Polyimide oligomer, preparation method thereof and cured product with low dielectric property prepared from polyimide oligomer

By combining dipolymer diamine with other monomers and performing free radical curing, the problem of insufficient heat resistance of polyimide materials is solved, high-frequency, low-dielectric characteristics and good electrical properties are achieved, and waste liquids and Solvent is suitable for high-frequency circuit board materials, taking into account material properties and environmental protection.

CN118930855APending Publication Date: 2024-11-12SWANCOR INNOVATION & INCUBATION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310521103.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing polyimide materials have shortcomings in heat resistance, and their purification is difficult to be easy during the preparation process and wastewater is generated in large quantities, making it difficult to take into account both electrical properties and environmental protection.

Method used

Radically curable polyimide oligomers are prepared by combining dimer diamine with other monomers and proportional adjustments. The polymerization is carried out using a series of dissolution, mixing and reaction steps, combined with a radical initiator for polymerization. Curing, avoiding purification steps, and forming a cured substance with good heat resistance and electrical properties.

Benefits of technology

It has achieved improvements in the heat resistance and electrical properties of polyimide oligomers, reduced waste liquid output and solvent use, and is suitable for high-frequency circuit board materials, balancing material performance and environmental protection needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930855A_ABST
    Figure CN118930855A_ABST
Patent Text Reader

Abstract

The invention provides a polyimide oligomer, a preparation method thereof and a cured product with low dielectric property prepared by the polyimide oligomer, the polyimide oligomer has a structure shown as a formula (I) or a formula (II), and each symbol in the formula (I) and the formula (II) is defined in the specification. Therefore, the dimer diamine is matched with a specific monomer and the proportion is adjusted to prepare the free radical curable polyimide oligomer, and the polyimide oligomer has good thermal property and excellent low dielectric property after being cured, so that the polyimide oligomer can be applied to the industry of high-frequency circuit boards. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an oligomer, a preparation method thereof and a cured product, and in particular to a polyimide oligomer derived from dimerized diamine, a preparation method thereof and a cured product prepared therefrom with low dielectric properties. Background Art

[0002] Nowadays, the rise of cloud technologies such as the Internet and data centers has made free radical curing systems highly valued in the application of printed circuit board materials. Noryl SA 9000 sold by SABIC is a polyphenylene ether oligomer with a terminal difunctional acrylic group. Due to its low molecular weight, it has good organic solubility and good construction properties in the impregnation process. Therefore, Noryl SA 9000 is endowed with basic physical properties through free radical curing of the terminal acrylic group, and the non-polar structure of polyphenylene ether itself and the fact that no polar groups are generated after free radical curing give its cured product excellent electrical performance, making Noryl SA 9000 gradually become one of the mainstream materials for today's high-end printed circuit board materials. However, the preparation process of Noryl SA 9000 is not easy to purify and produces a lot of wastewater. Based on environmental protection considerations, the development of usable materials with good electrical performance and low process pollution will help the development of printed circuit board materials while taking into account environmental protection issues.

[0003] In recent years, with the rise of environmental awareness and carbon reduction, many studies have begun to focus on the application of special bio-based diamines. For example, dimer diamine is mixed with aromatic diamine monomer m-tolidine and polymerized with 4,4'-bisphenol A dianhydride (BPADA) to obtain a high molecular weight polyimide (PI), or dimer diamine is reacted with dianhydride to prepare a polyimide oligomer or polymer with a reactive functional group at the end. Since the main structure of dimer diamine is a large diamine with a branched shape and a large free volume, it is expected to provide low dielectric properties when introduced into the material, so that the electrical properties of the above-mentioned polyimide materials are excellent, but there is still considerable room for improvement in heat resistance.

[0004] In view of this, how to synthesize a free radical-curable polyimide oligomer derived from bio-based dimerized diamine so that it can overcome the poor thermal properties of dimerized diamine derivatives and have high frequency and low dielectric properties has become the goal of relevant industry players. Summary of the invention

[0005] An object of the present invention is to provide a polyimide oligomer, a preparation method thereof and a cured product thereof with low dielectric properties. The free radical-curable polyimide oligomer is obtained by combining dimerized diamine with other monomers and adjusting the ratio. The cured product has heat resistance and excellent electrical properties.

[0006] One embodiment of the present invention provides a polyimide oligomer having a structure as shown in formula (I) or formula (II):

[0007]

[0008] Wherein, X is independently hydrogen or methyl, R1 is a cycloalkane having a total carbon number of 5 to 20 and having a carbon number of 5 or more, or a structure represented by formula (A), formula (B) or formula (C):

[0009]

[0010] R2 is independently a saturated or unsaturated hydrocarbon having 36 carbon atoms, and A is independently a benzene ring, a biphenyl ring, a naphthalene ring, a cycloalkane having 4 to 6 carbon atoms, or a structure represented by formula (a), formula (b), formula (c), formula (d), formula (e), formula (f), formula (g), formula (h) or formula (i):

[0011]

[0012] Wherein, n is any number from 0 to 10, and m / p is any number from 0.5 to 5.

[0013] According to the polyimide oligomer described in the preceding paragraph, the cycloalkanes having 5 or more carbon atoms may include a structure as shown in formula (D), formula (E) or formula (F):

[0014]

[0015] According to the polyimide oligomer described in the preceding paragraph, R2 may have a structure as shown in formula (G), formula (H), formula (I) or formula (J):

[0016]

[0017]

[0018] According to the polyimide oligomer described in the previous paragraph, it may have a structure as shown in formula (I-1) or formula (II-1):

[0019]

[0020] Another embodiment of the present invention provides a method for preparing the aforementioned polyimide oligomer, comprising performing a first dissolving step, performing a second dissolving step, performing a mixing step, and performing an adding step. The first dissolving step is to dissolve a dianhydride and a monoanhydride in a first solvent to form an anhydride solution, wherein the monoanhydride has an unsaturated double bond. The second dissolving step is to mix a dimerized diamine with a difunctional fatty amine and dissolve them in a second solvent to form a diamine solution, wherein the difunctional fatty amine has a rigid cyclic structure. The mixing step is to add the diamine solution to the anhydride solution and react at a polymerization temperature to form a mixed solution. The adding step is to add xylene to the mixed solution, and react and distill at a reaction distillation temperature to obtain the polyimide oligomer.

[0021] According to the preparation method of polyimide oligomer described in the previous paragraph, the first solvent and the second solvent can be selected from the group consisting of N,N-dimethylacetamide, N-methylpyrrolidone, dimethylformamide, anisole, dimethyl sulfoxide, cyclohexanone, and resorcinol.

[0022] According to the method for preparing the polyimide oligomer described in the previous paragraph, the polymerization temperature can be 0°C to 90°C.

[0023] According to the method for preparing the polyimide oligomer described in the preceding paragraph, the reaction distillation temperature may be 130° C. to 170° C.

[0024] According to the preparation method of the polyimide oligomer described in the preceding paragraph, the molar ratio of the dimerized diamine to the difunctional fatty amine may be 1:0.4 to 1:3.

[0025] According to the preparation method of the polyimide oligomer described in the preceding paragraph, the molar ratio of the diamine obtained by adding the diamine dimer to the difunctional fatty amine to the dianhydride can be 1.2:1 to 1.8:1.

[0026] Another embodiment of the present invention provides a cured product with low dielectric properties, which is prepared by adding a free radical initiator to the aforementioned polyimide oligomer and baking at a curing temperature.

[0027] According to the cured product with low dielectric properties described in the previous paragraph, the free radical initiator can be a peroxide, an azo initiator or a mixture thereof.

[0028] According to the cured product with low dielectric properties described in the previous paragraph, the amount of the free radical initiator added can be 0.3 weight percent to 2 weight percent of the polyimide oligomer content.

[0029] According to the cured material with low dielectric properties described in the previous paragraph, the curing temperature may be 160° C. to 240° C.

[0030] According to the cured material with low dielectric properties described in the previous paragraph, the curing temperature may be 180° C., 200° C. or 220° C.

[0031] Thus, the polyimide oligomer of the present invention is polymerized with dimer diamine as a raw material and a specific monomer without the need for a purification step, so that the molecular chain end has a reactive unsaturated double bond, can be directly free radical thermally cured, and has good heat resistance and excellent electrical performance after curing and forming, and can be used as a potential material in high-frequency circuit board applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to make the above and other objects, features, advantages and embodiments of the present invention more clearly understood, the following are the descriptions of the accompanying drawings:

[0033] Figure 1 FIG. 4 is a flow chart showing the steps of a method for preparing a polyimide oligomer according to one embodiment of the present invention. DETAILED DESCRIPTION

[0034] The following will discuss various embodiments of the present invention in more detail. However, this embodiment can be an application of various inventive concepts and can be specifically implemented in various specific scopes. The specific embodiments are for illustrative purposes only and are not limited to the scope of the disclosure.

[0035] In the present invention, the compound structure is sometimes represented by a skeleton formula, which may omit carbon atoms, hydrogen atoms, and carbon-hydrogen bonds. If the functional group is clearly drawn in the structural formula, the drawn one shall prevail.

[0036] In the present invention, "polyimide oligomer having a structure as shown in formula (I)" may be expressed as polyimide oligomer shown in formula (I) or polyimide oligomer (I) for the sake of brevity and fluency, and the representation of other compounds or groups may be deduced in the same manner.

[0037] In the present invention, if it is not particularly indicated whether a group is substituted, the group may represent a substituted or unsubstituted group. For example, "alkyl" may represent a substituted or unsubstituted alkyl group.

[0038] <Polyimide oligomer>

[0039] The present invention provides a polyimide oligomer having a structure as shown in formula (I) or formula (II):

[0040]

[0041] Wherein, X is independently hydrogen or methyl, R1 is a cycloalkane having a total carbon number of 5 to 20 and having a carbon number of 5 or more, or a structure represented by formula (A), formula (B) or formula (C):

[0042]

[0043] R2 is independently a saturated or unsaturated hydrocarbon having 36 carbon atoms. A is independently a benzene ring, a biphenyl ring, a naphthalene ring, a cycloalkane having 4 to 6 carbon atoms, or a structure represented by formula (a), formula (b), formula (c), formula (d), formula (e), formula (f), formula (g), formula (h) or formula (i):

[0044]

[0045]

[0046] Here, n is any number from 0 to 10, and m / p is any number from 0.5 to 5.

[0047] Specifically, the cycloalkanes having 5 or more carbon atoms may include a structure as shown in formula (D), formula (E) or formula (F):

[0048]

[0049] However, the present invention is not limited thereto. In addition, R2 may have a structure as shown in formula (G), formula (H), formula (I) or formula (J):

[0050]

[0051] For example, when in the polyimide oligomer represented by formula (I) or formula (II), X is hydrogen, R1 is the structure represented by formula (D), R2 is the structure represented by formula (J), and A is a benzene ring, the polyimide oligomer has a structure represented by formula (I-1) or formula (II-1):

[0052]

[0053] Thus, the polyimide oligomer of the present invention is derived from dimerized diamine, has a reactive unsaturated double bond at the end of the structure, and can be cured by free radical polymerization to form a cured product with good mechanical properties and heat resistance. Moreover, since the main structure is composed of a large number of aliphatic carbon chains, it can provide the material with good low dielectric properties and has considerable potential for application in printed circuit board materials.

[0054] <Method for preparing polyimide oligomer>

[0055] Mate Reference Figure 1 , which is a flow chart of the steps of a method 100 for preparing a polyimide oligomer according to one embodiment of the present invention. Figure 1In the present invention, the method 100 for preparing a polyimide oligomer includes step 110 , step 120 , step 130 and step 140 .

[0056] Step 110 is a first dissolution step, which is to dissolve a diacid anhydride and a monoanhydride in a first solvent to form an anhydride solution, and the monoanhydride has an unsaturated double bond to meet the subsequent free radical curing requirements. Specifically, the monoanhydride can be but is not limited to maleic anhydride or itaconic anhydride.

[0057] Step 120 is to perform a second dissolving step, which is to mix a dimerized diamine and a difunctional fatty amine and dissolve them in a second solvent to form a diamine solution, wherein the molar ratio of the dimerized diamine to the difunctional fatty amine can be 1:0.4 to 1:3, preferably 1:0.5 to 1:2. In detail, the dimerized diamine is a bio-based diamine, which is a diamine monomer derived from fatty acids, and the main structure is a multi-carbon aliphatic, and the difunctional fatty amine has a rigid cyclic structure to provide good heat resistance for subsequent free radical curing derivatives. Specifically, the difunctional fatty amine can be but is not limited to isophorone diamine or protobornene diamine.

[0058] In addition, the first solvent of step 110 and the second solvent of step 120 may be the same or different, and are selected from a group consisting of N,N-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), dimethylformamide (DMF), anisole, dimethyl sulfoxide (DMSO), cyclohexanone, and m-cresol.

[0059] Step 130 is a mixing step, which is to add the diamine solution into the anhydride solution and react at a polymerization temperature to form a mixed solution, wherein the polymerization temperature can be 0°C to 90°C, preferably 40°C to 80°C. After the diamine solution is added to the anhydride solution, polymerization is carried out at the polymerization temperature, and the molar ratio of the diamine obtained by adding the diamine to the dianhydride can be 1.2:1 to 1.8:1, preferably 1.4:1 to 1.6:1.

[0060] Step 140 is to perform an adding step, which is to add xylene to the mixed solution, and react and distill at a reaction distillation temperature to obtain polyimide oligomer, wherein the reaction distillation temperature can be 130° C. to 170° C., preferably 140° C. to 160° C. In detail, after xylene is added to the mixed solution, a Dean-Stark device is set up, and the temperature is raised to the reaction distillation temperature to perform a closed loop reaction and distillation to remove water, and the polyimide oligomer solution can be obtained after cooling, and the polyimide oligomer solution contains polyimide oligomer and solvent.

[0061] <Cured material with low dielectric properties>

[0062] The present invention provides a cured product with low dielectric properties, which is prepared by adding a free radical initiator to the aforementioned polyimide oligomer and baking at a curing temperature, wherein the free radical initiator can be a peroxide, an azo initiator or a mixture thereof, and the amount of the free radical initiator added can be 0.3 weight percent to 2 weight percent of the polyimide oligomer content, preferably 0.5 weight percent to 1.5 weight percent. In addition, the free radical curing reaction can be carried out by a step-by-step heating method, but is not limited to this heating method, and the curing temperature can be 160°C to 240°C, preferably 180°C, 200°C or 220°C.

[0063] Thus, the preparation method of the polyimide oligomer of the present invention can overcome the problem of poor thermal properties after the product is cured and maintain high-frequency and low-dielectric properties by selecting and matching amines and adjusting the proportions. In terms of process, the polyimide oligomer can be prepared without adding a catalyst due to the improvement of the selection of monomers and the feeding sequence, and can be directly used in the circuit board impregnation process, reducing the output of waste liquid and the use of solvents, so as to balance the development of the circuit board industry and the trend of carbon reduction.

[0064] The present invention is further illustrated by the following specific embodiments, which are used to facilitate those skilled in the art to which the present invention belongs, so that they can fully utilize and practice the present invention without excessive interpretation. These embodiments should not be regarded as limiting the scope of the present invention, but are used to illustrate how to implement the materials and methods of the present invention.

[0065] <Example / Comparative Example>

[0066] Example 1: 20 g (0.0917 mole) of pyromellitic anhydride (PMDA) and 8.99 g (0.0917 mole) of maleic anhydride were dissolved in 90 g of N,N-dimethylacetamide (DMAc) to prepare an anhydride solution. Then, 36.79 g (0.0688 mole) of Priamine 1075 (purchased from Croda) and 11.71 g (0.0688 mole) of isophoronediamine (IPDA) were dissolved in 73 g of N,N-dimethylacetamide to prepare a diamine solution. Afterwards, the diamine solution is slowly dripped into the anhydride solution, and the water bath temperature is controlled not to exceed 60°C. After the dripping is completed, the temperature is raised to 80°C for reaction for 3 hours. After the reaction is completed, 54 grams of xylene is added to form a mixed solution to be separated, and the polyimide oligomer solution is separated from the mixed solution to be separated by distillation. For example, the mixed solution to be separated is heated to 150°C for dehydration for 4 hours by a Dean-Stark device, and then further heated to 160°C for dehydration. After the distilled water volume reaches the expected dehydration volume, the temperature is lowered to obtain the polyimide oligomer solution of Example 1. Specifically, the polyimide oligomer in Example 1 has a structure as shown in formula (I-1), wherein m / p is 1, and after being measured by a gel chromatography permeameter (GPC), its number average molecular weight (Mn) is 2095 and its weight average molecular weight (Mw) is 4841.

[0067] Example 2: 20 grams (0.0917 mole) of pyromellitic anhydride and 8.99 grams (0.0917 mole) of maleic anhydride were dissolved in 90 grams of N,N-dimethylacetamide to prepare an anhydride solution. Then, 24.53 grams (0.0459 mole) of dimer diamine (Priamine 1075, purchased from Croda) and 15.62 grams (0.0917 mole) of isophorone diamine were dissolved in 56.54 grams of N,N-dimethylacetamide to prepare a diamine solution. After that, the diamine solution was slowly dripped into the anhydride solution, and the water bath temperature was controlled not to exceed 60°C. After the dripping was completed, the temperature was raised to 80°C for reaction for 3 hours. After the reaction was completed, 48.85 grams of xylene was added. The remaining steps were the same as those in Example 1 to obtain the polyimide oligomer solution of Example 2. Specifically, the polyimide oligomer in Example 2 has a structure as shown in formula (I-1), wherein m / p is 2, and after being measured by gel chromatography permeameter (GPC), its number average molecular weight (Mn) is 1448 and its weight average molecular weight (Mw) is 3049.

[0068] Example 3: 20 grams (0.0917 mole) of pyromellitic anhydride and 8.99 grams (0.0917 mole) of maleic anhydride were dissolved in 90 grams of N,N-dimethylacetamide (DMAc) to prepare an anhydride solution. Then, 49.05 grams (0.0917 mole) of dimer diamine (Priamine 1075, purchased from Croda) and 7.81 grams (0.0458 mole) of isophorone diamine were dissolved in 90.07 grams of N,N-dimethylacetamide to prepare a diamine solution. After that, the diamine solution was slowly dripped into the anhydride solution, and the water bath temperature was controlled not to exceed 60°C. After the dripping was completed, the temperature was raised to 80°C for reaction for 3 hours. After the reaction was completed, 60.02 grams of xylene were added. The remaining steps were the same as in Example 1 to obtain the polyimide oligomer solution of Example 3. Specifically, the polyimide oligomer in Example 3 has a structure as shown in formula (I-1), wherein m / p is 0.5, and after being measured by gel chromatography permeameter (GPC), its number average molecular weight (Mn) is 1050 and its weight average molecular weight (Mw) is 2373.

[0069] Example 4: 20 grams (0.0917 mole) of pyromellitic anhydride and 10.28 grams (0.0917 mole) of itaconic anhydride were dissolved in 90 grams of N,N-dimethylacetamide to prepare an anhydride solution. Then, 24.53 grams (0.0459 mole) of dimer diamine (Priamine 1075, purchased from Croda) and 15.62 grams (0.0917 mole) of isophorone diamine were dissolved in 56.54 grams of N,N-dimethylacetamide to prepare a diamine solution. After that, the diamine solution was slowly dripped into the anhydride solution, and the water bath temperature was controlled not to exceed 60°C. After the dripping was completed, the temperature was raised to 80°C for reaction for 3 hours. After the reaction was completed, 48.85 grams of xylene were added. The remaining steps were the same as those in Example 1 to obtain the polyimide oligomer solution of Example 4. Specifically, the polyimide oligomer in Example 4 has a structure as shown in formula (II-1), wherein m / p is 2, and after being measured by gel chromatography permeameter (GPC), its number average molecular weight (Mn) is 2235 and its weight average molecular weight (Mw) is 5669.

[0070] Comparative Example 1: 20 grams (0.0917 mole) of pyromellitic anhydride and 8.99 grams (0.0917 mole) of maleic anhydride were dissolved in 90 grams of N,N-dimethylacetamide to prepare an anhydride solution. Then, 23.42 grams (0.1375 mole) of isophorone diamine was dissolved in 24.14 grams of N,N-dimethylacetamide to prepare a diamine solution. After that, the diamine solution was slowly dripped into the anhydride solution, and the water bath temperature was controlled not to exceed 60°C. After the dripping was completed, the temperature was raised to 80°C for reaction for 3 hours. After the reaction was completed, 38.14 grams of xylene was added. The remaining steps were the same as those of Example 1 to obtain the polyimide oligomer solution of Comparative Example 1. Specifically, after the comparative example 1 was measured by gel chromatography permeameter (GPC), its number average molecular weight (Mn) was 2117 and the weight average molecular weight (Mw) was 2950.

[0071] Comparative Example 2: 20 g (0.0917 mole) of pyromellitic anhydride and 1.798 g (0.0813 mole) of maleic anhydride were dissolved in 80 g of N,N-dimethylacetamide to prepare an anhydride solution. Then, 26.98 g (0.0504 mole) of dimer diamine (Priamine 1075, purchased from Croda) and 8.59 g (0.0504 mole) of isophorone diamine were dissolved in 39.6 g of N,N-dimethylacetamide to prepare a diamine solution. Afterwards, the diamine solution was slowly dripped into the anhydride solution, and the water bath temperature was controlled not to exceed 60°C. After the dripping was completed, the temperature was raised to 80°C for reaction for 3 hours. After the reaction was completed, 39.87 grams of xylene was added. The remaining steps were the same as in Example 1. However, a large amount of salts were generated during the preparation process and were difficult to eliminate, resulting in the inability to successfully obtain the product. The reason was that the molar ratio of diamine to dianhydride was changed to 1.1:1.

[0072] Comparative Example 3: 20 g (0.0917 mole) of pyromellitic anhydride and 8.99 g (0.0917 mole) of maleic anhydride were dissolved in 90 g of N,N-dimethylacetamide to prepare an anhydride solution. Next, 36.79 g (0.0688 mole) of dimer diamine (Priamine 1075, purchased from Croda) and 11.71 g (0.0688 mole) of isophorone diamine were dissolved in 73 g of N,N-dimethylacetamide to prepare a diamine solution. Afterwards, the anhydride solution was slowly dripped into the diamine solution, but the reaction was violent during the dripping process, causing the reaction to gel rapidly and the product could not be obtained smoothly. The reason was that the diamine solution and the anhydride solution were added in a different order.

[0073] Comparative Example 4: 20 grams (0.0917 mole) of pyromellitic anhydride and 8.99 grams (0.0917 mole) of maleic anhydride were dissolved in 90 grams of N,N-dimethylacetamide to prepare an anhydride solution. Then, 73.58 grams (0.1375 mole) of diamine (Priamine 1075, purchased from Croda) was dissolved in 127.28 grams of N,N-dimethylacetamide to prepare a diamine solution. After that, the diamine solution was slowly dripped into the anhydride solution, and the water bath temperature was controlled not to exceed 60°C. After the dripping was completed, the temperature was raised to 80°C for reaction for 3 hours. After the reaction was completed, 72.43 grams of xylene was added. The remaining steps were the same as those in Example 1 to obtain the polyimide oligomer solution of Comparative Example 4. Specifically, after the comparative example 4 was measured by gel chromatography permeameter (GPC), its number average molecular weight (Mn) was 1937 and its weight average molecular weight (Mw) was 2480.

[0074] <Preparation of Cured Material>

[0075] Example 5: Add 0.015 g (1 wt% of the polyimide oligomer) of dicumyl peroxide (DCP) to 5 g of the polyimide oligomer solution of Example 1 (solid content 30%, solvent: DMAc) to prepare a prepolymer solution, which is then poured into a mold and slowly heated to 80°C to 140°C for baking to remove the solvent. The solution is then further heated to cure. The curing procedure is a staged heating process. This example is a three-stage curing process, which is performed at 180°C, 200°C, and 220°C for 2 hours each to obtain the cured product of Example 5.

[0076] Example 6: Add 0.015 g (1 wt% of the polyimide oligomer) of diisopropylbenzene peroxide to 5 g of the polyimide oligomer solution of Example 2 (solid content 30%, solvent: DMAc) to prepare a prepolymer solution, which is then poured into a mold. The remaining steps are the same as those of Example 5 to obtain the cured product of Example 6.

[0077] Example 7: Add 0.015 g (1 wt% of the polyimide oligomer) of diisopropylbenzene peroxide to 5 g of the polyimide oligomer solution of Example 3 (solid content 30%, solvent: DMAc) to prepare a prepolymer solution, which is then poured into a mold. The remaining steps are the same as in Example 5 to obtain the cured product of Example 7.

[0078] Example 8: Add 0.015 g (1 wt% of the polyimide oligomer) of diisopropylbenzene peroxide to 5 g of the polyimide oligomer solution of Example 4 (solid content 30%, solvent: DMAc) to prepare a prepolymer solution, which is then poured into a mold. The remaining steps are the same as in Example 5 to obtain the cured product of Example 8.

[0079] Comparative Example 5: 5 g of the polyimide oligomer solution of Comparative Example 1 (solid content 30%, solvent DMAc) was added with 0.015 g (1 wt% of the polyimide oligomer) of diisopropylbenzene peroxide to prepare a prepolymer solution, which was then poured into a mold. The remaining steps were the same as those in Example 5 to obtain the cured product of Comparative Example 5, but it had severe foaming and high brittleness, and a complete film could not be successfully prepared.

[0080] Comparative Example 6: 5 g of the polyimide oligomer solution of Comparative Example 4 (solid content 30%, solvent DMAc) was added with 0.015 g (1 wt% of the polyimide oligomer) of diisopropylbenzene peroxide to prepare a prepolymer solution, which was then poured into a mold. The remaining steps were the same as in Example 5 to obtain the cured product of Comparative Example 6.

[0081] Comparative Example 7: 5 g of polyphenylene ether resin (NorylSA 9000, purchased from SABIC) was added with 0.015 g of diisopropylbenzene peroxide to prepare a prepolymer solution, which was then poured into a mold. The remaining steps were the same as those in Example 5 to obtain a cured product of Comparative Example 7.

[0082] <Evaluation Test Method>

[0083] Glass transition temperature (T g ): A dynamic mechanical analyzer (DMA) was used to measure the glass transition temperature of the cured product, and the test was performed at a heating rate of 5°C / min.

[0084] Dielectric analysis method: In order to evaluate the dielectric properties of the cured product obtained by curing the polyimide oligomer of the present invention, the dielectric constant (D k ) and dielectric loss (D f ).

[0085] The above evaluation test method was performed on Examples 5 to 8 and Comparative Examples 6 to 7, and the results were recorded in Table 1.

[0086]

[0087] From the results in Table 1 above, it can be seen that after the polyimide oligomers of Examples 1 to 4 are cured by free radicals, the glass transition temperatures of the cured products of Examples 5 to 8 obtained are all higher than 100°C, and as the amount of rigid isophorone diamine used increases, the glass transition temperatures of Examples 6 and 8 can reach above 180°C. Although the heat resistance is poorer than that of Comparative Example 7 prepared by the currently widely used polyphenylene ether resin SA 9000, the heat resistance of the cured products of Examples 5 to 8 is indeed significantly improved compared to the cured product of Comparative Example 6 without adding rigid isophorone diamine.

[0088] In addition, the cured products of Examples 5 to 8 can show better insulation properties than Comparative Example 7 made of the currently widely used polyphenylene ether resin SA 9000 under high-frequency measurement. For Example 6 with the best heat resistance, its dielectric constant (D k ) can show a level similar to that of Comparative Example 7, but the dielectric loss (D f However, as the amount of diamine used increases, the resulting cured product can exhibit better insulation properties. For Example 7, in which the amount of diamine used is the highest, its dielectric constant (D k ) can reach 2.21, dielectric loss (D f ) can reach 0.0027, showing excellent electrical performance and can be used in the production of high-frequency printed circuit boards.

[0089] In addition, the dielectric constant (D k ) is not better than Example 7, but the dielectric loss (D f ) can be further optimized to 0.0018, indicating that the diamine structure has a certain effect on the dielectric constant (D k ) will gradually decrease, and the contribution of dielectric loss (D f ) can be further improved, but in terms of heat resistance, the heat resistance of Comparative Example 6 will also be greatly reduced, which limits its application in circuit boards with heat resistance requirements.

[0090] In summary, the polyimide oligomer of the present invention, which uses dimerized diamine as a raw material and is combined with a rigid bifunctional diamine monomer, does improve the problem of heat resistance and allows the material to retain good electrical properties, and even exhibits better electrical properties than the polyphenylene ether resin currently widely used in the industry. This shows that the polyimide oligomer proposed by the present invention has its application potential in the circuit board industry and can improve the environmental problems caused by material development.

[0091] Although the present invention has been disclosed in the above embodiments, it is not intended to limit the present invention. Anyone skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the following claims.

[0092] Explanation of symbols:

[0093] 100: Preparation method of polyimide oligomer

[0094] 110,120,130,140: Steps

Claims

1. A polyimide oligomer, characterized in that: Having a structure as shown in formula (I) or formula (II): Wherein, X is independently hydrogen or methyl, R1 is a cycloalkane having a total carbon number of 5 to 20 and having a carbon number of 5 or more, or a structure represented by formula (A), formula (B) or formula (C): R2 is independently a saturated or unsaturated hydrocarbon having 36 carbon atoms, and A is independently a benzene ring, a biphenyl ring, a naphthalene ring, a cycloalkane having 4 to 6 carbon atoms, or a structure represented by formula (a), formula (b), formula (c), formula (d), formula (e), formula (f), formula (g), formula (h) or formula (i): Wherein, n is any number from 0 to 10, and m / p is any number from 0.5 to 5.

2. The polyimide oligomer according to claim 1, wherein The cycloalkanes having 5 or more carbon atoms include a structure represented by formula (D), formula (E) or formula (F):

3. The polyimide oligomer according to claim 1, wherein R2 has a structure as shown in formula (G), formula (H), formula (I) or formula (J):

4. The polyimide oligomer according to claim 1, wherein Having a structure as shown in formula (I-1) or formula (II-1):

5. A method for preparing a polyimide oligomer as claimed in claim 1, characterized in that: Include: A first dissolving step is performed, wherein a dianhydride and a monoanhydride are dissolved in a first solvent to form an anhydride solution, wherein the monoanhydride has an unsaturated double bond; A second dissolving step is performed, wherein a dimerized diamine and a difunctional fatty amine are mixed and dissolved in a second solvent to form a diamine solution, wherein the difunctional fatty amine has a rigid cyclic structure; performing a mixing step, which is to add the diamine solution into the anhydride solution and react at a polymerization temperature to form a mixed solution; and An adding step is performed, in which xylene is added to the mixed solution, and the mixture is reacted and distilled at a reaction distillation temperature to obtain the polyimide oligomer.

6. The method for preparing a polyimide oligomer according to claim 5, characterized in that: The first solvent and the second solvent are selected from a group consisting of N,N-dimethylacetamide, N-methylpyrrolidone, dimethylformamide, anisole, dimethyl sulfoxide, cyclohexanone, and resorcinol.

7. The method for preparing a polyimide oligomer according to claim 5, characterized in that: The polymerization temperature is from 0°C to 90°C.

8. The method for preparing a polyimide oligomer according to claim 5, characterized in that: The reaction distillation temperature is 130°C to 170°C.

9. The method for preparing a polyimide oligomer according to claim 5, characterized in that: The molar ratio of the dimerized diamine to the difunctional fatty amine is 1:0.4 to 1:

3.

10. The method for preparing a polyimide oligomer according to claim 5, characterized in that: The molar ratio of the diamine obtained by adding the diamine to the difunctional fatty amine to the dianhydride is 1.2:1 to 1.8:

1.

11. A cured product with low dielectric properties, characterized in that: The polyimide oligomer is prepared by adding a free radical initiator to the polyimide oligomer according to any one of claims 1 to 4 and baking the polyimide oligomer at a curing temperature.

12. The cured product with low dielectric properties according to claim 11, wherein: The free radical initiator is a peroxide, an azo initiator or a mixture thereof.

13. The cured product with low dielectric properties according to claim 11, wherein: The amount of the free radical initiator added is 0.3 weight percent to 2 weight percent of the polyimide oligomer content.

14. The cured product with low dielectric properties according to claim 11, wherein: The curing temperature is 160°C to 240°C.

15. The cured product with low dielectric properties according to claim 14, wherein: The curing temperature is 180°C, 200°C or 220°C.