EPDM composition

By adding liquid polybutadiene and terpene resin to the EPDM composition, the problems of arching and reduced biomass quality in plant-derived components were solved, achieving good roll processability and maintenance of biomass quality.

CN118931048APending Publication Date: 2024-11-12NOK CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410568840.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-11
Filing Date
2024-05-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In EPDM compositions using at least some plant-derived components, existing technologies struggle to simultaneously suppress arching and maintain biomass density.

Method used

By adding liquid polybutadiene and terpene resin containing plant-derived components to the EPDM composition, the roll processability is improved and the biomass quality is maintained. Specifically, the ratio is 1 to 12 parts by weight of liquid polybutadiene and 1 to 12 parts by weight of terpene resin.

Benefits of technology

While suppressing arching during roll mixing, the biomass particle size variation rate of EPDM is kept within ±1.5%, achieving good roll workability and biomass particle size maintenance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004830234000000051
    Figure BDA0004830234000000051
  • Figure BDA0004830234000000071
    Figure BDA0004830234000000071
  • Figure BDA0004830234000000072
    Figure BDA0004830234000000072
Patent Text Reader

Abstract

The present application relates to an EPDM composition in which 1-12 parts by weight of a liquid polybutadiene and 1-12 parts by weight of a terpene resin containing a plant-derived component are blended with respect to 100 parts by weight of an ethylene-propylene-diene tripolymer containing a plant-derived component. According to the EPDM composition, liquid polybutadiene is added to EPDM (the liquid polybutadiene has good compatibility with the EPDM, and the viscosity of a blank can be reduced, so that the roller processability can be improved), and the EPDM composition can be used for producing a plant-derived component with a small environmental burden in at least a part of the EPDM. Further, a specific amount of a terpene resin containing a plant-derived component is used (suppressing an unavoidable decrease in biomass degree due to the addition of the liquid polybutadiene), whereby the occurrence of arching during roll kneading is suppressed and the biomass degree of the obtained EPDM is maintained, and specifically, the biomass degree of the EPDM is maintained. Compared with a composition in which liquid polybutadiene is not added and a terpene resin containing a plant-derived component, the composition has the advantages that the change rate of the biomass degree is less than + / -1.5%, and the effect is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an EPDM composition, and more particularly to an EPDM composition that can be effectively used as a vulcanization molding material such as a sealing material and a vibration-proof rubber. Background Art

[0002] Ethylene-propylene-diene terpolymer rubber (EPDM) has excellent heat resistance due to its polymer structure and is widely used as a vulcanization molding material for industrial parts.

[0003] Among these various parts, gaskets and valves in particular require good compression set resistance, so peroxide crosslinking is used. Here, since the peroxide crosslinking system has a short crosslinking induction time and a fast rise rate during crosslinking, it is necessary to add a plasticizer to improve its poor molding in products that require fluidity such as complex shapes and thin shapes.

[0004] As the above-mentioned EPDM composition, the applicant has previously proposed a sealing rubber composition, which satisfies molding processability and exhibits good compression set resistance in a crosslinked product, wherein the rubber composition comprises 32 to 60 parts by weight of (A) carbon black A having an average particle size of 60 to 100 nm, an iodine adsorption of 14 to 23 g / kg, and a DBP oil absorption of 100 ml / 100 g or more, 10 to 30 parts by weight of (B) carbon black B having an average particle size of 40 to 50 nm, an iodine adsorption of 35 to 49 g / kg, and a DBP oil absorption of 100 to 160 ml / 100 g, 2 to 10 parts by weight of (C) an ethylene-α-olefin copolymer, and 0 to 16 parts by weight of (D) silica, relative to 100 parts by weight of ethylene-propylene-diene copolymer rubber (Patent Document 1).

[0005] On the other hand, in recent years, in order to realize a sustainable society, plant-derived raw materials that absorb and fix carbon dioxide during their production process are superior to petroleum-based raw materials in that they do not change the total amount of carbon dioxide in the atmosphere and can be recycled, and are non-depletable raw materials, so their active use is considered to be extremely important.

[0006] Based on this viewpoint, there is a strong demand for the use of plant-derived raw materials also in rubber compositions, particularly EPDM compositions that are commonly used in sealing materials, anti-vibration rubbers, and the like.

[0007] In the rubber composition using EPDM, when the processability (hereinafter referred to as roller processability) is poor when the mixing operation is usually carried out with an open roller, the rubber wound on the roller is peeled off from the surface, and so-called bagging occurs. In order to suppress this bagging, a mineral oil plasticizer with good compatibility with EPDM is usually added. However, when using EPDM in which at least a portion of plant-derived components are used, the mineral oil plasticizer causes the biomass degree of the rubber composition to decrease. Therefore, it is required to maintain the biomass degree while suppressing the occurrence of bagging.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2023-30734 Summary of the invention

[0011] Technical problem to be solved by the invention

[0012] An object of the present invention is to provide an EPDM composition in which at least a part of the EPDM composition contains plant-derived components, the occurrence of cambering can be suppressed, and the biomass degree of the obtained EPDM can be maintained.

[0013] Means for solving problems

[0014] The above-mentioned object of the present invention is achieved by an EPDM composition, wherein 1 to 12 parts by weight of liquid polybutadiene and 1 to 12 parts by weight of a terpene resin containing a plant-derived component are blended with 100 parts by weight of an ethylene-propylene-diene terpolymer containing a plant-derived component.

[0015] Effects of the Invention

[0016] The EPDM composition of the present invention adds liquid polybutadiene to at least a portion of EPDM containing plant-derived components with low environmental impact (the liquid polybutadiene has good compatibility with the EPDM and reduces the viscosity of the billet, thereby improving roll processability), and further uses a specific amount of a terpene resin containing plant-derived components (suppressing the inevitable decrease in biomass due to the addition of the liquid polybutadiene). As a result, the biomass of the obtained EPDM is maintained while suppressing the occurrence of camber during roll kneading. Specifically, compared with a composition to which no liquid polybutadiene and no terpene resin containing plant-derived components are added, the change rate of the biomass is less than ±1.5%, thereby achieving excellent effects. DETAILED DESCRIPTION

[0017] As EPDM, EPDM obtained by copolymerizing various non-conjugated diene components with ethylene and propylene containing at least a part of plant-derived components, specifically 40 to 80% by weight of plant-derived components, is used. Here, as plant-derived components, ethylene refined from sugar cane and the like can be cited. As such EPDM, for example, commercially available products such as Keltan ECO 6950 (ratio of ethylene refined from sugar cane: 48% by weight), 5470 (ratio of ethylene refined from sugar cane: 70% by weight), and 8550 (ratio of ethylene refined from sugar cane: 55% by weight) of ARLANXEO can be used directly. As non-conjugated dienes, ethylidene norbornene (ENB), dicyclopentadiene (DCPD), and 1,4-hexadiene (HD) can be cited.

[0018] As liquid polybutadiene, a liquid polybutadiene having a 1,2-vinyl content of 25% by weight or more, preferably 28 to 99% by weight, is used. As a plasticizer, if other types of plasticizers or plasticizers having a 1,2-vinyl content less than this range are used, the desired molding processability cannot be satisfied. In fact, commercially available products such as NISSO-PB series of Nippon Soda and RICON series of Crayvalley can be used directly.

[0019] Liquid polybutadiene is used in a ratio of 1 to 12 parts by weight, preferably 2 to 10 parts by weight, per 100 parts by weight of EPDM. If the liquid polybutadiene is used in a ratio exceeding this range, the roll processability may be deteriorated due to the sticking of the blank during kneading. On the other hand, if the liquid polybutadiene is used in a ratio less than this range, the Mooney viscosity ML 1+4 (125℃) will become greater than 65, resulting in arching.

[0020] As the terpene resin containing plant-derived ingredients, a terpene resin containing at least a part of plant-derived ingredients, for example, a terpene resin obtained by further refining turpentine or orange oil obtained by refining from plants such as pine trees or orange peels, can be used. As the terpene resin containing plant-derived ingredients, for example, a YS resin series such as YS resin 105 (plant-derived ingredients: 70 wt%) produced by YASUHARA CHEMICAL is used in a ratio of 1 to 12 parts by weight, preferably 2 to 10 parts by weight, per 100 parts by weight of EPDM. If the terpene resin containing plant-derived ingredients is used in a ratio exceeding this range, deterioration in roll processability due to sticking of the blank is observed during kneading. On the other hand, if it is used in a ratio less than this range, the Mooney viscosity ML 1+4 (125°C) becomes greater than 65, bulging occurs, and it may be difficult to suppress the reduction of the biomass degree.

[0021] By using a terpene resin containing a plant-derived component, it is possible to compensate for the biomass content that is inevitably reduced due to the addition of liquid polybutadiene, and it is possible to suppress the occurrence of bulging during roll kneading while maintaining the biomass content of the resulting EPDM.

[0022] In the EPDM composition composed of the above essential components, an organic peroxide is blended as a crosslinking agent. Examples of the organic peroxide include tert-butyl peroxide, diisopropylbenzene peroxide, tert-butylisopropylbenzene peroxide, 1,1-di(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 1,3-di(tert-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, tert-butyl peroxybenzoate, tert-butylperoxyisopropyl carbonate, and n-butyl-4,4-di(tert-butylperoxy)valerate.

[0023] These organic peroxides are used in a ratio of about 1 to 8 parts by weight, preferably about 2 to 7 parts by weight, per 100 parts by weight of EPDM. If the mixing ratio is below this range, sufficient crosslinking density cannot be obtained, and heat resistance and compression set resistance characteristics deteriorate. On the other hand, if the ratio is used above this range, foaming occurs and a crosslinked molded product cannot be obtained.

[0024] In addition to the above components, various compounding agents commonly used in the rubber industry, such as fillers or reinforcing agents such as carbon black and silica, oxides or hydroxides of divalent metals such as zinc oxide and magnesium oxide, acid acceptors such as hydrotalcite, plasticizers other than liquid polybutadiene, and antioxidants, may be appropriately added to the composition within a range that does not impair the physical properties.

[0025] The composition can be prepared by kneading using a closed mixer or the like, and crosslinked by press vulcanization at about 150 to 220° C. for about 1 to 20 minutes and, if necessary, oven vulcanization (secondary vulcanization) at about 120 to 200° C. for about 0.1 to 20 hours.

[0026] Example

[0027] Next, the present invention will be described with reference to examples.

[0028] Example 1

[0029]

[0030] The above components were kneaded with a kneader and an open roll, and the kneaded product was crosslinked at 180°C at a crosslinking rate of t90×1.5 seconds, followed by post-curing at 150°C for 15 hours to obtain a test piece with a thickness of 2 mm.

[0031] Example 2

[0032] In Example 1, the amount of liquid polybutadiene was changed to 5 parts by weight, and the amount of terpene resin was changed to 2 parts by weight.

[0033] Example 3

[0034] In Example 1, the amount of liquid polybutadiene was changed to 5 parts by weight.

[0035] Example 4

[0036] In Example 1, the amounts of liquid polybutadiene and terpene resin were changed to 5 parts by weight and 10 parts by weight, respectively.

[0037] Example 5

[0038] In Example 1, the amount of liquid polybutadiene was changed to 10 parts by weight.

[0039] Example 6

[0040] In Example 1, the amounts of liquid polybutadiene and terpene resin were changed to 10 parts by weight and 10 parts by weight, respectively.

[0041] Comparative Example 1

[0042] In Example 1, liquid polybutadiene and terpene resin were not used.

[0043] Comparative Example 2

[0044] In Comparative Example 1, an equal amount (100 parts by weight) of EPDM containing no plant-derived component (Keltan 6950, a product of ARLANXEO) was used as EPDM.

[0045] Comparative Example 3

[0046] In Comparative Example 1, 10 parts by weight of a plasticizer (PW-380 manufactured by Idemitsu Kosan) was further used.

[0047] Comparative Example 4

[0048] In Comparative Example 2, 10 parts by weight of a plasticizer (PW-380 manufactured by Idemitsu Kosan) was further used.

[0049] Comparative Example 5

[0050] In Example 1, no terpene resin was used.

[0051] Comparative Example 6

[0052] In Example 5, no terpene resin was used.

[0053] Comparative Example 7

[0054] In Example 1, no liquid polybutadiene was used.

[0055] Comparative Example 8

[0056] In Example 4, no liquid polybutadiene was used.

[0057] Comparative Example 9

[0058] In Example 1, the amount of liquid polybutadiene was changed to 15 parts by weight.

[0059] Comparative Example 10

[0060] In Example 2, the amount of the terpene resin was changed to 20 parts by weight.

[0061] The kneaded products or test pieces obtained in the above examples and comparative examples were tested for roll processability, Mooney viscosity ML 1+4 , evaluation, determination and calculation of biomass density and normal physical properties.

[0062] Roll processability: Kneading was performed using a 10-inch open roll with a gap of 4 mm at a speed of 14 rpm for the front roll and 17 rpm for the rear roll, and the following criteria were used for evaluation:

[0063] ○: No problem, mixing can be done with rollers

[0064] ×: Difficult to mix due to arching

[0065] *: The blank sticks to the roller and is difficult to mix.

[0066] Mooney viscosity ML 1+4 :JIS K6300 standard corresponding to ISO 289 (125℃)

[0067] Biomass content: The content ratio of plant-derived ingredients (weight %), calculated by the following formula

[0068] {Weight of plant-derived components in EPDM composition (g) / weight of EPDM composition (g)}×100

[0069] Normal physical properties: The results obtained according to JIS K6253 corresponding to ISO 7619-1 and JIS K6251 corresponding to ISO 37 are shown in the following Tables 1 and 2.

[0070] Table 1

[0071]

[0072] Table 2

[0073]

[0074] Based on the above results, it is considered as follows:

[0075] (1) The EPDM composition obtained in each example has good processability during kneading, suppresses the occurrence of camber, and maintains the biomass content of the obtained EPDM.

[0076] (2) If liquid polybutadiene and / or terpene resin is not used, the Mooney viscosity ML 1+4 (125°C) became greater than 65, causing arching (Comparative Examples 1 to 2, 5, 7 to 8).

[0077] (3) Even without using liquid polybutadiene and terpene resin, by adding plasticizer, Mooney viscosity ML 1+4 (125°C) may be 65 or less, and the occurrence of bulging can be suppressed, and roll processability is also good, but a decrease in biomass degree cannot be avoided (Comparative Example 3).

[0078] (4) If the terpene resin is not used, a decrease in the biomass content cannot be avoided (Comparative Example 6).

[0079] (5) Even when using terpene resin containing plant-derived ingredients, if liquid polybutadiene is not used, the Mooney viscosity ML 1+4 (125°C) also becomes greater than 65, causing arching (Comparative Examples 1 to 2, 5, 7 to 8).

[0080] (6) Even when liquid polybutadiene or terpene resin containing plant-derived components is used, if it is used in a ratio exceeding a predetermined amount, deterioration in roll processability due to sticking of the blank during kneading is observed (Comparative Examples 9 and 10).

Claims

1. An EPDM composition, It is characterized in that 1 to 12 parts by weight of liquid polybutadiene and 1 to 12 parts by weight of terpene resin containing plant-derived components are blended with 100 parts by weight of ethylene-propylene-diene ternary copolymer containing plant-derived components.

2. The EPDM composition according to claim 1, in, The plant-derived ingredient is ethylene refined from sugar cane.

3. The EPDM composition according to claim 1 or 2, in, Ethylene containing 40 to 80% by weight of a plant-derived component is used as a copolymerization component.

4. The EPDM composition according to claim 1, in, Liquid polybutadiene having a 1,2-vinyl content of 25% by weight or more is used.

5. The EPDM composition according to claim 1, in, The terpene resin containing plant-derived ingredients is obtained by further refining turpentine oil or orange oil refined from plants.

6. The EPDM composition according to claim 1, in, Compared with the composition to which no liquid polybutadiene was added and the composition containing the terpene resin of plant origin, the change rate of the biomass degree was less than ±1.5%.

7. The EPDM composition according to claim 1, in, Mooney viscosity ML 1+4 (125°C) is 65 or less.

8. A vulcanized product, It is characterized in that A vulcanized molded product of the EPDM composition according to claim 1.

9. The vulcanized molded article according to claim 8, which is a sealing material or a vibration-proof rubber.