Special rubber material for high-performance pavement deceleration strip, preparation equipment and preparation method of special rubber material
By using high-performance rubber materials with ethylene-propylene rubber and other components and a double-stage mixing process, the problem of insufficient heat-resistant aging performance of existing rubber speed bumps in high temperature environments is solved, and the material's heat-resistant aging and ozone resistance is improved , suitable for a variety of environments and extends service life.
Patent Information
- Application Number
- CN202411011823.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
The existing rubber speed bumps have poor heat-resistant aging performance in high temperature environments, which affects their service life and traffic safety.
High-performance rubber materials using ethylene-propylene rubber, carbon black, environmentally friendly paraffin oil, zinc oxide, stearic acid, sulfur and environmentally friendly sulfur carriers, and improve the materials through the dual-stage mixing process of mixer and stirrer equipment. Thermal aging resistance and ozone resistance.
It achieves high-performance rubber materials with excellent high-temperature resistance and strong thermal aging resistance. It is suitable for a variety of environments, extends the service life of speed bumps and improves traffic safety.
Smart Images

Figure CN118931049A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of rubber technology, and in particular to a high-performance rubber material specially used for road speed bumps, a preparation device and a method thereof. Background Art
[0002] A speed bump is a raised strip or dot structure on the road surface. It is used to warn drivers to slow down in areas prone to traffic accidents. It is mainly made of metal, concrete, rubber, etc., and the surface is generally sprayed with black or yellow paint.
[0003] Compared with metal and concrete speed bumps, rubber speed bumps have better shock absorption, excellent compression resistance, less wear on tires, and less vibration on the frame, which greatly improves the driver's comfort and reduces the impact of vehicles on the road. In addition, they produce less noise and have a longer service life, making them very suitable for paving roads in densely populated areas such as schools, residences, and hospitals.
[0004] There are more and more vehicles in cities, and traffic accidents happen from time to time. Speed bumps, as a new type of special facility to improve traffic safety, can not only buffer and decelerate, improve traffic safety, but also have little impact on drivers and the surrounding environment.
[0005] In the prior art, speed bump rubber is mostly made of natural rubber, which has poor heat aging resistance. Especially in summer, when the road surface temperature is high, it will seriously affect its service life and become a safety hazard. For this reason, we propose a high-performance road speed bump special rubber material, preparation equipment and method thereof to solve the above problems. Summary of the invention
[0006] The object of the present invention is to provide a high-performance rubber material specially used for road speed bumps, a preparation device and a method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0007] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a high-performance rubber material specially used for road speed bumps, whose components, by mass, are as follows: 100 parts of ethylene-propylene rubber, 75-90 parts of carbon black, 0-40 parts of light calcium carbonate, 30-45 parts of environmentally friendly paraffin oil, 0-2 parts of microcrystalline paraffin, 5-10 parts of zinc oxide, 1 part of stearic acid, 0-2 parts of operating aid, 0.5-1 part of sulfur, 0.5-1.5 parts of environmentally friendly sulfur carrier CLD, and 1.9-2.5 parts of accelerators TT, CZ, and BZ in total.
[0008] The raw materials include, by mass: 60 parts of ethylene propylene rubber KEP570, 40 parts of ethylene propylene rubber KEP350, 65 parts of carbon black N550, 25 parts of carbon black N330, 45 parts of environmentally friendly paraffin oil, 1 part of microcrystalline paraffin, 5 parts of zinc oxide, 1 part of stearic acid, 1 part of operating aid, 0.5 parts of sulfur, 1.5 parts of environmentally friendly sulfur carrier CLD, and 2 parts of accelerators TT, CZ, and BZ.
[0009] The raw materials include, by mass: 60 parts of ethylene propylene rubber KEP570, 40 parts of ethylene propylene rubber KEP350, 75 parts of carbon black N550, 35 parts of environmentally friendly paraffin oil, 7 parts of zinc oxide, 1 part of stearic acid, 1 part of operating aid, 0.8 parts of sulfur, 1.2 parts of environmentally friendly sulfur carrier CLD, and 2 parts of accelerators TT, CZ, and BZ.
[0010] The raw materials include, by mass: 100 parts of ethylene propylene rubber KEP350, 80 parts of carbon black N550, 30 parts of environmentally friendly paraffin oil, 2 parts of microcrystalline paraffin, 10 parts of zinc oxide, 1 part of stearic acid, 1 part of operating aid, 1 part of sulfur, 1 part of environmentally friendly sulfur carrier CLD, and 1.9 parts of accelerators TT, CZ, and BZ.
[0011] The raw materials include, by mass: 60 parts of ethylene propylene rubber KEP570, 40 parts of ethylene propylene rubber KEP350, 65 parts of carbon black N550, 25 parts of carbon black N330, 40 parts of light calcium carbonate, 35 parts of environmentally friendly paraffin oil, 1 part of microcrystalline paraffin, 5 parts of zinc oxide, 1 part of stearic acid, 2 parts of operating aid, 0.5 parts of sulfur, 1.5 parts of environmentally friendly sulfur carrier CLD, and 2.5 parts of accelerators TT, CZ, and BZ.
[0012] The environmentally friendly paraffin oil is TUDALEN 16.
[0013] A method for preparing a high-performance rubber material for road speed bumps, comprising the following steps:
[0014] S1, the first stage of mixing, ethylene propylene rubber, microcrystalline wax, zinc oxide, stearic acid, and operating aids are put into an internal mixer and mixed for about 60 seconds, and then carbon black, environmentally friendly paraffin oil, and calcium carbonate are added and mixed to about 150°C for sheeting;
[0015] S2, the second mixing stage, adding the accelerator and the remaining raw materials to the material mixed in the previous stage, mixing for the second time, mixing thoroughly, mixing again after cleaning, and obtaining a high-performance rubber material for road speed bumps after sufficient dispersion.
[0016] A preparation device for high-performance rubber materials specially used for road speed bumps, comprising an internal mixer, a base plate arranged at the bottom of the internal mixer for installing the internal mixer, and an agitator, wherein the base plate is provided with a slide groove, a bracket is slidably engaged in the slide groove, a stirring seat is connected to one end of the bracket away from the slide groove, an agitator for stirring materials is provided on the stirring seat, and a sealing plate for movably sealing an opening at the bottom of the stirring seat is provided below the stirring seat.
[0017] A telescopic rod for pushing the bracket to move is arranged in the slide groove, the bracket is an L-shaped bracket, and the length of the bracket and the telescopic length of the telescopic rod are both greater than the length of the sealing plate.
[0018] The stirring seat is a pipe pile structure, and the bottom of the stirring seat and the top of the sealing plate are both provided with anti-stick and wear-resistant coatings. The sealing plate is arranged on one side of the internal mixer feed port, and the top of the sealing plate is on the same horizontal plane as the top of the internal mixer feed port.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. It has excellent high and low temperature resistance, strong heat aging resistance, strong ozone resistance, suitable for a variety of different environments, and suitable for use as a rubber material for road speed bumps.
[0021] 2. Pour the material into the mixing base, and use the sealing plate to limit the falling of the material in the mixing base. Start the agitator to mix the material in the mixing base. After mixing, drive the telescopic rod, and the telescopic rod extends to push the bracket to slide in the slide. The bracket moves and pushes the mixing base to move on the sealing plate. When the mixing base moves to the feed inlet of the internal mixer, the bottom of the mixing base and the sealing plate are gradually separated, and the gap between the mixing base and the sealing plate is gradually expanded. The material enters the internal mixer through the opening at the bottom of the mixing base for processing, so that the material can be pre-mixed, which improves the mixing effect of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the structure of the present invention.
[0023] In the figure: 1. internal mixer; 2. bottom plate; 3. slide; 4. bracket; 5. telescopic rod; 6. stirring seat; 7. stirrer; 8. sealing plate. DETAILED DESCRIPTION
[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] A high-performance rubber material specially used for road speed bumps. The rubber material has the following components by mass: 100 parts of ethylene-propylene rubber, 75-90 parts of carbon black, 0-40 parts of light calcium carbonate, 30-45 parts of environmentally friendly paraffin oil, 0-2 parts of microcrystalline paraffin, 5-10 parts of zinc oxide, 1 part of stearic acid, 0-2 parts of operating aid, 0.5-1 part of sulfur, 0.5-1.5 parts of environmentally friendly sulfur carrier CLD, and 1.9-2.5 parts of accelerators TT, CZ, and BZ in total.
[0026] Ethylene propylene rubber KEP570 uses medium-high ethylene EPDM as the main rubber, which makes the rubber have excellent heat aging resistance, low temperature resistance and ozone aging resistance, and no additional antioxidant is needed, so that the surface of the final product is bright and colorful. Carbon black mainly uses N550 to improve the physical and mechanical properties of the rubber. The environmentally friendly paraffin oil is TUDALEN 16. The use of environmentally friendly paraffin oil improves the process operation performance of the rubber and improves the processing technology of the later stage. The vulcanization system using sulfur and environmentally friendly sulfur carrier CLD further improves the heat aging resistance of the rubber and gives the rubber good elasticity.
[0027] Example 1
[0028] The raw materials include, by mass: 60 parts of ethylene propylene rubber KEP570, 40 parts of ethylene propylene rubber KEP350, 65 parts of carbon black N550, 25 parts of carbon black N330, 45 parts of environmentally friendly paraffin oil, 1 part of microcrystalline paraffin, 5 parts of zinc oxide, 1 part of stearic acid, 1 part of operating aid, 0.5 parts of sulfur, 1.5 parts of environmentally friendly sulfur carrier CLD, and 2 parts of accelerators TT, CZ, and BZ.
[0029] Ethylene propylene rubber KEP570 uses medium-high ethylene EPDM as the main rubber, which makes the rubber have excellent heat aging resistance, low temperature resistance and ozone aging resistance, and no additional antioxidant is needed, so that the surface of the final product is bright and colorful. Carbon black mainly uses N550 to improve the physical and mechanical properties of the rubber. The environmentally friendly paraffin oil is TUDALEN 16. The use of environmentally friendly paraffin oil improves the process operation performance of the rubber and improves the processing technology of the later stage. The vulcanization system using sulfur and environmentally friendly sulfur carrier CLD further improves the heat aging resistance of the rubber and gives the rubber good elasticity.
[0030] Example 2
[0031] The raw materials include, by mass: 60 parts of ethylene propylene rubber KEP570, 40 parts of ethylene propylene rubber KEP350, 75 parts of carbon black N550, 35 parts of environmentally friendly paraffin oil, 7 parts of zinc oxide, 1 part of stearic acid, 1 part of operating aid, 0.8 parts of sulfur, 1.2 parts of environmentally friendly sulfur carrier CLD, and 2 parts of accelerators TT, CZ, and BZ.
[0032] Ethylene propylene rubber KEP570 uses medium-high ethylene EPDM as the main rubber, which makes the rubber have excellent heat aging resistance, low temperature resistance and ozone aging resistance, and no additional antioxidant is needed, so that the surface of the final product is bright and colorful. Carbon black mainly uses N550 to improve the physical and mechanical properties of the rubber. The environmentally friendly paraffin oil is TUDALEN 16. The use of environmentally friendly paraffin oil improves the process operation performance of the rubber and improves the processing technology of the later stage. The vulcanization system using sulfur and environmentally friendly sulfur carrier CLD further improves the heat aging resistance of the rubber and gives the rubber good elasticity.
[0033] Example 3
[0034] The raw materials include, by mass: 100 parts of ethylene propylene rubber KEP350, 80 parts of carbon black N550, 30 parts of environmentally friendly paraffin oil, 2 parts of microcrystalline paraffin, 10 parts of zinc oxide, 1 part of stearic acid, 1 part of operating aid, 1 part of sulfur, 1 part of environmentally friendly sulfur carrier CLD, and 1.9 parts of accelerators TT, CZ, and BZ.
[0035] Ethylene propylene rubber KEP570 uses medium-high ethylene EPDM as the main rubber, which makes the rubber have excellent heat aging resistance, low temperature resistance and ozone aging resistance, and no additional antioxidant is needed, so that the surface of the final product is bright and colorful. Carbon black mainly uses N550 to improve the physical and mechanical properties of the rubber. The environmentally friendly paraffin oil is TUDALEN 16. The use of environmentally friendly paraffin oil improves the process operation performance of the rubber and improves the processing technology of the later stage. The vulcanization system using sulfur and environmentally friendly sulfur carrier CLD further improves the heat aging resistance of the rubber and gives the rubber good elasticity.
[0036] Example 4
[0037] The raw materials include, by mass: 60 parts of ethylene propylene rubber KEP570, 40 parts of ethylene propylene rubber KEP350, 65 parts of carbon black N550, 25 parts of carbon black N330, 40 parts of light calcium carbonate, 35 parts of environmentally friendly paraffin oil, 1 part of microcrystalline paraffin, 5 parts of zinc oxide, 1 part of stearic acid, 2 parts of operating aid, 0.5 parts of sulfur, 1.5 parts of environmentally friendly sulfur carrier CLD, and 2.5 parts of accelerators TT, CZ, and BZ.
[0038] Ethylene propylene rubber KEP570 uses medium-high ethylene EPDM as the main rubber, which makes the rubber have excellent heat aging resistance, low temperature resistance and ozone aging resistance, and no additional antioxidant is needed, so that the surface of the final product is bright and colorful. Carbon black mainly uses N550 to improve the physical and mechanical properties of the rubber. The environmentally friendly paraffin oil is TUDALEN 16. The use of environmentally friendly paraffin oil improves the process operation performance of the rubber and improves the processing technology of the later stage. The vulcanization system using sulfur and environmentally friendly sulfur carrier CLD further improves the heat aging resistance of the rubber and gives the rubber good elasticity.
[0039] A method for preparing a high-performance rubber material for road speed bumps, comprising the following steps:
[0040] S1, the first stage of mixing, ethylene propylene rubber, microcrystalline wax, zinc oxide, stearic acid, and operating aids are put into an internal mixer and mixed for about 60 seconds, and then carbon black, environmentally friendly paraffin oil, and calcium carbonate are added and mixed to about 150°C for sheeting;
[0041] S2, the second mixing stage, adding the accelerator and the remaining raw materials to the material mixed in the previous stage, mixing for the second time, mixing thoroughly, mixing again after cleaning, and obtaining a high-performance rubber material for road speed bumps after sufficient dispersion.
[0042] Table 1 shows the mass fractions of each component in Examples 1-4
[0043]
[0044] Table 2 shows the performance parameters of the rubber materials prepared in Examples 1-4
[0045]
[0046] From Table 2, we can see that the hardness of the rubber is above 65Shore A, the tensile strength is ≥10MPa, the elongation at break is ≥250%, and the basic physical and mechanical properties are excellent. At the same time, after hot air aging at 70℃×168h and water resistance test at 23℃×168h, the hardness is ≤85Shore A; the tensile strength is ≥9MPa and the elongation at break is ≥200%; the ozone resistance is 200pphm×40℃×96h×20%, no cracking, and the low temperature resistance is -40℃×3min without cracks; it has excellent high and low temperature resistance, strong heat aging resistance, strong ozone resistance, suitable for a variety of different environments, and suitable for use as a rubber compound for road speed bumps.
[0047] A preparation device for high-performance rubber materials specially used for road speed bumps, comprising an internal mixer 1 and a base plate 2 arranged at the bottom of the internal mixer 1 for installing the internal mixer 1, and an agitator 7. The base plate 2 is provided with a slide groove 3, in which a bracket 4 is slidably engaged, and the bracket 4 is connected to a stirring seat 6 at one end away from the slide groove 3. The stirring seat 6 is provided with an agitator 7 for stirring materials, and a sealing plate 8 for moving and blocking an opening at the bottom of the stirring seat 6 is provided below the stirring seat 6. A telescopic rod 5 for pushing the bracket 4 to move is provided in the slide groove 3, and a driving end of the telescopic rod 5 is connected to the bracket 4. The bracket 4 is an L-shaped bracket, and the length of the bracket 4 and the telescopic length of the telescopic rod 5 are both greater than the length of the sealing plate 8. The stirring seat 6 is a pipe pile structure, and the bottom of the stirring seat 6 and the top of the sealing plate 8 are both provided with anti-sticking and wear-resistant coatings. The sealing plate 8 is arranged on one side of the feed port of the internal mixer 1, and the top of the sealing plate 8 is in the same horizontal plane as the top of the feed port of the internal mixer 1.
[0048] The material is poured into the stirring seat 6, and the sealing plate 8 limits the falling of the material in the stirring seat 6. The stirrer 7 is started to stir and mix the material in the stirring seat 6. After the mixing is completed, the telescopic rod 5 is driven, and the telescopic rod 5 is extended to push the bracket 4 to slide in the slide groove 3. The bracket 4 moves and pushes the stirring seat 6 to move on the sealing plate 8. When the stirring seat 6 moves to the feeding port of the internal mixer 1, the bottom of the stirring seat 6 is gradually separated from the sealing plate 8, and the gap between the stirring seat 6 and the sealing plate 8 is gradually expanded. The material enters the internal mixer 1 through the bottom opening of the stirring seat 6 for processing, so that the material can be pre-mixed, thereby improving the mixing effect of the material.
[0049] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high-performance rubber material for road speed bumps, characterized in that: The components are as follows by mass: 100 parts of EPDM rubber, 75-90 parts of carbon black, 0-40 parts of light calcium carbonate, 30-45 parts of environmentally friendly paraffin oil, 0-2 parts of microcrystalline paraffin, 5-10 parts of zinc oxide, 1 part of stearic acid, 0-2 parts of operating aid, 0.5-1 parts of sulfur, 0.5-1.5 parts of environmentally friendly sulfur carrier CLD, and 1.9-2.5 parts of accelerators TT, CZ, and BZ.
2. The high-performance rubber material for road speed bumps according to claim 1, characterized in that: The raw materials include, by mass: 60 parts of ethylene propylene rubber KEP570, 40 parts of ethylene propylene rubber KEP350, 65 parts of carbon black N550, 25 parts of carbon black N330, 45 parts of environmentally friendly paraffin oil, 1 part of microcrystalline paraffin, 5 parts of zinc oxide, 1 part of stearic acid, 1 part of operating aid, 0.5 parts of sulfur, 1.5 parts of environmentally friendly sulfur carrier CLD, and 2 parts of accelerators TT, CZ, and BZ.
3. The high-performance rubber material for road speed bumps according to claim 1, characterized in that: The raw materials include, by mass: 60 parts of ethylene propylene rubber KEP570, 40 parts of ethylene propylene rubber KEP350, 75 parts of carbon black N550, 35 parts of environmentally friendly paraffin oil, 7 parts of zinc oxide, 1 part of stearic acid, 1 part of operating aid, 0.8 parts of sulfur, 1.2 parts of environmentally friendly sulfur carrier CLD, and 2 parts of accelerators TT, CZ, and BZ.
4. The high-performance rubber material for road speed bumps according to claim 1, characterized in that: The raw materials include, by mass: 100 parts of ethylene propylene rubber KEP350, 80 parts of carbon black N550, 30 parts of environmentally friendly paraffin oil, 2 parts of microcrystalline paraffin, 10 parts of zinc oxide, 1 part of stearic acid, 1 part of operating aid, 1 part of sulfur, 1 part of environmentally friendly sulfur carrier CLD, and 1.9 parts of accelerators TT, CZ, and BZ.
5. The high-performance rubber material for road speed bumps according to claim 1, characterized in that: The raw materials include, by mass: 60 parts of ethylene propylene rubber KEP570, 40 parts of ethylene propylene rubber KEP350, 65 parts of carbon black N550, 25 parts of carbon black N330, 40 parts of light calcium carbonate, 35 parts of environmentally friendly paraffin oil, 1 part of microcrystalline paraffin, 5 parts of zinc oxide, 1 part of stearic acid, 2 parts of operating aid, 0.5 parts of sulfur, 1.5 parts of environmentally friendly sulfur carrier CLD, and 2.5 parts of accelerators TT, CZ, and BZ.
6. A high-performance rubber material for road speed bumps according to claims 1-5, characterized in that: The environmentally friendly paraffin oil is TUDALEN 16.
7. A method for preparing a high-performance rubber material for road speed bumps according to any one of claims 1 to 5, characterized in that: The specific steps include: S1, the first stage of mixing, ethylene propylene rubber, microcrystalline wax, zinc oxide, stearic acid, and operating aids are put into an internal mixer and mixed for about 60 seconds, and then carbon black, environmentally friendly paraffin oil, and calcium carbonate are added and mixed to about 150°C for sheeting; S2, the second mixing stage, adding the accelerator and the remaining raw materials to the material mixed in the previous stage, mixing for the second time, mixing thoroughly, mixing again after cleaning, and obtaining a high-performance rubber material for road speed bumps after sufficient dispersion.
8. A preparation device for a high-performance rubber material for road speed bumps according to any one of claims 1 to 5, comprising an internal mixer (1), a bottom plate (2) provided at the bottom of the internal mixer (1) for mounting the internal mixer (1), and a stirrer (7), characterized in that: The bottom plate (2) is provided with a slide groove (3), a bracket (4) is slidably engaged in the slide groove (3), an end of the bracket (4) away from the slide groove (3) is connected to a stirring seat (6), a stirrer (7) for stirring materials is provided on the stirring seat (6), and a sealing plate (8) for moving and blocking the bottom opening of the stirring seat (6) is provided below the stirring seat (6).
9. The equipment for preparing the high-performance rubber material for road speed bumps according to claim 8, characterized in that: A telescopic rod (5) for pushing the bracket (4) to move is arranged in the slide groove (3); the bracket (4) is an L-shaped bracket; the length of the bracket (4) and the telescopic length of the telescopic rod (5) are both greater than the length of the sealing plate (8).
10. The equipment for preparing the high-performance rubber material for road speed bumps according to claim 8, characterized in that: The stirring seat (6) is a pipe pile structure, and the bottom of the stirring seat (6) and the top of the sealing plate (8) are both provided with anti-sticking and wear-resistant coatings. The sealing plate (8) is arranged on one side of the feed port of the internal mixer (1), and the top of the sealing plate (8) is on the same horizontal plane as the top of the feed port of the internal mixer (1).
Citation Information
Cited By
Light high-strength rubber covered roller and application