, and obtain a large-sized monodisperse polymer microsphere suspension; the large-sized monodisperse polymer microsphere suspension is centrifuged, washed, and dried to obtain large-sized monodisperse polystyrene microspheres.
[0050] Example 2
[0051] A method for preparing large-sized monodisperse polystyrene microspheres comprises the following steps:
[0052] S1. At room temperature, add 3 g of monodisperse polystyrene microspheres with a particle size of 2 μm, 1 g of sodium dodecyl sulfate, 0.2 g of ionic liquid, and 12 g of dichloromethane to 200 g of water, mix well, and stir and swell at 20° C. for 6 h to obtain a seed swelling solution;
[0053] The ionic liquid is obtained by mixing N-butyl-N-methylpiperidinium bromide and 1,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide in a mass ratio of 2:3;
[0054] S2, adding 1 g of benzoyl peroxide to 40 g of vinyl monomer, dispersing under ultrasound for 5 min to obtain a monomer mixture;
[0055] The vinyl monomer is obtained by mixing styrene and divinylbenzene in a mass ratio of 5:1;
[0056] S3, adding the monomer mixture to the seed swelling solution, stirring and swelling at 10° C. for 6 h to obtain a seed reaction solution;
[0057] S4. Bubble nitrogen into the seed reaction solution, first heat it to 65°C, react for 10 hours, then cool it to 40°C, react for 2 hours to obtain a large-sized monodisperse polymer microsphere suspension; the large-sized monodisperse polymer microsphere suspension is centrifuged, washed, and dried to obtain large-sized monodisperse polystyrene microspheres.
[0058] Example 3
[0059] A method for preparing large-sized monodisperse polystyrene microspheres comprises the following steps:
[0060] S1. At room temperature, add 3 g of monodisperse polystyrene microspheres with a particle size of 5 μm, 1 g of sodium dodecylbenzene sulfonate, 0.3 g of ionic liquid, and 12 g of cyclopentane to 200 g of water, mix well, and stir and swell at 20° C. for 6 h to obtain a seed swelling solution;
[0061] The ionic liquid is obtained by mixing N-butyl-N-methylpiperidinium bromide and 1,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide in a mass ratio of 1:1;
[0062] S2, adding 1.5 g of benzoyl peroxide to 50 g of vinyl monomer, dispersing under ultrasound for 5 min to obtain a monomer mixture;
[0063] The vinyl monomer is obtained by mixing styrene and divinylbenzene in a mass ratio of 5:1;
[0064] S3, adding the monomer mixture to the seed swelling solution, stirring and swelling at 10° C. for 6 h to obtain a seed reaction solution;
[0065] S4. Bubble nitrogen into the seed reaction solution, first heat it to 65°C, react for 8 hours, then cool it to 45°C, react for 1 hour, and obtain a large-sized monodisperse polymer microsphere suspension; the large-sized monodisperse polymer microsphere suspension is centrifuged, washed, and dried to obtain large-sized monodisperse polystyrene microspheres.
[0066] Example 4
[0067] A method for preparing large-sized monodisperse polystyrene microspheres comprises the following steps:
[0068] S1. At room temperature, add 3.5 g of monodisperse polystyrene microspheres with a particle size of 4 μm, 1 g of dehydrated sorbitol fatty acid, 0.4 g of ionic liquid, and 11 g of n-pentane to 200 g of water, mix well, and stir and swell at 15° C. for 7 h to obtain a seed swelling solution;
[0069] The ionic liquid is obtained by mixing N-butyl-N-methylpiperidinium bromide and 1,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide in a mass ratio of 4:3;
[0070] S2, adding 1.1 g of benzoyl peroxide to 45 g of vinyl monomer, dispersing under ultrasound for 8 min to obtain a monomer mixture;
[0071] The vinyl monomer is obtained by mixing styrene and divinylbenzene in a mass ratio of 5:1;
[0072] S3, adding the monomer mixture to the seed swelling solution, stirring and swelling at 15° C. for 10 h to obtain a seed reaction solution;
[0073] S4. Bubble nitrogen into the seed reaction solution, first heat it to 70°C, react for 9 hours, then cool it to 50°C, react for 1 hour to obtain a large-sized monodisperse polymer microsphere suspension; the large-sized monodisperse polymer microsphere suspension is centrifuged, washed, and dried to obtain large-sized monodisperse polystyrene microspheres.
[0074] Example 5
[0075] A method for preparing large-sized monodisperse polystyrene microspheres comprises the following steps:
[0076] S1. At room temperature, add 4 g of monodisperse polystyrene microspheres with a particle size of 5 μm, 1 g of polyoxyethylene sorbitan ester, 0.5 g of ionic liquid, and 12 g of cyclopentane to 200 g of water, mix well, and stir and swell at 20° C. for 6 h to obtain a seed swelling solution;
[0077] The ionic liquid is obtained by mixing N-butyl-N-methylpiperidinium bromide and 1,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide in a mass ratio of 5:3;
[0078] S2, adding 1.2 g of benzoyl peroxide to 50 g of vinyl monomer, dispersing under ultrasound for 10 min to obtain a monomer mixture;
[0079] The vinyl monomer is obtained by mixing styrene and divinylbenzene in a mass ratio of 5:1;
[0080] S3, adding the monomer mixture to the seed swelling solution, stirring and swelling at 20° C. for 6 hours to obtain a seed reaction solution;
[0081] S4. Bubble nitrogen into the seed reaction solution, first heat it to 70°C, react for 8 hours, then cool it to 40°C, react for 1.5 hours to obtain a large-sized monodisperse polymer microsphere suspension; the large-sized monodisperse polymer microsphere suspension is centrifuged, washed, and dried to obtain large-sized monodisperse polystyrene microspheres.
[0082] Example 6
[0083] A method for preparing large-sized monodisperse polystyrene microspheres comprises the following steps:
[0084] S1. At room temperature, add 3 g of monodisperse polystyrene microspheres with a particle size of 2 μm, 1 g of sodium dodecyl sulfate, 0.1 g of ionic liquid, and 10 g of low-boiling point organic matter to 200 g of water, mix well, and stir and swell at 5°C for 8 h to obtain a seed swelling solution;
[0085] The ionic liquid is obtained by mixing N-butyl-N-methylpiperidinium bromide and 1,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide in a mass ratio of 1:3;
[0086] The low boiling point organic matter is obtained by mixing dichloromethane and n-pentane in a mass ratio of 1:1;
[0087] S2, adding 0.8 g of benzoyl peroxide to 40 g of vinyl monomer, dispersing under ultrasound for 5 min to obtain a monomer mixture;
[0088] The vinyl monomer is obtained by mixing styrene and divinylbenzene in a mass ratio of 5:1;
[0089] S3, adding the monomer mixture to the seed swelling solution, stirring and swelling at 5° C. for 10 h to obtain a seed reaction solution;
[0090] S4. Bubble nitrogen into the seed reaction solution, first heat it to 60°C, react for 8 hours, then cool it to 40°C, react for 1 hour, and obtain a large-sized monodisperse polymer microsphere suspension; the large-sized monodisperse polymer microsphere suspension is centrifuged, washed, and dried to obtain large-sized monodisperse polystyrene microspheres.
[0091] Example 7
[0092] A method for preparing large-sized monodisperse polystyrene microspheres comprises the following steps:
[0093] S1. At room temperature, add 3 g of monodisperse polystyrene microspheres with a particle size of 2 μm, 1 g of sodium dodecyl sulfate, 0.1 g of ionic liquid, and 10 g of low-boiling point organic matter to 200 g of water, mix well, and stir and swell at 5°C for 8 h to obtain a seed swelling solution;
[0094] The ionic liquid is obtained by mixing N-butyl-N-methylpiperidinium bromide and 1,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide in a mass ratio of 1:3;
[0095] The low boiling point organic matter is obtained by mixing dichloromethane, n-pentane and cyclopentane in a mass ratio of 1:2:4;
[0096] S2, adding 0.8 g of benzoyl peroxide to 40 g of vinyl monomer, dispersing under ultrasound for 5 min to obtain a monomer mixture;
[0097] The vinyl monomer is obtained by mixing styrene and divinylbenzene in a mass ratio of 5:1;
[0098] S3, adding the monomer mixture to the seed swelling solution, stirring and swelling at 5° C. for 10 h to obtain a seed reaction solution;
[0099] S4. Bubble nitrogen into the seed reaction solution, first heat it to 60°C, react for 8 hours, then cool it to 40°C, react for 1 hour, and obtain a large-sized monodisperse polymer microsphere suspension; the large-sized monodisperse polymer microsphere suspension is centrifuged, washed, and dried to obtain large-sized monodisperse polystyrene microspheres.
[0100] In order to verify the performance of the large-sized monodisperse polystyrene microspheres provided by the present invention, the inventors set up comparative examples 1-5, wherein:
[0101] Comparative Example 1
[0102] Comparative Example 1 is the same as Example 1, except that N-N-dimethylformamide is used to replace dichloromethane, as follows:
[0103] A method for preparing large-sized monodisperse polystyrene microspheres comprises the following steps:
[0104] S1. At room temperature, add 3 g of monodisperse polystyrene microspheres with a particle size of 2 μm, 1 g of sodium dodecyl sulfate, and 10 g of NN dimethylformamide to 200 g of water, mix well, and stir and swell at 5°C for 8 h to obtain a seed swelling solution;
[0105] S2, adding 0.8 g of benzoyl peroxide to 40 g of vinyl monomer, dispersing under ultrasound for 5 min to obtain a monomer mixture;
[0106] The vinyl monomer is obtained by mixing styrene and divinylbenzene in a mass ratio of 5:1;
[0107] S3, adding the monomer mixture to the seed swelling solution, stirring and swelling at 5° C. for 10 h to obtain a seed reaction solution;
[0108] S4. Bubble nitrogen into the seed reaction solution, first heat it to 60°C, react for 8 hours, then cool it to 40°C, react for 1 hour, and obtain a large-sized monodisperse polymer microsphere suspension; the large-sized monodisperse polymer microsphere suspension is centrifuged, washed, and dried to obtain large-sized monodisperse polystyrene microspheres.
[0109] Comparative Example 2
[0110] Comparative Example 2 is the same as Example 1, except that no ionic liquid is added, as follows:
[0111] A method for preparing large-sized monodisperse polystyrene microspheres comprises the following steps:
[0112] S1. At room temperature, add 3 g of monodisperse polystyrene microspheres with a particle size of 2 μm, 1 g of sodium dodecyl sulfate, and 10 g of dichloromethane to 200 g of water, mix well, and stir and swell at 5° C. for 8 h to obtain a seed swelling solution;
[0113] S2, adding 0.8 g of benzoyl peroxide to 40 g of vinyl monomer, dispersing under ultrasound for 5 min to obtain a monomer mixture;
[0114] The vinyl monomer is obtained by mixing styrene and divinylbenzene in a mass ratio of 5:1;
[0115] S3, adding the monomer mixture to the seed swelling solution, stirring and swelling at 5° C. for 10 h to obtain a seed reaction solution;
[0116] S4. Bubble nitrogen into the seed reaction solution, first heat it to 60°C, react for 8 hours, then cool it to 40°C, react for 1 hour, and obtain a large-sized monodisperse polymer microsphere suspension; the large-sized monodisperse polymer microsphere suspension is centrifuged, washed, and dried to obtain large-sized monodisperse polystyrene microspheres.
[0117] Comparative Example 3
[0118] Comparative Example 3 is the same as Example 1, except that the ionic liquid is only N-butyl-N-methylpiperidinium bromide, specifically as follows:
[0119] A method for preparing large-sized monodisperse polystyrene microspheres comprises the following steps:
[0120] S1. At room temperature, add 3 g of monodisperse polystyrene microspheres with a particle size of 2 μm, 1 g of sodium dodecyl sulfate, 0.1 g of ionic liquid, and 10 g of dichloromethane to 200 g of water, mix well, and stir and swell at 5° C. for 8 h to obtain a seed swelling solution;
[0121] The ionic liquid is N-butyl-N-methylpiperidinium bromide;
[0122] S2, adding 0.8 g of benzoyl peroxide to 40 g of vinyl monomer, dispersing under ultrasound for 5 min to obtain a monomer mixture;
[0123] The vinyl monomer is obtained by mixing styrene and divinylbenzene in a mass ratio of 5:1;
[0124] S3, adding the monomer mixture to the seed swelling solution, stirring and swelling at 5° C. for 10 h to obtain a seed reaction solution;
[0125] S4. Bubble nitrogen into the seed reaction solution, first heat it to 60°C, react for 8 hours, then cool it to 40°C, react for 1 hour, and obtain a large-sized monodisperse polymer microsphere suspension; the large-sized monodisperse polymer microsphere suspension is centrifuged, washed, and dried to obtain large-sized monodisperse polystyrene microspheres.
[0126] Comparative Example 4
[0127] Comparative Example 4 is the same as Example 1, except that the ionic liquid is only 1,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide salt, specifically as follows:
[0128] A method for preparing large-sized monodisperse polystyrene microspheres comprises the following steps:
[0129] S1. At room temperature, add 3 g of monodisperse polystyrene microspheres with a particle size of 2 μm, 1 g of sodium dodecyl sulfate, 0.1 g of ionic liquid, and 10 g of dichloromethane to 200 g of water, mix well, and stir and swell at 5° C. for 8 h to obtain a seed swelling solution;
[0130] The ionic liquid is 1,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide salt;
[0131] S2, adding 0.8 g of benzoyl peroxide to 40 g of vinyl monomer, dispersing under ultrasound for 5 min to obtain a monomer mixture;
[0132] The vinyl monomer is obtained by mixing styrene and divinylbenzene in a mass ratio of 5:1;
[0133] S3, adding the monomer mixture to the seed swelling solution, stirring and swelling at 5° C. for 10 h to obtain a seed reaction solution;
[0134] S4. Bubble nitrogen into the seed reaction solution, first heat it to 60°C, react for 8 hours, then cool it to 40°C, react for 1 hour, and obtain a large-sized monodisperse polymer microsphere suspension; the large-sized monodisperse polymer microsphere suspension is centrifuged, washed, and dried to obtain large-sized monodisperse polystyrene microspheres.
[0135] Comparative Example 5
[0136] Comparative Example 5 is the same as Example 1, except that the specific operation of the temperature control reaction in S4 is to raise the temperature of the seed reaction solution to 60° C. and react for 9 hours, as follows:
[0137] A method for preparing large-sized monodisperse polystyrene microspheres comprises the following steps:
[0138] S1. At room temperature, add 3 g of monodisperse polystyrene microspheres with a particle size of 2 μm, 1 g of sodium dodecyl sulfate, and 10 g of dichloromethane to 200 g of water, mix well, and stir and swell at 5° C. for 8 h to obtain a seed swelling solution;
[0139] S2, adding 0.8 g of benzoyl peroxide to 40 g of vinyl monomer, dispersing under ultrasound for 5 min to obtain a monomer mixture;
[0140] The vinyl monomer is obtained by mixing styrene and divinylbenzene in a mass ratio of 5:1;
[0141] S3, adding the monomer mixture to the seed swelling solution, stirring and swelling at 5° C. for 10 h to obtain a seed reaction solution;
[0142] S4. Bubble nitrogen into the seed reaction solution, raise the temperature to 60° C., and react for 9 hours to obtain a large-sized monodisperse polymer microsphere suspension. The large-sized monodisperse polymer microsphere suspension is centrifuged, washed, and dried to obtain large-sized monodisperse polystyrene microspheres.
[0143] The morphologies of the polystyrene microspheres in Examples 1-7 and Comparative Examples 1-5 were observed using a scanning electron microscope, and the software Image J was used for image analysis. 100 microspheres were randomly selected from the scanning electron microscope images to measure the particle size. The average particle size and the coefficient of variation of the microspheres were calculated using the following formula according to the statistical method. The following results were obtained. Figure 1-12 And Table 1:
[0144] Average particle size
[0145] Coefficient of variation
[0146] The scanning electron microscopy images of the polystyrene microspheres prepared in Examples 1-7 are as follows: Figure 1-7 As shown, it can be seen that the polystyrene microspheres prepared by the present invention have good dispersibility, no microsphere aggregation and no specific microspheres appear, the surface is smooth, the sphericity is good, and they are in a monodisperse state. The scanning electron microscopy images of the polystyrene microspheres prepared in Comparative Examples 1-5 are as follows Figure 8-12 As shown, it can be seen that the polystyrene microspheres prepared in Comparative Examples 1-5 have uneven surfaces, wrinkles, and adhesion, and are relatively small in size; and the microspheres in Comparative Example 4 swell and rupture.
[0147] Table 1:
[0148]
[0149]
[0150] It can be seen from the data shown in Table 1 above that the polystyrene microspheres prepared in Examples 1-7 of the present invention have better dispersibility and larger size than those in Comparative Examples 1-5, no microsphere aggregation and no specific microspheres appear, good sphericity, monodisperse state, good reproducibility between particle sizes and small coefficient of variation.
[0151] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.
Claims
1. A method for preparing large-sized monodisperse polystyrene microspheres, characterized in that: The following steps are involved: S1. Add monodisperse polystyrene microspheres, stabilizer, ionic liquid and low-boiling point organic matter into water, mix well, and stir to swell at 5-20° C. for 6-8 hours to obtain a seed swelling solution; S2, adding the oil-soluble initiator to the vinyl monomer, dispersing under ultrasound for 5-10 minutes, to obtain a monomer mixture; S3, adding the monomer mixture to the seed swelling solution, stirring and swelling at 5-20° C. for 6-10 hours to obtain a seed reaction solution; S4. Bubble nitrogen into the seed reaction solution and control the temperature to obtain a suspension. After centrifugation, washing and drying, large-sized monodisperse polystyrene microspheres are obtained.
2. The method for preparing large-sized monodisperse polystyrene microspheres according to claim 1, characterized in that: The mass ratio of the monodisperse polystyrene microspheres, stabilizer, ionic liquid, low boiling point organic matter, water, oil-soluble initiator and vinyl monomer is (3-4):1:(0.1-0.5):(10-12):200:(0.8-1.2):(40-50).
3. The method for preparing large-sized monodisperse polystyrene microspheres according to claim 1, characterized in that: The particle size of the monodisperse polystyrene microspheres is 2-5 μm.
4. The method for preparing large-sized monodisperse polystyrene microspheres according to claim 1, characterized in that: The stabilizer is at least one of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sorbitan fatty acid, and polyoxyethylene sorbitan ester.
5. The method for preparing large-sized monodisperse polystyrene microspheres according to claim 1, characterized in that: The low boiling point organic matter is at least one of dichloromethane, n-pentane and cyclopentane.
6. The method for preparing large-sized monodisperse polystyrene microspheres according to claim 5, characterized in that: The low boiling point organic matter is obtained by mixing dichloromethane, n-pentane and cyclopentane in a mass ratio of 1:2:
4.
7. The method for preparing large-sized monodisperse polystyrene microspheres according to claim 1, characterized in that: The ionic liquid is obtained by mixing N-butyl-N-methylpiperidinium bromide and 1,3-dimethylimidazole bis(trifluoromethanesulfonyl)imide in a mass ratio of (1-5):
3.
8. The method for preparing large-sized monodisperse polystyrene microspheres according to claim 1, characterized in that: The oil-soluble initiator is benzoyl peroxide.
9. The method for preparing large-sized monodisperse polystyrene microspheres according to claim 1, characterized in that: The vinyl monomer is obtained by mixing styrene and divinylbenzene in a mass ratio of 5:
1.
10. The method for preparing large-sized monodisperse polystyrene microspheres according to claim 1, characterized in that: The specific operation of the temperature control reaction in S4 is: The seed reaction liquid is first heated to 60-70°C, reacted for 8-10 hours, and then cooled to 40-50°C, reacted for 1-2 hours to obtain a large-sized monodisperse polymer microsphere suspension.
Citation Information
Cited By
Monodisperse polymer porous microsphere and preparation method thereof
CN120464015A