Light / moisture-curable urethane compound, light / moisture-curable urethane prepolymer, and light / moisture-curable resin composition
By using urethane compounds and prepolymers with specific structures, combined with photopolymerization initiators and free radical polymerizable compounds, a photo-wet-curing resin composition was formed, which solved the problem of insufficient adhesion both initially and after wet curing, and achieved a balance between high adhesion and flexibility.
Patent Information
- Application Number
- CN202411165106.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2018-12-18
- Filing Date
- 2019-12-17
- Publication Date
- 2024-11-12
AI Technical Summary
Existing light-curing and moisture-curing resin compositions have insufficient initial adhesion and adhesion after moisture curing, making it difficult to meet high adhesion requirements.
A photocurable resin composition is formed by combining a photocurable urethane prepolymer with a photopolymerization initiator, a free radical polymerizable compound having a polyol backbone containing more than three hydroxyl groups in one molecule and more than two isocyanate groups and more than one free radical polymerizable group at the molecule end.
It significantly improves the initial adhesion and adhesion after wet curing of light-curing resin compositions, ensuring high adhesion and flexibility in complex environments.
Smart Images

Figure BDA0005007630220000341
Abstract
Description
[0001] The invention of the present application is a divisional application of the application with application number 201980083744.5, invention name “Light-curable urethane compounds, light-curable urethane prepolymers and light-curable resin compositions” and application date December 17, 2019. Technical Field
[0002] The present invention relates to a light moisture curable urethane compound, a light moisture curable urethane prepolymer, and a light moisture curable resin composition. Background Art
[0003] It is known that photocurable resins have the characteristics of excellent curing speed and simple curing process. However, photocurable resins have the problem that they are cured only in the range irradiated with light, and remain uncured if they enter the gaps and dark areas of the adherend. From this point of view, in recent years, in order to prevent the uncured parts from remaining, resins that are given moisture curing properties in addition to photocuring properties have been developed.
[0004] A method of using a light-curable moisture-curable resin composition containing a urethane prepolymer having at least one isocyanate group and at least one (meth)acryloyl group in a molecule and combining light curing and moisture curing is disclosed (Patent Documents 1 and 2).
[0005] However, when using a light moisture curable resin composition as disclosed in these documents, the initial adhesive strength immediately after photocuring and bonding to an adherend may be insufficient.
[0006] Patent Documents 3 to 5 disclose optical moisture curable resin compositions containing a radical polymerizable composition, an optical moisture curable urethane prepolymer as a compound having an isocyanate group and a reactive double bond, and a moisture curable urethane prepolymer, and show that initial adhesion is improved.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2008-274131
[0010] Patent Document 2: Japanese Patent Application Publication No. 2008-63406
[0011] Patent Document 3: Japanese Patent No. 5824597
[0012] Patent Document 4: Japanese Patent No. 2017-14518
[0013] Patent Document 5: International Publication No. 2013 / 016133 Summary of the invention
[0014] Problems to be solved by the invention
[0015] However, even when the above-mentioned conventional optical moisture-curable resin composition is used, it is found that the adhesive strength after moisture curing is insufficient and there is room for improvement.
[0016] Therefore, an object of the present invention is to provide a light moisture curable urethane compound having excellent initial adhesive force and adhesive force after moisture curing, a light moisture curable urethane prepolymer containing the light moisture curable urethane compound, and a light moisture curable resin composition.
[0017] Means for solving problems
[0018] The inventors of the present invention have conducted in-depth research to solve the above-mentioned problems. As a result, it is predicted that the above-mentioned problems are caused by the structure of the light moisture curable urethane compound. That is, the light moisture curable urethane prepolymer used in the past contains a urethane compound having a skeleton derived from a polyol containing two hydroxyl groups in one molecule and having one isocyanate group and one reactive double bond at the end of the molecule. It is predicted that such a structure has a small number of isocyanate groups that contribute to moisture curing, and the adhesive force after moisture curing is poor.
[0019] Based on such prediction, the present inventors have found that a carbamate compound having a skeleton derived from a polyol containing three or more hydroxyl groups in one molecule and having two or more isocyanate groups and one or more free radical polymerizable groups at the molecular end, a light moisture curable carbamate prepolymer containing the carbamate compound, and a light moisture curable resin composition can solve the above-mentioned problems, and have completed the present invention. That is, the present invention is as follows.
[0020] [1] An optical moisture curable urethane compound comprising a skeleton derived from a polyol (a) having three or more hydroxyl groups in one molecule and having two or more isocyanate groups and one or more radical polymerizable groups at a molecular terminal.
[0021] [2] The optical moisture curable urethane compound according to the above [1], which is obtained by reacting a polyol component (A) containing the above polyol (a), a compound (B) having an isocyanate group and having a free radical polymerizable group at the terminal, and a polyisocyanate compound (C).
[0022] [3] The optical moisture curable urethane compound according to [1] or [2] above, wherein the weight average molecular weight is 500 to 30,000.
[0023] [4] A light moisture curable urethane prepolymer comprising the light moisture curable urethane compound according to any one of [1] to [3] above.
[0024] [5] The optical moisture curable urethane prepolymer according to [4] above, which has a weight average molecular weight of 500 to 30,000.
[0025] [6] An optical moisture curable resin composition comprising the optical moisture curable urethane prepolymer according to [4] or [5] above, and a photopolymerization initiator.
[0026] [7] The optical moisture curable resin composition according to [6] above, further comprising a radical polymerizable compound.
[0027] [8] The optical moisture curable resin composition according to [6] or [7], further comprising a moisture curable urethane prepolymer.
[0028] [9] The optical moisture curable resin composition according to [7] or [8], wherein the radical polymerizable compound contains a monofunctional radical polymerizable compound and a polyfunctional radical polymerizable compound.
[0029]
[10] An adhesive for electronic components, comprising the optical moisture curable resin composition according to any one of [6] to [9].
[0030]
[11] An adhesive for a display element, comprising the optical moisture curable resin composition according to any one of [6] to [9].
[0031] Effects of the Invention
[0032] According to the present invention, there are provided a light moisture curable urethane compound having excellent initial adhesive force and adhesive force after moisture curing, a light moisture curable urethane prepolymer containing the light moisture curable urethane compound, and a light moisture curable resin composition. DETAILED DESCRIPTION
[0033] [Light moisture curable urethane compound]
[0034] The light-curable moisture-curable urethane compound of the present invention comprises a urethane compound having a skeleton derived from a polyol (a) having three or more hydroxyl groups in one molecule and having two or more isocyanate groups and one or more free radical polymerizable groups at the molecular end. The light-curable property is mainly exhibited by polymerization based on the free radical polymerizable group present at the molecular end, and the moisture-curable property is mainly exhibited by polymerization based on the isocyanate group present at the molecular end.
[0035] The light moisture curable urethane compound of the present invention has two or more isocyanate groups at the molecular end, so the adhesive force after moisture curing is effectively improved. In addition, the adhesive force after moisture curing of the urethane prepolymer containing the urethane compound and the light moisture curable resin composition containing the urethane prepolymer is also effectively improved.
[0036] The optical moisture curable urethane compound of the present invention has a free radical polymerizable group at the molecular end, so the initial adhesion is also good. In addition, the urethane prepolymer containing the urethane compound and the optical moisture curable resin composition containing the urethane prepolymer also have good initial adhesion.
[0037] In this specification, the initial adhesive strength refers to the adhesive strength at 25°C immediately after the optical moisture curing resin composition is photocured and bonded to an adherend, and the adhesive strength after moisture curing refers to the adhesive strength at 25°C after light curing and moisture curing.
[0038] (Polyol skeleton)
[0039] The light moisture curable urethane compound in the present invention contains a skeleton derived from a polyol having three or more hydroxyl groups in one molecule. As described later, the light moisture curable urethane prepolymer preferably uses a polyol (a) containing three or more hydroxyl groups in one molecule as a raw material in its manufacturing process, and introduces a free radical polymerizable group and an isocyanate group by the reaction of the hydroxyl group with an isocyanate group. Therefore, the light moisture curable urethane compound has a skeleton derived from a polyol containing three or more hydroxyl groups in one molecule.
[0040] The light moisture curable urethane compound contains a skeleton derived from a polyol having three or more hydroxyl groups, and thus a large number of functional groups involved in light curing and moisture curing can be introduced into the molecule, so that the initial adhesive strength and the adhesive strength after moisture curing become excellent.
[0041] Furthermore, from the viewpoint of preventing gelation during storage, the light moisture curable urethane compound preferably has a skeleton derived from a polyol containing 10 or less hydroxyl groups in one molecule, more preferably has a skeleton derived from a polyol containing 8 or less hydroxyl groups in one molecule, and further preferably has a skeleton derived from a polyol containing 6 or less hydroxyl groups in one molecule.
[0042] Furthermore, from the viewpoint of improving the elongation and flexibility of the cured product of the optical moisture curable urethane prepolymer, the optical moisture curable urethane compound particularly preferably has a skeleton derived from a polyol having three hydroxyl groups in one molecule.
[0043] The polyol having three or more hydroxyl groups in one molecule in the optical moisture curable urethane compound of the present invention is preferably a polyol (a) having three or more hydroxyl groups in one molecule described below. The details of the polyol (a) will be described later.
[0044] (isocyanate group)
[0045] The optical moisture curable urethane compound of the present invention has two or more isocyanate groups at the molecular terminal. This facilitates the curing of the optical moisture curable urethane prepolymer during moisture curing, thereby improving the adhesive strength.
[0046] The number of isocyanates at the molecular end of the optical moisture curable urethane compound is preferably 2 to 5, more preferably 2 to 4, and even more preferably 2. When the number of isocyanates at the molecular end is 5 or less, gelation during storage can be suppressed, and excessive curing can be prevented, thereby maintaining good flexibility and adhesive strength.
[0047] The ratio of isocyanate groups in the light moisture curable urethane compound of the present invention is preferably 1.5% by mass or more, more preferably 2% by mass or more, preferably 7% by mass or less, more preferably 5% by mass or less. By being 1.5% by mass or more, sufficient adhesion and flexibility are easily obtained during moisture curing. If it is 7% by mass or less, the initial adhesion during photocuring is easy to become good. From the viewpoint of the balance between light curing and moisture curing, the ratio of isocyanate groups is preferably 2 to 5% by mass.
[0048] As a method for introducing an isocyanate group into a molecular terminal, a method of reacting the above-mentioned polyol (a) with a polyisocyanate compound is preferably mentioned.
[0049] The polyisocyanate compound may be an aliphatic polyisocyanate compound or an aromatic polyisocyanate compound, but an aromatic polyisocyanate compound is preferred because of its high reactivity.
[0050] Examples of the aromatic polyisocyanate compound include diphenylmethane diisocyanate, liquid modified products of diphenylmethane diisocyanate, polymeric MDI (methane diisocyanate), toluene diisocyanate, naphthalene-1,5-diisocyanate, etc. The polyisocyanate compound may be used alone or in combination of two or more.
[0051] (Free Radical Polymerization Group)
[0052] The optical moisture curable urethane compound of the present invention has one or more radical polymerizable groups at the molecular terminal, thereby improving the initial adhesive force.
[0053] The number of radical polymerizable groups at the molecular end of the carbamate compound is preferably 1 to 4, more preferably 1 to 2, and even more preferably 1. When the number of radical polymerizable groups at the molecular end is 4 or less, gelation during storage can be suppressed, and excessive curing can be prevented, thereby maintaining good flexibility and adhesiveness.
[0054] As a method for introducing a radical polymerizable group into a molecular terminal, the following method is preferred. That is, a polyol compound (a) and a compound (B) having an isocyanate group and having a radical polymerizable group at the terminal can be used to react the hydroxyl group of the polyol compound (a) with the isocyanate group of the compound (B) to obtain a carbamate compound having a radical polymerizable group at the molecular terminal.
[0055] The type of radical polymerizable group is not particularly limited, and from the viewpoint of photocurability, examples thereof include (meth)acryloyl, vinyl, and allyl groups, among which (meth)acryloyl is preferred. It should be noted that the so-called (meth)acryloyl group refers to an acryloyl group or a methacryloyl group.
[0056] When the number of radical polymerizable groups at the molecular terminal in the optical moisture curable urethane compound is 2 or more, the plurality of radical polymerizable groups may be of the same type or of different types.
[0057] The weight average molecular weight of the optical moisture curable urethane compound is preferably 500 or more, more preferably 1,000 or more, further preferably 2,000 or more, particularly preferably 5,000 or more, and is preferably 30,000 or less, more preferably 20,000 or less, further preferably 15,000 or less, particularly preferably 12,000 or less.
[0058] If the weight average molecular weight is 500 or more, the crosslinking density when curing the optical moisture curable resin composition containing the carbamate compound described below will not be too high, and the flexibility can be improved. If it is 30,000 or less, the coating property of the optical moisture curable resin composition containing the carbamate compound described below can be improved.
[0059] In the present invention, the weight average molecular weight is a value obtained by gel permeation chromatography (GPC) measurement and conversion of polystyrene. As a column when the weight average molecular weight obtained by polystyrene conversion is measured by GPC, for example, Shodex LF-804 (Showa Denko Co., Ltd.) etc. can be mentioned. In addition, as the solvent used in GPC, tetrahydrofuran etc. can be mentioned.
[0060] [Light moisture curable resin composition]
[0061] The optical moisture curable resin composition of the present invention contains an optical moisture curable urethane prepolymer and a photopolymerization initiator.
[0062] <Light-moisture-curable urethane prepolymer>
[0063] The optical moisture curable urethane prepolymer of the present invention contains the optical moisture curable urethane compound described above.
[0064] The optical moisture curable urethane prepolymer of the present invention is preferably obtained by reacting a polyol component (A) containing a polyol (a) having three or more hydroxyl groups in one molecule, a compound (B) having an isocyanate group and having a radical polymerizable group at a terminal, and a polyisocyanate compound (C).
[0065] The multiple hydroxyl groups of the polyol (a) react with the isocyanate groups of the compound (B) and the isocyanate groups of the compound (C), thereby obtaining a light moisture curable urethane prepolymer containing a light moisture curable urethane compound.
[0066] In such a reaction, in addition to the above-mentioned light moisture curable urethane compound, a urethane compound of another structure can also be simultaneously produced. Therefore, the light moisture curable urethane prepolymer can be present as a mixture containing the light moisture curable urethane compound.
[0067] The content of the optical moisture curable urethane compound in the optical moisture curable urethane prepolymer can be adjusted by adjusting the types and composition ratio of the polyol component (A), the compound (B), and the compound (C).
[0068] The weight average molecular weight of the light moisture curable urethane prepolymer is preferably 500 or more, more preferably 1,000 or more, further preferably 2,000 or more, particularly preferably 5,000 or more, preferably 30,000 or less, more preferably 20,000 or less, further preferably 15,000 or less, particularly preferably 12,000 or less. If the weight average molecular weight is 500 or more, the crosslinking density when curing the light moisture curable resin composition will not become too high, and the flexibility can be improved. If it is 30,000 or less, the coating property of the light moisture curable resin composition can be made good.
[0069] The weight average molecular weight of the photocurable urethane prepolymer is measured by GPC as described above. It should be noted that, in the molecular weight distribution curve obtained by GPC measurement, when multiple peaks derived from the photocurable urethane prepolymer are confirmed, the weight average molecular weight can be calculated based on the multiple peaks.
[0070] (Polyol component (A))
[0071] The polyol component (A) contains a polyol (a) having three or more hydroxyl groups in one molecule. As the polyol (a) containing three or more hydroxyl groups in one molecule, preferably, polyether polyols, polyester polyols, polyalkylene polyols, polycarbonate polyols, etc. having three or more hydroxyl groups can be cited. Among them, polyether polyols and polyester polyols having three or more hydroxyl groups are more preferred, and polyether polyols are further preferred.
[0072] From the viewpoint of improving the initial adhesion of the urethane prepolymer and the adhesive strength after moisture curing, the polyether polyol having three or more hydroxyl groups is preferably a trifunctional polyether polyol, a tetrafunctional polyether polyol, a pentafunctional polyether polyol, or a hexafunctional polyether polyol. Among them, from the viewpoint of improving the elongation of the cured product of the urethane prepolymer and the viewpoint of easy availability, a trifunctional polyether polyol (triol component) is preferred.
[0073] It should be noted that the term "trifunctional" means having three hydroxyl groups, and the same applies to the others.
[0074] The polyether polyol having three or more hydroxyl groups is preferably obtained by adding alkylene oxide to a polyol having three or more hydroxyl groups such as trimethylolpropane, glycerol, and pentaerythritol. Here, the alkylene oxide is preferably any one of ethylene oxide and propylene oxide, but more preferably propylene oxide. In addition, the alkylene oxide added may be both ethylene oxide and propylene oxide, in which case, it is preferred that propylene oxide is mainly added. The propylene oxide in all the added alkoxides is preferably 55% by mass or more, and more preferably 75% by mass or more. As such a polyether polyol, for example, terminal ethylene oxide addition type polyoxypropylene glycol can be cited.
[0075] Examples of the trifunctional polyether polyol include "Preminol 7012", "Preminol 7001K", "Preminol S3025" and "Excenol 430" manufactured by Asahi Glass Co., Ltd.
[0076] Examples of the tetrafunctional polyether polyol include "Excenol 410NE" manufactured by Asahi Glass Co., Ltd. and the like.
[0077] Examples of the hexafunctional polyether polyol include "Excenol 385SO" manufactured by Asahi Glass Co., Ltd., and the like.
[0078] As the polyester polyol having three or more hydroxyl groups, trifunctional polyester polyol, tetrafunctional polyester polyol, pentafunctional polyester polyol, and hexafunctional polyester polyol are preferred from the viewpoint of improving initial adhesion and adhesion after moisture curing. Among them, trifunctional polyester polyol is preferred from the viewpoint of improving the elongation of the cured product of the optical moisture curable resin composition and from the viewpoint of easy availability.
[0079] The polyester polyol having three or more hydroxyl groups can generally be obtained by reacting a low molecular weight diol, a low molecular weight dicarboxylic acid, and a triol.
[0080] Examples of the low molecular weight diol include ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butadiene glycol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, and cyclohexanediol.
[0081] Examples of the low molecular weight dicarboxylic acid include terephthalic acid, isophthalic acid, 1,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, decamethylene dicarboxylic acid, and dodecamethylene dicarboxylic acid.
[0082] Examples of the triol include trimethylolpropane and glycerin.
[0083] Examples of the trifunctional polyester polyol include "Kuraray Polyol F-1010" manufactured by Kuraray Corporation.
[0084] The weight average molecular weight of the polyol (a) is preferably 500 or more, more preferably 5,000 or more, and preferably 30,000 or less, more preferably 25,000 or less. When the weight average molecular weight is within such a range, photocurability becomes good and initial adhesive strength tends to be improved.
[0085] The weight average molecular weight can be measured by gel permeation chromatography (GPC).
[0086] The optical moisture curable urethane compound contained in the optical moisture curable urethane prepolymer of the present invention is preferably a compound obtained by reacting 5 to 50 mol % of the hydroxyl groups of all the terminal hydroxyl groups of the polyol (a) with the compound (B) described below. The optical moisture curable composition containing such an optical moisture curable urethane prepolymer has excellent initial adhesion and adhesive strength after moisture curing.
[0087] The polyol component (A) preferably includes a polyol (a) containing three or more hydroxyl groups in one molecule and a polyol (b) containing two hydroxyl groups in one molecule. In this case, the content of the polyol (b) containing two hydroxyl groups in one molecule is preferably 50 parts by mass or more, more preferably 100 parts by mass or more, preferably 15,000 parts by mass or less, more preferably 1,500 parts by mass or less, and further preferably 1000 parts by mass or less relative to 100 parts by mass of the polyol (a) containing three or more hydroxyl groups in one molecule. In this way, by containing the polyol (b), the initial adhesion of the optical moisture curable resin composition of the present invention obtained is improved, and gelation during storage can be suppressed.
[0088] The weight average molecular weight of the polyol (b) is preferably 500 or more, more preferably 1,000 or more, preferably 3,500 or less, more preferably 3,000 or less, and further preferably 2,000 or less. When the weight average molecular weight is within such a range, the adhesion of the optical moisture curable resin composition is improved and the elongation of the cured product is improved.
[0089] The type of the polyol (b) is not particularly limited, and examples thereof include polyester polyols, polyether polyols, polyalkylene polyols, polycarbonate polyols, and the like, with polyether polyols and polyester polyols being preferred.
[0090] The polyester polyol as the polyol (b) can be produced by polycondensation of a polycarboxylic acid and a polyol, and other examples thereof include poly-ε-caprolactone polyol obtained by ring-opening polymerization of ε-caprolactam.
[0091] As the polycarboxylic acid used for producing the polyester polyol, generally used are dicarboxylic acids such as terephthalic acid, isophthalic acid, 1,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, decamethylene dicarboxylic acid, and dodecamethylene dicarboxylic acid.
[0092] In addition, as the polyol used for producing the polyester polyol, generally, diols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butadiene glycol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, and cyclohexanediol can be used.
[0093] Examples of the polyether polyol as the polyol (b) include polyethylene glycol, polypropylene glycol, etc. In addition, examples include ring-opening polymerized compounds of tetrahydrofuran, ring-opening polymerized compounds of 3-methyltetrahydrofuran, random copolymers or block copolymers thereof or derivatives thereof, and bisphenol-type polyoxyalkylene modified products.
[0094] The above-mentioned bisphenol-type polyoxyalkylene modified body is a polyether polyol obtained by allowing an oxyalkylene to react with the active hydrogen part of the bisphenol-type molecular skeleton, and can be a random copolymer or a block copolymer. As the above-mentioned oxyalkylene, for example, ethylene oxide, propylene oxide, butylene oxide, isobutylene oxide, etc. can be mentioned. The above-mentioned bisphenol-type polyoxyalkylene modified body is preferably added with one or more oxyalkylenes at both ends of the bisphenol-type molecular skeleton. As the bisphenol type, there is no particular limitation, and A type, F type, S type, etc. can be mentioned, preferably bisphenol A type. From the viewpoint of the ease of introduction of reactive double bonds and the storage stability and flexibility of the prepolymer, it is more preferably an addition polymerization compound using a multifunctional diol as a starting material.
[0095] Examples of the polyalkylene polyol as the polyol (b) include polybutadiene polyol, hydrogenated polybutadiene polyol, hydrogenated polyisoprene polyol, and the like.
[0096] As polycarbonate polyol as a polyol (b), polyhexamethylene carbonate polyol, polycyclohexanedimethylene carbonate polyol, etc. are mentioned, for example.
[0097] Among the polyols (b), from the viewpoint of improving the initial adhesion, adhesive strength after moisture curing, and toughness of the optical moisture curable resin composition, preferred are ring-opening polymerized compounds of tetrahydrofuran and ring-opening polymerized compounds of 3-methyltetrahydrofuran, and more preferred is polytetramethylene ether glycol.
[0098] When the polyol (b) is used, as described above, it is preferred to use a triol component having three hydroxyl groups in one molecule as the polyol (a), and polyoxypropylene glycol using glycerol as a starting material and terminal ethylene oxide addition type polypropylene glycol are particularly preferred. On the other hand, as the diol component (polyol (b)) combined with the triol component, a ring-opening polymerization compound of tetrahydrofuran, a ring-opening polymerization compound of 3-methyltetrahydrofuran, or a random copolymer or block copolymer of these or their derivatives is preferred.
[0099] In addition, when polyol (a) and polyol (b) are used together, substances with similar structures can be combined. Polyol (a) and polyol (b) have similar structures, so that polyol (a) and polyol (b) are easily compatible. Specifically, when polyether polyol is used as polyol (a), polyether polyol is also preferably used as polyol (b). Similarly, when polyester polyol is used as polyol (a), polyester polyol is preferably used as polyol (b).
[0100] (Compound (B))
[0101] By using a compound (B) having an isocyanate group and having a radical polymerizable group at a terminal, the hydroxyl group of the polyol compound (a) reacts with the isocyanate group of the compound (B) to obtain a light moisture curable urethane prepolymer containing a urethane compound having a radical polymerizable group at a molecular terminal.
[0102] As compound (B), for example, vinyl isocyanate etc. can be mentioned. In addition, compounds synthesized by reacting various diisocyanate compounds with compounds having a hydroxyl group and a (meth) acryloyl group in a ratio of isocyanate group / hydroxyl group (molar ratio) of 2 can also be used. Among them, 2-isocyanate ethyl methacrylate, 2-isocyanate ethyl acrylate, 1,1-(bisacryloyloxymethyl) ethyl isocyanate, 1,1-(bismethacryloyloxymethyl) ethyl isocyanate etc. can be mentioned from the viewpoint of easy availability, and 2-isocyanate ethyl acrylate is more preferred from the viewpoint of photoreactivity.
[0103] The amount of the compound (B) is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, based on 100 parts by mass of the polyol component (A).
[0104] (Compound (C))
[0105] By using a polyisocyanate compound (C), the hydroxyl group of the polyol compound (a) reacts with a part of the isocyanate groups of the compound (C), thereby obtaining a urethane prepolymer having an isocyanate group of the compound (C) different from the reacted isocyanate group at the molecular end. The polyisocyanate compound (C) can be the one described above.
[0106] The amount of the polyisocyanate compound (C) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and preferably 150 parts by mass or less, more preferably 100 parts by mass or less, based on 100 parts by mass of the polyol component (A).
[0107] The method for producing the optical moisture curable urethane prepolymer of the present invention is preferably a method for reacting (A) to (C) as described above. More preferably, it is a method for producing the prepolymer comprising the following steps: a first step of reacting a polyol component (A) with a compound (B) having an isocyanate group and having a terminal free radical polymerizable group to produce a terminal free radical polymerizable group-modified polyol compound; and a second step of reacting the terminal free radical polymerizable group-modified polyol compound with a polyisocyanate compound (C).
[0108] In the first step, the hydroxyl groups are present in excess relative to the isocyanate groups, and the conditions are preferably such that all the isocyanate groups disappear by the reaction. Specifically, it is preferred that the NCO / OH equivalent ratio be adjusted to a range of 0.05 to 0.5.
[0109] Using the above-mentioned compound (B) having an isocyanate group and a free radical polymerizable group at the end, the ratio of the terminal hydroxyl group of the polyol component (A) being replaced by a reactive double bond is preferably 5 mol% relative to 100 mol% of the polyol component, and the preferred lower limit is 5 mol%, and the preferred upper limit is 50 mol%. If it is 5 mol% or more, the photocuring can be carried out well, and if it is 50 mol% or less, the photocuring is suppressed from being excessively carried out, and the initial bonding strength can be ensured. In view of the above, the more preferred lower limit is 10 mol%, the more preferred upper limit is 40 mol%, the further preferred lower limit is 15 mol%, and the further preferred upper limit is 35 mol%. If it is the above range, it is preferred to obtain the performance of the initial bonding produced by the photocuring, and the balance of bonding and flexibility produced by the crosslinking reaction carried out by the moisture curing.
[0110] Next, the preferred scheme in the above-mentioned process is described. As a polyol component, relative to the total 1 mole of the polyol (b) having 2 hydroxyls in 1 molecule, the content of the polyol (a) having 3 hydroxyls in 1 molecule is preferably 0.0005 mole or more, more preferably 0.001 mole or more. In addition, relative to the total 1 mole of the polyol (b) having 2 hydroxyls in 1 molecule, the content of the polyol (a) having 3 hydroxyls in 1 molecule is preferably 0.5 mole or less, more preferably 0.2 mole or less, and further preferably 0.15 mole or less. In the case of 0.0005 mole or more, the softness of the cured product after moisture curing improves, and if it is 0.5 mole or less, the viscosity of the light moisture curing prepolymer can be prevented from becoming too high, and gelation is not easy to occur.
[0111] In the second step, the NCO / OH equivalent ratio is preferably 1.5 or more, more preferably 1.8 or more, preferably 3 or less, more preferably 2.5 or less. If the NCO / OH equivalent ratio is 1.8 or more, a highly transparent prepolymer can be obtained, and if it is 2.5 or less, the initial adhesion of the prepolymer and the adhesion of the final bonded product become good.
[0112] The content of the optical moisture curable urethane prepolymer of the present invention in the optical moisture curable resin composition is not particularly limited, but is preferably 1% by mass or more, more preferably 5% by mass or more, and further preferably 8% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, and further preferably 60% by mass or less, based on the total amount of the optical moisture curable resin composition.
[0113] <Other light moisture curable urethane prepolymers>
[0114] The optical moisture curable resin composition of the present invention may contain other optical moisture curable urethane prepolymers in addition to the optical moisture curable urethane prepolymer described below, wherein the optical moisture curable urethane prepolymer comprises: an optical moisture curable urethane compound having a skeleton derived from a polyol (a) having three or more hydroxyl groups in one molecule and having two or more isocyanate groups and one or more free radical polymerizable groups at the molecular terminal.
[0115] As other optical moisture curable urethane prepolymers, optical moisture curable urethane prepolymers having one isocyanate group and one or more radical polymerizable groups at the molecular terminal are mentioned.
[0116] The optical moisture curable urethane prepolymer having one isocyanate group and one or more radical polymerizable groups at the molecular terminal is not particularly limited, and may be a low molecular weight monomer or a high molecular weight polymer.
[0117] Examples of the substance having one isocyanate group and one radical polymerizable group at the molecular terminal include 2-acryloyloxyethyl isocyanate, 2-methacryloyloxyethyl isocyanate, and Carens MOI-EG (manufactured by Showa Denko K.K.).
[0118] As a substance which has one isocyanate group and two radical polymerizable groups at a molecular terminal, Kalenzu BEI (made by Showa Denko K.K.) etc. are mentioned, for example.
[0119] <Moisture-curable urethane prepolymer>
[0120] The optical moisture curable resin composition of the present invention preferably contains a moisture curable urethane prepolymer. It should be noted that in this specification, the so-called moisture curable urethane prepolymer refers to a compound having an isocyanate group and no free radical polymerizable group, unlike the optical moisture curable urethane prepolymer.
[0121] The isocyanate group in the moisture-curable urethane prepolymer reacts with moisture in the air or in the adherend to cure. Therefore, the optical moisture-curable resin composition of the present invention can improve the adhesive strength after moisture curing by containing the moisture-curable urethane prepolymer.
[0122] The moisture-curable urethane prepolymer may contain a compound having only one isocyanate group in one molecule, or may contain a compound having two or more isocyanate groups in one molecule. Among them, the moisture-curable urethane prepolymer preferably contains a compound having isocyanate groups at both terminals.
[0123] The moisture-curable urethane prepolymer is preferably obtained by reacting a polyol having two or more hydroxyl groups in one molecule with a polyisocyanate compound. As the polyol having two or more hydroxyl groups in one molecule, any one or both of the above-mentioned polyol (a) and polyol (b) can be used, and as the polyisocyanate compound, the above-mentioned polyisocyanate compound (C) can be used.
[0124] Among the polyols having two or more hydroxyl groups in one molecule, ring-opening polymerization compounds of tetrahydrofuran and ring-opening polymerization compounds of 3-methyltetrahydrofuran are preferred, and polytetramethylene ether glycol is more preferred.
[0125] The reaction of a polyol having two or more hydroxyl groups in one molecule with a polyisocyanate compound is usually performed in a range where the molar ratio [(NCO) / (OH)] of hydroxyl groups (OH) to polyisocyanate groups (NCO) in the polyol is 2.0 to 2.5.
[0126] The weight average molecular weight of the moisture-curable urethane prepolymer is preferably 800 or more, preferably 10,000 or less. If the weight average molecular weight is 800 or more, the crosslinking density when the light moisture-curable resin composition is cured will not become too high, and the flexibility can be improved. If it is 10,000 or less, the coating property of the light moisture-curable resin composition can be improved.
[0127] From the viewpoint of improving both the photocurability and moisture curability of the optical moisture curable resin composition, the moisture curable urethane prepolymer is preferably 5% by mass or more, more preferably 10% by mass or more, and is preferably 95% by mass or less, more preferably 80% by mass or less, based on the total amount of the optical moisture curable urethane prepolymer and the moisture curable urethane prepolymer.
[0128] <Radical polymerizable compounds>
[0129] The optical moisture curable resin composition of the present invention preferably contains a radical polymerizable compound. In addition, the radical polymerizable compound in this specification refers to a compound having a radical polymerizable group and having no isocyanate group.
[0130] By containing a free radical polymerizable compound, the light-curable resin composition has good light curability. In addition, the cured product of the light moisture curable urethane prepolymer, the moisture curable urethane prepolymer, and the free radical polymerizable compound has excellent softness and adhesion. It can be considered that this is because the light moisture curable urethane prepolymer reacts with both the moisture curable urethane prepolymer and the free radical polymerizable compound, thereby suppressing phase separation.
[0131] As the radical polymerizable compound, a compound having an unsaturated double bond as a radical polymerizable group is suitable, and a compound having a (meth)acryloyl group is particularly suitable from the viewpoint of reactivity.
[0132] Examples of the compound having a (meth)acryloyl group include ester compounds obtained by reacting a compound having a hydroxyl group with (meth)acrylic acid. In addition to the ester compounds, epoxy (meth)acrylates obtained by reacting (meth)acrylic acid with an epoxy compound, and urethane (meth)acrylates obtained by reacting a (meth)acrylic acid derivative having a hydroxyl group with an isocyanate compound may be mentioned.
[0133] It should be noted that in this specification, the so-called "(meth)acrylate" refers to acrylate or methacrylate. In addition, the isocyanate groups of the isocyanate compound that is the raw material of the urethane (meth)acrylate are all used to form urethane bonds, and the urethane (meth)acrylate does not have any residual isocyanate groups.
[0134] Examples of the monofunctional ester compounds include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, isooctyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, , methoxyethylene glycol (meth)acrylate, 2-ethoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate, ethyl carbitol (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiglycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, 1H (meth)acrylate ,1H,5H-octafluoropentyl ester, imide (meth) acrylate, methyl (meth) acrylate, ethyl (meth) acrylate, n-butyl (meth) acrylate, propyl (meth) acrylate, cyclohexyl (meth) acrylate, 2-ethylhexyl (meth) acrylate, n-octyl (meth) acrylate, isononyl (meth) acrylate, isomyristyl (meth) acrylate, 2-butoxyethyl (meth) acrylate, 2-phenoxyethyl (meth) acrylate, dicyclopentenyl (meth) acrylate, propyl (meth) acrylate, cyclohexyl (meth) acrylate, 2-ethylhexyl (meth) acrylate, n-octyl (meth) acrylate, isononyl (meth) acrylate, isomyristyl (meth) acrylate, 2-butoxyethyl (meth) acrylate, 2-phenoxyethyl (meth) acrylate, dicyclopentenyl (meth) acrylate, Phthalimide acrylates such as isodecyl acrylate, diethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl 2-hydroxypropyl phthalate, glycidyl (meth)acrylate, 2-(meth)acryloyloxyethyl phosphate, N-acryloyloxyethyl hexahydrophthalimide, and various imide acrylates.
[0135] Examples of bifunctional ester compounds include 1,4-butanediol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 2-n-butyl-2-ethyl-1,3-propanediol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, and polyethylene glycol di(meth)acrylate. di(meth)acrylate, propylene oxide-added bisphenol A di(meth)acrylate, ethylene oxide-added bisphenol A di(meth)acrylate, ethylene oxide-added bisphenol F di(meth)acrylate, dimethylol dicyclopentadienyl di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethylene oxide-modified isocyanuric acid di(meth)acrylate, 2-hydroxy-3-(meth)acryloxypropyl (meth)acrylate, carbonate diol di(meth)acrylate, polyether diol di(meth)acrylate, polyester diol di(meth)acrylate, polycaprolactone diol di(meth)acrylate, polybutadiene diol di(meth)acrylate, and the like.
[0136] Examples of the trifunctional or higher-functional ester compounds include pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, propylene oxide-added trimethylolpropane tri(meth)acrylate, ethylene oxide-added trimethylolpropane tri(meth)acrylate, caprolactone-modified trimethylolpropane tri(meth)acrylate, ethylene oxide-added isocyanuric acid tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, glycerol tri(meth)acrylate, propylene oxide-added glycerol tri(meth)acrylate, and tri(meth)acryloyloxyethyl phosphate.
[0137] Examples of the epoxy (meth)acrylate include those obtained by reacting an epoxy compound and (meth)acrylic acid in the presence of a basic catalyst according to a conventional method.
[0138] Examples of the epoxy compound used as a raw material for synthesizing the epoxy (meth)acrylate include bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, 2,2'-diallylbisphenol A type epoxy resin, hydrogenated bisphenol type epoxy resin, propylene oxide added bisphenol A type epoxy resin, resorcinol type epoxy resin, biphenyl type epoxy resin, sulfide type epoxy resin, diphenyl ether type epoxy resin, dicyclopentadiene type epoxy resin, naphthalene type epoxy resin, phenol novolac type epoxy resin, o-cresol novolac type epoxy resin, dicyclopentadiene novolac type epoxy resin, biphenyl novolac type epoxy resin, naphthol novolac type epoxy resin, glycidylamine type epoxy resin, alkyl polyol type epoxy resin, rubber modified epoxy resin, glycidyl ester compound, bisphenol A type episulfide resin, and the like.
[0139] Examples of commercially available products of the bisphenol A-type epoxy resin include jER828EL, jER1001, and jER1004 (all manufactured by Mitsubishi Chemical Corporation) and Epiclone 850-S (manufactured by DIC Corporation).
[0140] As what is marketed among the said bisphenol F type epoxy resin, jER806, jER4004 (all are manufactured by Mitsubishi Chemical Corporation) etc. are mentioned, for example.
[0141] As what is marketed among the said bisphenol S type epoxy resin, Epiclone EXA1514 (made by DIC Corporation) etc. are mentioned, for example.
[0142] As what is marketed among the said 2,2'-diallylbisphenol A type epoxy resin, RE-810NM (made by Nippon Kayaku Co., Ltd.) etc. are mentioned, for example.
[0143] As what is marketed among the said hydrogenated bisphenol type epoxy resin, Epichrome EXA7015 (made by DIC Corporation) etc. are mentioned, for example.
[0144] As what is marketed among the said propylene oxide addition bisphenol A type epoxy resin, EP-4000S (made by ADEKA) etc. are mentioned, for example.
[0145] As what is marketed among the said resorcinol type epoxy resin, EX-201 (made by Nagase Chemtex Co., Ltd.) etc. are mentioned, for example.
[0146] As what is marketed among the said biphenyl type epoxy resin, jERYX-4000H (made by Mitsubishi Chemical Corporation) etc. are mentioned, for example.
[0147] As what is marketed among the said sulfide type epoxy resin, YSLV-50TE (made by Nippon Steel Sumigin Chemical Co., Ltd.) etc. are mentioned, for example.
[0148] As what is marketed among the said diphenyl ether type epoxy resin, YSLV-80DE (made by Nippon Steel Sumigin Chemical Co., Ltd.) etc. are mentioned, for example.
[0149] As what is marketed among the said dicyclopentadiene type epoxy resin, EP-4088S (made by ADEKA) etc. are mentioned, for example.
[0150] As a commercial item among the said naphthalene type epoxy resin, Epicron HP4032, Epicron EXA-4700 (all are manufactured by DIC Corporation), etc. are mentioned, for example.
[0151] As what is marketed among the said phenol novolac type epoxy resin, Epiclone N-770 (made by DIC Corporation) etc. are mentioned, for example.
[0152] As what is marketed among the said o-cresol novolac epoxy resin, Epiclone N-670-EXP-S (made by DIC Corporation) etc. are mentioned, for example.
[0153] As what is marketed among the said dicyclopentadiene novolac epoxy resin, Epiclone HP7200 (made by DIC Corporation) etc. are mentioned, for example.
[0154] As what is marketed among the said biphenyl novolac epoxy resin, NC-3000P (made by Nippon Kayaku Co., Ltd.) etc. are mentioned, for example.
[0155] As what is marketed among the said naphthol novolac epoxy resin, ESN-165S (made by Nippon Steel Sumikin Chemical Co., Ltd.) etc. are mentioned, for example.
[0156] Examples of commercially available products of the glycidylamine epoxy resins include jER630 (manufactured by Mitsubishi Chemical Corporation), Epiclone 430 (manufactured by DIC Corporation), and TETRAD-X (manufactured by Mitsubishi Gas Chemical Corporation).
[0157] Examples of commercially available products of the alkyl polyol epoxy resins include ZX-1542 (manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.), Epiclone 726 (manufactured by DIC Corporation), Epilight 80MFA (manufactured by Kyoeisha Chemical Co., Ltd.), and Denacol EX-611 (manufactured by Nagase Chemtex Co., Ltd.).
[0158] Examples of commercially available products of the rubber-modified epoxy resins include YR-450 and YR-207 (all manufactured by Nippon Steel & Sumitomo Chemical Co., Ltd.) and Epilide PB (manufactured by Daicel Corporation).
[0159] As a commercial item among the said glycidyl ester compound, Denacol EX-147 (made by Nagase Chemtex Co., Ltd.) etc. are mentioned, for example.
[0160] As what is marketed among the said bisphenol A type episulfide resin, jERYL-7000 (made by Mitsubishi Chemical Corporation) etc. are mentioned, for example.
[0161] Other commercially available products of the above-mentioned epoxy resins include, for example, YDC-1312, YSLV-80XY, and YSLV-90CR (all manufactured by Nippon Steel & Sumitomo Chemical Co., Ltd.), XAC4151 (manufactured by Asahi Kasei Corporation), jER1031 and jER1032 (all manufactured by Mitsubishi Chemical Corporation), EXA-7120 (manufactured by DIC Corporation), and TEPIC (manufactured by Nissan Chemical Co., Ltd.).
[0162] Examples of commercially available products of the epoxy (meth)acrylates include EBECRYL 860, EBECRYL 3200, EBECRYL 3201, EBECRYL 3412, EBECRYL 3600, EBECRYL 3700, EBECRYL 3701, EBECRYL 3702, EBECRYL 3703, EBECRYL 3800, EBECRYL 6040, and EBECRYL RDX63182 (all made by ダイセル・オルネクス Co., Ltd.), EA-1010, EA-1020, EA-5323, EA-5520, EA-CHD, EMA-1020 (all made by Shin-Nakamura Chemical Industry Co., Ltd. Made in Japan A. エポキシエステル200PA, エポキシエステル80MFA, エポキシエステル3002 M, エポキシエステル3002A, エポキシエステル1600A, エポキシエステル300 0M, エポキシエステル3000A, エポキシエステル200EA, エポキシエステル400 EA (both made by Gyoeisha Chemical Industry Co., Ltd.), Dorothy DA-141, DorothyトDA-314, デナコールアクリレートDA-911 (all made by ナガセケム テックス Co., Ltd.), etc.
[0163] The urethane (meth)acrylate can be obtained, for example, by reacting a (meth)acrylic acid derivative having a hydroxyl group with a compound having an isocyanate group in the presence of a catalytic amount of a tin-based compound.
[0164] Examples of the isocyanate compound used as a raw material for the urethane (meth)acrylate include isophorone diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 1,6-hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, diphenylmethane-4,4′-diisocyanate (MDI), hydrogenated MDI, polymeric MDI, 1,5-naphthalene diisocyanate, norbornane diisocyanate, tolidine diisocyanate, xylylene diisocyanate (XDI), hydrogenated XDI, lysine diisocyanate, triphenylmethane triisocyanate, tris(isocyanatophenyl)phosphorothioate, tetramethylxylene diisocyanate, and 1,6,11-undecane triisocyanate.
[0165] In addition, as the above-mentioned isocyanate compound, a chain-extended isocyanate compound obtained by reacting a polyol with an excess of an isocyanate compound can also be used. As the polyol, for example, ethylene glycol, glycerol, sorbitol, trimethylolpropane, (poly)propylene glycol, carbonate diol, polyether diol, polyester diol, polycaprolactone diol, etc. can be mentioned.
[0166] Examples of the (meth)acrylic acid derivative having a hydroxyl group, which is a raw material for the urethane (meth)acrylate, include mono(meth)acrylates of diols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, and polyethylene glycol; mono(meth)acrylates or di(meth)acrylates of triols such as trimethylolethane, trimethylolpropane, and glycerol; and epoxy (meth)acrylates such as bisphenol A epoxy (meth)acrylate.
[0167] As commercially available products among the above-mentioned urethane (meth)acrylates, for example, M-1100, M-1200, M-1210, M-1600 (all manufactured by Toagosei Co., Ltd.), EBECRYL230, EBECRYL270, EBECRYL4858, EBECRYL8402, EBECRYL8411, EBECRYL8412, EBECRYL8413, EBECRYL8804, EBECRYL8803, EBECRYL8807, EBECRYL9260, EBECRYL1290, EBECRYL5129, EBECRYL4842, EBECRYL210, EBECRYL4827, EBECRYL6700, EBECRYL220, EBECRYL2220, KRM7735, KRM-8295 (all manufactured by Daicel Ornex Co., Ltd.), Art Resin UN-9000H, Art Resin UN-9000A, Art Resin UN-7100, Art Resin UN-1255, Art Resin UN-330, Art Resin UN-3320HB, Art Resin UN-1200TPK, Art Resin SH-500B (all manufactured by Negami Kogyo Co., Ltd.), U-2HA, U-2PHA, U-3HA, U-4HA, U-6H, U-6LPA, U-6HA, U-10H, U-15HA, U-122A, U-122P, U-108, U-108A, U-324A, U-340A, U-340P, U-1084A, U-2061BA, UA-340P, UA-4100, UA-4000, UA-4200, UA-4400, UA-5201P, UA-7100, UA-7200, UA-W2A (all manufactured by Shin-Nakamura Chemical Co., Ltd.), AI-600, AH-600, AT-600, UA-101I, UA-101T, UA-306H, UA-306I, UA-306T (all manufactured by Kyoeisha Chemical Co., Ltd.), etc.
[0168] In addition, other radically polymerizable compounds other than the above can also be appropriately used.
[0169] As the above-mentioned other radically polymerizable compounds, for example, (meth)acrylamide compounds such as N,N-dimethyl(meth)acrylamide, N-(meth)acryloylmorpholine, N-hydroxyethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, vinyl compounds such as styrene, α-methylstyrene, N-vinylpyrrolidone, N-vinylcaprolactone, etc.
[0170] From the viewpoint of adjusting curability, the above-mentioned free radical polymerizable compound preferably contains a monofunctional free radical polymerizable compound and a polyfunctional free radical polymerizable compound. By using the two together, the curability and initial adhesion of the obtained light moisture curable resin composition are easy to become good. In addition, the above-mentioned polyfunctional free radical polymerizable compound is preferably difunctional or trifunctional, and more preferably difunctional.
[0171] The content of the radical polymerizable compound is preferably 20% by mass or more, more preferably 25% by mass or more, and preferably 80% by mass or less, more preferably 70% by mass or less, based on the total amount of the radical polymerizable compound, the light moisture curable urethane prepolymer, and the moisture curable urethane prepolymer. Within such a range, the balance between the initial adhesive force of the light moisture curable resin composition and the adhesive strength after moisture curing becomes good.
[0172] <Photopolymerization initiator>
[0173] The optical moisture curable resin composition of the present invention must contain a photopolymerization initiator.
[0174] As the above-mentioned photopolymerization initiator, for example, benzophenone compounds, acetophenone compounds, acylphosphine oxide compounds, titanocene compounds, oxime ester compounds, benzoin ether compounds, thioxanthone, maleimide compounds and other photoradical polymerization initiators can be mentioned. In view of good deep curing properties, acylphosphine oxide compounds and oxime ester compounds are preferred.
[0175] The content of the above-mentioned photopolymerization initiator is preferably 0.01 parts by mass and the preferred upper limit is 10 parts by mass relative to the total 100 parts by mass of the above-mentioned free radical polymerizable compound and the light moisture curable urethane prepolymer. If the content of the above-mentioned photopolymerization initiator is 0.01 parts by mass or more, the obtained light moisture curable resin composition can be fully photocured. If the content of the above-mentioned light free radical polymerization initiator is 10 parts by mass or less, the storage stability of the obtained light moisture curable resin composition becomes good. The more preferred lower limit of the content of the above-mentioned photopolymerization initiator is 0.1 parts by mass, and the more preferred upper limit is 5 parts by mass.
[0176] <Moisture curing catalyst>
[0177] The optical moisture curable resin composition of the present invention preferably contains a moisture curing accelerator. By containing a moisture curing accelerator, the curing speed during moisture curing can be increased. In addition, since the generation of bubbles can be suppressed, the resulting optical moisture curable resin composition can be used for adhesives for electronic components, adhesives for display elements, etc., and the disconnection during coating caused by the bubbles can be prevented.
[0178] Examples of the moisture curing accelerating catalyst include a compound having a morpholine skeleton, a compound having a piperidine skeleton, a compound having a piperazine skeleton, and the like.
[0179] Examples of the compound having a morpholine skeleton include 4-methylmorpholine, 4-ethylmorpholine, 4-phenylmorpholine, 4-cyclohexylmorpholine, 4-cycloheptylmorpholine, 4-tritylmorpholine, 4-acylmorpholine, 4-(meth)acryloylmorpholine, 4-(meth)acryloyloxymorpholine, 4-(meth)acryloyloxyethylmorpholine, 4-morpholinomethylmorpholine, 4-morpholinoethylmorpholine, 4-morpholinopropylmorpholine, and 2,2′-dimorpholinodiethyl ether.
[0180] Examples of commercially available products of the compound having a morpholine skeleton include U-CAT 651M, U-CAT 660M, U-CAT 2041, and U-CAT 2046 (all manufactured by Sanapro Corporation).
[0181] Examples of the compound having a piperidine skeleton include 1-methylpiperidine, 1-ethylpiperidine, 1,2,2,6,6-pentamethylpiperidine, 1-cyclopentylpiperidine, and 1-cyclohexylpiperidine.
[0182] Examples of the compound having a piperazine skeleton include 1,4-dimethylpiperazine, 1,4-diethylpiperazine, 1,4-diphenylpiperazine, 1-acyl-4-methylpiperazine, 2-ethoxycarbonyl-1,4-dimethylpiperazine, and 1,4-diazabicyclo[2.2.2]octane.
[0183] The molecular weight and the number of functional groups of the moisture curing accelerator of the present invention are not particularly limited, but preferably have two or more morpholine skeletons, piperidine skeletons, or piperazine skeletons in one molecule. As a compound having two or more morpholine skeletons, piperidine skeletons, or piperazine skeletons in one molecule, for example, 4-morpholinopropylmorpholine, 2,2'-dimorpholinodiethylether, etc. can be cited, and as a commercial product, for example, U-CAT 651M, U-CAT 660M, U-CAT 2041, U-CAT 2046 (all manufactured by Sanapro) and the like can be cited.
[0184] The content of the moisture curing accelerator catalyst of the present invention in the optical moisture curing composition is preferably 0.025 mass % or more, more preferably 0.05 mass % or more, preferably 3 mass % or less, more preferably 1 mass % or less. If the content of the moisture curing accelerator catalyst is within this range, the optical moisture curing resin composition obtained can maintain excellent storage stability while having better rapid curing properties during moisture curing.
[0185] The optical moisture curable resin composition of the present invention may contain a coupling agent from the viewpoint of improving adhesion and creep resistance.
[0186] The coupling agent preferably has a reactive functional group that can react with any one of a free radical polymerizable compound, a light moisture curable urethane prepolymer, and a moisture curable urethane prepolymer. By having the reactive functional group, the coupling agent is introduced into the cured product obtained by curing the light moisture curable resin composition of the present invention, and the adhesion and creep resistance are further improved.
[0187] As the reactive functional group possessed by the coupling agent, for example, groups having unsaturated double bonds such as (meth)acryloyl, epoxy, isocyanate, thiol, amino, etc. can be cited. Among them, groups having unsaturated double bonds, epoxy, and isocyanate are preferred from the viewpoint of excellent effects of improving adhesion and creep resistance.
[0188] As the coupling agent, for example, silane coupling agent, titanate coupling agent, aluminate coupling agent, zirconate coupling agent, etc. can be cited. Among them, silane coupling agent is preferred because of its excellent effect of improving adhesion and creep resistance. The coupling agent can be used alone or in combination of two or more.
[0189] Examples of the silane coupling agent include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropylmethyl 3-(Meth)acryloxypropyltrimethoxysilane, 3-(Meth)acryloxypropyltriethoxysilane, 3-(Meth)acryloxypropylmethyldimethoxysilane, 3-(Meth)acryloxypropylmethyldiethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 3-isocyanatepropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, etc.
[0190] Examples of the titanate coupling agent include tetraisopropyl titanate, tetra-n-butyl titanate, butyl titanate dimer, tetraoctyl titanate, tetra-tert-butyl titanate, tetrastearyl titanate, and titanium acetoacetate.
[0191] Examples of the aluminate coupling agent include alkylaluminum acetoacetate diisopropyl and the like.
[0192] Examples of the zirconate coupling agent include n-propyl zirconate and zirconium ethyl acetate.
[0193] The content of the coupling agent is preferably limited to 5 parts by mass relative to 100 parts by mass of the total of the light moisture curable urethane prepolymer, the moisture curable urethane prepolymer, and the free radical polymerizable compound. If the content of the coupling agent is less than 5 parts by mass, the storage stability of the obtained light moisture curable resin composition becomes good. The more preferred upper limit of the content of the coupling agent is 1.5 parts by mass.
[0194] In addition, the content of the coupling agent is preferably limited to 0.05 parts by mass relative to 100 parts by mass of the total of the light moisture curable urethane prepolymer, the moisture curable urethane prepolymer, and the free radical polymerizable compound. If the content of the coupling agent is 0.05 parts by mass or more, adhesion and creep resistance can be improved. The more preferred lower limit of the content of the coupling agent is 0.5 parts by mass.
[0195] The optical moisture curable resin composition of the present invention may contain a filler from the viewpoint of adjusting the coating properties, shape retaining properties, and the like of the optical moisture curable resin composition obtained.
[0196] The preferred lower limit of the primary particle size of the filler is 1 nm, and the preferred upper limit is 50 nm. If the primary particle size of the filler is 1 nm or more, the coating property of the obtained light moisture curable resin composition becomes good. If the primary particle size of the filler is 50 nm or less, the shape retention of the obtained light moisture curable resin composition after coating is good. The more preferred lower limit of the primary particle size of the filler is 5 nm, and the more preferred upper limit is 30 nm.
[0197] The primary particle size of the filler can be measured by dispersing the filler in a solvent (water, an organic solvent, etc.) using NICOMP 380ZLS (manufactured by PARTICLESIZING SYSTEMS).
[0198] In addition, the filler is sometimes present in the form of secondary particles (a substance formed by a plurality of primary particles) in the optical moisture curable resin composition of the present invention, and the preferred lower limit of the particle size of such secondary particles is 5 nm, the preferred upper limit is 500 nm, the more preferred lower limit is 10 nm, and the more preferred upper limit is 100 nm. The particle size of the secondary particles of the filler can be measured by observing the optical moisture curable resin composition of the present invention or its cured product using a transmission electron microscope (TEM).
[0199] Examples of the filler include silicon dioxide, talc, titanium oxide, zinc oxide, etc. Among them, silicon dioxide is preferred because the resulting optical moisture curable resin composition has excellent UV light transmittance. These fillers may be used alone or in combination of two or more.
[0200] The filler is preferably subjected to a hydrophobic surface treatment. The hydrophobic surface treatment can provide the obtained optical moisture curable resin composition with better shape retention after application.
[0201] Examples of the hydrophobic surface treatment include silylation, alkylation, epoxidation, etc. Among them, silylation is preferred, and trimethylsilylation is more preferred, because it is excellent in improving the shape retention.
[0202] Examples of a method for subjecting the filler to a hydrophobic surface treatment include a method of treating the surface of the filler using a surface treatment agent such as a silane coupling agent.
[0203] Specifically, the trimethylsilylated silica can be prepared, for example, by the following operations. For example, the trimethylsilylated silica can be prepared by the following methods: synthesizing silica by a sol-gel method or the like, spraying hexamethyldisilazane while the silica is in a fluidized state; adding silica to an organic solvent such as alcohol or toluene, further adding hexamethyldisilazane and water, and then evaporating and drying the water and the organic solvent using an evaporator, etc.
[0204] The content of the above-mentioned filler is preferably 1 part by mass in the entire 100 parts by mass of the optical moisture curable resin composition of the present invention, and the preferred upper limit is 20 parts by mass. If the content of the above-mentioned filler is 1 part by mass or more, the shape retention of the obtained optical moisture curable resin composition after coating becomes good. If the content of the above-mentioned filler is 20 parts by mass or less, the coating property of the obtained optical moisture curable resin composition becomes good. The more preferred lower limit of the content of the above-mentioned filler is 2 parts by mass, the more preferred upper limit is 15 parts by mass, the further preferred lower limit is 3 parts by mass, the further preferred upper limit is 10 parts by mass, and the particularly preferred lower limit is 4 parts by mass.
[0205] The optical moisture curable resin composition of the present invention may contain a light shielding agent. By containing the light shielding agent, the optical moisture curable resin composition of the present invention has excellent light shielding properties and can prevent light leakage of a display element.
[0206] In addition, in this specification, the said "light shielding agent" refers to the material which has the ability to make the light of the visible light region difficult to transmit.
[0207] Examples of the light shielding agent include iron oxide, titanium black, aniline black, cyanine black, fullerene, carbon black, resin-coated carbon black, etc. The light shielding agent may not be black, but if it is a material that has the ability to make light in the visible light region difficult to transmit, materials listed as fillers such as silicon dioxide, talc, and titanium oxide are also included in the light shielding agent. Among them, titanium black is preferred.
[0208] The titanium black is a substance having a high transmittance to light near the ultraviolet region, especially light of 370 to 450 nm in wavelength, compared to the average transmittance to light of 300 to 800 nm in wavelength. That is, the titanium black is a light-shielding agent that imparts light-shielding properties to the light-curable resin composition of the present invention by fully shielding light of wavelengths in the visible light region, and on the other hand, has the property of transmitting light of wavelengths near the ultraviolet region. Therefore, by using a substance that can initiate a reaction by light of a wavelength (370 to 450 nm) with a high transmittance of the titanium black as a photo-radical polymerization initiator, the photocurability of the light-curable resin composition of the present invention can be further increased. In addition, on the other hand, as a light-shielding agent contained in the light-curable resin composition of the present invention, it is preferably a substance with high insulating properties, and titanium black is also suitable as a light-shielding agent with high insulating properties.
[0209] The optical density (OD value) of the titanium black is preferably 3 or more, more preferably 4 or more. In addition, the blackness (L value) of the titanium black is preferably 9 or more, more preferably 11 or more. The higher the light shielding property of the titanium black, the better. There is no particular upper limit on the OD value of the titanium black, but it is usually 5 or less.
[0210] The titanium black described above can fully exert its effect even if it is a material that has not been surface treated, but titanium black that has been surface treated with an organic component such as a coupling agent, or a material that has been coated with an inorganic component such as silicon oxide, titanium oxide, germanium oxide, aluminum oxide, zirconium oxide, or magnesium oxide can also be used. Among them, the material that has been treated with an organic component is preferred in that the insulation can be further improved.
[0211] Furthermore, the display element produced using the optical moisture curable resin composition of the present invention has a high contrast without leakage of light, and has excellent image display quality, because the optical moisture curable resin composition has sufficient light shielding properties.
[0212] Examples of commercially available products of the titanium black include 12S, 13M, 13M-C, and 13R-N (all manufactured by Mitsubishi Material Co., Ltd.) and Titanium D (manufactured by Akaho Chemicals Co., Ltd.).
[0213] The preferred lower limit of the specific surface area of the titanium black is 5 m 2 / g, the preferred upper limit is 40m 2 / g, and a more preferred lower limit is 10m 2 / g, and the more preferred upper limit is 25m 2 / g.
[0214] The preferred lower limit of the sheet resistance of the titanium black when mixed with a resin (70% blending) is 10 9 Ω / □, the more preferred lower limit is 10 11 Ω / □.
[0215] In the light moisture curable resin composition of the present invention, the primary particle size of the above-mentioned light-shielding agent is less than the distance between the substrates of the display element, etc., and is appropriately selected according to the purpose, but the preferred lower limit is 30nm, and the preferred upper limit is 500nm. If the primary particle size of the above-mentioned light-shielding agent is more than 30nm, the viscosity and thixotropy of the obtained light moisture curable resin composition are not too increased, and the workability becomes good. If the primary particle size of the above-mentioned light-shielding agent is less than 500nm, the dispersibility of the light-shielding agent in the obtained light moisture curable resin composition becomes good, and the light-shielding property is improved. The more preferred lower limit of the primary particle size of the above-mentioned light-shielding agent is 50nm, and the more preferred upper limit is 200nm.
[0216] The particle size of the light-shielding agent can be measured by dispersing the light-shielding agent in a solvent (water, an organic solvent, etc.) using NICOMP 380ZLS (manufactured by PARTICLESIZING SYSTEMS) and obtaining an average particle size.
[0217] The content of the above-mentioned sunscreen in the whole optical moisture curable resin composition of the present invention is not particularly limited, but the preferred lower limit is 0.05% by mass, and the preferred upper limit is 10% by mass. If the content of the above-mentioned sunscreen is 0.05% by mass or more, the light-shielding property becomes good. If the content of the above-mentioned sunscreen is 10% by mass or less, the adhesion of the obtained optical moisture curable resin composition to the substrate, the strength after curing can be improved, and the drawing property can be made good. The more preferred lower limit of the content of the above-mentioned sunscreen is 0.1% by weight, the more preferred upper limit is 2% by weight, and the further preferred upper limit is 1% by weight.
[0218] The optical moisture curable resin composition of the present invention may further contain additives such as a colorant, an ionic liquid, a solvent, metal-containing particles, and a reactive diluent as necessary.
[0219] Examples of a method for producing the optical moisture curable resin composition of the present invention include a method of mixing the components using a mixer such as a homodisperser, a homomixer, a universal mixer, a planetary mixer, a kneader, or a three-roll mixer.
[0220] The optical moisture curable resin composition of the present invention has a viscosity measured at 25°C and 1 rpm using a cone-plate viscometer with a preferred lower limit of 30 Pa·s and a preferred upper limit of 500 Pa·s. If it is within such a range, the workability when the optical moisture curable resin composition is applied to an adherend such as a substrate when used as an adhesive for electronic components or an adhesive for display elements becomes good. The more preferred lower limit of the above viscosity is 50 Pa·s, the more preferred upper limit is 300 Pa·s, and the further preferred upper limit is 200 Pa·s.
[0221] The preferred lower limit of the thixotropic index of the optical moisture curable resin composition of the present invention is 1.3, and the preferred upper limit is 5.0. If the thixotropic index is in such a range, the workability when the optical moisture curable resin composition is applied to an adherend such as a substrate when used as an adhesive for electronic components or an adhesive for display elements becomes good. The more preferred lower limit of the above thixotropic index is 1.5. The more preferred upper limit is 4.0.
[0222] In this specification, the thixotropic index refers to a value obtained by dividing the viscosity measured at 25° C. and 1 rpm using a cone-plate viscometer by the viscosity measured at 25° C. and 10 rpm using a cone-plate viscometer.
[0223] The lower limit of the tensile modulus of the cured product of the optical moisture curable resin composition of the present invention at 25°C is preferably 0.5 kgf / cm 2 The upper limit is preferably 20kgf / cm 2 If the above tensile elastic modulus is 0.5kgf / cm 2 If the tensile modulus is 20 kgf / cm 2 The lower limit of the tensile modulus is more preferably 1 kgf / cm 2 The more preferred upper limit is 10 kgf / cm 2 .
[0224] In this specification, the “tensile modulus” refers to a value measured as the force at 50% elongation by stretching the cured product at a rate of 10 mm / min using a tensile tester (for example, “EZ-Graph” manufactured by Shimadzu Corporation).
[0225] The above-mentioned "tensile modulus" refers to the test results of a test conducted by a mercury lamp at 3000 mJ / cm 2 The value is obtained by measuring a cured product obtained by irradiating a curable resin composition and then leaving it to stand in an environment of 23° C. and 50 RH % for 3 days.
[0226] Examples of adherends that can be bonded using the optical moisture curable resin composition of the present invention include various adherends such as metals, glass, and plastics.
[0227] Examples of the shape of the adherend include a film, a sheet, a plate, a panel, a disk, a rod (rod-like body), a box, and a shell.
[0228] Examples of the metal include steel, stainless steel, aluminum, copper, nickel, chromium, and alloys thereof.
[0229] Examples of the glass include alkali glass, alkali-free glass, and quartz glass.
[0230] Examples of the plastic include high-density polyethylene, ultra-high molecular weight polyethylene, isotactic polypropylene, syndiotactic polypropylene, and polyolefin resins such as ethylene-propylene copolymer resins; polyamide resins such as nylon 6 (N6), nylon 66 (N66), nylon 46 (N46), nylon 11 (N11), nylon 12 (N12), nylon 610 (N610), nylon 612 (N612), nylon 6 / 66 copolymer (N6 / 66), nylon 6 / 66 / 610 copolymer (N6 / 66 / 610), nylon MXD6 (MXD6), nylon 6T, nylon 6 / 6T copolymer, nylon 66 / PP copolymer, and nylon 66 / PPS copolymer; polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polyethylene isophthalate (PEI), PET / P Aromatic polyester resins such as EI copolymer, polyarylate (PAR), polybutylene naphthalate (PBN), liquid crystal polyester, polyoxyalkylene imide diacid / polybutyrate terephthalate copolymer, polyacrylonitrile (PAN), polymethacrylonitrile, acrylonitrile / styrene copolymer (AS), methacrylonitrile / styrene copolymer, methacrylonitrile / styrene / butadiene copolymer, polycarbonate, polymethyl methacrylate (PMMA), polyethyl methacrylate vinyl acetate (EVA), polyvinyl alcohol (PVA), vinyl alcohol / ethylene copolymer (EVOH), polyvinylidene chloride (PVDC), polyvinyl chloride (PVC), vinyl chloride / 1,1-dichloroethylene copolymer, vinyl chloride / methyl acrylate copolymer, etc.
[0231] Furthermore, the adherend may be a composite material having a metal-plated layer on the surface, and the base material for plating the composite material may be the metals, glass, plastic, etc., for example.
[0232] Furthermore, as the adherend, there can be cited materials in which a passive film is formed on the metal surface by passivation treatment, and the passivation treatment can be, for example, heat treatment, anodizing treatment, etc. In particular, in the case of aluminum alloys such as the material of the International Aluminum Alloy No. 6000, the adhesion can be improved by performing sulfuric acid aluminum treatment or phosphoric acid aluminum treatment as the passivation treatment.
[0233] The optical moisture curable resin composition of the present invention can be particularly suitably used as an adhesive for electronic components and an adhesive for display elements. An adhesive for electronic components formed using the optical moisture curable resin composition of the present invention and an adhesive for display elements formed using the optical moisture curable resin composition of the present invention are also one of the present inventions.
[0234] Example
[0235] Hereinafter, the present invention will be described in further detail with reference to Examples, but the present invention is not limited to these Examples.
[0236] (Synthesis Example 1 (Synthesis of light moisture curable urethane prepolymer A))
[0237] As polyols, 100 parts by mass of polytetramethylene ether glycol (2-functional, molecular weight 1,000, hydroxyl value 115, "PTG-L1000" manufactured by Hodogaya Chemical Co., Ltd.) and 10 parts by mass of terminal ethylene oxide addition type polyoxypropylene glycol (3-functional, molecular weight 10,000, hydroxyl value = 16.9, "Preminol 7012" manufactured by Asahi Glass Co., Ltd.) were prepared. These were added to a 1000 mL separable flask, dehydrated at 100° C. for 2 hours under vacuum (20 mmHg or less), and then returned to normal pressure and cooled to 70° C. under a nitrogen atmosphere.
[0238] While maintaining the liquid temperature at 70°C, 0.06 parts by mass of bismuth tri(2-ethylhexanoate) ("Neostan U-600" manufactured by Nitto Chemical Industry Co., Ltd.) as a urethane catalyst was added with stirring, and the mixture was stirred until uniform. Next, while maintaining the liquid temperature at 70°C, 4.24 parts by mass of 2-isocyanate ethyl acrylate ("Karenzu AOI" manufactured by Showa Denko K.K.) was added dropwise in a manner such that the liquid temperature was not higher than 75°C. After all the amount was added dropwise, the mixture was reacted at 70°C under a nitrogen flow with stirring for 1 hour to obtain a terminal free radical polymerizable group-modified polyol compound. After the reaction was completed, a Fourier transform infrared spectrophotometer (manufactured by Shimadzu Corporation) was used to confirm the presence of 2250 cm-1 derived from the isocyanate group. -1 The peak disappears.
[0239] Next, after the reaction was completed, 53.3 parts by mass of diphenylmethane diisocyanate (Desmodium 44S manufactured by Sumika Cobalt Corporation) as a polyisocyanate compound was added, and the mixture was stirred at 70° C. for 1 hour under a nitrogen stream to react. Thus, a light moisture curable urethane prepolymer A (weight average molecular weight 8,300) containing a urethane compound having a skeleton derived from a polyol having three hydroxyl groups in one molecule and having two isocyanate groups and one radical polymerizable group at the molecular terminal was obtained.
[0240] (Synthesis Example 2 (Synthesis of light moisture curable urethane prepolymer B))
[0241] As a polyol, 100 parts by mass of polypropylene glycol (bifunctional, molecular weight 3,000, hydroxyl value 37, "Extron 3020" manufactured by Asahi Glass Co., Ltd.) was added to a 1000 mL separable flask, dehydrated at 100° C. for 2 hours under vacuum (20 mmHg or less), then returned to normal pressure and cooled to 70° C. under a nitrogen atmosphere. While the liquid temperature was maintained at 70° C., 0.06 parts by mass of bismuth tris(2-ethylhexanoate) ("Neoster U-600" manufactured by Nitto Kasei Co., Ltd.) as a urethanization catalyst was added with stirring, and the mixture was stirred until it became uniform. Next, while the liquid temperature was maintained at 70°C, 4.54 parts by mass of 2-isocyanate ethyl acrylate ("Karenzu AOI" manufactured by Showa Denko Co., Ltd.) was added dropwise in a manner that the liquid temperature was not higher than 75°C. After the entire amount was added dropwise, the mixture was reacted at 70°C under a nitrogen stream for 1 hour while stirring to obtain a terminal free radical polymerizable group-modified polyol compound. After the reaction was completed, a Fourier transform infrared spectrophotometer (manufactured by Shimadzu Corporation) was used to confirm the presence of 2250 cm-1 derived from the isocyanate group. -1 The peak disappeared. Then, after the reaction was completed, 8.45 parts by mass of diphenylmethane diisocyanate ("Desmodium 44S" manufactured by Sumika Cobalt Corporation) as a polyisocyanate compound was added, and the mixture was stirred at 70°C for 1 hour under a nitrogen stream to react. Thus, a light moisture-curable urethane prepolymer B (weight average molecular weight 6,000) containing a urethane compound having a skeleton derived from a polyol having two hydroxyl groups in one molecule and having one isocyanate group and one free radical polymerizable group at the molecular end was obtained.
[0242] (Synthesis Example 3 (Moisture Curable Urethane Prepolymer C))
[0243] 100 parts by mass of polytetramethylene ether glycol (difunctional, "PTMG-2000" manufactured by Mitsubishi Chemical Co., Ltd.) as a polyol and 0.01 parts by mass of dibutyltin dilaurate were added to a 500 mL removable flask, and stirred at 100°C for 30 minutes under vacuum (below 20 mmHg) to mix. Then, the mixture was set to normal pressure, and 26.5 parts by mass of diphenylmethane diisocyanate (manufactured by Nissou Shoji Co., Ltd., "Pure MDI") as a polyisocyanate compound was added, and the mixture was stirred at 80°C for 3 hours to react. Thus, a moisture-curable urethane prepolymer C (weight average molecular weight 2,700) containing a urethane compound having isocyanate groups at both ends was obtained.
[0244] (Examples 1 to 5, Comparative Examples 1 to 2)
[0245] The materials were stirred with a planetary stirring device (manufactured by Shinki Co., Ltd., "Awato Ri Rentaro") according to the mixing ratios listed in Table 1, and then uniformly mixed with a ceramic triple roll to obtain optical moisture curable resin compositions of Examples 1 to 5 and Comparative Examples 1 to 2. The optical moisture curable resin compositions were subjected to the evaluations described below, and the results are shown in Table 1.
[0246] <Evaluation>
[0247] (Adhesion after moisture curing)
[0248] Using a dispensing device, a light moisture curable resin composition was applied to an aluminum substrate in a manner of 1.0±0.1 mm in width, 25±2 mm in length, and 0.4±0.1 mm in thickness, and irradiated with a mercury lamp at 1000 mJ / cm2 in an environment of 25°C and 50 RH% to photocure. Then, a glass plate was bonded to the aluminum substrate, a 100 g weight was placed from above for 10 seconds, and the composition was left at 25°C and 50 RH% for 3 days to moisture cure, thereby obtaining a sample for an adhesion test.
[0249] The obtained adhesion test sample was stretched at a rate of 5 mm / sec in the shear direction at 25°C and 50% RH using a tensile tester Autograph AG-X (Shimadzu Corporation), and the strength when the aluminum substrate and the glass plate peeled off was measured to measure the "adhesion after moisture curing".
[0250] The case where the measured value of the adhesive force was 50 N or more was evaluated as A, the case where it was 20 N or more and less than 50 N was evaluated as B, and the case where it was less than 20 N was evaluated as C.
[0251] (Evaluation just after UV treatment)
[0252] Using a dispensing device, a light moisture curable resin composition is applied to an aluminum substrate in a manner of 1.0 ± 0.1 mm in width, 25 ± 2 mm in length, and 0.4 ± 0.1 mm in thickness, and a mercury lamp is used to irradiate with 1000 mJ / cm2 to photocuring. Then, a glass plate is bonded to the aluminum substrate, and a 100 g weight is placed from above for 10 seconds to obtain a sample for evaluating adhesion. Then, within 10 minutes, a 10 g weight is suspended in a shear direction under an atmosphere of 25 ° C and 50% RH, and the time until the aluminum substrate falls is measured. The situation of not falling for more than 30 minutes is set to A, the situation of falling for 10 minutes to 30 minutes is set to B, and the situation of falling within 10 minutes is set to C.
[0253] (Viscosity)
[0254] The viscosity of the optical moisture curable resin composition was measured using a cone-plate viscometer at 25° C. and 1 rpm.
[0255] [Table 1]
[0256]
[0257] The optical moisture curable resin composition of each example includes an optical moisture curable urethane prepolymer containing a urethane compound of the present invention having two isocyanate groups and one free radical polymerizable group, and has excellent adhesion just after UV (initial adhesion) and adhesion after moisture curing. On the other hand, in Comparative Examples 1 and 2 using an optical moisture curable resin composition not containing such a specific urethane compound, the adhesion just after UV or the adhesion after moisture curing is low.
Claims
1. A light moisture curable urethane compound comprising a skeleton derived from a polyol (a) having three or more hydroxyl groups in one molecule and having two or more isocyanate groups and one or more radical polymerizable groups at a molecular terminal.
2. The optical moisture curable urethane compound according to claim 1, which is obtained by reacting a polyol component (A) containing the polyol (a), a compound (B) having an isocyanate group and having a free radical polymerizable group at the terminal, and a polyisocyanate compound (C). 3 . The optical moisture curable urethane compound according to claim 1 , which has a weight average molecular weight of 500 to 30,000. 4 . A light moisture curable urethane prepolymer comprising the light moisture curable urethane compound according to claim 1 . 5 . The optical moisture curable urethane prepolymer according to claim 4 , which has a weight average molecular weight of 500 to 30,000. 6 . A light moisture curable resin composition comprising the light moisture curable urethane prepolymer according to claim 4 or 5 and a photopolymerization initiator. 7 . The optical moisture curable resin composition according to claim 6 , further comprising a radical polymerizable compound. 8 . The optical moisture curable resin composition according to claim 6 , further comprising a moisture curable urethane prepolymer. 9 . The optical moisture curable resin composition according to claim 7 , wherein the radical polymerizable compound contains a monofunctional radical polymerizable compound and a polyfunctional radical polymerizable compound. 10 . An adhesive for electronic components, comprising the optical moisture curable resin composition according to claim 6 . 11 . An adhesive for display elements, comprising the optical moisture curable resin composition according to claim 6 .