Leather surface treating agent and preparation method thereof

By introducing end-hydroxyl-terminated polyisobutene into the leather surface treatment agent, combined with organic silicon and other components, the interface compatibility problem in traditional leather surface treatment agents is solved, and the effects of self-matching, folding and wear resistance are achieved, and the leather is improved Comprehensive performance and service life.

CN118979127APending Publication Date: 2024-11-19MINGHAI CHEM ENTERPRISE
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411374187.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In traditional leather surface treatment agents, there is an interface compatibility problem with inorganic silica and organic polyurethane resin, resulting in uneven white markings on the surface of synthetic leather, affecting the aesthetics of the product. The water-based resin is difficult to meet the water resistance, solvent resistance of synthetic leather and Wear resistance requirements limit the development of water-bearing of synthetic leather surface treatment agents.

Method used

Using self-efficulated water-based polyurethane as the main component, the polyurethane main chain is introduced with end hydroxyl-terminated polyisobutene, combined with silicone wetting agent, defoaming agent, thickening agent and hand feel agent to form a micro-phase separation effect and improve flexibility and stability, and a leather surface treatment agent with excellent comprehensive performance is prepared by specific preparation methods.

Benefits of technology

It realizes the self-fading effect of the leather surface, significantly improves folding and wear resistance, has strong adhesion, and has a smoother and softer feel. It is suitable for low-temperature applications and extends the service life of leather products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of coating compositions, in particular to a leather surface treatment agent and a preparation method thereof. The surface treating agent comprises the following components in parts by weight: 40-60 parts of self-extinction waterborne polyurethane, 0.5-2 parts of a wetting agent, 0.5-1 part of a defoaming agent, 1-5 parts of a thickening agent, 1-5 parts of a hand feeling agent and 30-40 parts of water. The invention also provides a preparation method of the composition. Compared with the prior art, the surface treating agent provided by the invention is remarkable in effect, excellent in comprehensive performance, good in folding resistance, wear resistance and low-temperature performance, high in adhesiveness and good in permeability and leveling property, and leather subjected to surface treatment is smoother and softer in hand feeling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coating compositions, and in particular to a leather surface treatment agent and a preparation method thereof. Background Art

[0002] Leather surface treatment agents are chemicals used to improve the texture, softness and durability of leather. They are widely used in the production of leather products such as furniture, shoes, handbags and car seats. This treatment agent can penetrate into the leather fiber structure, change its physical and chemical properties, and improve the quality and performance of the leather. The main functions of leather surface treatment agents include increasing the softness and glossiness of leather, improving its resistance to water, pollution and wear, and preventing oxidation, fading and aging of the leather surface, thereby extending the service life of leather products.

[0003] CN103205898A provides a skin-feel polyurethane leather surface treatment agent, which is mixed with solvent-based PU, additive silicone, wax and solvent. The proportion of each component is calculated by weight: 30-40 parts of solvent-based PU, 4-9 parts of silicone, 3-6 parts of wax, and 45-60 parts of solvent; wherein the solvent-based PU is prepared from diisocyanate, polyol, chain extender, reactive silicone, antioxidant and catalyst in the presence of an organic solvent. The molar ratio of diisocyanate, polyol, chain extender and reactive silicone used to prepare solvent-based PU is: diisocyanate: polyol: chain extender: reactive silicone = (3.5-4.5): (2-3.5): 1: (0.1-0.2). When used on synthetic leather, it can significantly improve the touch of synthetic leather, making the synthetic leather have strong skin-feeling properties, while improving the scratch resistance and wear resistance of synthetic leather.

[0004] CN116751513A relates to a water-based surface treatment agent, a highly flexible skin-feeling PVC leather and a preparation method, wherein the surface treatment agent comprises a water-based polymer resin, a reactive POSS, a polysiloxane and a cross-linking agent. The invention innovatively adopts a reactive POSS in the water-based surface treatment agent, which can not only be evenly dispersed in the system, but also form a uniform and stable dispersion system together with polysiloxane and polymer resin. At the same time, the reactive POSS, polysiloxane, polymer resin and cross-linking agent are used in combination, and the viscoelastic coefficient of the coating formed by curing of the finally prepared water-based surface treatment agent is close to that of human skin, and can give a flexible and pleasant touch under the stress of touch pressure, and can also maintain the wear resistance and chemical resistance of the coating. When used on PVC leather, it effectively reduces the plastic feel of traditional PVC surface treatment, obtains a high degree of skin recognition from consumers, and also has excellent wear resistance and chemical resistance.

[0005] At present, the surface post-treatment of synthetic leather mostly adopts the three-printing process, which is an open production system. However, the surface treatment agent currently used mainly uses solvent-based polyurethane as a film-forming agent, which contains a large amount of harmful organic solvents. These organic solvents are not only harmful to the environment, but also because most of them are difficult to dissolve in water, the current spraying method for recycling is not ideal. Water-based leather surface treatment agents can fundamentally solve the pollution and harm problems caused by solvent-based surface treatment agents. However, the transition of synthetic leather surface treatment agents to water-based is relatively slow, mainly due to the lack of water-based resins suitable for synthetic leather surface treatment. The top treatment agent of the synthetic leather surface needs to have excellent water resistance, solvent resistance, wear resistance and scratch resistance, and general water-based resins are difficult to meet these requirements. Therefore, the development of water-based synthetic leather surface treatment agents has been restricted to a certain extent. Summary of the invention

[0006] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to provide a leather surface treatment agent and a preparation method thereof.

[0007] Matting treatment is a common surface effect technology and is widely used in synthetic leather manufacturing. It can bring a soft natural gloss and excellent touch to synthetic leather. However, the traditional matting technology uses inorganic silica particles mixed with polyurethane resin. Although it can provide excellent matting effect, it has some limitations. Since silica is an inorganic material, there are differences in properties with the organic polyurethane resin in synthetic leather, which leads to interfacial compatibility issues between the two. When synthetic leather is stretched, this matting agent composed of inorganic silica and organic polyurethane is prone to separation. This separation will cause uneven white streaks on the surface of synthetic leather, affecting the appearance and aesthetics of the product. Therefore, the present invention provides a self-matting waterborne polyurethane as the main component in the leather surface treatment agent, and introduces a terminal hydroxyl-terminated polyisobutylene in the polyurethane main chain, which can not only be used as a soft segment to adjust the flexibility of the polyurethane due to its excellent low-temperature flexibility, thermal stability, hydrolysis stability, chemical resistance, air tightness, hydrophobicity and watertightness, but also can affect its performance at low temperatures, flexibility, stability, etc. due to its own characteristics, and the non-polar long carbon chain in the terminal hydroxyl-terminated polyisobutylene structure can form an obvious microphase separation between the soft and hard segments, so that the coating surface obtained by the waterborne polyurethane is roughened to achieve self-matting. The surface treatment agent provided by the present invention has significant effect, excellent comprehensive performance, folding resistance and wear resistance, good low-temperature performance, strong adhesion, good permeability and leveling, and the leather feels smoother and softer after surface treatment.

[0008] To achieve the above object, the present invention provides a leather surface treatment agent, comprising the following components in parts by weight: 40-60 parts of self-matting water-based polyurethane, 0.5-2 parts of wetting agent, 0.5-1 parts of defoaming agent, 1-5 parts of thickener, 1-5 parts of hand feeling agent and 30-40 parts of water.

[0009] Furthermore, the wetting agent is a silicone wetting agent.

[0010] Furthermore, the defoaming agent is a silicone defoaming agent.

[0011] Furthermore, the thickener is carboxymethyl cellulose.

[0012] Furthermore, the feel agent is a silicone feel agent.

[0013] The method for preparing the self-matting waterborne polyurethane comprises the following steps: The terminal hydroxyl-terminated polyisobutylene and polytetrahydrofuran ether are mixed and dehydrated, and then methyl propanediol and isophorone diisocyanate are added at 80-90°C, and the temperature is lowered to 70-80°C, and a solution of 3-hydroxy-2-hydroxymethyl-2-methylpropionic acid in N-methylpyrrolidone is added, and bismuth neododecanoate is added after stirring for 1-2 hours, and isopropanol is added to dilute after continuing to stir for 3-4 hours, and a mixed aqueous solution of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt and ethylenediamine is added after cooling to 30-40°C, and triethylamine is added after cooling to 20-30°C to adjust the pH to neutral, and the mixture is emulsified and concentrated under reduced pressure to remove isopropanol to obtain the product.

[0014] Furthermore, the mass ratio of the terminal hydroxyl-terminated polyisobutylene to polytetramethyleneimine, methyl propanediol, isophorone diisocyanate, 3-hydroxy-2-hydroxymethyl-2-methylpropionic acid, bismuth neododecanoate, 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt, and ethylenediamine is 1-5:1:0.01-0.03:2-3:0.02-0.03:0.001-0.003:0.02-0.03:0.01-0.02.

[0015] Furthermore, the concentration of the N-methylpyrrolidone solution of 3-hydroxy-2-hydroxymethyl-2-methylpropionic acid is 20-30wt%.

[0016] Furthermore, the concentration of the aqueous solution of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt and ethylenediamine is 10-30wt%.

[0017] A method for preparing a leather surface treatment agent comprises the following steps: The self-matting water-based polyurethane is mixed with a wetting agent, a defoaming agent, a thickener, a feel agent and water, and then stirred evenly to obtain a leather surface treatment agent.

[0018] Beneficial effects of the present invention: The present invention provides a self-matting waterborne polyurethane as the main component of a leather surface treatment agent, and introduces a terminal hydroxyl-terminated polyisobutylene into the main chain of the polyurethane, which can not only be used as a soft segment to adjust the flexibility of the polyurethane, but also can affect its performance at low temperatures, flexibility, stability, etc. due to its own characteristics. The surface treatment agent provided by the present invention has significant effects, excellent comprehensive performance, good folding and wear resistance, good low-temperature performance, strong adhesion, good permeability and leveling properties, and the leather feels smoother and softer after surface treatment. DETAILED DESCRIPTION

[0019] Hydroxyl-terminated polyisobutylene, Mw=2000, product number: Q-0003289, Xi'an Qiyue Biological.

[0020] Polytetramethylenetetrahydrofuran ether, Mw=2000.

[0021] 3-hydroxy-2-(hydroxymethyl)-2-methylpropanoic acid, CAS No.: 123384-67-8.

[0022] Silicone wetting agent, HT-309, Guangzhou Huitu New Materials.

[0023] Silicone defoamer, E32, Guangzhou Lai Ke Bao New Materials.

[0024] Silicone feel agent, DC-51, Shenzhen Dayang New Materials. Example

[0025] A method for preparing a leather surface treatment agent comprises the following steps, measured in parts by weight: Mix 55 parts of self-matting waterborne polyurethane, 1 part of silicone wetting agent, 0.5 parts of silicone defoaming agent, 3 parts of carboxymethyl cellulose, 5 parts of silicone feel agent and 30 parts of water, and stir evenly to obtain a leather surface treatment agent.

[0026] The method for preparing the self-matting waterborne polyurethane comprises the following steps, measured in parts by weight: 40 parts of hydroxyl-terminated polyisobutylene and 10 parts of polytetrahydrofuran ether are mixed and dehydrated, and then 0.2 parts of methyl propanediol and 25 parts of isophorone diisocyanate are added at 85°C, and after cooling to 75°C, 1 part of 30wt% N-methylpyrrolidone solution of 3-hydroxy-2-hydroxymethyl-2-methylpropionic acid is added, and after stirring for 1 hour, 0.01 parts of bismuth neododecanoate are added, and after continuing to stir for 4 hours, an equal volume of isopropanol is added for dilution, and after cooling to 35°C, 1 part of 30wt% aqueous solution of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt and ethylenediamine (the mass ratio of the two is 2:1) is added, and after cooling to 25°C, triethylamine is added to adjust the pH to neutral, and the mixture is emulsified and concentrated under reduced pressure to remove isopropanol to obtain the product. Example

[0027] The method is basically the same as Example 1, except that the weight portion of the hydroxyl-terminated polyisobutylene is 10 parts. Example

[0028] The method is basically the same as Example 1, except that the weight portion of the hydroxyl-terminated polyisobutylene is 20 parts. Example

[0029] The method is basically the same as Example 1, except that the weight portion of the hydroxyl-terminated polyisobutylene is 30 parts. Example

[0030] The method is basically the same as Example 1, except that the weight portion of the hydroxyl-terminated polyisobutylene is 50 parts.

[0031] A method for preparing a leather surface treatment agent comprises the following steps, measured in parts by weight: Mix 55 parts of waterborne polyurethane, 1 part of silicone wetting agent, 10 parts of silicon dioxide, 0.5 parts of silicone defoaming agent, 3 parts of carboxymethyl cellulose, 5 parts of silicone feel agent and 20 parts of water, and stir evenly to obtain a leather surface treatment agent.

[0032] The preparation method of the waterborne polyurethane comprises the following steps, measured in parts by weight: Dehydrate 50 parts of polytetrahydrofuran ether, then add 0.2 parts of methyl propanediol and 25 parts of isophorone diisocyanate at 85°C, cool to 75°C, add 1 part of 30wt% N-methylpyrrolidone solution of 3-hydroxy-2-hydroxymethyl-2-methylpropionic acid, stir for 1 hour, add 0.01 parts of bismuth neododecanoate, continue stirring for 4 hours, add an equal volume of isopropanol for dilution, cool to 35°C, add 1 part of 30wt% aqueous solution of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt and ethylenediamine (mass ratio 2:1), cool to 25°C, add triethylamine to adjust the pH to neutral, emulsify the mixture, and concentrate under reduced pressure to remove isopropanol to obtain the product.

[0033] According to the standard QB / T 3514-2005 "Determination of folding fastness of leather in physical and mechanical experiments", the following test steps are carried out: Use a surface treatment coating roller to evenly apply the leather surface treatment agent on the surface of the leather sample, dry it at 120℃ and then take it out. Select 3 surface-treated specimens in each group, and ensure that the surface of the specimen faces inward. Use a light leather folding instrument to perform folding tests on the specimens for different times. After the test, use the naked eye and a magnifying glass to carefully check the folding of the coating under sufficient light conditions. The key points for evaluating the test results include: Check whether the surface coating remains intact and is not damaged. Observe whether the color of the coating changes during the test. Count the number of cracks in the coating. Evaluate whether there are abnormal changes in the adhesion of the coating. Check whether there are abnormalities in the adhesion between the coatings. Observe whether there are powder or flaky substances on the surface of the coating. Check whether there are cracks, powder or flaky substances on the coating. In order to ensure the accuracy of the test results, three groups of parallel tests are carried out, and the lowest level in the sample is used as the final test result.

[0034] Table 1 Folding resistance test of leather after surface treatment

[0035] By comparing the comparative example 1 with the embodiment, it can be found that the folding resistance of the leather treated with the surface treatment agent of adding silica as the matting agent is significantly worse. This may be because silica is added to the solution as a matting agent, which is different from the polyurethane resin in properties, which leads to the interface compatibility problem between the two. When the synthetic leather is bent, the matting agent composed of inorganic silica and organic polyurethane is prone to separation, which is more likely to cause creases. The self-matting polyurethane is more uniform after film formation on the leather surface, and its matting effect comes from the microphase separation formed by the incompatible components in the main chain, so it will not affect the strength of the film. From the comparison of Examples 1 to 5, it can be seen that Example 1 has the best folding resistance. This may be because although the non-polar long carbon chain in the polyisobutylene structure terminated with terminal hydroxyl groups can form obvious microphase separation between the soft and hard segments, when its content increases, the effect of microphase separation will be intensified, thereby weakening the interaction between the soft and hard segments and improving flexibility. However, when the content is too much, the continuous increase in microphase separation will lead to a decrease in the interaction between the soft and hard segments, presenting a discontinuous state, thereby affecting flexibility.

[0036] According to the standard QB / T 2726-2005 "Determination of wear resistance of leather in physical and mechanical experiments", the test process is as follows: First, use a surface treatment coating roller to evenly apply the leather surface treatment agent on the surface of the leather sample, dry it at 120℃ and take it out. Select 3 surface treated specimens cut according to the standard for each group and fix them on the specimen platform. In the experiment, the rotation speed is set to 60 revolutions per minute, and an error of 5 revolutions is allowed. A load of 250 grams is applied to the specimen, and a wear test is performed using a standard H22 grinding wheel. After setting the number of rotations, start the instrument for testing. After the test is completed, remove the specimen, measure and record its damage, and exclude damage within 2 mm of the edge of the test area and extrusion damage caused by starting or stopping the machine. If necessary, use a gray sample card to measure the color change within the test area. When the leather surface substrate is exposed, record the corresponding number of turns as a basis for judgment. Finally, conduct multiple groups of parallel tests, and take the lowest number of turns of the specimen as the final test result.

[0037] Table 2 Abrasion resistance test of leather after surface treatment

[0038] By comparing the control example 1 with the embodiment, it can be found that the surface treatment agent of the self-matting waterborne polyurethane has a better effect on the wear resistance of the leather. This is because the addition of silicon dioxide will reduce the strength of the polyurethane coating, and silicon dioxide as an inorganic particle itself has poor compatibility with the resin, so it is easier to precipitate after friction, which further reduces the wear resistance of the coating. The self-matting polyurethane in the embodiment has improved mechanical properties due to the addition of polyisobutylene terminated with terminal hydroxyl groups, and the coating is not easily worn.

[0039] With reference to GB / T 528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber, the surface treatment agent is prepared into specimens of corresponding size and then its tensile properties at room temperature and low temperature are tested. The test temperature is 25°C and -50°C, and the minimum tensile rate is 100mm / min.

[0040] Table 3 Mechanical properties of leather surface treatment agent after film formation

[0041] From the comparison between the control example 1 and the embodiment, it can be seen that the polyisobutylene terminated with terminal hydroxyl groups is introduced into the main chain of the polyurethane, and the mechanical properties of the polyurethane film formed at low temperature are better. This is because the polyisobutylene terminated with terminal hydroxyl groups has excellent low temperature flexibility, thermal stability, hydrolysis stability, chemical resistance, air tightness, hydrophobicity and impermeability. Therefore, it can not only be used as a soft segment to adjust the flexibility of the polyurethane, but also can affect its performance at low temperature, flexibility, stability, etc. due to its own characteristics. The polyisobutylene terminated with terminal hydroxyl groups is mainly composed of long non-polar carbon chains. Its addition not only weakens the hydrogen bonding effect between the soft and hard segments, but also increases the content of the soft segment, thereby improving the flexibility of the polyurethane main chain. When its content increases, the effect of microphase separation will be aggravated, thereby weakening the interaction between the soft and hard segments and improving flexibility. However, when the content is too much, the continuous increase in microphase separation will lead to a decrease in the interaction between the soft and hard segments, presenting a discontinuous state, so that the elongation at break first increases and then decreases. The introduction of hydroxyl-terminated polyisobutylene makes the polyurethane film have good flexibility even at low temperatures. Therefore, applying it to leather surface treatment can improve the performance of leather at low temperatures and make its application range wider.

[0042] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A leather surface treatment agent, characterized in that: The invention comprises the following components in parts by weight: 40-60 parts of self-matting waterborne polyurethane, 0.5-2 parts of wetting agent, 0.5-1 parts of defoaming agent, 1-5 parts of thickener, 1-5 parts of hand feeling agent and 30-40 parts of water; The preparation method of the self-matting waterborne polyurethane comprises the following steps: The terminal hydroxyl-terminated polyisobutylene and polytetrahydrofuran ether are mixed and dehydrated, and then methyl propanediol and isophorone diisocyanate are added at 80-90°C, and the temperature is lowered to 70-80°C, and a solution of 3-hydroxy-2-hydroxymethyl-2-methylpropionic acid in N-methylpyrrolidone is added, and bismuth neododecanoate is added after stirring for 1-2 hours, and isopropanol is added to dilute after continuing to stir for 3-4 hours, and a mixed aqueous solution of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt and ethylenediamine is added after cooling to 30-40°C, and triethylamine is added after cooling to 20-30°C to adjust the pH to neutral, and the mixture is emulsified and concentrated under reduced pressure to remove isopropanol to obtain the product.

2. The leather surface treatment agent according to claim 1, characterized in that The wetting agent is an organic silicon wetting agent.

3. The leather surface treatment agent according to claim 1, characterized in that The defoamer is an organosilicon defoamer.

4. The leather surface treatment agent according to claim 1, characterized in that The thickener is carboxymethyl cellulose.

5. The leather surface treatment agent according to claim 1, characterized in that The feel agent is an organic silicone feel agent.

6. The leather surface treatment agent according to claim 1, characterized in that The mass ratio of the terminal hydroxyl-terminated polyisobutylene to polytetramethyleneimine, methyl propanediol, isophorone diisocyanate, 3-hydroxy-2-hydroxymethyl-2-methylpropionic acid, bismuth neododecanoate, 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt, and ethylenediamine is 1-5:1:0.01-0.03:2-3:0.02-0.03:0.001-0.003:0.02-0.03:0.01-0.

02.

7. The leather surface treatment agent according to claim 1, characterized in that The concentration of the N-methylpyrrolidone solution of 3-hydroxy-2-hydroxymethyl-2-methylpropionic acid is 20-30 wt %.

8. The leather surface treating agent according to claim 1, characterized in that The concentration of the aqueous solution mixed with 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt and ethylenediamine is 10-30 wt %.

9. A method for preparing a leather surface treatment agent according to any one of claims 1 to 8, characterized in that: The steps include: The self-matting water-based polyurethane is mixed with a wetting agent, a defoaming agent, a thickener, a feel agent and water, and then stirred evenly to obtain a leather surface treatment agent.

Citation Information

Patent Citations

  • Synthetic leather surface conditioning agent

    CN105064034A

  • Waterborne polyurethane surface treating agent for synthetic leather and preparation method thereof

    CN106634524A

  • Method for preparing hydroxyl-terminated liquid rubber modified waterborne polyurethane matting resin

    CN107141442A

  • Water-based matting finishing agent used for surface treatment of artificial leather and containing no inorganic matting powder, and preparation method thereof

    CN108300058A

  • Scrubbing-resistant polyurethane water-based surface treating agent

    CN108978238A