Preparation and temporary shape control method of degradable shape memory polyester copolymer

Through esterification reaction and melt polymerization technology, polyester copolymers with both shape memory and degradability were prepared, which solved the problem that shape memory materials in the prior art were difficult to take into account both degradation performance, and realized the food and medical field. application.

CN118930827AActive Publication Date: 2024-11-12淮北矿业绿色化工新材料研究院有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411020405.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

While maintaining the shape memory performance of the material, it is difficult to take into account the degradability of the material. Traditional methods such as increasing the crosslink density or introducing rigid chain segments will affect the degradability and safety of the material, limiting its use in food. Applications in packaging, medical and other fields.

Method used

Hard and soft segment prepolymers are prepared through esterification reaction, and their proportions are adjusted during melt polymerization, and degradable shape memory polyester copolymers with different shape fixation and recovery temperatures are prepared, using hard segments and soft chains The combination of segments controls the shape memory performance and degradability of the material.

Benefits of technology

It has achieved the preparation of shape memory polyester copolymers with good mechanical properties, adjustable deformation temperature range, and degradable shape memory polyester copolymers, suitable for food and tableware packaging, fracture fixing materials, etc., and expanded the application field of degradable polymer materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930827A_ABST
    Figure CN118930827A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and a temporary shape control method of a degradable shape memory polyester copolymer. The preparation method of the polyester copolymer comprises the following steps: by taking one of lactide, lactic acid, glycolide, methyl glycolate and glycollic acid as a monomer, carrying out esterification reaction to prepare a hard chain segment prepolymer; adipic acid or succinic acid and butanediol are subjected to an esterification reaction to prepare a soft chain segment prepolymer; or caprolactone is used as a polymeric monomer to prepare a soft segment prepolymer; and carrying out melt polymerization reaction on the hard chain segment prepolymer and the soft chain segment prepolymer to obtain the degradable shape memory polyester copolymer. The degradable shape memory polyester copolymer prepared by the invention has the advantages of good mechanical property, adjustable deformation temperature interval, degradability and the like, and can be used as a raw material of products such as food and tableware packages, fracture fixation materials, intelligent fabrics and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the preparation and application of a degradable shape memory macromolecular polymer, in particular to a preparation and temporary shape control method of a degradable shape memory polyester copolymer. Background Art

[0002] Shape memory polymer materials can deform under external stimuli (temperature, force, light, humidity, etc.) and fix the deformed temporary shape under specific conditions, and can return to the original shape when stimulated again. Shape memory polymers are widely used as heat shrink films, heat shrink tubes, smart fabrics, medical materials, etc. due to their advantages such as light weight and low price, easy molding, large deformation, and adjustable memory temperature.

[0003] Degradable polymer materials are environmentally friendly materials because they can be quickly degraded into small molecules such as water and carbon dioxide under natural conditions. They have been used in agricultural mulch, packaging bags, medical materials and other fields. Using degradable polymer materials to replace traditional plastics and other polymer products is an effective way to reduce the impact of plastics on the environment.

[0004] Most shape memory polymer materials are new polymers with special structures formed by in-situ polymerization. These polymer materials are targeted at specific needs in special occasions, have a narrow application field, and generally do not consider degradation performance. The heat shrinkable films and tubes used in daily life are mostly made of modified general-purpose resins as raw materials, and these shape memory polymers are not degradable.

[0005] The use of degradable polymers to prepare shape memory materials has little impact on the ecological environment while maintaining the shape memory properties of the materials, greatly broadening the application field of degradable polymer materials. However, shape memory polymer materials usually contain two structures, "stationary phase" and "reversible phase". In order to make the material have a strong shape recovery force, two methods are usually adopted: one is to increase the cross-linking density of the "stationary phase" to store more entropy energy of the molecular chain during the stretching process. As the temperature rises, the stored entropy energy is released to drive the material back to its original shape. However, cross-linking of degradable polymers will inevitably weaken or even completely destroy its degradable properties. The other is to introduce rigid segments to increase the entropy energy of the molecular chain when stretched, thereby providing a high recovery force for shape recovery. However, like increasing the cross-linking density, this method is also not conducive to polymer degradation, and the introduction of rigid segments may reduce the safety of the material, making it no longer suitable for use in food packaging, medical and health fields. Summary of the invention

[0006] Purpose of the invention: The purpose of the present invention is to provide a method for preparing a degradable shape memory polyester copolymer, and solve the problem of how to prepare a degradable shape memory polyester copolymer. Another purpose of the present invention is to propose a temporary shape control method for a degradable shape memory polyester copolymer, and solve the problem of how to restore and fix the shape of the polyester copolymer.

[0007] Technical solution: The method for preparing a degradable shape memory polyester copolymer described in the present invention comprises the following steps:

[0008] (1) using one of lactide, lactic acid, glycolide, methyl glycolate, and glycolic acid as a monomer, and carrying out an esterification reaction to prepare a hard segment prepolymer;

[0009] (2) preparing a soft segment prepolymer by esterification reaction of adipic acid or succinic acid with butanediol; or preparing a soft segment prepolymer by using caprolactone as a polymerization monomer;

[0010] (3) The hard segment prepolymer and the soft segment prepolymer are subjected to melt polymerization reaction to obtain a degradable shape memory polyester copolymer.

[0011] The invention uses degradable polyester monomer as main raw material, obtains hard and soft segment prepolymers through esterification reaction, and adjusts the ratio of soft and hard segments in the polymerization stage to obtain degradable shape memory polyester copolymers with different shape fixing temperatures and recovery temperatures as well as different shape fixing rates and recovery rates.

[0012] Preferably, the method of esterification reaction in step (1) is: after mixing the monomer and 0.1-0.25% of the total weight of the monomer, heating to 140-180° C. in an inert atmosphere for esterification reaction, and obtaining the hard segment prepolymer after reacting for 3-7 hours.

[0013] Preferably, the first catalyst is one or more of tin isooctanoate, stannous isooctanoate, stannous oxide, stannous chloride, stannous oxalate, tin tetrachloride butoxide titanium, p-toluenesulfonic acid monohydrate, anhydrous zinc acetate, triethoxytetrafluoroborate, boron trifluoride, trifluoroacetic acid, and antimony trioxide.

[0014] Preferably, in step (2), the esterification reaction method is: adding a second catalyst to a mixture of adipic acid and butanediol or a mixture of succinic acid and butanediol, heating to 160-200° C. under an inert atmosphere to carry out an esterification reaction, and reacting for 4-8 hours to obtain a soft segment prepolymer;

[0015] The method for preparing a soft segment prepolymer using caprolactone as a polymerization monomer comprises: adding a second catalyst to caprolactone, carrying out an esterification reaction under vacuum and heating conditions, and obtaining the soft segment prepolymer.

[0016] Preferably, the molar ratio of adipic acid to butanediol is 1-1.2:1-1.2, the molar ratio of succinic acid to butanediol is 1-1.2:1-1.2, the second catalyst comprises one or more of tetrabutyl titanate, tetraphenyltin, and stannous octoate, and the added amount of the second catalyst is 0.1-0.25wt% of the mixture of adipic acid and butanediol or the mixture of succinic acid and butanediol or caprolactone.

[0017] Preferably, in step (3), the molar ratio of the hard segment prepolymer to the soft segment prepolymer is 1-9:1-9.

[0018] Preferably, in step (3), the method of melt polymerization reaction is: under an inert atmosphere, the hard segment prepolymer and the soft segment prepolymer are mixed and melted, and then a third catalyst, triphenyl phosphate and an antioxidant are added, and an esterification reaction is carried out at 180-220°C under vacuum conditions for 3-7 hours to obtain a degradable shape memory polyester copolymer; the weight ratio of the total weight of the hard segment prepolymer and the soft segment prepolymer: the third catalyst: triphenyl phosphate: the antioxidant is 100: 0.1-0.25: 0.1-0.3: 0.1-0.3.

[0019] Preferably, the third catalyst includes one or more of antimony trioxide, tetrabutyl titanate, tin isooctanoate, and stannous octoate. The method for mixing and melting the hard segment prepolymer and the soft segment prepolymer is: first, the soft segment prepolymer is heated to 175-195°C under stirring conditions, kept warm for 0.5-1.5h, then cooled to 130-150°C and added to the hard segment prepolymer, and kept warm until the soft segment prepolymer and the hard segment prepolymer are completely melted.

[0020] Another aspect of the present invention discloses a method for controlling the temporary shape of the degradable shape memory polyester copolymer prepared by the above preparation method, comprising the following steps:

[0021] The polyester copolymer is stretched at a temperature higher than the crystallization temperature of its soft segment and lower than the crystallization temperature of its hard segment, and then cooled to a temperature lower than the crystallization temperature of its soft segment to fix the stretched shape.

[0022] Preferably, the crystallization temperature of the soft segment is 30-45°C, and the crystallization temperature of the hard segment is 65-160°C.

[0023] The degradable shape memory polyester copolymer of the present invention contains two kinds of segments, hard and soft. The hard segment is used as a "stationary phase", which is cold-drawn to a highly oriented structure under the action of a tensile force above the transition temperature (between the crystallization temperature of the "reversible phase" and the crystallization temperature of the "stationary phase"), and the molecular chain is arranged along the force direction, the conformational entropy of the molecular chain is reduced, and the entropy energy is increased; as the temperature drops below the transition temperature, the molecular chain is frozen and the movement is hindered, and the conformation of the molecular chain remains unchanged after the external force is removed, and the entropy energy is stored; when the temperature rises above the transition temperature again, the mobility of the molecular chain is activated, the entropy energy is released, and the molecular chain is driven back to the state with the maximum conformational entropy, and the material returns to its original shape. The soft chain segment acts as a "reversible phase" and is stretched above the transition temperature. Since the molecular chains of this phase have strong mobility at this temperature, the stretched molecular chains quickly rearrange themselves. As the temperature drops below the transition temperature, all the molecular chains of the two phases are frozen, and the temporary shape is fixed after the external force is removed. When the temperature rises above the transition temperature again, on the one hand, the "stationary phase" molecular chains are activated and entropy energy is released. On the other hand, the "reversible phase" molecular chains are unfrozen, and the hindering effect on the "stationary phase" molecular chains is weakened, and the material returns to its original shape driven by entropy energy.

[0024] In the present invention, polylactic acid or polyglycolic acid is used as a hard segment, as the "stationary phase" in the shape memory polyester copolymer, which is used to provide a driving force for shape recovery and fix the original shape of the polyester; polybutylene adipate, polybutylene succinate or polycaprolactone is used as a soft segment, as the "reversible phase" in the shape memory polyester copolymer, which is used to control the fixation and recovery of the temporary shape of the polyester.

[0025] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the degradable shape memory polyester copolymer prepared by the present invention has the advantages of good mechanical properties, adjustable deformation temperature range, and degradability, and can be used as a raw material for food and tableware packaging, fracture fixation materials, smart fabrics and other products. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a test curve of shape memory performance of butylene lactate adipate copolymer;

[0027] Figure 2 is the stress-strain curve of butylene lactate adipate copolymer;

[0028] Figure 3 These are the weight loss curves of lactic acid and adipate butylene glycol copolymer in water, soil burial, and CALB enzyme environments respectively. DETAILED DESCRIPTION

[0029] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0030] Example 1: A method for preparing a degradable shape memory polyester copolymer is as follows:

[0031] (1) Preparation of lactic acid prepolymer:

[0032] A certain mass of lactic acid was weighed into a reactor, and anhydrous zinc acetate as a catalyst was added at 0.2% of the weight of the lactic acid. Nitrogen was passed through the reactor for protection, the temperature was raised to 160° C., stirring was started, the nitrogen was turned off after reacting for 5 hours, and the reactor was vacuumed for 10 minutes to finally obtain a lactic acid prepolymer.

[0033] (2) Preparation of butanediol adipate prepolymer:

[0034] Adipic acid and 1,4-butanediol in a molar ratio of 1:1 were added to a reactor, and a catalyst tetrabutyl titanate was added with a total weight of 0.2% of adipic acid and butanediol. After evacuation, nitrogen was used to replace the residual air and nitrogen protection was continued. The temperature was raised to 180°C, stirring was started, and the nitrogen was turned off after reacting for 6 hours to obtain adipic acid butanediol prepolymer with a number average molecular weight of 8917.

[0035] (3) Melt polymerization of lactic acid prepolymer and butanediol adipate prepolymer:

[0036] Add butylene adipate prepolymer into a reactor, replace air with nitrogen, set the temperature to 50°C, start stirring, gradually heat up to 185°C and keep warm for 1 hour, cool down to 140°C and add lactic acid prepolymer in the same mole as butylene adipate prepolymer, then add 0.2% of the total weight of butylene adipate prepolymer and lactic acid prepolymer as catalyst antimony trioxide, 0.2% of the total weight of butylene adipate prepolymer and lactic acid prepolymer as stabilizer triphenyl phosphate, and 0.2% of the total weight of butylene adipate prepolymer and lactic acid prepolymer as antioxidant 1010. Evacuate, gradually heat up to 200°C, keep warm for 5 hours, and obtain lactic acid butylene adipate copolymer, which is a degradable shape memory polyester copolymer.

[0037] Example 2: A method for preparing a degradable shape memory polyester copolymer is as follows:

[0038] (1) Preparation of lactic acid prepolymer:

[0039] Weigh a certain mass of lactic acid into a reactor, add anhydrous zinc acetate at 0.25% of the weight of the lactic acid, pass nitrogen protection, heat to 140°C, start stirring, turn off nitrogen after reacting for 7 hours, evacuate for 10 minutes, and finally obtain a lactic acid prepolymer.

[0040] (2) Preparation of butylene succinate prepolymer:

[0041] Succinic acid and 1,4-butanediol in a molar ratio of 1.2:1 were added to a reactor, and a catalyst tetrabutyl titanate with a total weight of 0.25% of succinic acid and butanediol was added. After evacuation, nitrogen was used to replace the residual air and nitrogen protection was continued. The temperature was raised to 160°C, stirring was started, and the nitrogen was turned off after reacting for 8 hours to obtain a succinic acid butanediol prepolymer with a number average molecular weight of 7825.

[0042] (3) Melt polymerization of lactic acid prepolymer and butanediol succinate prepolymer:

[0043] The butylene succinate prepolymer is added to the reactor, the air is replaced by nitrogen, the temperature is set to 50°C, stirring is started, the temperature is gradually raised to 175°C and then kept warm for 1.5 hours, the temperature is lowered to 130°C and then the lactic acid prepolymer is added, the molar ratio of the lactic acid prepolymer to the butylene succinate prepolymer is 1:9, and then 0.1% of the total weight of the butylene succinate prepolymer and the lactic acid prepolymer is added. The catalyst antimony trioxide, 0.1% of the total weight of the butylene succinate prepolymer and the lactic acid prepolymer, the stabilizer triphenyl phosphate, and the antioxidant 1010 are added. Vacuuming, gradually raising the temperature to 220°C, and keeping warm for 3 hours to obtain a lactic acid butylene succinate copolymer, that is, a degradable shape memory polyester copolymer.

[0044] Example 3: A method for preparing a degradable shape memory polyester copolymer is as follows:

[0045] (1) Preparation of lactic acid prepolymer:

[0046] Weigh a certain mass of lactic acid into a reactor, add 0.1% of the weight of lactic acid anhydrous zinc acetate, pass nitrogen protection, heat to 180°C, start stirring, turn off nitrogen after reacting for 3 hours, evacuate for 10 minutes, and finally obtain a lactic acid prepolymer.

[0047] (2) Preparation of butanediol adipate prepolymer:

[0048] Adipic acid and 1,4-butanediol in a molar ratio of 1:1.2 were added to a reactor, and a catalyst tetrabutyl titanate was added at a total weight of 0.1% of adipic acid and butanediol. After evacuation, nitrogen was used to replace the residual air and nitrogen protection was continued. The temperature was raised to 200°C, stirring was started, and the nitrogen was turned off after reacting for 4 hours to obtain adipic acid butanediol prepolymer with a number average molecular weight of 9451.

[0049] (3) Melt polymerization of lactic acid prepolymer and butanediol adipate prepolymer:

[0050] Add butylene adipate prepolymer to the reactor, replace air with nitrogen, set the temperature to 50°C, start stirring, gradually heat up to 195°C and keep warm for 0.5 hours, cool down to 150°C and add lactic acid prepolymer, the molar ratio of lactic acid prepolymer to butylene adipate prepolymer is 9:1, then add 0.25% of the total weight of butylene adipate prepolymer and lactic acid prepolymer as catalyst antimony trioxide, 0.3% of the total weight of butylene adipate prepolymer and lactic acid prepolymer as stabilizer triphenyl phosphate, and 0.3% of the total weight of butylene adipate prepolymer and lactic acid prepolymer as antioxidant 1010. Evacuate, gradually heat up to 180°C, keep warm for 7 hours, and obtain lactic acid butylene adipate copolymer, which is a degradable shape memory polyester copolymer.

[0051] Embodiment 4: All other aspects are the same as Embodiment 1, except that:

[0052] In step (1), lactic acid is replaced by lactide; anhydrous zinc acetate is replaced by tin isooctanoate to obtain a lactide prepolymer.

[0053] In step (2), adipic acid and butanediol are replaced by caprolactone; tetrabutyl titanate is replaced by tetraphenyltin; and the amount of tetraphenyltin added is 0.15 wt% of the weight of caprolactone to obtain a caprolactone prepolymer.

[0054] In step (3), the butanediol adipate prepolymer is replaced by caprolactone prepolymer, and the molar ratio of the caprolactone prepolymer to the lactide prepolymer is 3:5; and antimony trioxide is replaced by tetrabutyl titanate.

[0055] Embodiment 5: All other aspects are the same as Embodiment 1, except that:

[0056] In step (1), lactic acid is replaced by glycolide; anhydrous zinc acetate is replaced by tin tetrachloride titanium butoxide to obtain a glycolide prepolymer.

[0057] In step (2), adipic acid and butanediol are replaced by caprolactone; tetrabutyl titanate is replaced by stannous octoate; and the amount of stannous octoate added is 0.15 wt% of the weight of caprolactone to obtain a caprolactone prepolymer.

[0058] In step (3), the butanediol adipate prepolymer is replaced by caprolactone prepolymer, and the molar ratio of the caprolactone prepolymer to the glycolide prepolymer is 1:4; and antimony trioxide is replaced by tin isooctanoate.

[0059] Embodiment 6: All other aspects are the same as those of Embodiment 1, except that:

[0060] In step (1), lactic acid is replaced by methyl glycolate; anhydrous zinc acetate is replaced by triethoxytetrafluoroborate to obtain methyl glycolate prepolymer.

[0061] In step (3), the molar ratio of the butanediol adipate prepolymer to the methyl glycolate prepolymer is 7:2; antimony trioxide is replaced by stannous octoate.

[0062] Embodiment 7: All other aspects are the same as Embodiment 1, except that:

[0063] In step (1), lactic acid is replaced by glycolic acid; anhydrous zinc acetate is replaced by p-toluenesulfonic acid monohydrate to obtain a glycolic acid prepolymer.

[0064] In step (3), the molar ratio of the butanediol adipate prepolymer to the glycolic acid prepolymer is 1:2; antimony trioxide is replaced by tetrabutyl titanate.

[0065] Embodiment 8: All other aspects are the same as those of Embodiment 1, except that:

[0066] In step (1), lactic acid is replaced by glycolide.

[0067] Comparative Example 1: The rest is the same as Example 1, except that:

[0068] In step (1), lactic acid is replaced by a mixture of glycolide and lactide in a molar ratio of 5:1.

[0069] Comparative Example 2: The rest is the same as Example 1, except that:

[0070] In step (1), lactic acid is replaced by a mixture of glycolide and lactide in a molar ratio of 5:1.

[0071] At the same time, the butylene adipate prepolymer prepared in step (2) is replaced by polybutylene adipate with a number average molecular weight of 2000.

[0072] Comparative Example 3: The rest is the same as Example 1, except that:

[0073] The butylene adipate prepolymer prepared in step (2) is replaced by polybutylene adipate having a number average molecular weight of 2000.

[0074] Comparative Example 4: A polymer was prepared as follows:

[0075] Under nitrogen protection, lactic acid, adipic acid and 1,4-butanediol were mixed in a molar ratio of 2:1:1, and then 0.5% of the total weight of the catalyst (composed of antimony trioxide, tetrabutyl titanate and anhydrous zinc acetate in a weight ratio of 1:1:1) of lactic acid, adipic acid and 1,4-butanediol; 0.2% of the total weight of triphenyl phosphate of lactic acid, adipic acid and 1,4-butanediol; 0.2% of the total weight of antioxidant 1010 of lactic acid, adipic acid and 1,4-butanediol were added. Vacuum was evacuated, and the temperature was gradually raised to 200°C, and the temperature was kept for 5 hours to obtain the final product.

[0076] Shape memory properties test of degradable shape memory polyester copolymer

[0077] The polylactic acid-butylene adipate copolymer obtained in Example 1 was sampled and molded into a 0.7 mm thick sheet using a flat vulcanizer, and then cut into dumbbell-shaped strips with a length of 75 mm and a width of 4 mm in the middle using a punching machine.

[0078] Shape memory performance testing in a dynamic thermomechanical analyzer

[0079] Fix the specimen with a clamp, heat it to 80°C, keep it at this temperature for 1 minute, and mark the strain at this time as ε0.

[0080] Stress is applied to stretch the spline to 100%, and the strain at this time is marked as ε1.

[0081] Keeping the strain constant, the specimen was cooled to 25°C and kept at this temperature for 5 minutes.

[0082] Remove the stress and record the strain ε2 after 5 minutes.

[0083] The sample was heated to 80°C again and kept at this temperature for 30 minutes to restore the sample to its original shape and generate residual strain ε3.

[0084] The values ​​of shape fixation rate (Rf) and shape recovery rate (Rr) are calculated according to the formula and The shape memory test curve is as follows: Figure 1 As shown, the calculated Rf is 97.4% and the Rr is 98.0%.

[0085] Experimental example Mechanical properties test

[0086] The same preparation method as the shape memory performance test was used to prepare the sample, and the tensile mechanical performance test was carried out on an electronic universal testing machine. The sample was pulled to fracture at a tensile rate of 5mm / min at room temperature of 25°C. Its stress-strain curve is shown in Figure 2 As shown, it can be seen that the tensile strength is 43.5 MPa and the tensile strain at break is 535%.

[0087] Degradation performance test: The molded specimens were subjected to corresponding degradation experiments in water, soil burial, and CALB enzyme conditions. The mass loss was weighed every week and the mass loss rate was calculated. The results are as follows Figure 3 As shown, the experiment was carried out for 10 weeks, from which it can be seen that the mass loss rates of hydrolysis, soil burial and enzymatic hydrolysis after ten weeks were 4.9%, 2.3% and 10%, respectively.

[0088] The properties of the final products obtained in Examples 2-8 and Comparative Examples 1-4 were tested using the same test method as above, and the results were as follows:

[0089] Table 1 Effects of different preparation methods on the shape memory properties and degradation properties of polymers

[0090]

[0091]

[0092] As can be seen from the results in Table 1, when the raw materials of the hard segment prepolymer in Comparative Example 1 are two lactides, the shape memory performance of the polymer is poor. It can be seen from the comparison between Comparative Examples 1 and 2 that the reason for the poor performance of Comparative Example 1 may be related to the number average molecular weight of the soft segment prepolymer. The hard segment prepolymer made of two lactides may rely on the soft segment prepolymer with a lower number average molecular weight, and is not compatible with the soft segment prepolymer with a higher number average molecular weight. The wrong match leads to a significant reduction in the degradability and shape memory performance of the final product. Comparative Example 3 is compared with Example 1 to show that the smaller the number average molecular weight of the soft segment prepolymer, the better the degradability. Therefore, the enzymatic mass loss rate of Comparative Example 3 is greater than that of Example 1, but the shape memory performance and strength of the final product are significantly lower than those of Example 1, indicating that although the selection of a soft segment prepolymer with a smaller number average molecular weight can slightly improve the degradability, it has a greater negative impact on the shape memory performance. Comparative Example 4 uses the same raw materials to prepare the polymer through a one-pot process. Due to the disordered esterification reaction between the monomers, it is difficult to form ordered and functionalized hard and soft segments. Therefore, the product of Comparative Example 4 does not have shape memory function and has poor degradability.

Claims

1. A method for preparing a degradable shape memory polyester copolymer, It is characterized in that The steps include: (1) using one of lactide, lactic acid, glycolide, methyl glycolate, and glycolic acid as a monomer, and carrying out an esterification reaction to prepare a hard segment prepolymer; (2) preparing a soft segment prepolymer by esterification reaction of adipic acid or succinic acid with butanediol; or preparing a soft segment prepolymer by using caprolactone as a polymerization monomer; (3) The hard segment prepolymer and the soft segment prepolymer are subjected to melt polymerization reaction to obtain a degradable shape memory polyester copolymer.

2. The method for preparing the degradable shape memory polyester copolymer according to claim 1, It is characterized in that The method of the esterification reaction in step (1) is: after mixing the monomer and 0.1-0.25% of the total weight of the monomer, heat to 140-180° C. in an inert atmosphere for esterification reaction, and obtain the hard segment prepolymer after reacting for 3-7 hours.

3. The method for preparing the degradable shape memory polyester copolymer according to claim 2, It is characterized in that The first catalyst is one or more of tin isooctanoate, stannous isooctanoate, stannous oxide, stannous chloride, stannous oxalate, tin tetrachloride titanium butoxide, p-toluenesulfonic acid monohydrate, anhydrous zinc acetate, triethoxytetrafluoroborate, boron trifluoride, trifluoroacetic acid, and antimony trioxide.

4. The method for preparing the degradable shape memory polyester copolymer according to claim 1, It is characterized in that In step (2), the esterification reaction method is: adding a second catalyst to a mixture of adipic acid and butanediol or a mixture of succinic acid and butanediol, heating to 160-200° C. under an inert atmosphere for esterification reaction, and reacting for 4-8 hours to obtain a soft segment prepolymer; The method for preparing a soft segment prepolymer using caprolactone as a polymerization monomer comprises the following steps: adding a second catalyst to caprolactone, carrying out an esterification reaction under vacuum and heating conditions, and obtaining the soft segment prepolymer.

5. The method for preparing the degradable shape memory polyester copolymer according to claim 4, It is characterized in that The molar ratio of adipic acid to butanediol is 1-1.2:1-1.2, the molar ratio of succinic acid to butanediol is 1-1.2:1-1.2, the second catalyst comprises one or more of tetrabutyl titanate, tetraphenyltin, and stannous octoate, and the added amount of the second catalyst is 0.1-0.25wt% of the mixture of adipic acid and butanediol or the mixture of succinic acid and butanediol or caprolactone.

6. The method for preparing the degradable shape memory polyester copolymer according to claim 1, It is characterized in that In step (3), the molar ratio of the hard segment prepolymer to the soft segment prepolymer is 1-9:1-9.

7. The method for preparing the degradable shape memory polyester copolymer according to claim 1, It is characterized in that In step (3), the method of melt polymerization reaction is: under an inert atmosphere, the hard segment prepolymer and the soft segment prepolymer are mixed and melted, and then a third catalyst, triphenyl phosphate and an antioxidant are added, and an esterification reaction is carried out at 180-220° C. under vacuum conditions for 3-7 hours to obtain a degradable shape memory polyester copolymer; the weight ratio of the total weight of the hard segment prepolymer and the soft segment prepolymer: the third catalyst: triphenyl phosphate: the antioxidant is 100: 0.1-0.25: 0.1-0.3: 0.1-0.

3.

8. The method for preparing the degradable shape memory polyester copolymer according to claim 7, It is characterized in that The third catalyst includes one or more of antimony trioxide, tetrabutyl titanate, tin isooctanoate, and stannous octoate. The method for mixing and melting the hard segment prepolymer and the soft segment prepolymer is: firstly heat the soft segment prepolymer to 175-195°C under stirring conditions, keep it warm for 0.5-1.5h, then cool it to 130-150°C, add the hard segment prepolymer, and keep it warm until the soft segment prepolymer and the hard segment prepolymer are completely melted.

9. A method for controlling the temporary shape of a degradable shape memory polyester copolymer prepared by the preparation method according to any one of claims 1 to 8, It is characterized in that The steps include: The polyester copolymer is stretched at a temperature higher than the crystallization temperature of its soft segment and lower than the crystallization temperature of its hard segment, and then cooled to a temperature lower than the crystallization temperature of its soft segment to fix the stretched shape.

10. The temporary shape control method of the degradable shape memory polyester copolymer according to claim 9, It is characterized in that The crystallization temperature of the soft segment is 30-45°C, and the crystallization temperature of the hard segment is 65-160°C.

Citation Information

Patent Citations

  • Preparation method of polylactic acid-based thermoplastic elastomer with shape memory property

    CN108559088A

  • Degradable polymer with shape memory function and synthesis method thereof

    CN114835877A

  • Photoinduced biodegradable shape memory material

    CN115073698A

  • Preparation method of poly (butylene succinate) and polylactic acid biodegradable block copolyester material

    CN118047938A

  • Biodegradable shape memory polymeric sutures

    US20040015187A1