Preparation method and application of high-melt-strength poly (butylene succinate) / butylene adipate
By introducing branching agents into PBSA for esterification and polycondensation reactions, a micro-crosslinked structure is formed, which solves the problem of low melt strength of PBSA, significantly improves its melt strength and tensile strength, and expands the application range.
Patent Information
- Application Number
- CN202411322029.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-12
AI Technical Summary
The melt strength of PBSA is relatively low, which affects its forming and processing and mechanical properties, limiting its use in applications requiring higher strength.
By introducing high-efficiency branching agents, their types and content are regulated, and esterification and polycondensation reactions are carried out to form a micro-crosslinked structure to improve the melt strength and tensile strength of PBSA.
The melt strength and tensile strength of PBSA are significantly improved, the application range is expanded, and the mechanical properties are optimized, with the melt index below 10 g/min and the tensile strength reaches 45-62 MPa.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a preparation method of high melt strength polybutylene succinate / adipate (PBSA) and application thereof. Background Art
[0002] Currently, polybutylene succinate (PBS), as a typical aliphatic polyester, is valued for its excellent mechanical properties. These properties make it an ideal choice for packaging, fibers, films and composite materials. Although PBS has many advantages, it still has some significant defects. First, compared with some traditional plastics, the production cost of PBS is higher, which may limit its competitiveness in a price-sensitive market environment. In addition, the degradation rate of PBS is low. Although it is a biodegradable material, its degradation rate in the natural environment may not be sufficient to meet the growing environmental protection needs.
[0003] In order to further improve its performance, the researchers explored the method of chemical modification by introducing adipic acid (AA). By esterifying and polycondensing 1,4-butanediol (BDO) and succinic acid (SA) with adipic acid, a new copolyester polybutylene succinate / adipate (PBSA) was successfully synthesized. This chemical modification brought about a series of significant performance improvements.
[0004] First, PBSA, due to the introduction of adipic acid units, improves the flexibility of the macromolecular chain, destroys the regularity of the macromolecular chain, and reduces the crystallinity of the polymer. Therefore, PBSA has higher elongation at break and impact strength than PBS. In addition, PBSA degrades faster than PBS. This is because the introduction of adipic acid units reduces the crystallinity of the polymer and increases the content of amorphous regions. The amorphous region has a loose structure and is the first to be attacked and degraded by microorganisms during the degradation process. This feature is of great significance for reducing the persistence of plastics in the environment, especially in disposable products that require rapid biodegradation.
[0005] Although PBSA has shown its potential as a biodegradable material due to its excellent flexibility and fast degradation rate, it is still facing some challenges, especially its macromolecules are completely linear, and the molecular weight is low, which makes the polymer melt strength of PBSA low, seriously affecting its molding process, such as injection molding, blow molding, etc. Low melt strength causes melt fracture during the blow molding process of polymer materials, and bubbles and collapse occur during the injection molding process, affecting the quality and consistency of the final product. Molecular weight also directly affects the various mechanical properties of the material. High molecular weight materials with low molecular weight are more likely to break or fracture when stretched or bent, limiting their use in applications requiring higher strength. The performance of the material can be improved by introducing polyols or using a composite material method. Patent CN102477216A provides a composite material blended with starch and hyperbranched polyester, which uses a new type of compatibilizer to improve the tensile strength of the composite material. Because the abundant hydroxyl groups on the surface of the hyperbranched polyester are easy to hydrogen bond with the hydroxyl groups of the starch molecular chain, the intermolecular and intramolecular hydrogen bond forces of the starch are weakened, resulting in a decrease in the melt index and a decrease in the melt strength. Patent CN118184846A introduces a melt strength enhancer into the polymerization system, which can form a certain micro-crosslinked structure during the polymerization process and has a long side chain, so that the melt strength of the polymer is greatly improved. However, the addition of the melt strength enhancer reduces the catalytic effect of the catalyst, reduces the molecular weight of the polymer, and deteriorates the mechanical properties. Patent CN114409939A introduces inorganic nanoparticles into polyester and uses them as grafting points to form a branched structure, thereby improving the melt strength of the polymer. However, the inorganic nanoparticles are prone to agglomeration in polyester, resulting in a decrease in mechanical properties.
[0006] In order to improve the melt strength and mechanical properties of PBSA, the present invention adopts a branching agent to modify the PBSA copolyester, and synthesizes a new PBSA copolyester by adjusting the type and content of the branching agent, thereby providing a branched PBSA copolyester with high tensile strength and high melt strength and a preparation method thereof.
[0007] In view of this, the present invention is proposed. Summary of the invention
[0008] In order to solve the problems existing in the above-mentioned technology, the present invention provides a branched PBSA with high tensile strength and high melt strength and a preparation method thereof.
[0009] The invention improves the disadvantages of low melt strength, poor mechanical properties and the like of PBSA polyester by introducing a high-efficiency branching agent, thereby expanding the application range of PBSA polyester.
[0010] To achieve the above object, the present invention provides the following technical solution, comprising the following steps: S1, mixing succinic acid, adipic acid, 1,4-butanediol, an esterification catalyst, a heat stabilizer, and a branching agent, and then performing an esterification reaction; S2. After the esterification reaction is completed, a polycondensation catalyst and a heat stabilizer are added to carry out a prepolymerization reaction at a certain temperature, and then the temperature is further increased to carry out a polycondensation reaction under a certain vacuum degree to obtain a PBSA copolyester with high tensile strength and high melt strength.
[0011] Preferably, in the above technical solution, in step S1, the molar ratio of the diacid monomer to butanediol is 1:1-2, and the molar ratio of succinic acid to adipic acid is 3:7.
[0012] Preferably, in the above technical solution, in step S1, the esterification reaction temperature is 150-190° C., and the reaction time is 2-4 h.
[0013] Preferably, in the above technical scheme, in step S1, the amount of the esterification catalyst added is 0.001-1% of the sum of the mass of the dibasic acid and the diol, the amount of the heat stabilizer added is 0.001-1% of the sum of the mass of the dibasic acid and the diol, and the branching agent accounts for less than 2% of the molar percentage of the diacid monomer.
[0014] Preferably, in the above technical scheme, in step S1, the esterification catalyst is selected from one or more of zinc acetate, tetrabutyl titanate, tetrabutyl zirconate, and manganese acetate, preferably zinc acetate and tetrabutyl titanate. The heat stabilizer is selected from one or more of triphenyl phosphate, trimethyl phosphate, sodium hydrogen phosphate, sodium dihydrogen phosphate, potassium hydrogen phosphate, potassium dihydrogen phosphate, potassium phosphate, magnesium hydrogen phosphate, magnesium dihydrogen phosphate, magnesium phosphate, triphenyl phosphite, and trimethyl phosphite, preferably trimethyl phosphate and triphenyl phosphate. The branching agent is selected from one or more of trihydroxypropane, trihydroxyethane, malic acid, citric acid, tartaric acid, pentaerythritol, and glycerol. Preferably, glycerol and pentaerythritol.
[0015] Preferably, in the above technical solution, in step S2, the temperature of the pre-polycondensation reaction is 180-250°C, and the reaction time is 0.5-1 h.
[0016] Preferably, in the above technical solution, in step S2, the temperature of the polycondensation reaction is 210-290°C, the pressure is 10-200 Pa, and the time is 1-4 h.
[0017] Preferably, in the above technical solution, in step S2, the amount of the polycondensation catalyst added is 0.001-1% of the sum of the mass of the dibasic acid and the diol, and the amount of the heat stabilizer added is 0.001-1% of the sum of the mass of the dibasic acid and the diol.
[0018] Preferably, in the above technical solution, in step S2, the polycondensation catalyst is selected from one or more of zinc acetate, tetrabutyl titanate, tetrabutyl zirconate, and manganese acetate, preferably zinc acetate and tetrabutyl titanate. The heat stabilizer is selected from one or more of triphenyl phosphate, trimethyl phosphate, sodium hydrogen phosphate, sodium dihydrogen phosphate, potassium hydrogen phosphate, potassium dihydrogen phosphate, potassium phosphate, magnesium hydrogen phosphate, magnesium dihydrogen phosphate, magnesium phosphate, triphenyl phosphite, and trimethyl phosphite, preferably trimethyl phosphate and triphenyl phosphate.
[0019] The present invention provides a high melt strength polybutylene succinate / adipate. Compared with pure diacid monomers, polyols are used as branching agents to achieve faster reaction and higher reaction degree in the esterification reaction stage. The branching agent forms a micro-crosslinking structure in the polymer system to improve the melt strength of the polymer, but excessive use may lead to performance deterioration and reduced tensile strength. The present invention controls the amount of branching agent to be less than 2% of the molar percentage of the diacid monomer, thereby not only improving the melt strength and molecular weight, but also reducing the content of oligomers. The final weight average molecular weight ( M w ) is 25×10 4 g / mol-30×10 4 g / mol, tensile strength range of 45-62 MPa, intrinsic viscosity ≥2.0 dL / g, melt index (MFR) of 5-10 g / min, polybutylene succinate / adipate, while obtaining high mechanical properties polyester, the melt strength is improved to a certain extent.
[0020] Compared with the prior art, the present invention has the following advantages: 1. The present invention achieves the maximum branching effect by controlling the structure, content and addition time of the branching agent, and obtains a copolyester with a tensile strength of up to 62 MPa and a melt index of less than 10 g / 10min.
[0021] 2. The present invention introduces a branching agent of polyols that can participate in the reaction, without considering the loss of mechanical properties caused by poor compatibility and agglomeration, thereby extending the service life of the material. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments.
[0023] The embodiments are only a part of the embodiments of the present invention, rather than all the embodiments, and are only used to explain the present invention, not to limit the present invention.
[0024] In the examples, unless otherwise specified, all the means used are conventional means in the art.
[0025] In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0026] In the embodiments of the present invention, the raw materials used are all commercially available products and are used directly without special treatment.
[0027] In the embodiments of the present invention, the analytical test methods used are described as follows: 1. Intrinsic viscosity: Determined according to GB / T 14190-2017, the solvent used is phenol / 1,1,2,2-tetrachloroethane (mass ratio is 1:1) solution.
[0028] 2. Melt index: According to GB / T 3682-2000, the test was carried out under the conditions of load 2.16 kg and temperature 190°C. The test was repeated 5 times and the average value was taken as the test result.
[0029] 3. Tensile strength: According to GB / T 1040.2-2006 standard, the tensile test was carried out using an Instron 1122 tensile testing machine at 25 °C and a tensile rate of 50 mm / min. The test was performed 5 times, and the average value was taken as the test result.
[0030] 4. Weight average molecular weight ( M w ): The weight average molecular weight of the sample was determined by gel permeation chromatography at a temperature of 45 °C, a solvent of chromatographic grade chloroform, a flow rate of 1.0 ml / min, and polystyrene was used as a reference standard.
[0031] Example 1 Example 1 A total of 4 experiments were conducted, namely Example 1.1, Example 1.2, Example 1.3 and Example 1.4.
[0032] In Example 1.1, the synthesis method of PBSA copolyester specifically includes: Adipic acid (7 mol), succinic acid (3 mol) and 1,4-butanediol (20 mol) were added into a reactor, and 0.05 wt% of tetrabutyl titanate based on the total mass of the dibasic acid and the diol and 0.03 wt% of trimethyl phosphate based on the total mass of the dibasic acid and the diol were added. Before esterification, 0.2% of pentaerythritol based on the molar number of the diacid monomer was added. Under nitrogen protection, the temperature was raised to 190°C for normal pressure esterification reaction for 3 h. After the esterification reaction was completed, 0.15 wt% of tetrabutyl titanate based on the total mass of the dibasic acid and the diol and 0.3 wt% of trimethyl phosphate based on the total mass of the dibasic acid and the diol were added. The temperature was raised to 210°C, the pressure was reduced to 200 Pa, and the reaction was carried out for 30 min for pre-polycondensation. The temperature was raised to 230°C, the pressure was reduced to 50 Pa, and the reaction was carried out for 4 h for polycondensation. Finally, the polymer PBSA-1 was obtained by discharging, pelletizing, cooling and drying.
[0033] The difference between Example 1.2 and Example 1.1 is that in step S1, the molar ratio of the diacid monomer to 1,4-butanediol is 1:1, and the polymer PBSA-2 is obtained.
[0034] The difference between Example 1.3 and Example 1.1 is that in step S1, the molar ratio of the diacid monomer to 1,4-butanediol is 1:1.5, and the polymer PBSA-3 is obtained.
[0035] The difference between Example 1.4 and Example 1.1 is that in step S1, the molar ratio of the diacid monomer to 1,4-butanediol is 1:2.5, and the polymer PBSA-4 is obtained.
[0036] Example 2 Example 2 was carried out in Example 2.1, Example 2.2, Example 2.3, Example 2.4, There are 6 tests in total for Example 2.5 and Example 2.6.
[0037] The difference between Example 2.1 and Example 1.1 is that in step S1, pentaerythritol is added after esterification reaction for 30 min to obtain polymer PBSA-5.
[0038] The difference between Example 2.2 and Example 1.1 is that in step S1, pentaerythritol is added after 60 min of esterification reaction to obtain polymer PBSA-6.
[0039] The difference between Example 2.3 and Example 1.1 is that in step S1, pentaerythritol is added after 90 min of esterification reaction to obtain polymer PBSA-7.
[0040] The difference between Example 2.4 and Example 1.1 is that in step S1, pentaerythritol is added after 120 min of esterification reaction to obtain polymer PBSA-8.
[0041] The difference between Example 2.5 and Example 1.1 is that in step S1, pentaerythritol is added after esterification reaction for 150 min to obtain polymer PBSA-9.
[0042] The difference between Example 2.6 and Example 1.1 is that pentaerythritol is added after the esterification reaction is completed in step S1 to obtain polymer PBSA-10.
[0043] Example 3 Example 3 A total of 3 experiments were conducted, namely Example 3.1, Example 3.2 and Example 3.3.
[0044] The difference between Example 3.1 and Example 1.1 is that in step S1, 0.1% of trihydroxypropane based on the molar number of the diacid monomer is added before esterification to obtain the polymer PBSA-11.
[0045] The difference between Example 3.2 and Example 1.1 is that in step S1, 0.4% of pentaerythritol based on the molar number of the diacid monomer is added before esterification to obtain the polymer PBSA-12.
[0046] The difference between Example 3.3 and Example 1.1 is that in step S1, 0.8% of propylene glycol based on the molar number of the diacid monomer is added before esterification to obtain the polymer PBSA-13.
[0047] Comparative Example 1 Adipic acid (7 mol), succinic acid (3 mol) and 1,4-butanediol (20 mol) were added to the reactor, and 0.05 wt% of tetrabutyl titanate based on the total mass of the dibasic acid and the diol and 0.03 wt% of trimethyl phosphate based on the total mass of the dibasic acid and the diol were added. Under nitrogen protection, the temperature was raised to 190 ° C for normal pressure esterification reaction for 3 hours. After the esterification reaction was completed, 0.15 wt% of tetrabutyl titanate based on the total mass of the dibasic acid and the diol and 0.3 wt% of trimethyl phosphate based on the total mass of the dibasic acid and the diol were added. The temperature was raised to 210 ° C, the pressure was reduced to 200 Pa, and the reaction was carried out for 30 min for pre-condensation. The temperature was raised to 230 ° C, the pressure was reduced to 50 Pa, and the reaction was carried out for 4 h for the condensation stage. Finally, the polymer PBSA-14 was obtained by discharging, pelletizing, cooling and drying.
[0048] All examples use a new reaction system to prepare PBSA, and Comparative Example 1 uses an acid method and does not introduce a branching agent to prepare PBSA, as shown in Table 1.
[0049] Table 1 PBSA performance test sample <![CDATA[M w (10 4 g / mol)]]> Melt index (g / 10min) Viscosity (dL / g) Tensile strength (MPa) PBSA-1 26.6 7.21 2.4 47.2 PBSA-2 26.2 7.46 2.2 47.4 PBSA-3 26.3 7.65 2.4 47.4 PBSA-4 26.5 7.54 2.4 47.6 PBSA-5 26.9 10.41 2.4 45.8 PBSA-6 26.4 11.52 2.4 45.3 PBSA-7 26.1 11.96 2.3 45.1 PBSA-8 25.9 12.27 2.3 44.8 PBSA-9 25.5 12.29 2.3 44.2 PBSA-10 26.9 13.52 2.5 43.7 PBSA-11 27.2 8.45 2.5 44.4 PBSA-12 27.9 7.17 2.6 62.6 PBSA-13 26.8 7.36 2.3 45.1 PBSA-14 25.3 20.36 2.3 28.1 Table 1 shows the performance of all the PBSA prepared in the experiment. With the continuous increase of the amount of branching agent added, the melt strength and mechanical properties of PBSA have increased significantly, and the tensile strength has increased by 50%. At the same time, the molecular weight has little effect, and the branching agent is added before the esterification reaction. The improvement of melt strength and mechanical properties has a wide range of application value for PBSA in blow molding. Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing high melt strength polybutylene succinate / adipate, comprising the following steps: S1. Mix succinic acid, adipic acid, 1,4-butanediol, an esterification catalyst, a heat stabilizer, and a branching agent, and then perform an esterification reaction at a certain temperature; S2. After the esterification reaction is completed, a pre-polycondensation reaction is carried out with a polycondensation catalyst and a heat stabilizer at a certain temperature, and then the temperature is further increased to carry out a polycondensation reaction under a certain vacuum degree.
2. The method for preparing high melt strength polybutylene succinate / adipate according to claim 1, characterized in that: The molar ratio of the diacid monomer to 1,4-butanediol is 1:1-2.
3. The method for preparing high melt strength polybutylene succinate / adipate according to claim 1, characterized in that: The molar ratio of succinic acid to adipic acid is 3:
7.
4. The method for preparing high melt strength polybutylene succinate / adipate according to claim 1, characterized in that: The branching agent is selected from one or more of trihydroxypropane, trihydroxyethane, malic acid, citric acid, tartaric acid, pentaerythritol and glycerol.